Copolymer, method for producing acrylic rubber, and acrylic rubber
A copolymer with thermally decomposable and crosslinkable monomers, heat-treated at 70 to 250°C, addresses the issue of uniform functional group distribution in acrylic rubber, enhancing mechanical properties and fatigue resistance for automotive applications.
Patent Information
- Application Number
- JP2023093326
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2038-05-31
AI Technical Summary
Existing acrylic rubber compositions face challenges in achieving uniform distribution of crosslinkable functional groups, leading to deteriorated mechanical properties, compression set, and bending fatigue resistance, which are critical for high-performance automotive applications.
Incorporating a specific copolymer containing a thermally decomposable monomer unit, such as tert-butyl acrylate or tert-butyl 2-ethyl acrylate, along with a crosslinkable monomer unit having functional groups like carboxy or epoxy groups, and heat-treating the copolymer at 70 to 250°C to generate crosslinking sites, thereby improving mechanical properties and fatigue resistance.
The method results in acrylic rubber with enhanced mechanical properties, compression set of 27% or less, and bending fatigue resistance of 1.3 million cycles or more, suitable for automotive rubber hoses and seals.
Smart Images

Figure 0007569537000001 
Figure 0007569537000002 
Figure 0007569537000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer, a method for producing an acrylic rubber, an acrylic rubber, an acrylic rubber composition, a vulcanizate of the acrylic rubber composition, and uses of the vulcanizate. [Background technology]
[0002] Acrylic rubber and its vulcanizates have excellent physical properties such as heat aging resistance, oil resistance, mechanical properties and compression set properties, and are therefore widely used as materials for hose components and seal components in the engine compartments of automobiles, where heat resistance is required.
[0003] However, in recent years, against the backdrop of higher performance in automobiles, the characteristics required for acrylic rubber parts have become increasingly strict, and there is a strong demand for improved physical properties of acrylic rubber, such as flex fatigue resistance for hose applications and compression set for sealing applications.
[0004] Acrylic rubber is usually used by imparting rubber elasticity through cross-linking, and for this purpose cross-linking monomers having cross-linkable functional groups are copolymerized. The cross-linkable functional groups mainly used are epoxy groups, carboxy groups, active chlorine groups, etc., and are used according to the characteristics.
[0005] (Meth)acrylic acid monomers, which are cross-linking monomers with good copolymerizability with (meth)acrylic acid ester monomers, the main component of acrylic rubber, are highly water-soluble and it is difficult for them to react sufficiently in the semi-batch emulsion polymerization commonly used in the production of acrylic rubber.
[0006] Since uneven distribution of crosslinkable functional groups is a factor in reducing mechanical properties, compression set, and flex fatigue resistance, improvements are required.
[0007] For example, Patent Document 1 and Non-Patent Document 1 disclose pressure sensitive adhesives in which tert-butyl acrylate monomers are copolymerized, followed by a thermal modification reaction to generate carboxyl groups, thereby changing the adhesive properties. Tert-butyl acrylate monomers have good copolymerizability with (meth)acrylic acid ester monomers, and it is believed that the use of this monomer can achieve a uniform distribution of crosslinkable functional groups. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Special Publication No. 2006-511640 [Non-patent literature]
[0009] [Non-Patent Document 1] Shoichi Matsumoto, "Synthesis of degradable polymers by radical polymerization and design of dismantlable adhesive materials", Journal of the Adhesion Society of Japan, Japan Adhesion Society, 2014, Vol. 50, No. 3, pp. 72-81 Summary of the Invention [Problem to be solved by the invention]
[0010] The main object of the present invention is to provide an acrylic rubber having excellent mechanical properties, compression set and flex fatigue resistance. [Means for solving the problem]
[0011] As a result of intensive research into achieving the above object, the inventors have discovered that the above object can be achieved by using a specific copolymer containing a thermally decomposable monomer unit in a production method for acrylic rubber, and have thus completed the present invention.
[0012] That is, the present invention provides a copolymer containing (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units), at least one of tert-butyl (meth)acrylate monomer units and tert-butyl 2-ethylacrylate monomer units as thermally decomposable monomer units, and a crosslinkable monomer unit having a crosslinkable functional group, in which the thermally decomposable monomer units are 0.1 to 10 parts by mass and the crosslinkable monomer units are 5 parts by mass or less per 100 parts by mass of the (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units). The copolymer may contain an ethylene monomer unit, and the ethylene monomer unit in the copolymer may be 0.1 to 10 parts by mass per 100 parts by mass of the (meth)acrylic acid ester monomer unit (excluding tert-butyl (meth)acrylate monomer unit). The crosslinkable monomer unit may have, as the crosslinkable functional group, at least one selected from a carboxy group, an epoxy group, and a halogen group. The present invention provides a method for producing an acrylic rubber, comprising the step of heat-treating the copolymer at 70 to 250°C. In the above production method, the heat treatment may be carried out in the presence of an acid catalyst having an acid dissociation constant (pKa) in water at 25° C. of 5 to −10. The acid catalyst may be p-toluenesulfonic acid. The present invention provides an acrylic rubber produced by the above-mentioned production method. The present invention provides an acrylic rubber composition containing 100 parts by mass of the acrylic rubber and 30 to 80 parts by mass of carbon black. The present invention provides a vulcanizate obtained by vulcanizing the acrylic rubber composition, which has a compression set of 27% or less and a flex fatigue resistance of 1.3 million or more cycles. The present invention provides a rubber hose using the vulcanizate. The present invention provides a sealing part using the vulcanizate. Effect of the Invention
[0013] According to the present invention, it is possible to obtain an acrylic rubber having excellent mechanical properties, compression set and resistance to flex fatigue. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below, but the present invention is not limited to the embodiments shown below.
[0015] In the method for producing an acrylic rubber according to the present embodiment, a copolymer containing (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units) and at least one of tert-butyl (meth)acrylate monomer units and tert-butyl 2-ethylacrylate monomer units as thermally decomposable monomer units is heat-treated at 70 to 250°C to thermally decompose the thermally decomposable monomer units to generate crosslinking units having a carboxy group, thereby producing an acrylic rubber. The copolymer may further contain a crosslinking monomer unit having a crosslinkable functional group.
[0016] <Copolymer> The (meth)acrylic acid ester monomer becomes the backbone of the acrylic rubber, and is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers and (meth)acrylic acid alkoxyalkyl ester monomers.
[0017] The (meth)acrylic acid alkyl ester monomer is not particularly limited, but examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-methylpentyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Among these (meth)acrylic acid alkyl ester monomers, (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 1 to 8 carbon atoms are preferred, methyl (meth)acrylate, ethyl (meth)acrylate, and n-butyl (meth)acrylate are more preferred, and ethyl acrylate and n-butyl acrylate are particularly preferred. These may be used alone or in combination of two or more.
[0018] The (meth)acrylic acid alkoxyalkyl ester monomer is not particularly limited, but examples thereof include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 2-(2-ethoxyethoxy)ethyl (meth)acrylate. Among these (meth)acrylic acid alkoxyalkyl ester monomers, (meth)acrylic acid alkoxyalkyl ester monomers having a linear alkoxyalkyl group having 2 to 8 carbon atoms are preferred, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, and 2-(2-ethoxyethoxy)ethyl (meth)acrylate are more preferred, and 2-methoxyethyl acrylate and 2-(2-ethoxyethoxy)ethyl acrylate are particularly preferred. These may be used alone or in combination of two or more.
[0019] The content of the (meth)acrylic acid ester monomer unit is preferably 50 to 99.9 mass%, more preferably 60 to 99.5 mass%, and particularly preferably 70 to 99 mass%, based on 100 mass% of the copolymer. By setting the content of the (meth)acrylic acid ester monomer unit within the above range, the heat resistance and oil resistance of the obtained acrylic rubber vulcanizate can be made more excellent.
[0020] The thermally decomposable monomer unit includes at least one of a tert-butyl (meth)acrylate monomer unit and a tert-butyl 2-ethylacrylate monomer unit. The thermally decomposable monomer unit generates a carboxyl group, which is a crosslinkable functional group that enables intermolecular crosslinking of acrylic rubber, by heat treatment at 70 to 250°C. This intermolecular crosslinking can adjust the hardness and elongation properties of the obtained acrylic rubber vulcanizate. In addition, this thermally decomposable monomer has excellent copolymerizability with a (meth)acrylic acid ester monomer, and by uniformly disposing the crosslinkable functional groups in the acrylic rubber molecule, the mechanical properties, compression set, and flex fatigue resistance of the obtained acrylic rubber vulcanizate can be made excellent. These may be used alone or in combination of two or more types.
[0021] The total content of the thermally decomposable monomer units in the copolymer is 0.1 to 10 parts by mass relative to 100 parts by mass of the (meth)acrylic acid ester monomer units (excluding the (meth)acrylate tert-butyl monomer units). The upper limit of the total content of the thermally decomposable monomer units is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 2 parts by mass or less. The lower limit of the total content of the thermally decomposable monomer units is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, even more preferably 0.4 parts by mass or more, and particularly preferably 0.5 parts by mass or more. By setting the total content of the thermally decomposable monomer units within the above range, scorching during processing in a state where a vulcanizing agent or the like is added can be suppressed, and the mechanical properties of the obtained acrylic rubber vulcanizate can be made excellent.
[0022] The copolymer preferably further contains a crosslinkable monomer unit having a crosslinkable functional group, which enables intermolecular crosslinking of the resulting acrylic rubber.
[0023] The crosslinkable functional group is not particularly limited, but examples thereof include an epoxy group, a carboxy group, a halogen group, an amino group, a hydroxyl group, a phenol group, a hydrazide group, and an unsaturated carbon bond group. Among these crosslinkable functional groups, an epoxy group, a carboxy group, and a halogen group are preferred, and a carboxy group is more preferred. The crosslinkable monomer having these crosslinkable functional groups may be used alone or in combination of two or more types.
[0024] The crosslinking monomer having a carboxy group is a monomer copolymerizable with a (meth)acrylic acid ester monomer. Examples include carboxylic acid monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid; carboxylic acid ester monomers such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, monomethyl maleate, monoethyl maleate, mono-n-butyl maleate, monomethyl fumarate, monoethyl fumarate, and mono-n-butyl fumarate; and carboxylic acid anhydride monomers such as maleic anhydride having a carboxylic acid anhydride group; and the like. Among these crosslinking monomers having a carboxy group, carboxylic acid ester monomers are preferred, butenedioic acid monoester monomers such as fumaric acid monoester and maleic acid monoester are more preferred, maleic acid monoalkyl ester monomers are even more preferred, and maleic acid monobutyl is particularly preferred.
[0025] The crosslinking monomer having a halogen group is a monomer that can be copolymerized with the (meth)acrylic acid ester monomer. For example, it can include unsaturated alcohol esters of halogen-containing saturated carboxylic acids such as vinyl chloroacetate, allyl chloroacetate, vinyl fluoroacetate, and allyl fluoroacetate; halogen-containing unsaturated ethers such as chloromethyl vinyl ether, 2-chloroethyl vinyl ether, and 2-fluoroethyl vinyl ether; halogen-containing aromatic vinyls such as p-chlorostyrene, p-fluorostyrene, and vinylbenzyl chloride; halogen-containing (meth)acrylic acid esters such as trifluoromethyl (meth)acrylate and trifluoroethyl 2,2,2-(meth)acrylate; and the like.
[0026] The crosslinking monomer having an epoxy group is a monomer that can be copolymerized with the (meth)acrylic acid ester monomer. For example, unsaturated glycidyl esters such as glycidyl (meth)acrylate, unsaturated glycidyl ethers such as vinyl glycidyl ether and allyl glycidyl ether, etc. are included. Among these crosslinking monomers having an epoxy group, unsaturated glycidyl esters are preferred, and glycidyl methacrylate is more preferred.
[0027] The total content of the crosslinking monomer units in the copolymer is 0% by mass or more and 5 parts by mass or less, based on 100 parts by mass of the (meth)acrylic acid ester monomer units (excluding the (meth)acrylate tert-butyl monomer units). The upper limit of the total content of the crosslinking monomer units is preferably 4.7 parts by mass or less, more preferably 4.5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 3 parts by mass or less. The lower limit of the total content of the crosslinking monomer units is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.3 parts by mass or more, and particularly preferably 0.5 parts by mass or more. By setting the crosslinking monomer units in the above range, scorching during processing in a state where a vulcanizing agent or the like is added can be suppressed, and the mechanical properties of the obtained acrylic rubber vulcanizate can be made excellent.
[0028] In order to improve the mechanical properties of the obtained acrylic rubber vulcanizate, the copolymer preferably contains an ethylene monomer unit. The content of the ethylene monomer unit in the copolymer is preferably 10 parts by mass or less relative to 100 parts by mass of the (meth)acrylic acid ester monomer unit (excluding the (meth)acrylate tert-butyl monomer unit). The upper limit of the content of the ethylene monomer is more preferably 5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 3 parts by mass or less. The lower limit of the content of the ethylene monomer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. By setting the content of the ethylene monomer unit in the copolymer within this numerical range, an acrylic rubber composition having improved elongation and cold resistance of the vulcanizate can be obtained.
[0029] The above copolymer may contain other monomers copolymerizable with the (meth)acrylic acid ester monomer and the crosslinking monomer, as long as the object of the present invention is not impaired. Examples of other copolymerizable monomers include, but are not limited to, alkyl vinyl ketones such as vinyl acetate and methyl vinyl ketone; vinyl and allyl ethers such as vinyl ethyl ether and allyl methyl ether; vinyl aromatic compounds such as styrene, α-methylstyrene, vinyl toluene, and vinyl naphthalene; ethylenically unsaturated compounds such as vinyl nitriles such as acrylonitrile and methacrylonitrile, acrylamide, propylene, butadiene, isoprene, pentadiene, vinyl propionate, maleic acid diesters such as dimethyl maleate, fumaric acid dialkyl esters such as dimethyl fumarate, itaconic acid dialkyl esters such as dimethyl itaconate, citraconic acid dialkyl esters such as dimethyl citraconic acid, mesaconic acid dialkyl esters such as dimethyl mesaconic acid, 2-pentenedioic acid dialkyl esters such as dimethyl 2-pentenedioic acid, and acetylenedicarboxylic acid dialkyl esters such as dimethyl acetylenedicarboxylate. These may be used alone or in combination of two or more. In the copolymer, the content of other monomer units copolymerizable with the (meth)acrylic acid ester monomer and the crosslinking monomer is preferably 40 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units).
[0030] The copolymer is obtained by copolymerizing a (meth)acrylic acid ester monomer, a thermally decomposable monomer, a crosslinkable monomer having a crosslinkable functional group, and another monomer copolymerizable therewith, which is used as necessary. As the form of the polymerization reaction, any of emulsion polymerization, suspension polymerization, bulk polymerization, and solution polymerization can be used. From the viewpoint of ease of control of the polymerization reaction, polymerization by emulsion polymerization, which is generally used as a method for producing conventionally known acrylic rubber, is preferred.
[0031] In the case of polymerization by emulsion polymerization, a conventional method may be used. As the polymerization initiator, polymerization terminator, emulsifier, etc., conventionally known ones that are generally used may be used.
[0032] Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile; organic peroxides such as diisopropylbenzene hydroperoxide, cumene hydroperoxide, and benzoyl peroxide; and inorganic peroxides such as sodium persulfate and ammonium persulfate. These polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.01 to 1.0 part by mass relative to 100 parts by mass of the total monomers used in the polymerization.
[0033] The peroxide initiator can be used as a redox polymerization initiator in combination with a reducing agent. The reducing agent is not particularly limited, but includes compounds containing reduced metal ions such as ferrous sulfate and cuprous naphthenate; sulfonic acid compounds such as sodium methanesulfonate; and amine compounds such as dimethylaniline. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 0.03 to 10 parts by mass relative to 1 part by mass of the peroxide initiator.
[0034] Examples of the polymerization terminator include hydroxylamine, hydroxylamine sulfate, diethylhydroxyamine, hydroxylamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, etc. The amount of the polymerization terminator used is not particularly limited, but is preferably 0.1 to 2 parts by mass relative to 100 parts by mass of the total monomers used in the polymerization.
[0035] Examples of emulsifiers include nonionic emulsifiers such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, polyoxyethylene alkyl ether, polyoxyethylene alkylphenol ether, polyoxyethylene alkyl ester, and polyoxyethylene sorbitan alkyl ester; salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; anionic emulsifiers such as higher alcohol sulfates and alkyl sulfosuccinates; cationic emulsifiers such as alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride; and copolymerizable emulsifiers such as sulfoesters of α,β-unsaturated carboxylic acids, sulfate esters of α,β-unsaturated carboxylic acids, and sulfoalkylaryl ethers. Among these, partially saponified polyvinyl alcohol is preferred. These emulsifiers may be used alone or in combination of two or more. The amount of emulsifier used is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the total monomers used in the polymerization.
[0036] The amount of water used is preferably 80 to 500 parts by mass, and more preferably 100 to 300 parts by mass, based on 100 parts by mass of all the monomers used in the polymerization.
[0037] In the emulsion polymerization, polymerization auxiliary materials such as a molecular weight regulator, a particle size regulator, a chelating agent, an oxygen scavenger, etc. may be used, if necessary.
[0038] Examples of the molecular weight regulator include mercaptans such as n-butyl mercaptan and t-dodecyl mercaptan; sulfides such as tetraethylthiuram sulfide and dipentamethylenethiuram hexasulfide; α-methylstyrene dimer; and carbon tetrachloride.
[0039] The emulsion polymerization may be any of a batch system, a semi-batch system, and a continuous system. The polymerization is preferably carried out in the temperature range of 0 to 80°C, more preferably 20 to 70°C.
[0040] <Acrylic rubber manufacturing method> The method for producing an acrylic rubber according to the present embodiment includes a step of heat-treating the copolymer, whereby the heat-decomposable monomer units are thermally decomposed to generate crosslinking site units having a carboxy group.
[0041] The copolymer to be heat-treated may be in the form of a rubber emulsion, a rubber solution, or a rubber. The heat treatment temperature is 70 to 250°C, preferably 70 to 230°C, and more preferably 75 to 200°C. The heat treatment time is preferably 5 minutes or more, more preferably 5 minutes to 4 hours, and even more preferably 10 minutes to 2 hours. By carrying out the heat treatment step, the mechanical properties of the obtained acrylic rubber vulcanizate can be made excellent.
[0042] In addition, the heat treatment time can be shortened by using an acid catalyst in the heat treatment step. The acid catalyst is preferably an acid catalyst having an acid dissociation constant (pKa) of 5 to -10 in water at 25°C, more preferably an acid catalyst having a pKa of 0 to -9, and even more preferably an acid catalyst having a pKa of -1 to -5. Here, pKa is a value defined by the formula: pKa = -log10Ka (Ka is an acid dissociation constant). For an acid compound containing an acid catalyst, the pKa can be calculated from its molecular structure.
[0043] The acid catalyst having a pKa in the range of 5 to -10 is not particularly limited, and examples thereof include carboxylic acids such as acetic acid, benzoic acid, and trifluoroacetic acid; sulfonic acids such as trifluoromethanesulfonic acid, sulfuric acid, monoalkylbenzenesulfonic acid, dialkylbenzenesulfonic acid, trialkylbenzenesulfonic acid, and alkylnaphthalenesulfonic acid; inorganic acids such as phosphoric acid, hydrochloric acid, aluminum silicate, and zeolite; and phenol. These acid catalysts can be used alone or in combination of two or more. Among these, sulfonic acids and carboxylic acids are preferred, monoalkylbenzenesulfonic acid is more preferred, and p-toluenesulfonic acid is particularly preferred. By using these acid catalysts, it is possible to efficiently proceed with the decomposition reaction of the thermally decomposable monomer unit in the heat treatment step, thereby shortening the heat treatment time.
[0044] The upper limit of the amount of the acid catalyst having a pKa of 5 to -10 added is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the copolymer. The lower limit of the amount of the acid catalyst added is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the copolymer. By setting the amount of the acid catalyst added within this range, the heat treatment time can be efficiently shortened.
[0045] <Acrylic rubber> The acrylic rubber of this embodiment is produced by the above-mentioned production method. That is, the acrylic rubber of this embodiment is obtained by heat treating the above-mentioned copolymer at 70 to 250° C. The acrylic rubber contains crosslinking site units having a carboxy group, which are generated by thermally decomposing the above-mentioned thermally decomposable monomer units.
[0046] The upper limit of the carboxyl group content in the acrylic rubber is preferably 10% by mass or less, more preferably 5% by mass or less, based on 100% by mass of the acrylic rubber. The lower limit of the carboxyl group content is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, based on 100% by mass of the acrylic rubber.
[0047] <Acrylic rubber composition> The acrylic rubber composition of the present embodiment includes the acrylic rubber and carbon black. By using the acrylic rubber, the mechanical properties and heat resistance of the obtained acrylic rubber vulcanizate can be improved. The carbon black is not particularly limited, but examples thereof include acetylene black, ketjen black, thermal black, channel black, furnace black, lamp black, and graphitized carbon black. In order to further improve the mechanical properties and heat resistance, among these carbon blacks, furnace black and acetylene black are preferred, and furnace black is more preferred.
[0048] The content of the carbon black in the acrylic rubber composition is preferably 30 to 80 parts by mass, more preferably 40 to 75 parts by mass, and further preferably 45 to 70 parts by mass, relative to 100 parts by mass of the acrylic rubber. By setting the carbon black content within the above range, it is possible to obtain an acrylic rubber composition having a good balance between tensile strength and elongation at break and excellent mechanical properties.
[0049] The acrylic rubber composition may further contain a vulcanizing agent and a vulcanization accelerator.
[0050] The vulcanizing agent may be appropriately selected depending on the type of crosslinking monomer contained in the acrylic rubber and the molding application of the acrylic rubber composition, and is not particularly limited as long as it can crosslink the above-mentioned acrylic rubber. As such a vulcanizing agent, for example, a conventionally known vulcanizing agent such as a polyamine compound such as a diamine compound and its carbonate, sulfur, a sulfur donor, a triazine thiol compound, a polyepoxy compound, an organic carboxylic acid ammonium salt, a dithiocarbamic acid metal salt, a polycarboxylic acid, a quaternary onium salt, an imidazole compound, an isocyanuric acid compound, or an organic peroxide may be used. These vulcanizing agents may be used alone or in combination of two or more.
[0051] The acrylic rubber that is the raw material of the acrylic rubber composition according to the present embodiment contains a carboxyl group generated by heat-treating the thermally decomposable monomer unit, and therefore, the vulcanizing agent is preferably a polyamine compound or a carbonate thereof.
[0052] The polyamine compounds and carbonates of polyamine compounds are not particularly limited, but include aliphatic polyamine compounds and carbonates thereof, and aromatic polyamine compounds, etc. Among these, aliphatic polyamine compounds and carbonates thereof are particularly preferred.
[0053] The aliphatic polyamine compound and its carbonate are not particularly limited, but examples thereof include hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine. Among these, hexamethylenediamine carbamate is preferred.
[0054] The aromatic polyvalent amine compound is not particularly limited, but examples thereof include 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, and 1,3,5-benzenetriamine. Among these, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane is preferred.
[0055] In addition, when the acrylic rubber contains an epoxy group, the vulcanizing agent may be an aliphatic polyamine compound such as hexamethylenediamine or hexamethylenediamine carbamate, or a carbonate thereof; an aromatic polyamine compound such as 4,4'-methylenedianiline; an ammonium carboxylate such as ammonium benzoate or ammonium adipate; a metal dithiocarbamate such as zinc dimethyldithiocarbamate; a polycarboxylic acid such as tetradecanoic acid; a quaternary onium salt such as cetyltrimethylammonium bromide; an imidazole compound such as 2-methylimidazole; or an isocyanuric acid compound such as ammonium isocyanurate. Among these, ammonium carboxylate and metal dithiocarbamate are preferred, and ammonium benzoate is more preferred.
[0056] When the acrylic rubber contains a halogen group, the vulcanizing agent is preferably sulfur, a sulfur donor or a triazine thiol compound.
[0057] Specific examples of sulfur donors include dipentamethylene thiuram hexasulfide and triethylthiuram disulfide.
[0058] Specific examples of triazine thiol compounds include 1,3,5-triazine-2,4,6-trithiol, 6-anilino-1,3,5-triazine-2,4-dithiol, 6-dibutylamino-1,3,5-triazine-2,4-dithiol, 6-diallylamino-1,3,5-triazine-2,4-dithiol, and 6-octylamino-1,3,5-triazine-2,4-dithiol. Among these, 1,3,5-triazine-2,4,6-trithiol is preferred.
[0059] The content of the vulcanizing agent is not particularly limited, but is preferably 0.1 to 10 parts by mass, and more preferably 0.3 to 5 parts by mass, relative to 100 parts by mass of the acrylic rubber. By setting it within this range, necessary and sufficient vulcanization treatment can be performed.
[0060] When the acrylic rubber composition of the present embodiment contains a vulcanizing agent, the acrylic rubber composition preferably further contains a vulcanization accelerator. The vulcanization accelerator is added to adjust the vulcanization rate. The vulcanization accelerator is not particularly limited, but examples thereof include aliphatic monovalent secondary amine compounds, aliphatic monovalent tertiary amine compounds, guanidine compounds, imidazole compounds, quaternary onium salts, tertiary phosphine compounds, alkali metal salts of weak acids, and diazabicycloalkene compounds. Among these, diazabicycloalkene compounds are preferred.
[0061] The amount of the vulcanization accelerator added may be set within a range that does not impair the properties of the vulcanizate obtained from the acrylic rubber composition of the present embodiment.
[0062] The aliphatic monovalent secondary amine compound is a compound in which two hydrogen atoms of ammonia are replaced with an aliphatic hydrocarbon group. The aliphatic hydrocarbon group replacing the hydrogen atom is not particularly limited, but preferably has 1 to 30 carbon atoms, more preferably has 8 to 20 carbon atoms. Specific examples of the aliphatic monovalent secondary amine compound include dimethylamine, diethylamine, di-n-propylamine, diallylamine, diisopropylamine, di-n-butylamine, di-t-butylamine, di-sec-butylamine, dipentylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, diundecylamine, didodecylamine, ditridecylamine, ditetradecylamine, dipentadecylamine, dicetylamine, di-2-ethylhexylamine, dioctadecylamine, di-cis-9-octadecenylamine, and dinonadecyamine.
[0063] The aliphatic monovalent tertiary amine compound is a compound in which all three hydrogen atoms of ammonia are substituted with an aliphatic hydrocarbon group. The aliphatic hydrocarbon group substituting the hydrogen atom is not particularly limited, but is preferably one having 1 to 30 carbon atoms, and more preferably one having 1 to 22 carbon atoms. Specific examples of the aliphatic monovalent tertiary amine compound include trimethylamine, triethylamine, tri-n-propylamine, triallylamine, triisopropylamine, tri-n-butylamine, tri-t-butylamine, tri-sec-butylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, triundecylamine, tridodecylamine, tridecylamine, tritetradecylamine, tripentadecylamine, tricetylamine, tri-2-ethylhexylamine, ...ethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, triethylamine, tri Examples of the amines include thioctadecylamine, tri-cis-9-octadecenylamine, trinonadecylamine, N,N-dimethyldecylamine, N,N-dimethyldodecylamine, N,N-dimethyltetradecylamine, N,N-dimethylcetylamine, N,N-dimethyloctadecylamine, N,N-dimethylbehenylamine, N-methyldidecylamine, N-methyldidodecylamine, N-methylditetradecylamine, N-methyldicetylamine, N-methyldioctadecylamine, N-methyldibehenylamine, and dimethylcyclohexylamine.
[0064] Specific examples of the guanidine compound include 1,3-di-o-tolylguanidine and 1,3-diphenylguanidine.
[0065] Specific examples of the imidazole compound include 2-methylimidazole and 2-phenylimidazole.
[0066] Specific examples of quaternary onium salts include tetra-n-butylammonium bromide and octadecyltri-n-butylammonium bromide.
[0067] Specific examples of the tertiary phosphine compound include triphenylphosphine and tri-p-tolylphosphine.
[0068] Specific examples of alkali metal salts of weak acids include inorganic weak acid salts such as sodium or potassium phosphate or carbonate; and organic weak acid salts such as sodium or potassium stearate or laurate.
[0069] Specific examples of the diazabicycloalkene compound include 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) and 1,5-diazabicyclo[4.3.0]non-5-ene (DBN).
[0070] When sulfur is used as a vulcanizing agent, it is preferable to use an alkali metal carboxylate or a thiazole compound as a vulcanization accelerator. Examples of the alkali metal carboxylate include sodium stearate, potassium stearate, sodium laurate, and potassium laurate. Examples of the thiazole compound include mercaptobenzothiazole and dibenzothiazyl disulfide.
[0071] When a triazine thiol compound is used as a vulcanizing agent, it is preferable to use a thiuram-based accelerator or a dithiocarbamate-based accelerator as a vulcanization accelerator. Examples of the thiuram-based accelerator include tetraethyl thiuram disulfide and tetrabutyl thiuram disulfide. As the dithiocarbamate-based accelerator, at least one selected from zinc salts, copper salts, iron salts and tellurium salts of dithiocarbamic acids is preferable, zinc salts are more preferable, and zinc diethyldithiocarbamate and zinc dibutyldithiocarbamate are even more preferable.
[0072] The acrylic rubber composition of the present embodiment may contain a filler, a reinforcing agent, a plasticizer, a lubricant, an antioxidant, a stabilizer, a silane coupling agent, and the like depending on the purpose of practical use.
[0073] The filler and reinforcing agent may be any filler and reinforcing agent that is used in ordinary rubber applications other than carbon black, such as silica, talc, calcium carbonate, etc. The total content of the filler and reinforcing agent is preferably within the range of 20 to 100 parts by mass per 100 parts by mass of the acrylic rubber composition.
[0074] The plasticizer may be any one that is commonly used in rubber applications, such as ester-based plasticizers, polyoxyethylene ether-based plasticizers, trimellitate-based plasticizers, etc. The content of the plasticizer is preferably 50 parts by mass or less per 100 parts by mass of the acrylic rubber composition.
[0075] The antiaging agent may be any agent used in ordinary rubber applications, such as amine-based antiaging agents such as 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, N,N'-di-2-naphthyl-p-phenylenediamine, and N-phenyl-N'-isopropyl-p-phenylenediamine; phenol-based antiaging agents such as 2,5-di-tert-butylhydroquinone and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]; sulfur-based antiaging agents such as 2-mercaptobenzimidazole; and phosphorus-based antiaging agents such as tris(nonylphenyl)phosphite. The content of the antiaging agent is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the acrylic rubber composition.
[0076] The acrylic rubber composition of the present embodiment may further contain a polymer other than the acrylic rubber described above, as long as the effect of the present invention is not impaired. Examples of the polymer other than the acrylic rubber include rubbers such as acrylic rubbers other than the acrylic rubbers, natural rubbers, polybutadiene rubbers, polyisoprene rubbers, styrene-butadiene rubbers, acrylonitrile-butadiene rubbers, silicone rubbers, and fluororubbers; and resins such as polyester polyolefin resins, polystyrene resins, polyphenylene ether resins, polyester resins, polycarbonate resins, polyamide resins, vinyl chloride resins, and fluororesins. The amount of the polymer other than the acrylic rubber is preferably 50 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 1 part by mass or less, relative to 100 parts by mass of the acrylic rubber.
[0077] The method for producing the acrylic rubber composition of the present embodiment is not particularly limited. For example, the acrylic rubber and each component except for the vulcanizing agent and the thermally unstable vulcanizing aid are kneaded in a mixer such as a Banbury mixer, a Brabender mixer, an intermixer, or a kneader at preferably 10 to 200°C, more preferably 20 to 170°C, and then transferred to a roll or the like to add the vulcanizing agent and the thermally unstable vulcanizing aid, and then secondary kneading is performed preferably under the condition of 10 to 80°C to produce the composition.
[0078] <Vulcanizate of acrylic rubber composition> The vulcanizate of the acrylic rubber composition according to this embodiment is obtained by vulcanizing the above-mentioned acrylic rubber composition.
[0079] The vulcanizate of the acrylic rubber composition according to the present embodiment is produced by using the above acrylic rubber composition, for example, molding the composition into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, or a roll, and then heating the composition to perform a vulcanization reaction (primary vulcanization) and fix the shape as a vulcanizate. In this case, the composition may be vulcanized after molding in advance, or may be vulcanized simultaneously with molding. The molding temperature is preferably 10 to 200°C, more preferably 25 to 120°C. The vulcanization temperature is preferably 100 to 200°C, more preferably 130 to 190°C. The vulcanization time is preferably 1 minute to 24 hours, more preferably 2 minutes to 12 hours, and particularly preferably 3 minutes to 6 hours.
[0080] Depending on the shape, size, etc. of the vulcanizate, the inside may not be sufficiently vulcanized even if the surface is vulcanized, so secondary vulcanization may be performed by further heating.
[0081] As the vulcanization method, a general method used for vulcanizing rubber, such as steam vulcanization, press vulcanization, or oven vulcanization, can be appropriately selected.
[0082] The vulcanizate of the acrylic rubber composition according to the present embodiment preferably has a compression set of 27% or less when heated for 22 hours at 150° C. in accordance with JIS K6262: 2013. Such a vulcanizate of the acrylic rubber composition is suitable for use in sealing parts.
[0083] The vulcanizate of the acrylic rubber composition according to the present embodiment preferably has a flex fatigue number of 1.3 million or more until cracks occur, as measured in accordance with JIS K6260: 2010. Such a vulcanizate of the acrylic rubber composition is suitable for rubber hoses and seal parts.
[0084] The vulcanizate of the acrylic rubber composition according to the present embodiment is suitably used as a rubber hose and sealing parts such as a gasket and packing. The rubber hose and sealing parts may consist of only the vulcanizate of the acrylic rubber composition, or may be combined with other parts.
[0085] Examples of rubber hoses include transmission oil cooler hoses, engine oil cooler hoses, air duct hoses, turbo intercooler hoses, hot air hoses, radiator hoses, power steering hoses, fuel system hoses, and drain system hoses for automobiles, construction machinery, hydraulic equipment, and the like.
[0086] The rubber hose may be configured in such a way that reinforcing threads or wires are provided in the middle of the hose or in the outermost layer of the rubber hose, as is commonly done, or may have a laminated structure with rubber such as fluororubber or silicone rubber.
[0087] Examples of sealing parts include engine head cover gaskets, oil pan gaskets, oil seals, lip seal packings, O-rings, transmission seal gaskets, crankshafts, camshaft seal gaskets, valve stems, power steering seal belt cover seals, constant velocity joint boot materials, and rack and pinion boot materials. EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0089] A rubber-like copolymer was prepared under the conditions shown below. <Copolymer A> In a pressure-resistant reaction vessel with an internal volume of 40 liters, 17 kg of a 4% by mass aqueous solution of partially saponified polyvinyl alcohol, 22 g of sodium acetate, 56 g of ascorbic acid, 1.12 g of ethylenediaminetetraacetic acid, and 0.56 g of iron (II) sulfate heptahydrate were charged, and the air in the upper part of the vessel was replaced with nitrogen while mixing well with a stirrer, and then 0.95 kg of ethylene was forced into the upper part of the vessel, and the pressure was adjusted to 3.5 MPa. Stirring was continued, and the vessel was kept at 55°C, and then a monomer mixture of 7.84 kg of ethyl acrylate, 3.36 kg of n-butyl acrylate, 168 g of tert-butyl acrylate, and 2.7 g of tert-dodecyl mercaptan was forced into the vessel over 6 hours. At the same time, a t-butyl hydroperoxide aqueous solution (0.25% by mass, 2 liters) was forced into the vessel over 6 hours from a separate inlet, and polymerization was carried out until the final polymerization rate reached 95%. To the resulting polymerization solution, an aqueous sodium borate solution (3.5% by mass, 7 liters) was added as a coagulant to solidify the polymer, which was then dehydrated and dried to obtain copolymer A.
[0090] <Copolymer B> Copolymer B was obtained by polymerization in the same manner as copolymer A, except that ethylene was not injected.
[0091] <Copolymer C> Copolymer C was obtained in the same manner as for copolymer A, except that the amount of tert-butyl acrylate was changed to 784 g.
[0092] <Copolymer D> Copolymer D was obtained by the same method as for copolymer A, except that the amount of tert-butyl acrylate was changed to 112 g and 180 g of monobutyl maleate was further added.
[0093] <Copolymer E> Copolymer E was obtained by the same method as for copolymer A, except that the amount of tert-butyl acrylate was changed to 112 g, and 112 g of glycidyl methacrylate was further added.
[0094] <Copolymer F> Copolymer F was obtained in the same manner as for copolymer A, except that tert-butyl acrylate was changed to 205 g of tert-butyl 2-ethylacrylate.
[0095] <Copolymer G> Copolymer G was obtained by the same method as for copolymer A, except that the amount of tert-butyl acrylate was changed to 112 g, and 95 g of tert-butyl 2-ethylacrylate was further added.
[0096] <Copolymer H> Copolymer H was obtained in the same manner as for copolymer A, except that the amount of ethyl acrylate was changed to 10.4 kg and the amount of n-butyl acrylate was changed to 0.8 kg.
[0097] <Copolymer I> Copolymer I was obtained in the same manner as for copolymer A, except that the amount of ethyl acrylate was changed to 2.4 kg and the amount of n-butyl acrylate was changed to 8.9 kg.
[0098] <Copolymer J> Copolymer J was obtained in the same manner as for copolymer A, except that tert-butyl acrylate was replaced with 275 g of monobutyl maleate.
[0099] <Copolymer K> Copolymer K was obtained in the same manner as for copolymer A, except that tert-butyl acrylate was replaced with 224 g of glycidyl methacrylate.
[0100] <Copolymer L> Copolymer L was obtained in the same manner as for copolymer A, except that the amount of tert-butyl acrylate was changed to 1.5 kg.
[0101] <Copolymer M> Copolymer M was obtained by the same method as for copolymer A, except that the amount of tert-butyl acrylate was changed to 112 g and 1,070 g of monobutyl maleate was further added.
[0102] <Acrylic Rubber N> Copolymer N was obtained by the same method as for copolymer A, except that the amount of tert-butyl acrylate was changed to 112 g and 870 g of glycidyl methacrylate was further added.
[0103] <Identification of copolymer composition> The compositions of the obtained copolymers were identified by 13C NMR and are shown in Tables 2 to 4 below.
[0104] <Manufacture of acrylic rubber> The copolymer obtained by the above method was heat-treated at the temperature and time shown in Tables 2 to 4 below using a gear oven (TG-100 manufactured by Suga Test Instruments Co., Ltd.) to produce an acrylic rubber. The obtained acrylic rubber was then left to cool in the air at 23°C for 5 hours. When an acid catalyst shown in Tables 2 to 4 below was added in the heat treatment step, 3% by mass of the acid catalyst was added to the emulsion of the copolymer obtained by the above method before it solidified, and the emulsion was solidified, dehydrated, and dried to obtain the copolymer. The copolymer was then heat-treated according to the procedure described above.
[0105] In addition, with regard to the acid catalysts described in Tables 2 to 4 below, "PTSA" is p-toluenesulfonic acid monohydrate manufactured by Wako Pure Chemical Industries, Ltd., and "TfOH" is trifluoromethanesulfonic acid manufactured by Wako Pure Chemical Industries, Ltd.
[0106] <Measurement of carboxyl group amount> The copolymer before heat treatment and the acrylic rubber after heat treatment were dissolved in toluene, and the amount of carboxyl groups was measured by neutralization titration using potassium hydroxide. The reaction rate of the heat treatment was calculated by dividing the difference in the amount of carboxyl groups before and after heat treatment by the amount of tert-butyl (meth)acrylate monomer units and tert-butyl 2-ethylacrylate monomer units.
[0107] <Production of Acrylic Rubber Composition> The acrylic rubber obtained by the above method was kneaded for 15 minutes in a 0.5 L pressure kneader and then kneaded for 20 minutes using a 6-inch open roll in the composition shown in Table 1 below to produce an acrylic rubber composition. The units of the values shown in Table 1 are "parts by mass".
[0108] [Table 1]
[0109] The reagents used in preparing the acrylic rubber composition are as follows: FEF carbon black: Seast SO manufactured by Tokai Carbon Co., Ltd. Stearic acid: Kao Corporation's Lunac S-90 4,4'-Bis(α,α-dimethylbenzyl)diphenylamine: Addivant's Nauguard 445 (anti-aging agent) Liquid paraffin: Kaneda Hi-Col K-230 Stearylamine: Kao Corporation's Farmin 80 6-Aminohexylcarbamic acid: DuPont Diak#1 (vulcanizing agent) 1,8-Diazabicyclo[5.4.0]undec-7-ene (DBU): LANXESS XLA-60 (vulcanization accelerator) Trimethylthiourea (TMU): Noccela TMU manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 1-Benzyl-2-methylimidazole: Shikoku Chemical Industry Co., Ltd. SB-25 Stearyl trimethylammonium bromide (STB): Catinal STB-100 manufactured by Toho Chemical Industry Co., Ltd.
[0110] <Production of vulcanizate of acrylic rubber composition> The obtained acrylic rubber composition was cut into a sheet having a thickness of 2.4 mm, and then subjected to primary vulcanization at 170°C for 40 minutes in a press vulcanizer, and then secondary vulcanization at 170°C for 4 hours in a Geer oven to produce a vulcanizate.
[0111] <Physical property testing> The scorch time of the obtained acrylic rubber composition, and the tensile strength, elongation at break, hardness, compression set and flex fatigue resistance of the vulcanizate were evaluated under the following conditions, and the measurement results are shown in Tables 2 to 4 below. (1) Scorch Time Measured at 125°C in accordance with JIS K6300:2013. (2) Tensile strength, elongation at break Measurements were performed in accordance with JISK6251:2010. (3)Hardness Measurements were performed using a Type A durometer in accordance with JIS K6253:2012. (4) Compression set Measurements were made in accordance with JIS K6262: 2013. If the compression set when heated at 150°C for 22 hours was within 27%, it was determined that the material was suitable for use in sealing parts. (5) Flexural fatigue resistance (flexural crack initiation test) Measurements were performed in accordance with JIS K6260: 2010. The more times the material can be flexed until cracks appear, the better its resistance to flex fatigue is, and a material that can be flexed more than 1.3 million times is considered suitable for use in rubber hoses and seal parts.
[0112] [Table 2] [Table 3]
[0113] [Table 4]
[0114] As shown in Tables 2 to 4, it was confirmed that the vulcanizate of the acrylic rubber composition according to the present invention has a good balance between tensile strength and elongation at break, and has excellent mechanical properties, and further has excellent compression set and flex fatigue resistance. It was also suggested that the vulcanizate of the acrylic rubber composition is suitable for use in rubber hoses and seals.
[0115] In Comparative Examples 1 and 2, where the heat treatment temperature was 280°C, the copolymer decomposed. In Comparative Examples 3 and 4, where the heat treatment temperature was 50°C, vulcanization did not occur. In Comparative Example 5, where no heat treatment was performed, vulcanization did not occur. For this reason, in Comparative Examples 1 to 5, the desired acrylic rubber composition and its vulcanizate were not obtained. From these results, it was confirmed that the step of heat treating the copolymer at 70 to 250°C is essential.
[0116] In Comparative Examples 6 and 7, which used copolymers not containing a thermally decomposable monomer unit, the compression set and flex fatigue resistance of the vulcanizates were poor. These results confirmed that the thermally decomposable monomer unit is essential.
[0117] Comparative Example 8, which used a copolymer containing more than 10 parts by mass of thermally decomposable monomer units per 100 parts by mass of (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units), had inferior elongation at break, compression set, and flex fatigue resistance of the vulcanizate. This result suggests that the content of thermally decomposable monomer units in the copolymer is preferably 10 parts by mass or less per 100 parts by mass of (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units).
[0118] In Comparative Examples 9 and 10, which used copolymers containing more than 5 parts by mass of crosslinking monomer units per 100 parts by mass of (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units), the elongation at break, compression set and flex fatigue resistance of the vulcanizate were inferior. These results suggested that the content of crosslinking monomer units in the copolymer is preferably 5 parts by mass or less per 100 parts by mass of (meth)acrylic acid ester monomer units (excluding tert-butyl (meth)acrylate monomer units).
Claims
1. The polymerizable composition contains (meth)acrylic acid ester monomer units (excluding (meth)acrylate tert-butyl monomer units), at least one of (meth)acrylate tert-butyl monomer units and 2-ethylacrylate tert-butyl monomer units as thermally decomposable monomer units, and an ethylene monomer unit, A random copolymer, wherein the thermally decomposable monomer unit is 0.1 to 10 parts by mass and the ethylene monomer unit is 0.1 to 10 parts by mass relative to 100 parts by mass of the (meth)acrylic acid ester monomer unit (excluding the (meth)acrylate tert-butyl monomer unit).
2. A method for producing an acrylic rubber, comprising a step of heat-treating the copolymer according to claim 1 at 70 to 250°C.
3. The method for producing an acrylic rubber according to claim 2, wherein the heat treatment is carried out in the presence of an acid catalyst having an acid dissociation constant (pKa) in water at 25° C. of 5 to −10.
4. The method for producing an acrylic rubber according to claim 3, wherein the acid catalyst is p-toluenesulfonic acid.
5. A method for producing an acrylic rubber composition, comprising a step of kneading 100 parts by mass of the acrylic rubber produced by the production method described in any one of claims 2 to 4 and 30 to 80 parts by mass of carbon black.
6. A method for producing a vulcanizate, comprising a step of vulcanizing the acrylic rubber composition produced by the method for producing an acrylic rubber composition according to claim 5 to obtain a vulcanizate having a compression set of 27% or less and a flex fatigue resistance of 1.3 million or more.
7. A method for manufacturing a rubber hose using the vulcanizate, comprising a step of vulcanizing the acrylic rubber composition produced by the method for producing an acrylic rubber composition described in claim 5 to obtain a vulcanizate having a compression set of 27% or less and a flexural fatigue resistance of 1.3 million or more times.
8. A method for manufacturing a sealing part using the vulcanizate, comprising a step of vulcanizing the acrylic rubber composition produced by the method for producing an acrylic rubber composition described in claim 5 to obtain a vulcanizate having a compression set of 27% or less and a flexural fatigue resistance of 1.3 million or more cycles.
Citation Information
Patent Citations
Ethylene-acrylic acid ester based copolymer and production thereof
JP1989158014A
Resin composition and its use
JP2002241451A
(METH)acrylic block copolymer
JP2005281459A
glue
JP2006511640A
Acrylic rubber, acrylic rubber composition, and acrylic rubber crosslinked product
JP2008214418A