Curable composition for hard coat
A curable composition with specific chemical components forms a hard coat layer that balances scratch resistance, abrasion resistance, and slipperiness, addressing the trade-off in existing technologies and enhancing durability and liquid repellency.
Patent Information
- Application Number
- JP2022542584
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-26
- Filing Date
- 2021-06-09
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-06-09
AI Technical Summary
Existing hard coat layers for touch panels face a trade-off between durability properties such as scratch resistance and abrasion resistance, and slipperiness, making it difficult to achieve both at a high level, while also maintaining high liquid repellency.
A curable composition comprising an active energy ray-curable polyfunctional monomer, a perfluoropolyether with a poly(oxyperfluoroalkylene) group at the molecular chain end, and a polymerization initiator, which forms a hard coat layer with excellent scratch resistance, abrasion resistance, and slipperiness, using specific chemical structures and formulations to balance these properties.
The composition achieves a hard coat layer with both high scratch resistance and abrasion resistance, along with excellent slipperiness and liquid repellency, even in thin films, providing enhanced durability and performance.
Smart Images

Figure 0007569021000001 
Figure 0007569021000002 
Figure 0007569021000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition useful as a material for forming a hard coat layer applied to the surface of various display elements, and relates to a homogeneous curable composition capable of forming a hard coat layer having excellent slip properties, scratch resistance, abrasion resistance and water repellency, and free of suspended matter and sediment. [Background technology]
[0002] In recent years, touch panels have been introduced in various fields such as mobile phones, tablet computers, and other portable information terminal devices, notebook computers, home appliances, and automobile interior and exterior products, and the surface of a touch panel of a display element such as a liquid crystal display or an organic electroluminescence display is often touched with a finger or a pen to operate it. When it is assumed that the touch panel is operated with a finger, the surface of the touch panel is required to have water and oil repellency to facilitate the removal of attached fingerprints, and is also required to have abrasion resistance to maintain the water and oil repellency even when repeatedly rubbed with a finger. In addition, when the surface of the touch panel is operated with a finger or a pen, slipperiness is required from the viewpoint of the touch feeling of the finger or pen. In addition, scratch resistance is required to prevent the surface of the touch panel from being scratched. In order to impart these properties to the surface of the touch panel, a surface coating layer, for example a hard coating layer, is provided.
[0003] Fluorine-containing compounds are used as materials for forming hard coat layers because they exhibit high slipperiness and water and oil repellency, and for example, a method is used in which a small amount of a fluorine-based surface modifier is added to a coating liquid for forming a hard coat layer. It is known that the fluorine-based surface modifier segregates on the surface of the hard coat layer due to the low surface energy of fluorine atoms.
[0004] In general, in order to impart scratch resistance and abrasion resistance to a hard coat layer, a method is adopted in which a high-density crosslinked structure is formed to increase the surface hardness of the hard coat layer and provide resistance to external forces. Currently, as a material for forming such a hard coat layer, a multifunctional acrylate-based material that undergoes three-dimensional crosslinking by radicals generated by irradiation with active energy rays is most commonly used. As a fluorine-based surface modifier added to a coating liquid for forming a hard coat layer, a material having an active energy ray polymerizable group is generally used to impart scratch resistance and abrasion resistance to the hard coat layer (Patent Document 1).
[0005] On the other hand, as described in Patent Document 2, when a fluorine-based surface modifier having a crosslinkable group is used to obtain durability such as scratch resistance and abrasion resistance in a hard coat layer, the molecular chain containing fluorine atoms is fixed, and the slipperiness of the hard coat layer is reduced. In other words, there is a trade-off between durability such as scratch resistance and abrasion resistance and slipperiness, and it is difficult to achieve high levels of properties at the same time. As a method for improving the trade-off relationship, there is a method of introducing a crosslinkable group into one end of a molecular chain, for example, a molecular chain containing a fluorine atom, but the level of properties is not satisfactory. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 163479 [Patent Document 2] Patent No. 6497449 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a curable composition capable of forming a hard coat layer that has both durability and slipperiness at a high level, which are in a trade-off relationship. In addition, in consideration of practical use, the hard coat layer needs to have high liquid repellency. [Means for solving the problem]
[0008] The first aspect of the present invention is a curable composition comprising: (a) 100 parts by mass of an active energy ray-curable polyfunctional monomer; (b) 0.05 to 5 parts by mass of a perfluoropolyether (excluding the (c) perfluoropolyether described below) having an active energy ray-polymerizable group at an end of a molecular chain containing a poly(oxyperfluoroalkylene) group; (c) 0.05 to 5 parts by mass of a perfluoropolyether having a molecular weight of 1000 or more and having a group represented by the following formula [1], formula [2] or formula [3] at an end of a molecular chain containing a poly(oxyperfluoroalkylene) group; and (d) 1 to 20 parts by mass of a polymerization initiator that generates radicals by active energy rays. [ka] (In the above formula [1], formula [2] and formula [3], R 1 represents a trifluoromethyl group, a fluoro group, a trifluoromethoxy group, or a nitro group; R 1 represents a trifluoromethyl group, a trifluoromethoxy group, or a nitro group, m represents an integer of 1 to 5, R 1 represents a fluoro group, m represents an integer from 2 to 5, R 2 represents a methyl group or a methoxy group, n represents 1, 2, or 3, R 3 represents an alkyl group having 3 to 10 carbon atoms, and * represents a bond to the molecular chain containing the poly(oxyperfluoroalkylene) group of the (c) perfluoropolyether.
[0009] The (c) perfluoropolyether has, for example, a group represented by the formula [1], [2] or [3] at each of both ends of a molecular chain containing the poly(oxyperfluoroalkylene) group.
[0010] The (c) perfluoropolyether has, for example, a group represented by the formula [1], [2] or [3] at one end of a molecular chain containing the poly(oxyperfluoroalkylene) group.
[0011] The (c) perfluoropolyether does not have, for example, the active energy ray-polymerizable group.
[0012] The poly(oxyperfluoroalkylene) group of the (b) perfluoropolyether and the poly(oxyperfluoroalkylene) group of the (c) perfluoropolyether have, for example, the repeating unit -[CF2O]- and / or the repeating unit -[CF2CF2O]-. When having both repeating units, these repeating units are bonded in a block bond, a random bond, or a block bond and a random bond.
[0013] The (b) perfluoropolyether molecular chain containing a poly(oxyperfluoroalkylene) group and the (c) perfluoropolyether molecular chain containing a poly(oxyperfluoroalkylene) group have, for example, a structure represented by the following formula [4] or formula [5]. [ka] (In the above formula [4] and formula [5], p is the total number of the repeating units -[CF2CF2O]- and the repeating units -[CF2O]- and represents an integer of 3 to 30, the repeating units -[CF2CF2O]- and the repeating units -[CF2O]- are bonded to each other through a block bond, a random bond, or a combination of a block bond and a random bond, and q is the number of oxyethylene groups and represents an integer of 0 to 10.)
[0014] The ratio of the content of the perfluoropolyether (b) to the content of the perfluoropolyether (c) is, for example, 0.5 to 4.
[0015] The curable composition of the first aspect of the present invention may further comprise (e) a solvent.
[0016] A second aspect of the present invention is a cured film obtained from the curable composition of the first aspect of the present invention.
[0017] A third aspect of the present invention is a hardcoat film comprising a hardcoat layer on at least one surface of a film substrate, the hardcoat layer comprising the cured film according to the second aspect of the present invention.
[0018] The hard coat layer is formed, for example, by a method including a step of applying the curable composition of the first aspect of the present invention onto a film substrate to form a coating film, and a step of irradiating the coating film with active energy rays to cure it.
[0019] The hard coat layer is formed, for example, by a method including a step of applying the curable composition of the first aspect of the present invention onto a film substrate to form a coating film, a step of removing the solvent from the coating film by heating, and a step of irradiating the coating film with active energy rays to cure it.
[0020] The film substrate is, for example, composed of a plurality of layers, and has, for example, a lower layer of the hard coat layer on the surface of a resin film.
[0021] The hard coat layer has a thickness of, for example, 1 μm to 20 μm.
[0022] A fourth aspect of the present invention is a method for producing a laminate of a film substrate and a hard coat layer, comprising the steps of applying the curable composition of the first aspect of the present invention onto a film substrate to form a coating film, and irradiating the coating film with active energy rays to cure the coating film.
[0023] The film substrate is, for example, composed of a plurality of layers, and has, for example, a lower layer of the hard coat layer on the surface of a resin film.
[0024] A fifth aspect of the present invention is a perfluoropolyether compound having a group represented by the above formula [1], formula [2] or formula [3] at an end of a molecular chain containing a poly(oxyperfluoroalkylene) group.
[0025] The molecular chain containing the poly(oxyperfluoroalkylene) group has, for example, a structure represented by the formula [4] or [5].
[0026] The perfluoropolyether compound has, for example, a group represented by the formula [1], [2] or [3] at each of both ends of a molecular chain containing the poly(oxyperfluoroalkylene) group.
[0027] The perfluoropolyether compound has, for example, a group represented by the formula [1], [2] or [3] at one end of a molecular chain containing the poly(oxyperfluoroalkylene) group.
[0028] The perfluoropolyether compound does not have, for example, an active energy ray-polymerizable group.
[0029] A sixth aspect of the present invention is a surface modifier comprising the perfluoropolyether compound of the fifth aspect of the present invention and a perfluoropolyether compound having the active energy ray-polymerizable group at an end of a molecular chain including a poly(oxyperfluoroalkylene) group having a structure represented by the formula [4] or the formula [5]. Effect of the Invention
[0030] According to the present invention, it is possible to provide a curable composition useful for forming a cured film and a hard coat layer that have excellent scratch resistance, abrasion resistance, and excellent slippage even in a thin film having a thickness of 1 μm to 20 μm. In addition, according to the present invention, it is possible to provide a hard coat film having a cured film obtained from the curable composition or a hard coat layer made of the cured film, and it is possible to provide a hard coat film having excellent durability properties such as scratch resistance and abrasion resistance, and slippage, which are in a trade-off relationship. Furthermore, according to the present invention, it is possible to provide a curable composition useful for forming a cured film and a hard coat layer that is imparted with high liquid repellency in addition to the compatibility of both of the above-mentioned properties, and a hard coat film having a hard coat layer excellent in these properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] <Curable composition> Each component of the curable composition of the present invention will be described below. [(a) Active energy ray-curable polyfunctional monomer] The active energy ray-curable polyfunctional monomer of the component (a) (hereinafter, also simply referred to as "(a) polyfunctional monomer") refers to a monomer having two or more active energy ray-polymerizable groups that undergo a polymerization reaction and harden when irradiated with active energy rays such as ultraviolet rays. Examples of the active energy ray-polymerizable group include a (meth)acryloyl group and a vinyl group.
[0032] In the curable composition of the present invention, preferred examples of the polyfunctional monomer (a) include a monomer selected from the group consisting of polyfunctional (meth)acrylate compounds, and further include a monomer selected from the group consisting of polyfunctional urethane (meth)acrylate compounds and a monomer selected from the group consisting of lactone-modified polyfunctional (meth)acrylate compounds, which will be described later. In the present invention, the polyfunctional monomer (a) may be one selected from the group consisting of the polyfunctional (meth)acrylate compounds, or two or more selected from the group consisting of the polyfunctional (meth)acrylate compounds may be used in combination. In the present invention, the (meth)acrylate compound includes both an acrylate compound and a methacrylate compound, and for example, (meth)acrylic acid includes acrylic acid and methacrylic acid.
[0033] The (a) polyfunctional monomer may be an oxyalkylene-modified polyfunctional monomer, and examples of the oxyalkylene-modified monomer include oxymethylene-modified, oxyethylene-modified, and oxypropylene-modified monomers. The oxyalkylene-modified polyfunctional monomer may include the above-mentioned polyfunctional (meth)acrylate compound or polyfunctional urethane (meth)acrylate compound modified with oxyalkylene. The oxyalkylene-modified polyfunctional monomer may be used alone or in combination of two or more.
[0034] In the present invention, the (a) polyfunctional monomer may be a polyfunctional monomer having at least three, for example at least four, active energy ray polymerizable groups. In the present invention, the (a) polyfunctional monomer may be a monomer selected from the group consisting of oxyalkylene-modified polyfunctional (meth)acrylate compounds having at least three active energy ray polymerizable groups.
[0035] Examples of the polyfunctional (meth)acrylate compound (but not having a urethane bond) include trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, glycerin tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, ethoxylated glycerin tri(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, 1,3-propanediol di(meth)acrylate, acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-methyl-1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, bis(2-hydroxyethyl)isocyanurate di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, tricyclo[5.2.1.02,6 ] decanedimethanol di(meth)acrylate, dioxane glycol di(meth)acrylate, 2-hydroxy-1-acryloyloxy-3-methacryloyloxypropane, 2-hydroxy-1,3-di(meth)acryloyloxypropane, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, bis[4-(meth)acryloylthiophenyl]sulfide, bis[2-(meth)acryloylthioethyl]sulfide, 1,3-adamantanediol di(meth)acrylate, 1,3-adamantanedimethanol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate can be mentioned. Among these, preferred polyfunctional (meth)acrylate compounds include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0036] The oxyalkylene-modified polyfunctional (meth)acrylate compound may be, for example, a (meth)acrylate compound of a polyol modified with an oxyalkylene.The polyol may be, for example, glycerin, diglycerin, triglycerin, tetraglycerin, pentaglycerin, hexaglycerin, decaglycerin, polyglycerin, trimethylolpropane, ditrimethylolpropane, pentaerythritol, or dipentaerythritol.
[0037] The above-mentioned polyfunctional urethane (meth)acrylate compound is a compound having a plurality of acryloyl groups or methacryloyl groups in one molecule and having one or more urethane bonds [-NHC(=O)O-]. Examples of the polyfunctional urethane (meth)acrylate compound include a compound obtained by reacting a polyfunctional isocyanate with a (meth)acrylate having a hydroxyl group, and a compound obtained by reacting a polyfunctional isocyanate with a (meth)acrylate having a hydroxyl group and a polyol, but the polyfunctional urethane (meth)acrylate compound usable in the present invention is not limited to these examples.
[0038] Examples of the polyfunctional isocyanate include tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate. Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and tripentaerythritol hepta(meth)acrylate. Examples of the polyol include diols such as ethylene glycol, propylene glycol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, and dipropylene glycol; polyester polyols which are reaction products of these diols with aliphatic dicarboxylic acids or dicarboxylic anhydrides such as succinic acid, maleic acid, and adipic acid; polyether polyols; and polycarbonate diols.
[0039] The (a) polyfunctional monomer may be a lactone-modified polyfunctional (meth)acrylate compound, and the lactone to be modified is preferably ε-caprolactone. Examples of the lactone-modified polyfunctional (meth)acrylate compound include ε-caprolactone-modified pentaerythritol tri(meth)acrylate, ε-caprolactone-modified pentaerythritol tetra(meth)acrylate, ε-caprolactone-modified dipentaerythritol penta(meth)acrylate, and ε-caprolactone-modified dipentaerythritol hexa(meth)acrylate.
[0040] [(b) Perfluoropolyether having an active energy ray polymerizable group at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group] The perfluoropolyether having an active energy ray polymerizable group at the end of the molecular chain containing the poly(oxyperfluoroalkylene) group of the component (b) is also referred to simply as "(b) perfluoropolyether" below. The (b) perfluoropolyether excludes the (c) perfluoropolyether described below. The (b) perfluoropolyether preferred in the curable composition of the present invention has an active energy ray polymerizable group at the end of the molecular chain containing the poly(oxyperfluoroalkylene) group via a urethane bond. The end of the molecular chain containing the poly(oxyperfluoroalkylene) group may be either all ends or some ends of the molecular chain. When the molecular chain is linear, all ends and some ends of the molecular chain are both ends and one end of the linear molecular chain, respectively. As the linking group between the poly(oxyperfluoroalkylene) group and the urethane bond, for example, a hydrocarbon group having an ether bond may be mentioned, and at least one hydrogen atom of the hydrocarbon group may be substituted with a fluorine atom.
[0041] The perfluoropolyether (b), together with the component (c) described below, serves as a surface modifier in the hard coat layer formed from the curable composition of the present invention. In addition, the perfluoropolyether (b) has excellent compatibility with the polyfunctional monomer (a), and therefore enables the formation of a hard coat layer that is suppressed from becoming cloudy and exhibits a transparent appearance.
[0042] As the poly(oxyperfluoroalkylene) group, from the viewpoint of obtaining a cured film with good scratch resistance, a group having both -[CF2O]- (oxyperfluoromethylene group) and -[CF2CF2O]- (oxyperfluoroethylene group) as repeating units is preferred. In this case, the bond of these oxyperfluoroalkylene groups may be either block bond or random bond.
[0043] The molecular chain containing the poly(oxyperfluoroalkylene) group preferably has a structure represented by the following formula [4] or [5]. [ka] In the above formula [4] and formula [5], p is the total number of the repeating units -[CF2CF2O]- and the repeating units -[CF2O]-, and is, for example, an integer of 3 to 30, preferably 7 to 21, and the bond between the repeating units -[CF2CF2O]- and the repeating units -[CF2O]- may be either a block bond or a random bond. In the above formula [5], q is the number of oxyethylene groups and is an integer of 0 to 10.
[0044] Examples of the active energy ray polymerizable group include (meth)acryloyl group and vinyl group. (b) Perfluoropolyether is not limited to those having one active energy ray polymerizable group at the end of the molecular chain containing poly(oxyperfluoroalkylene) group, but may have two or more active energy ray polymerizable groups. Examples of the end structure containing active energy ray polymerizable group include the structures of formulas [A1] to [A5] shown below, and structures in which the acryloyl group in these structures is replaced with a methacryloyl group. Among these structures, the structures of formulas [A3], [A4] and [A5] having two or more active energy ray polymerizable groups, and structures in which the acryloyl group in these structures is replaced with a methacryloyl group are preferred. [ka]
[0045] In the curable composition of the present invention, the content of (b) perfluoropolyether is 0.05 to 5 parts by mass, preferably 0.1 to 5 parts by mass, more preferably 0.1 to 1 part by mass, based on 100 parts by mass of the (a) polyfunctional monomer. By making the content of (b) perfluoropolyether 0.05 parts by mass or more, sufficient scratch resistance can be imparted to the hard coat layer, and by making the content of (b) perfluoropolyether 5 parts by mass or less, sufficient compatibility with (a) polyfunctional monomer can be obtained, resulting in a hard coat layer with little cloudiness.
[0046] (b) Perfluoropolyether can be used alone or in combination of two or more. When two or more types are combined, perfluoropolyether having an active energy ray polymerizable group via a urethane bond at one end (one end) of a molecular chain containing a poly(oxyperfluoroalkylene) group and having a hydroxyl group at the other end (the other end) of the molecular chain may be included.
[0047] [(c) Perfluoropolyether having a molecular weight of 1000 or more and having a group represented by formula [1], formula [2] or formula [3] at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group] Perfluoropolyethers having a molecular weight of 1000 or more, for example 1000 to 4000, and having a group represented by formula [1], formula [2] or formula [3] at the end of the molecular chain containing the poly(oxyperfluoroalkylene) group of the component (c) are hereinafter also referred to simply as "(c) perfluoropolyethers". (c) perfluoropolyethers differ from the (b) perfluoropolyethers in that they have a group represented by the following formula [1], formula [2] or formula [3] at the end of the molecular chain containing the poly(oxyperfluoroalkylene) group, and have a molecular weight of 1000 or more. On the other hand, the definitions of the molecular chain containing the poly(oxyperfluoroalkylene) group of (c) perfluoropolyether and its end are the same as those of the (b) perfluoropolyether. Therefore, it is preferable that the molecular chain containing the poly(oxyperfluoroalkylene) group has a structure represented by the formula [4] or formula [5]. [ka] R in the above formula [1] 1 represents a trifluoromethyl group, a fluoro group, a trifluoromethoxy group, or a nitro group; R 1 represents a trifluoromethyl group, a trifluoromethoxy group, or a nitro group, m represents an integer of 1 to 5, R 1 When R represents a fluoro group, m represents an integer of 2 to 5. 2 represents a methyl group or a methoxy group, preferably a methyl group, and n represents 1, 2, or 3. 3 represents an alkyl group having 3 to 10 carbon atoms, for example, an alkyl group having 3 to 6 carbon atoms. In the above formulas [1], [2] and [3], * represents a bond to the molecular chain containing the poly(oxyperfluoroalkylene) group.
[0048] (c) Perfluoropolyether can be obtained, for example, by reacting a perfluoropolyether having a hydroxy group at the end of the structure represented by the above formula [4] or formula [5] with an isocyanate compound represented by the following formula [1a], formula [2a] or formula [3a]. [ka] R in the above formula [1a] 1 and m, R in the above formula [2a] 2 and n, and R in the above formula [3a] 3 R in the above formula [1], formula [2] and formula [3] respectively 1 , R 2 , R 3 , m and n are defined as the same.
[0049] The perfluoropolyether (c) plays a role as a surface modifier in the hard coat layer formed from the curable composition of the present invention together with the perfluoropolyether (b). In addition, the perfluoropolyether (c) has excellent compatibility with the perfluoropolyether (b), and therefore, it is possible to form a hard coat layer that is suppressed from becoming cloudy and has a transparent appearance.
[0050] When the molecular weight of (c) perfluoropolyether is 1000 or more, the (c) perfluoropolyether is likely to remain on the surface of the hard coat layer obtained from the curable composition of the present invention, and a hard coat layer with excellent slipperiness can be obtained. In addition, when the molecular weight of (c) perfluoropolyether is, for example, 4000 or less, it is sufficiently compatible with (a) polyfunctional monomer, and a hard coat layer with little cloudiness can be obtained.
[0051] In the curable composition of the present invention, the content of the (c) perfluoropolyether is 0.05 to 5 parts by mass relative to 100 parts by mass of the (a) polyfunctional monomer, and the ratio of the content of the (b) perfluoropolyether to the content of the (c) perfluoropolyether is preferably 0.5 to 4. When the content of the (c) perfluoropolyether is 0.05 parts by mass or more, the (c) perfluoropolyether is sufficiently present on the surface of the hard coat layer obtained from the curable composition of the present invention, so that a hard coat layer with excellent slip properties can be obtained. In addition, when the content of the (c) perfluoropolyether is 5 parts by mass or less, the (c) perfluoropolyether is sufficiently compatible with the (b) perfluoropolyether, so that a hard coat layer with little cloudiness can be obtained.
[0052] (c) perfluoropolyether can be used alone or in combination of two or more. When two or more types are combined, perfluoropolyethers having a group represented by the formula [1], formula [2] or formula [3] at one end (one end) of a molecular chain containing a poly(oxyperfluoroalkylene) group and having an active energy ray polymerizable group or a hydroxyl group at the other end (the other end) of the molecular chain may be included. In addition, (c) perfluoropolyether is more preferably one that does not have the active energy ray polymerizable group that the (b) perfluoropolyether has.
[0053] [(d) Polymerization initiator] The (d) polymerization initiator preferred in the curable composition of the present invention is, for example, a polymerization initiator that generates radicals when exposed to active energy rays such as electron beams, ultraviolet rays, and X-rays, particularly when exposed to ultraviolet rays.
[0054] Examples of the (d) polymerization initiator include benzoins, alkylphenones, thioxanthones, azos, azides, diazos, o-quinone diazides, acylphosphine oxides, oxime esters, organic peroxides, benzophenones, biscoumarins, bisimidazoles, titanocenes, thiols, halogenated hydrocarbons, trichloromethyltriazines, and onium salts such as iodonium salts and sulfonium salts. These polymerization initiators may be used alone or in combination of two or more. In the present invention, from the viewpoints of transparency, surface curability, and thin film curability, it is preferable to use alkylphenones as the (d) polymerization initiator. By using alkylphenones, a cured film with improved scratch resistance can be obtained.
[0055] Examples of the alkylphenones include α-hydroxyalkylphenones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-1-(4-(2-hydroxyethoxy)phenyl)-2-methylpropan-1-one, and 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one; α-aminoalkylphenones such as 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropan-1-one and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one; 2,2-dimethoxy-1,2-diphenylethan-1-one; and methyl phenylglyoxylate.
[0056] In the curable composition of the present invention, the content of the polymerization initiator (d) is 1 to 20 parts by mass, preferably 2 to 10 parts by mass, based on 100 parts by mass of the polyfunctional monomer (a).
[0057] [(e) Solvent] The curable composition of the present invention may contain a solvent (e) as an optional component, i.e., may be in the form of a varnish. The solvent (e) may be appropriately selected in consideration of the solubility and dispersibility of the components (a) to (d), the workability during application of the curable composition for forming a cured film (hard coat layer) described below, the drying properties before and after curing, etc.
[0058] Examples of the solvent (e) include aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, and tetralin; aliphatic or alicyclic hydrocarbons such as n-hexane, n-heptane, mineral spirits, and cyclohexane; halides such as methyl chloride, methyl bromide, methyl iodide, dichloromethane, chloroform, carbon tetrachloride, trichloroethylene, perchloroethylene, and o-dichlorobenzene; esters or ester ethers such as ethyl acetate, propyl acetate, butyl acetate, methoxybutyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, and propylene glycol monomethyl ether acetate (PGMEA); diethyl ether, tetrahydrofuran (THF), 1,4-dioxane, methyl cellosolve, ethyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and the like. Examples of the solvent include ethers such as polypropylene glycol ether (PGME), propylene glycol mono-n-propyl ether, propylene glycol monoisopropyl ether, and propylene glycol mono-n-butyl ether; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), di-n-butyl ketone, and cyclohexanone; alcohols such as methanol, ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol, tert-butyl alcohol, 2-ethylhexyl alcohol, benzyl alcohol, and ethylene glycol; amides such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methyl-2-pyrrolidone (NMP); and sulfoxides such as dimethyl sulfoxide (DMSO), as well as mixtures of two or more of these solvents.
[0059] The content of the (e) solvent in the curable composition of the present invention is not particularly limited, but is, for example, a concentration such that the solid content concentration of the curable composition of the present invention is 1% by mass to 70% by mass, preferably 5% by mass to 50% by mass. Here, the solid content concentration (also referred to as non-volatile content concentration) represents the content of the solid content (all components excluding the solvent component) relative to the total mass (total mass) of the (a) to (e) components and other additives in the curable composition of the present invention.
[0060] [Other additives] Furthermore, to the curable composition of the present invention, generally added additives may be appropriately blended as necessary, such as a polymerization inhibitor, a photosensitizer, a leveling agent, a surfactant, an adhesion imparting agent, a plasticizer, an ultraviolet absorber, a storage stabilizer, an antistatic agent, an inorganic filler, a pigment, a dye, etc., either alone or in combination of two or more kinds, so long as the effects of the present invention are not impaired.
[0061] <Cured film> The curable composition of the present invention can be applied (coated) on a substrate to form a coating film, and the coating film can be polymerized (cured) by irradiating the coating film with active energy rays to form a cured film, which is also the subject of the present invention. In addition, the above-mentioned cured film can be used as a hard coat layer in a hard coat film described later.
[0062] Examples of the substrate include various resins (polycarbonate, polymethacrylate, polystyrene, polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyurethane, thermoplastic polyurethane (TPU), polyolefin, polyamide, polyimide, epoxy resin, melamine resin, triacetyl cellulose (TAC), acrylonitrile-butadiene-styrene copolymer (ABS), acrylonitrile-styrene copolymer (AS), norbornene resin), metal, wood, paper, glass, and slate. The shape of these substrates may be a plate, a film, or a three-dimensional molded body. In addition, on the surface of the substrate, for example, a primer layer, an ultraviolet absorbing layer, an infrared absorbing layer, a near infrared absorbing layer, an electromagnetic wave absorbing layer, a color correction layer, a refractive index adjusting layer, a weather-resistant layer, an antireflection layer, an antistatic layer, a discoloration prevention layer, a gas barrier layer, a water vapor barrier layer, a light scattering layer, an electrode layer, etc. may be formed as a lower layer of the hard coat layer, and a plurality of lower layers of the hard coat layer may be laminated. The layer formed on the surface of the substrate is not particularly limited as long as it does not impair the effects of the present invention.
[0063] The coating method on the substrate may be appropriately selected from cast coating, spin coating, blade coating, dip coating, roll coating, spray coating, bar coating, die coating, inkjet printing, printing (letterpress printing, intaglio printing, lithographic printing, screen printing, etc.), among which the roll-to-roll method can be used. From the viewpoint of thin film coating, it is preferable to use letterpress printing, particularly gravure coating. It is preferable to filter the curable composition of the present invention using a filter having a pore size of about 0.2 μm before coating. When coating, a solvent may be further added to the curable composition as necessary. Examples of the solvent in this case include the various solvents listed in [(e) Solvent] above.
[0064] After the curable composition of the present invention is applied onto a substrate to form a coating film, the coating film is pre-dried with a heating means such as a hot plate or oven as necessary to remove the solvent (solvent removal step). The conditions for the heat drying at this time are preferably, for example, 40°C to 120°C and about 30 seconds to 10 minutes. After drying, the coating film is cured by irradiating it with active energy rays such as ultraviolet rays. Examples of active energy rays include ultraviolet rays, electron beams, and X-rays, and ultraviolet rays are particularly preferred. Examples of light sources used for ultraviolet irradiation include sunlight, chemical lamps, low-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, xenon lamps, and UV-LEDs. Furthermore, the polymerization may be completed by performing post-baking, specifically by heating using a heating means such as a hot plate or oven.
[0065] The thickness of the cured film formed after drying and curing is usually 0.1 to 50 μm, preferably 0.5 to 20 μm.
[0066] <Hard coat film> The curable composition of the present invention can be used to produce a hard coat film having a hard coat layer on at least one side (surface) of a film substrate. The hard coat film is also an object of the present invention, and the hard coat film is suitably used to protect the surfaces of various display elements such as touch panels and liquid crystal displays.
[0067] The hard coat layer in the hard coat film of the present invention can be formed by a method including a step of applying the curable composition of the present invention onto a film substrate to form a coating film, a step of removing the solvent by heating as necessary, and a step of irradiating the coating film with active energy rays such as ultraviolet rays to cure the coating film. A method for producing a hard coat film having a hard coat layer on at least one side of a film substrate, including these steps, is also within the scope of the present invention.
[0068] The film substrate may be any of the transparent resin films usable for optical applications among the substrates listed in the above-mentioned <Cured film>. Preferred resin films include, for example, films of polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN), polyurethane, thermoplastic polyurethane (TPU), polycarbonate, polymethacrylate, polystyrene, polyolefin, polyamide, polyimide, and triacetyl cellulose (TAC).
[0069] The film substrate may be formed by laminating a plurality of layers. For example, a layer different from the resin film may be laminated on the surface of the resin film as a lower layer of the hard coat layer, such as a primer layer, an ultraviolet absorbing layer, an infrared absorbing layer, a near infrared absorbing layer, an electromagnetic wave absorbing layer, a color correction layer, a refractive index adjustment layer, a weather resistant layer, an antireflection layer, an antistatic layer, a discoloration prevention layer, a gas barrier layer, a water vapor barrier layer, a light scattering layer, an electrode layer, etc., or a plurality of lower layers of the hard coat layer may be laminated. The layer laminated on the surface of the resin film is not particularly limited as long as it does not impair the effects of the present invention.
[0070] The method for applying the curable composition of the present invention onto the film substrate (coating film forming step) and the method for irradiating the coating film with active energy rays (curing step) can be the methods listed in the above-mentioned <cured film>. When the curable composition of the present invention contains a solvent (in the form of a varnish), the coating film may be dried to remove the solvent after the coating film forming step, if necessary. In this case, the method for drying the coating film (solvent removal step) listed in the above-mentioned <cured film> can be used.
[0071] The hard coat layer thus obtained has a thickness (film thickness) of, for example, 1 μm to 20 μm, and preferably 1 μm to 10 μm.
[0072] <Surface modifier> The present invention also includes a surface modifier comprising a perfluoropolyether compound having a group represented by the formula [1], formula [2] or formula [3] at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group, and a perfluoropolyether compound having an active energy ray polymerizable group at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group having a structure represented by the formula [4] or formula [5]. The active energy ray polymerizable group is the active energy ray polymerizable group of the (b) perfluoropolyether. The former perfluoropolyether compound is preferably one that does not have the active energy ray polymerizable group. Furthermore, the former perfluoropolyether compound itself is also a subject of the present invention. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the apparatus and conditions used for preparing samples and analyzing physical properties are as follows.
[0074] (1) Coating with a bar coater Equipment: PM-9050MC manufactured by SMT Co., Ltd. Bar: OSG System Products Co., Ltd. A-Bar OSP-30, maximum wet film thickness 30 μm Coating speed: 4m / min (2) Oven Equipment: Sanki Instruments Co., Ltd. 2-layer clean oven (upper and lower type) PO-250-45-D (3)UV curing Equipment: Heraeus CV-110QC-G Lamp: Heraeus H-bulb electrodeless lamp (4) Scratch resistance test and abrasion resistance test Equipment: Reciprocating wear tester TRIBOGEAR TYPE:30S manufactured by Shinto Scientific Co., Ltd. Scanning speed: 3200mm / min Scanning distance: 50mm (5) Contact angle Equipment: DropMaster DM-501 manufactured by Kyowa Interface Science Co., Ltd. Measurement temperature: 23℃ (6) Dynamic friction coefficient μk measurement Equipment: Shinto Scientific Co., Ltd., variable load friction and wear test system, TRIBOGEAR (registered trademark) TYPE: HHS2000 Probe: 0.6mmR sapphire pin Load: 200g Scanning speed: 2mm / sec Scanning distance: 10mm (7) Total light transmittance, haze Equipment: Haze meter NDH5000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0075] The abbreviations have the following meanings: Multifunctional acrylate PA1: Dipentaerythritol pentaacrylate / hexaacrylate mixture [Aronix (registered trademark) M-403, manufactured by Toagosei Co., Ltd., pentagonal ratio 50% to 60% (catalog value)] Multifunctional acrylate PA2: Oxyethylene-modified multifunctional acrylate [New Frontier (registered trademark) MF-001, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.] Multifunctional acrylate PA3: Multifunctional urethane acrylate [Art Resin (registered trademark) UN-3320HS, manufactured by Negami Chemical Industries, Ltd.] Multifunctional acrylate PA4: Caprolactone-modified dipentaerythritol hexaacrylate [DPCA30 manufactured by Nippon Kayaku Co., Ltd.] PFPE1: Perfluoropolyether having two hydroxyl groups at each end of a molecular chain containing a poly(oxyperfluoroalkylene) group, without a poly(oxyalkylene) group [Fomblin (registered trademark) T4 manufactured by Solvay Specialty Polymers, number average molecular weight calculated from the results of NMR analysis: 2200] PFPE2: Perfluoropolyether having two hydroxyl groups at each end of a molecular chain containing a poly(oxyperfluoroalkylene) group via a poly(oxyalkylene) group [Fluorolink (registered trademark) E10 manufactured by Solvay Specialty Polymers, number average molecular weight calculated from the results of H NMR analysis: 1818] PFPE3: Perfluoropolyether having one hydroxyl group at each end of the molecular chain containing a poly(oxyperfluoroalkylene) group, without a poly(oxyalkylene) group [Fomblin (registered trademark) D2 manufactured by Solvay Specialty Polymers, number average molecular weight calculated from the results of NMR analysis: 1500] PFPE4: Perfluoropolyether (1H,1H-perfluoro-3,6,9-trioxatridecan-1-ol) having one hydroxyl group at one end without a poly(oxyalkylene) group [C10GOL manufactured by Exfluor Research, molecular weight 548.1 (catalog value)] N1: 1,1-bis(acryloyloxymethyl)ethyl isocyanate [Karenz (registered trademark) BEI, manufactured by Showa Denko K.K.] N2: Propyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N3: Butyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N4: Hexyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N5: 2,4-Difluorophenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N6: 4-(Trifluoromethyl)phenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N7: 3-(Trifluoromethyl)phenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N8: 3-(Trifluoromethoxy)phenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N9: Para-toluenesulfonyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N10: 4-Nitrophenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N11: 4-Fluorophenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N12: Phenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N13: Para-tolyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N14: Para-methoxyphenyl isocyanate [Tokyo Chemical Industry Co., Ltd.] N15: 3,5-Dimethylphenylisocyanate [Tokyo Chemical Industry Co., Ltd.] N16: 2,6-Dimethylphenylisocyanate [Tokyo Chemical Industry Co., Ltd.] DOTDD: Dioctyltin dineodecanoate [Neostan (registered trademark) U-830, manufactured by Nitto Kasei Co., Ltd.] SMA2: Perfluoropolyether having a total of four active energy ray polymerizable groups at both ends of the molecular chain containing a poly(oxyperfluoroalkylene) group [Fluorolink (registered trademark) AD-1700 manufactured by Solvay Specialty Polymers, 70% by weight non-volatile solution] SMA3: Perfluoropolyether having an active energy ray polymerizable group at one end of the molecular chain containing a poly(oxyperfluoroalkylene) group [Optool DAC-HP manufactured by Daikin Co., Ltd., 20% by mass non-volatile content solution] O2959: 2-hydroxy-1-(4-(2-hydroxyethoxy)phenyl)-2-methylpropan-1-one [OMNIRAD (registered trademark) 2959, manufactured by IGM Resins] MEK: Methyl ethyl ketone PGME: Propylene glycol monomethyl ether
[0076] [Production Example 1] Production of SMA1, a component of the surface modifier In a screw tube, 1.19g (0.5mmol) of PFPE1, 0.52g (2.0mmol) of N1, 0.017g of DOTDD (0.01 times the total mass of PFPE1 and N1), and 1.67g of MEK were charged. This mixture was stirred for 72 hours at room temperature (approximately 23°C) using a stirrer tip to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMA1. The obtained SMA1 corresponds to the (b) component of the curable composition of the present invention.
[0077] [Example 1] Preparation of surface modifier component SMB1 In a screw tube, 2.22g (1.5mmol) of PFPE2, 0.25g (3.0mmol) of N2, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N2), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB1. The obtained SMB1 corresponds to the (c) component of the curable composition of the present invention.
[0078] [Example 2] Preparation of surface modifier component SMB2 In a screw tube, 2.19g (1.5mmol) of PFPE2, 0.29g (3.0mmol) of N3, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N3), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB2. The obtained SMB2 corresponds to the (c) component of the curable composition of the present invention.
[0079] [Example 3] Preparation of surface modifier component SMB3 In a screw tube, 2.12g (1.4mmol) of PFPE2, 0.36g (2.8mmol) of N4, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N4), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB3. The obtained SMB3 corresponds to the (c) component of the curable composition of the present invention.
[0080] [Example 4] Preparation of surface modifier component SMB4 In a screw tube, 2.05g (1.4mmol) of PFPE2, 0.42g (2.8mmol) of N5, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N5), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB4. The obtained SMB4 corresponds to the (c) component of the curable composition of the present invention.
[0081] [Example 5] Preparation of surface modifier component SMB5 In a screw tube, 1.98g (1.3mmol) of PFPE2, 0.49g (2.6mmol) of N6, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N6), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB5. The obtained SMB5 corresponds to the (c) component of the curable composition of the present invention.
[0082] [Example 6] Preparation of SMB6, a component of the surface modifier In a screw tube, 1.98g (1.3mmol) of PFPE2, 0.49g (2.6mmol) of N7, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N7), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB6. The obtained SMB6 corresponds to the (c) component of the curable composition of the present invention.
[0083] [Example 7] Preparation of surface modifier component SMB7 In a screw tube, 2.34g (1.6mmol) of PFPE2, 0.63g (3.2mmol) of N8, 0.030g of DOTDD (0.01 times the total mass of PFPE2 and N8), and 3.0g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB7. The obtained SMB7 corresponds to the component (c) of the curable composition of the present invention.
[0084] [Example 8] Preparation of SMB8, a component of the surface modifier In a screw tube, 4.09g (2.2mmol) of PFPE2, 1.10g (4.4mmol) of N9, 0.052g of DOTDD (0.01 times the total mass of PFPE2 and N9), and 5.3g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB8. The obtained SMB8 corresponds to the (c) component of the curable composition of the present invention.
[0085] [Example 9] Preparation of SMB9, a component of the surface modifier In a screw tube, 2.44g (1.6mmol) of PFPE2, 0.53g (3.2mmol) of N10, 0.030g of DOTDD (0.01 times the total mass of PFPE2 and N10), and 3.0g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB9. The obtained SMB9 corresponds to the component (c) of the curable composition of the present invention.
[0086] [Example 10] Preparation of surface modifier component SMB10 In a screw tube, 1.87g (0.8mmol) of PFPE1, 0.41g (3.2mmol) of N6, 0.025g of DOTDD (0.01 times the total mass of PFPE1 and N6), and 2.5g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB10. The obtained SMB10 corresponds to the (c) component of the curable composition of the present invention.
[0087] [Example 11] Preparation of SMB11, a component of the surface modifier In a screw tube, 4.17g (2.1mmol) of PFPE3, 1.01g (4.2mmol) of N6, 0.052g of DOTDD (0.01 times the total mass of PFPE3 and N6), and 5.2g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB11. The obtained SMB11 corresponds to the (c) component of the curable composition of the present invention.
[0088] [Example 12] Preparation of SMB12, a component of the surface modifier In a screw tube, 4.34g (2.2mmol) of PFPE3, 0.86g (4.4mmol) of N9, 0.052g of DOTDD (0.01 times the total mass of PFPE3 and N9), and 5.3g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB12. The obtained SMB12 corresponds to the (c) component of the curable composition of the present invention.
[0089] [Example 13] Preparation of surface modifier component SMB13 Into a screw tube, 4.11g (2.7mmol) of PFPE2, 0.51g (2.7mmol) of N6, 0.66g (2.7mmol) of N1, 0.053g of DOTDD (0.01 times the total mass of PFPE2, N6 and N1), and 4.67g of MEK were charged. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB13. The obtained SMB13 corresponds to the (c) component of the curable composition of the present invention.
[0090] [Example 14] Preparation of SMB14, a component of the surface modifier In a screw tube, 4.85 g (3.4 mmol) of PFPE4, 0.63 g (3.4 mmol) of N6, 0.025 g of DOTDD (0.01 times the total mass of PFPE4 and N6), and 2.5 g of MEK were charged. The resulting mixture was stirred with a stirrer tip at room temperature (approximately 23° C.) for 72 hours to obtain a 50 mass % MEK solution of the target perfluoropolyether compound SMB14.
[0091] [Comparative Example 1] Production of SMB15 2.09g (1.4mmol) of PFPE2, 0.38g (2.8mmol) of N11, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N11), and 2.5g of MEK were charged into a screw tube. The resulting mixture was stirred at room temperature (approximately 23°C) for 72 hours using a stirrer tip to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB15.
[0092] [Comparative Example 2] Production of SMB16 2.14g (1.4mmol) of PFPE2, 0.34g (2.8mmol) of N12, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N12), and 2.5g of MEK were charged into a screw tube. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB16.
[0093] [Comparative Example 3] Production of SMB17 In a screw tube, 2.10 g (1.4 mmol) of PFPE2, 0.37 g (2.8 mmol) of N13, 0.025 g of DOTDD (0.01 times the total mass of PFPE2 and N13), and 2.5 g of MEK were charged. The resulting mixture was stirred with a stirrer tip at room temperature (approximately 23° C.) for 72 hours to obtain a 50 mass % MEK solution of the target perfluoropolyether compound SMB17.
[0094] [Comparative Example 4] Production of SMB18 2.48g (1.7mmol) of PFPE2, 0.49g (3.4mmol) of N14, 0.030g of DOTDD (0.01 times the total mass of PFPE2 and N14), and 3.0g of MEK were charged into a screw tube. The resulting mixture was stirred at room temperature (approximately 23°C) for 72 hours using a stirrer tip to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB18.
[0095] [Comparative Example 5] Production of SMB19 2.07g (1.4mmol) of PFPE2, 0.41g (2.8mmol) of N15, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N15), and 2.5g of MEK were charged into a screw tube. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB19.
[0096] [Comparative Example 6] Production of SMB20 2.07g (1.4mmol) of PFPE2, 0.41g (2.8mmol) of N16, 0.025g of DOTDD (0.01 times the total mass of PFPE2 and N16), and 2.5g of MEK were charged into a screw tube. The resulting mixture was stirred using a stirrer tip at room temperature (approximately 23°C) for 72 hours to obtain a 50% by mass MEK solution of the target perfluoropolyether compound SMB20.
[0097] [Examples 1 to 14, Comparative Examples 1 to 6] The homogeneity of a 50% by mass MEK solution of each perfluoropolyether compound was evaluated. The evaluation procedure is shown below. The results are also shown in Table 1. [Solution homogeneity] The appearance of the resulting 50% by mass MEK solution of each perfluoropolyether compound was visually inspected and evaluated according to the following criteria. A: Transparent solution (no floating matter or sediment) C: Both floating matter and sediment are present [Table 1]
[0098] As shown in Table 1, the perfluoropolyether compounds SMB1 to SMB14 of Examples 1 to 14 (Example 13 was further reacted with isocyanate compound N1) obtained by reacting any one of perfluoropolyethers PFPE1 to PFPE4 with at least one of the isocyanate compounds N2 to N10 below had relatively weak cohesive strength and therefore high solubility. [ka]
[0099] On the other hand, as shown in Table 1, the perfluoropolyether compounds SMB15 to SMB20 of Comparative Examples 1 to 6 obtained by reacting the perfluoropolyether PFPE2 with any one of the following isocyanate compounds N11 to N16 showed high cohesive strength and low solubility. [ka]
[0100] [Examples 15 to 38, Comparative Examples 7 to 15] The components shown in Table 2 were mixed to prepare a curable composition having a solid content concentration shown in Table 2. Here, the solid content refers to components other than the solvent. In Table 2, [parts] means [parts by mass], and [%] means [% by mass]. In Table 2, the multifunctional acrylate and surface modifier each represent a solid content.
[0101] [Table 2]
[0102] These curable compositions were applied by a bar coater onto an A4-sized PET film [Lumirror (registered trademark) U403 (also known as U40), manufactured by Toray Industries, Inc., thickness 100 μm] on which a primer layer had been formed by easy-adhesion treatment on both sides, to obtain a coating film. This coating film was dried in an oven at 60° C. for 8 minutes to remove the solvent. The obtained film was then exposed to light at an exposure dose of 300 mJ / cm under a nitrogen atmosphere. 2 A hard coat film having a hard coat layer (cured film) was produced by exposing the film to UV light.
[0103] The homogeneity of each curable composition, and the scratch resistance, water repellency, abrasion resistance, slippage, and haze of the obtained hard coat film were evaluated. The evaluation procedures are shown below. The results are also shown in Table 3. [Composition homogeneity] The appearance of each of the prepared curable compositions was visually inspected and evaluated according to the following criteria. A: Clear solution (no floating matter, sediment or phase separation) C: Any of floating matter, sediment, and phase separation is present. [Scratch resistance] The surface of the hard coat layer of the obtained hard coat film was rubbed 5000 times with a steel wool [BONSTAR (registered trademark) #0000 (ultrafine)] attached to a reciprocating abrasion tester, with a load of 1 kg and a stroke of 50 mm. After that, the degree of damage in the area excluding the range of 5 mm width at both ends of the stroke of 50 mm was visually confirmed and evaluated according to the following criteria A, B, and C. Note that, when assuming actual use as a hard coat layer, at least B is required, and A is preferable. A: No scratches (0 scratches) B: Scratches (1 to 4 scratches, 1 to 9 mm long) C: Scratches (5 or more scratches measuring 1 to 9 mm in length, or 1 or more scratches measuring 1 cm or longer) [Water repellency] 1 μL of water was applied to the surface of the hard coat layer, and the contact angle θ was measured 5 times after 10 seconds. The average value was used to evaluate the hard coat layer according to the following criteria. When considering practical use as a hard coat layer, at least B is required, and A is desirable. A: θ≧105° B: 90°≦θ<105° C:θ<90° [Wear resistance] The surface of the hard coat layer was rubbed back and forth 2,500 times with a cylindrical eraser [Minoan RUBBER STICK, φ6.0mm] attached to a reciprocating abrasion tester, with a load of 1 kg. 1μL of water was applied to the rubbed part, and the contact angle θ was measured at 5 points after 5 seconds, and the average value was taken as the contact angle value and evaluated according to the following criteria. In addition, when assuming actual use as a hard coat layer, at least B is required, and A is preferable. A: θ≧90° B: 80°≦θ<90° C:80°<θ [Slipperiness] The dynamic friction coefficient μk was measured at five points on the surface of the hard coat layer, and the average value was used to evaluate the surface according to the following criteria. The smaller the dynamic friction coefficient value, the smaller the friction with the probe used, and the smoothness of the surface is measured. The smaller the dynamic friction coefficient value, the better the smoothness when touched, so the smaller the dynamic friction coefficient value, the better. A: μk≦0.05 B: 0.05<μk≦0.07 C:μk>0.07 [Haze] For reference, the haze was measured at three points on the surface of the hard coat layer, and the average value was calculated. The haze of the PET film used as the substrate this time [Lumirror (registered trademark) U403 (also known as U40), manufactured by Toray Industries, Inc., thickness 100 μm] was 1.6.
[0104] [Table 3]
[0105] As shown in Table 2, the curable compositions of Examples 15 to 36 include perfluoropolyether compounds SMB1 to SMB12 obtained by reacting any one of the isocyanate compounds N2 to N10 with any one of the multifunctional acrylates PA1 to PA4, perfluoropolyether compounds SMA1 to SMA3, and perfluoropolyethers PFPE1 to PFPE3.And, as shown in Table 3, the curable compositions of Examples 15 to 36 show excellent homogeneity, and the hard coat films having hard coat layers obtained from the curable compositions show excellent slip properties, scratch resistance, water repellency and abrasion resistance.
[0106] As shown in Table 2, the curable compositions of Example 37 and Example 38 contain multifunctional acrylate PA1, perfluoropolyether compound SMA1, and perfluoropolyether PFPE2, which are reacted with isocyanate compounds N6 and N1 to obtain perfluoropolyether compound SMB13. As shown in Table 3, the curable compositions of Example 37 and Example 38 show excellent homogeneity, and the hard coat film having a hard coat layer obtained from the curable composition shows excellent slip property, scratch resistance, water repellency and abrasion resistance.
[0107] On the other hand, as shown in Table 2, the curable compositions of Comparative Examples 7 to 9 contain the multifunctional acrylate PA1 and the perfluoropolyether compounds SMA1 to SMA3, and do not contain the component (c) such as SMB1 to SMB13. As shown in Table 3, the curable compositions of Comparative Examples 7 to 9 show the same level of homogeneity as the curable compositions of Examples 15 to 38, and the hard coat films having the hard coat layers obtained from the curable compositions of Comparative Examples 7 to 9 show the same level of scratch resistance and water repellency as the hard coat films having the hard coat layers obtained from the curable compositions of Examples 15 to 38, but are inferior in slipperiness.
[0108] In addition, as shown in Table 2, the curable compositions of Comparative Examples 10 and 11 contain perfluoropolyether compounds SMB6 or SMB7 obtained by reacting the isocyanate compound N7 or N8 with the polyfunctional acrylate PA1 and perfluoropolyether PFPE2, and do not contain the component (b) such as SMA1 to SMA3. As shown in Table 3, the curable compositions of Comparative Examples 10 and 11 are cloudy due to the generation of floating matter, and are inferior in homogeneity compared to the curable compositions of Examples 15 to 38, and the hard coat films having hard coat layers obtained from Comparative Examples 10 and 11 are inferior in slipperiness, scratch resistance, water repellency and abrasion resistance compared to the hard coat films having hard coat layers obtained from the curable compositions of Examples 15 to 38.
[0109] Furthermore, as shown in Table 2, the curable compositions of Comparative Examples 12 to 14 contain the multifunctional acrylate PA1, the perfluoropolyether compound SMA1, and the perfluoropolyethers PFPE1 to PFPE3. As shown in Table 3, the curable compositions of Comparative Examples 12 to 14 have poor homogeneity compared to the curable compositions of Examples 15 to 38, because the solubility of the perfluoropolyethers PFPE1 to PFPE3 is low, the curable compositions have cloudiness and phase separation due to the generation of suspended matter.
[0110] In addition, as shown in Table 2, the curable composition of Comparative Example 15 contains the perfluoropolyether compound SMB14 obtained by reacting the isocyanate compound N6 with the multifunctional acrylate PA1, the perfluoropolyether compound SMA1, and the perfluoropolyether PFPE4 having a molecular weight of 548.1. As shown in Table 3, the curable composition of Comparative Example 15 shows the same level of homogeneity as the curable compositions of Examples 15 to 38, and the hard coat film having a hard coat layer obtained from the curable composition of Comparative Example 15 shows the same level of scratch resistance, water repellency, and abrasion resistance as the hard coat film having a hard coat layer obtained from the curable composition of Examples 15 to 38, but the slipperiness is inferior. The perfluoropolyether compound SMB14 has a molecular weight of less than 1000 and is a low molecular weight compared to the other perfluoropolyether compounds SMB1 to SMB13, so the mobility of the molecules of SMB14 themselves is high and they are unlikely to remain on the surface of the hard coat layer, which is thought to result in the poor slipperiness.
Claims
1. (a) 100 parts by mass of an active energy ray-curable polyfunctional monomer, (b) 0.05 to 5 parts by mass of a perfluoropolyether (excluding the perfluoropolyether (c) described below) having an active energy ray-polymerizable group at the end of a molecular chain containing a poly(oxyperfluoroalkylene) group, (c) 0.05 to 5 parts by mass of a perfluoropolyether having a molecular weight of 1,000 or more and having a group represented by the following formula [1], formula [2] or formula [3] at each end of a molecular chain containing a poly(oxyperfluoroalkylene) group, and (d) A curable composition comprising 1 part by mass to 20 parts by mass of a polymerization initiator that generates radicals when exposed to active energy rays. 【Chemistry 1】 (In the above formula [1], formula [2] and formula [3], R 1 represents a trifluoromethyl group, a fluoro group, a trifluoromethoxy group, or a nitro group; R 1 represents a trifluoromethyl group, a trifluoromethoxy group, or a nitro group, m represents an integer of 1 to 5, R 1 represents a fluoro group, m represents an integer of 2 to 5, R 2 represents a methyl group or a methoxy group, n represents 1, 2 or 3, R 3 represents an alkyl group having 3 to 10 carbon atoms, and * represents a bond to the molecular chain containing the poly(oxyperfluoroalkylene) group of the (c) perfluoropolyether.
2. The curable composition according to claim 1 , wherein the perfluoropolyether (c) does not have the active energy ray-polymerizable group.
3. The poly(oxyperfluoroalkylene) group of the perfluoropolyether (b) and the poly(oxyperfluoroalkylene) group of the perfluoropolyether (c) each have a repeating unit -[CF 2 O]- and / or repeating unit -[CF 2 CF 2 3. The curable composition according to claim 1, wherein the repeating units are each a group having a repeating unit selected from the group consisting of a repeating unit ...
4. The (b) perfluoropolyether molecular chain containing a poly(oxyperfluoroalkylene) group and the (c) perfluoropolyether molecular chain containing a poly(oxyperfluoroalkylene) group have a structure represented by the following formula [4] or formula [5]. The curable composition according to claim 3. 【Chemistry 2】 (In the above formula [4] and formula [5], p represents a repeating unit -[CF 2 CF 2 O]- and the number of repeating units -[CF 2 The total number of the repeating units -[CF 2 CF 2 O]- and the repeating unit -[CF 2 O]- is bonded via a block bond, a random bond, or a block bond and a random bond, and q is the number of oxyethylene groups and represents an integer of 0 to 10.
5. The curable composition according to claim 1 , wherein the ratio of the content of the perfluoropolyether (b) to the content of the perfluoropolyether (c) is 0.5 to 4.
6. The curable composition according to claim 1 , further comprising: (e) a solvent.
7. A cured film obtained from the curable composition according to any one of claims 1 to 6.
8. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer comprising the cured film according to claim 7.
9. 7. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer being formed by a method including the steps of: applying the curable composition according to claim 1 onto a film substrate to form a coating film; and irradiating the coating film with active energy rays to cure the coating film.
10. 7. A hard coat film comprising a hard coat layer on at least one surface of a film substrate, the hard coat layer being formed by a method including the steps of: applying the curable composition according to claim 6 onto a film substrate to form a coating film; removing the solvent from the coating film by heating; and irradiating the coating film with active energy rays to cure the coating film.
11. The hard coat film according to claim 8 , wherein the film substrate is made of a plurality of layers.
12. The hard coat film according to claim 8 , wherein the film substrate has a lower layer of the hard coat layer on a surface of a resin film.
13. 13. The hard coat film according to claim 8, wherein the hard coat layer has a thickness of 1 μm to 20 μm.
14. The method includes the steps of applying the curable composition according to any one of claims 1 to 6 onto a film substrate to form a coating film, and irradiating the coating film with active energy rays to cure the coating film. A method for producing a laminate of a film substrate and a hard coat layer.
15. The method for producing a laminate according to claim 14, wherein the film substrate is made of a plurality of layers.
16. The method for producing a laminate according to claim 14 or 15, wherein the film substrate has a lower layer of the hard coat layer on a surface of a resin film.
17. A surface modifier comprising: a perfluoropolyether compound having a molecular weight of 1000 or more and having a group represented by the following formula [1], formula [2] or formula [3] at each end of a molecular chain containing a poly(oxyperfluoroalkylene) group, and a perfluoropolyether compound (excluding perfluoropolyether compounds having a molecular weight of 1000 or more) having an active energy ray-polymerizable group at an end of a molecular chain containing a poly(oxyperfluoroalkylene) group having a structure represented by the following formula [4] or formula [5]: 【Chemistry 3】 (In the above formulas [1], [2] and [3], R 1 represents a trifluoromethyl group, a fluoro group, a trifluoromethoxy group or a nitro group; when R 1 represents a trifluoromethyl group, a trifluoromethoxy group or a nitro group, m represents an integer of 1 to 5; when R 1 represents a fluoro group, m represents an integer of 2 to 5; R 2 represents a methyl group or a methoxy group; n represents 1, 2 or 3; R 3 represents an alkyl group having 3 to 10 carbon atoms; and * represents a bond to a molecular chain containing a poly(oxyperfluoroalkylene) group of the (c) perfluoropolyether.) 【Chemistry 4】 (In the above formula [4] and formula [5], p represents a repeating unit -[CF 2 CF 2 O]- and the number of repetitions Repeat unit - [CF 2 The total number of the repeating units -[CF 2 CF 2 O]- and the repeating unit -[CF 2 O]- is bonded via a block bond, a random bond, or a block bond and a random bond, and q is the number of oxyethylene groups and represents an integer of 0 to 10.
18. The surface modifier described in claim 17, wherein a molecular chain containing a poly(oxyperfluoroalkylene) group of the perfluoropolyether compound having a molecular weight of 1,000 or more has a structure represented by formula [4] or formula [5].
19. A surface modifier described in claim 17 or claim 18, wherein the perfluoropolyether compound having a molecular weight of 1,000 or more does not have the active energy ray-polymerizable group.
Citation Information
Patent Citations
Sperm injection method to pig and sperm injector for pig
JP1989097449A
Primer composition
JP2004331704A
Curable resin composition
JP2012241060A
Polyurethane resins from hydroxy terminated perfluoro ethers
US3671497A
Wash-out resistant underwater grease
US9441183B1