Ceramic wiring board, ceramic green sheet for ceramic wiring board, and glass ceramic powder for ceramic wiring board
A ceramic wiring board with glass, willemite, and alumina fillers addresses the challenge of thermal expansion mismatch and mechanical strength, achieving low thermal expansion and high strength for semiconductor wafer inspection.
Patent Information
- Application Number
- JP2021537276
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-06
- Filing Date
- 2020-07-30
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-07-30
AI Technical Summary
Existing ceramic wiring boards face challenges in achieving a low thermal expansion coefficient and high mechanical strength, particularly when used as interposer substrates for semiconductor wafers, due to difficulties in material composition and thermal expansion mismatch with test heads and semiconductor wafers.
A ceramic wiring board composition comprising glass, willemite filler, and alumina filler, with willemite having a larger average particle size than alumina, is used to achieve a low thermal expansion coefficient and high mechanical strength, utilizing a specific glass composition and filler ratios to optimize thermal expansion and strength properties.
The ceramic wiring board achieves a thermal expansion coefficient of 4 ppm/°C or less and a three-point bending strength of 100 MPa or more, ensuring accurate semiconductor wafer inspection across a wide temperature range.
Smart Images

Figure 0007569018000002 
Figure 0007569018000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic wiring board, a ceramic green sheet for a ceramic wiring board, and a glass ceramic powder for a ceramic wiring board. [Background technology]
[0002] Conventionally, when testing a semiconductor wafer, a probe card is placed on the semiconductor wafer and the semiconductor wafer is electrically connected to a tester via the probe card. A probe card usually has a test head that contacts the semiconductor wafer, a printed ceramic wiring board that is connected to the tester, and a ceramic wiring board called an interposer board that connects the printed ceramic wiring board and the test head.
[0003] For example, Patent Document 1 describes a ceramic wiring board that can be fired at a low temperature, which is made of low-temperature fired ceramics containing glass. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-074823 A Summary of the Invention [Problem to be solved by the invention]
[0005] The distance between the electrode pads on the printed ceramic wiring board is greater than the distance between the electrode pads on the test head. One main surface of the interposer board is provided with electrode pads corresponding to the electrode pads on the printed ceramic wiring board, and the other main surface is provided with electrode pads corresponding to the electrode pads on the test head. The electrode pads on one main surface and the electrode pads on the other main surface are connected by internal conductors. Therefore, it is important that the positional accuracy of the electrode pads on both main surfaces of the interposer board is high.
[0006] Furthermore, inspections using a probe card are performed over a wide temperature range, for example, from -40°C to +125°C. For this reason, it is preferable to approximate the thermal expansion coefficient of the interposer substrate to that of the test head or the printed ceramic wiring board so that there is no difference between the distance between the electrode pads of the interposer substrate and the distance between the electrode pads of the test head or the printed ceramic wiring board when the inspection temperature changes. Therefore, it is preferable that the interposer substrate is made of a material whose thermal expansion coefficient can be adjusted to suit the usage environment.
[0007] Furthermore, since the thermal expansion coefficient of the test head is usually close to that of the semiconductor wafer, there is a demand to reduce the thermal expansion coefficient of the interposer substrate to approximately the same as that of the semiconductor wafer.
[0008] However, the ceramic wiring board described in Patent Document 1 has a problem in that it is difficult to achieve a thermal expansion coefficient as low as that of a semiconductor wafer.
[0009] Furthermore, there is a demand to ensure the mechanical strength of the interposer substrate.
[0010] A primary object of the present invention is to provide a ceramic wiring board which can be fired at a low temperature, has a thermal expansion coefficient which can be adjusted to be low, and has high mechanical strength. [Means for solving the problem]
[0011] The ceramic wiring board of the present invention comprises a ceramic substrate and an internal conductor disposed within the ceramic substrate, the ceramic substrate containing glass, willemite filler and alumina filler, and the average particle size of the willemite filler is larger than the average particle size of the alumina filler. Here, "willemite" refers to a silicon-zinc composite oxide, generally known as ZnSiO 4 The "average particle size" is defined as D50, which is calculated based on the volume of the particles when the particle size of any powder is measured by a laser diffraction scattering method.
[0012] In the ceramic wiring board of the present invention, the ceramic board preferably contains, by mass %, 30 to 65% glass, 14 to 56% willemite filler, and 7 to 42% alumina filler.
[0013] In the ceramic wiring board of the present invention, the glass is preferably borosilicate glass.
[0014] In the ceramic wiring board of the present invention, the borosilicate glass has a glass composition consisting of, by mass%, SiO 2 60~80%, B 2 O 3 10-30%, Li 2 O+Na 2 O+K 2 It is preferable that the content of "LiO" is 1 to 5% and that of "MgO+CaO+SrO+BaO" is 0 to 20%. 2 O+Na 2 O+K 2 "O" stands for Li 2 O, Na 2 O and K 2 "MgO+CaO+SrO+BaO" means the total amount of MgO, CaO, SrO and BaO.
[0015] The ceramic green sheet for a ceramic wiring board of the present invention contains, by mass%, 30 to 65% glass powder, 14 to 56% willemite filler, and 7 to 42% alumina filler, and is characterized in that the average particle diameter of the willemite filler is larger than the average particle diameter of the alumina filler.
[0016] The glass ceramic powder for ceramic wiring board of the present invention contains, by mass%, 30 to 65% glass powder, 14 to 56% willemite filler, and 7 to 42% alumina filler, and is characterized in that the average particle diameter of the willemite filler is larger than the average particle diameter of the alumina filler. Effect of the Invention
[0017] According to the present invention, it is possible to provide a ceramic wiring board which can be fired at a low temperature, has a low thermal expansion coefficient, and has high mechanical strength. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view of a ceramic wiring board according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an example of a preferred embodiment of the present invention will be described. However, the following embodiment is merely an example, and the present invention is not limited to the following embodiment.
[0020] Fig. 1 is a schematic cross-sectional view of a ceramic wiring board according to this embodiment. The ceramic wiring board 1 shown in Fig. 1 can be used as a ceramic wiring board that is required to have a low thermal expansion coefficient and high mechanical strength. The ceramic wiring board 1 can be used, for example, as an interposer substrate for a probe card.
[0021] The ceramic wiring board 1 has a ceramic substrate 10. The ceramic substrate 10 has first and second main surfaces 10a, 10b. The ceramic substrate 10 is composed of a laminate of a plurality of ceramic layers 11.
[0022] A plurality of internal conductors 20 are disposed inside the ceramic substrate 10. Each internal conductor 20 has an interlayer electrode 21 located between adjacent ceramic layers 11, and a via-hole electrode 22 that penetrates the ceramic layer 11 and connects the interlayer electrodes 21 that face each other in the stacking direction of the ceramic layers 11 via the ceramic layer 11.
[0023] The multiple internal conductors 20 are provided across the first main surface 10a and the second main surface 10b of the ceramic substrate 10. Ends of the internal conductors 20 on the first main surface 10a side are connected to electrode pads 31 provided on the first main surface 10a. Ends of the internal conductors 20 on the second main surface 10b side are connected to electrode pads 32 provided on the second main surface 10b.
[0024] The distance between adjacent electrode pads 32 on the second main surface 10b is longer than the distance between adjacent electrode pads 31 on the first main surface 10a. Therefore, when the ceramic wiring board 1 is used as an interposer board, a test head is connected to the first main surface 10a side, and a printed ceramic wiring board is connected to the second main surface 10b side.
[0025] The internal conductor 20 and the electrode pads 31, 32 may be made of an appropriate conductive material. The internal conductor 20 and the electrode pads 31, 32 may each be made of at least one metal such as Pt, Au, Ag, Cu, Ni, or Pd.
[0026] The ceramic substrate 10 preferably contains glass, willemite filler, and alumina filler. Specifically, by mass%, it contains 30 to 65% glass, 14 to 56% willemite filler, and 7 to 42% alumina filler. In the following description of the contents, "%" means "mass%" unless otherwise specified.
[0027] Glass increases the denseness (relative density) and mechanical strength of the ceramic substrate 10. The glass content is preferably 30 to 65%, particularly 30 to 50%. If the glass content is too low or too high, it becomes difficult to obtain the desired thermal expansion coefficient and mechanical strength.
[0028] The willemite filler reduces the thermal expansion coefficient of the ceramic substrate 10. The content of the willemite filler is preferably 14 to 56%, and particularly preferably 20 to 40%. If the content of the willemite filler is too small or too large, it becomes difficult to obtain the desired thermal expansion coefficient and mechanical strength.
[0029] The alumina filler increases the mechanical strength of the ceramic substrate 10. The content of the alumina filler is preferably 7 to 42%, and particularly preferably 20 to 40%. If the content of the alumina filler is too small or too large, it becomes difficult to obtain the desired thermal expansion coefficient and mechanical strength.
[0030] The average particle size of the willemite filler is larger than that of the alumina filler, and is preferably at least 1.2 times that of the alumina filler. If the average particle size of the willemite filler is smaller than that of the alumina filler, the willemite filler and the alumina filler react with each other during firing, and gahnite is likely to precipitate. As a result, it becomes difficult to control the thermal expansion coefficient of the ceramic substrate 10 within a desired range.
[0031] The average particle size of the willemite filler is preferably 2 to 5 μm, particularly 2 to 3 μm. If the average particle size of the willemite filler is too small, the number of microcracks at the crystal grain boundaries caused by the anisotropic expansion of the crystal grains decreases, and the thermal expansion coefficient of the willemite filler tends to increase. As a result, it becomes difficult to control the thermal expansion coefficient of the ceramic substrate 10 within a desired range. On the other hand, if the average particle size of the willemite filler is too large, the mechanical strength of the ceramic substrate 10 is likely to decrease.
[0032] The thermal expansion coefficient of the ceramic substrate 10 is preferably 4 ppm / °C or less, particularly 3.6 ppm / °C or less, in the temperature range of -40°C to +125°C. If the thermal expansion coefficient of the ceramic substrate is too high, it will be higher than the thermal expansion coefficient of the semiconductor wafer, making it difficult to accurately inspect the semiconductor wafer. There is no particular lower limit to the thermal expansion coefficient, but in reality it is preferably 3 ppm / °C or more.
[0033] In this specification, the thermal expansion coefficient of the ceramic substrate in the temperature range of −40° C. to +125° C. is measured by a method in accordance with JIS R3102.
[0034] The three-point bending strength of the ceramic substrate 10 is preferably 100 MPa or more, and particularly preferably 150 MPa or more. If the three-point bending strength is too low, the ceramic substrate 10 becomes easily damaged. There is no particular upper limit to the three-point bending strength, but in reality, it is preferably 600 MPa or less. The three-point bending strength of the ceramic substrate in this specification is measured by a method in accordance with JIS R1601.
[0035] The thermal expansion coefficient of the ceramic filler in the temperature range of -40°C to +125°C is measured in accordance with JIS R3102 using a sheet-like sintered body prepared by the following method. The three-point bending strength of the ceramic filler in the present specification is measured in accordance with JIS R1601 using a sheet-like sintered body prepared by the following method.
[0036] The sheet-shaped sintered body used for measuring the thermal expansion coefficient and three-point bending strength of the ceramic filler is prepared by the following method. First, 100 parts by mass of ceramic filler (such as willemite filler or alumina filler) with an average particle size of 2 μm is mixed and kneaded with 15 parts by mass of polyvinyl butyral (PVB), 3 parts by mass of benzyl butyl phthalate, and 50 parts by mass of toluene to prepare a slurry. Next, the slurry is formed into a circular sheet shape with a diameter of 20.32 cm (8 inches) and a thickness of 150 μm by a doctor blade method to prepare a green sheet. Next, 30 green sheets are stacked and thermocompressed at 90°C and 30 MPa, and then heat-treated at 450°C for degreasing, and sintered at 1600°C to prepare a sintered body. Finally, the sintered body is polished to a thickness of 3.0 mm to obtain a sheet-shaped sintered body.
[0037] The ceramic substrate 10 may contain three or more types of ceramic fillers, that is, ceramic fillers other than the willemite filler and the alumina filler.
[0038] In this case, it is preferable that the willemite filler has the lowest thermal expansion coefficient among the three or more types of ceramic fillers in the temperature range of -40°C to +125°C, and the alumina filler has the highest three-point bending strength among the three or more types of ceramic fillers.
[0039] The glass in the ceramic substrate 10 is preferably borosilicate glass. By using borosilicate glass, it is easy to reduce the thermal expansion coefficient of the ceramic substrate 10. In addition, it is possible to increase the mechanical strength of the ceramic substrate 10.
[0040] Specifically, borosilicate glass has a glass composition of, by mass%, SiO 2 60~80%, B 2 O 3 10-30%, Li 2 O+Na 2 O+K 2It is preferable that the composition contains 1 to 5% of O and 0 to 20% of MgO+CaO+SrO+BaO. In the following description of the contents, "%" means "mass %" unless otherwise specified.
[0041] SiO 2 is a component that forms the skeleton of glass. SiO 2 The content is preferably 60 to 80%. 2 When the content of SiO is low, vitrification may be difficult. 2 If the content of SiO is large, the melting temperature becomes high and melting may become difficult. 2 The content is more preferably in the range of 65 to 75%.
[0042] B 2 O 3 B is a component that forms the glass framework, expands the vitrification range, and stabilizes the glass. 2 O 3 The content of is preferably 10 to 30%. 2 O 3 When the content of B is low, the melting temperature becomes high and melting tends to become difficult. 2 O 3 When the content of B increases, the thermal expansion coefficient of the ceramic substrate 10 tends to increase. 2 O 3 The content is more preferably in the range of 15 to 25%.
[0043] Alkali metal oxide (Li 2 O, Na 2 OK 2 O) is a component that reduces the viscosity of the molten glass and makes it easier to melt. The content (total amount) of alkali metal oxides is preferably 1 to 5%. If the content of alkali metal oxides is low, the effect of reducing viscosity may be reduced. On the other hand, if the content of alkali metal oxides is high, water resistance tends to decrease. The content of alkali metal oxides is more preferably in the range of 2 to 4%.
[0044] Alkaline earth metal oxides (MgO, CaO, SrO, BaO) are components that reduce the viscosity of molten glass and make it easier to melt. The content (total) of alkaline earth metal oxides is preferably 0 to 20%. If the content of alkaline earth metal oxides is too high, the glass tends to become unstable and to be easily devitrified when melted. The content of alkaline earth metal oxides is more preferably in the range of 5 to 15%.
[0045] Next, a method for manufacturing the ceramic wiring board 1 will be described.
[0046] First, a glass-ceramic powder for ceramic wiring boards is prepared, which contains, by mass%, 30 to 65% glass, 14 to 56% willemite filler, and 7 to 42% alumina filler. As described above, the average particle size of the willemite filler is larger than the average particle size of the alumina filler.
[0047] The glass is preferably a borosilicate glass having the above composition, and the average particle size of the glass powder is preferably 1 to 5 μm.
[0048] Next, a binder containing a resin, a plasticizer, a solvent, etc. is added to the glass ceramic powder for ceramic wiring boards and kneaded to prepare a slurry. The slurry is formed into a sheet by a doctor blade method or the like to prepare a ceramic green sheet for ceramic wiring boards containing glass, Willemite filler, and alumina filler.
[0049] Next, via holes are formed in the ceramic green sheets by, for example, irradiation with laser light, mechanical punching, or the like.
[0050] Next, the formed via holes are filled with a conductive paste for forming the via-hole electrodes 22. Also, a conductive paste for forming the interlayer electrodes 21 and the electrode pads 31, 32 is applied onto the ceramic green sheets.
[0051] Thereafter, the ceramic green sheets are appropriately laminated to obtain a laminate, which is then fired to complete the ceramic wiring board 1. EXAMPLES
[0052] The present invention will be described in more detail below based on specific examples, but the present invention is not limited to the following examples in any way.
[0053] Table 1 shows examples of the present invention (samples No. 1 to 6) and a comparative example (sample No. 7).
[0054] [Table 1]
[0055] SiO 2 70%, B 2 O 3 28%, K 2 Glass raw materials were mixed so that the O content was 2%, and the glass raw materials were placed in a platinum crucible and melted at 1600°C to obtain molten glass. The molten glass was supplied between two water-cooled rotating rolls and stretched to obtain a film-like glass.
[0056] The glass thus obtained was pulverized and classified to obtain a glass powder having the average particle size shown in Table 1.
[0057] 100 parts by mass of the prepared mixed powder was mixed with 12 parts by mass of acrylic resin, 3 parts by mass of plasticizer (benzyl butyl phthalate), and 35 parts by mass of solvent (toluene) so that the contents of glass powder, willemite powder, and alumina powder were as shown in Table 1, and then kneaded. A green sheet with a thickness of 150 μm was obtained by a doctor blade method. The average particle diameters of the willemite powder and alumina powder are as shown in Table 1.
[0058] The green sheet was punched to obtain a circular green sheet compact with a diameter of 20.32 cm (8 inches). Next, through holes with a diameter of 100 μm and intervals of 500 μm were formed in this green sheet compact using a laser punching machine, and via conductors were embedded by printing. In addition, interlayer electrodes and electrode pads were formed by printing a conductive paste. Thereafter, the green sheet compacts were stacked, and an alumina green sheet made of an alumina filler was further stacked as a restraining member to produce a laminate.
[0059] Next, the laminate was thermocompressed at 90° C. and 30 MPa. The laminate was then heat-treated at 450° C. to degrease it, and then sintered at 850° C. to obtain a sintered body. The obtained sintered body was polished to remove the restraining members, and a ceramic wiring board with a thickness of 3.0 mm was produced.
[0060] The thermal expansion coefficient and three-point bending strength of the produced ceramic wiring board were evaluated.
[0061] The thermal expansion coefficient in the temperature range of −40 to +125° C. was measured by a method conforming to JIS R3102.
[0062] The three-point bending strength was measured according to the method compliant with JIS R1601.
[0063] As is clear from Table 1, samples No. 1 to No. 6, which are examples of the present invention, have a thermal expansion coefficient of 3.6 to 4.0 ppm / °C in the temperature range of -40 to +125°C, which is almost the same as the thermal expansion coefficient of a semiconductor wafer. Also, the three-point bending strength was 232 to 273 MPa, which was sufficient strength. On the other hand, sample No. 7, which is a comparative example, had a thermal expansion coefficient of 4.3 ppm / °C, which was larger than the thermal expansion coefficient of a semiconductor wafer.
[0064] Next, when the samples No. 1 to 6 of the embodiment were used as a probe card and a semiconductor wafer was inspected with this probe card in a temperature range of -40 to +125° C., the semiconductor wafer could be inspected without any problems. On the other hand, when the sample No. 7 of the comparative example was used as a probe card and a semiconductor wafer was inspected with this probe card in a temperature range of -40 to +125° C., the semiconductor wafer could not be inspected accurately due to the expansion of the ceramic wiring board. [Explanation of symbols]
[0065] 1: Ceramic wiring board 10: Ceramic substrate 10a: First main surface 10b: second main surface 11: Ceramic layer 20: Inner conductor 21: Interlayer electrode 22: Via hole electrode 31, 32: Electrode pads
Claims
1. A ceramic substrate and an internal conductor disposed within the ceramic substrate, the ceramic substrate contains glass, a willemite filler and an alumina filler; A ceramic wiring board, characterized in that the average particle size of the willemite filler is larger than the average particle size of the alumina filler.
2. 2. The ceramic wiring board according to claim 1, characterized in that the ceramic board contains, by mass %, 30 to 65% of glass, 14 to 56% of willemite filler, and 7 to 42% of alumina filler.
3. 3. The ceramic wiring board according to claim 1, wherein the glass is borosilicate glass.
4. The borosilicate glass has a glass composition, in mass%, of SiO 2 60-80%, B 2 O 3 10-30%, Li 2 O+Na 2 O+K 2 4. The ceramic wiring board according to claim 3, further comprising 1 to 5% O and 0 to 20% MgO+CaO+SrO+BaO.
5. The composition contains, by mass%, 30 to 65% glass powder, 14 to 56% willemite filler, and 7 to 42% alumina filler. A ceramic green sheet for a ceramic wiring substrate, characterized in that the average particle size of the willemite filler is larger than the average particle size of the alumina filler.
6. The composition contains, by mass%, 30 to 65% glass powder, 14 to 56% willemite filler, and 7 to 42% alumina filler. A glass ceramic powder for ceramic wiring substrates, characterized in that the average particle size of the willemite filler is larger than the average particle size of the alumina filler.
Citation Information
Patent Citations
Glass-ceramic substrate fired at low temperature
JP1994116019A
Dielectric ceramic material
JP2000182881A
Measuring wiring substrate, probe card, and evaluation device
JP2006284541A
Polyethylene molding powder and porous articles made therefrom
JP2008501850A
Wiring board for electronic component inspection device, and its manufacturing method
JP2009074823A