Surface coated cutting tools
The surface-coated cutting tool with controlled lattice constants and Co content in the WC-based cemented carbide tool base addresses durability issues by enhancing adhesion and toughness, ensuring resistance to chipping and peeling during continuous stainless steel cutting.
Patent Information
- Application Number
- JP2021038651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-10
AI Technical Summary
Existing coated cutting tools face challenges in maintaining long-term durability and resistance to chipping and peeling during continuous cutting of stainless steel, particularly due to increased load and unique abrasion from hard burrs in interrupted cutting processes.
A surface-coated cutting tool with a WC-based cemented carbide tool base, where the lattice constant difference between the internal and surface bonded phases of Co is controlled to 0.002 Å or more, and the Co content is maintained between 4.5 to 12.0% by mass, along with a coating layer thickness of 1.0 to 20.0 μm, to enhance adhesion and toughness.
The tool achieves long-term durability and resistance to chipping and peeling during continuous cutting of stainless steel by suppressing local plastic deformation and maintaining tool integrity.
Smart Images

Figure 0007570598000001 
Figure 0007570598000002 
Figure 0007570598000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-coated cutting tool (hereinafter sometimes referred to as a coated tool). [Background technology]
[0002] In order to improve the cutting performance of cutting tools, there have been coated tools in which a coating layer is formed by vapor deposition on the surface of a tool substrate such as a tungsten carbide (hereinafter referred to as WC)-based cemented carbide. These coated tools are known to exhibit excellent wear resistance. Although the coated tools having the above-mentioned conventional coating layers are excellent in wear resistance, various proposals have been made to further improve the wear resistance.
[0003] For example, Patent Document 1 describes a coated tool having a coating layer provided on a tool substrate, in which a surface region within a depth of 2 μm from the surface has a structure in which WC particles exist in a phase consisting of a composite carbide of Co and W, and the density of the WC particles in the surface region is 1 to 5 particles per 10 μm in length of the surface region in a cross section of the substrate cut along a plane containing any normal to the tool substrate surface, and this coated tool is said to have excellent adhesion between the tool substrate and the coating layer.
[0004] Furthermore, for example, Patent Document 2 describes a coated tool in which a coating layer containing AlTiN and Cr(V, Si, Ti)N is provided on a WC-based cemented carbide having a Co content of 5 to 13 mass %, a coercive force of 19.8 kA / m or more, and a lattice constant calculated from the (111) plane of Co of 3.565 Å or more, and this coated tool is said to have excellent resistance to plastic deformation. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5900800 [Patent Document 2] Patent No. 3598035 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, there has been a strong demand for labor-saving and energy-saving cutting, even for difficult-to-cut materials such as stainless steel, and the load on coated tools during cutting has increased significantly. As a result, coated tools are required to have even greater resistance to abnormal damage, such as chipping resistance, fracture resistance, and peeling resistance, as well as excellent wear resistance for long-term use.
[0007] As a result of studying the coated tools described in the above-mentioned patent documents, the present inventors have recognized the following points (1) and (2).
[0008] (1) The coated tool described in Patent Document 1 has improved adhesion between the tool substrate and the coating layer, and therefore improved peeling resistance of the coating layer. However, when used in cutting stainless steel, for example, adhesion chipping occurs originating from the W-Co composite carbide in the WC-based cemented carbide.
[0009] (2) Although the coated tool described in Patent Document 2 has improved resistance to plastic deformation, when used in cutting stainless steel, for example, the toughness of the Co phase decreases, and chipping is likely to occur at the boundary of cuts where cutting is interrupted due to abrasion by hard burrs, which are specific to cutting stainless steel.
[0010] The present inventors have made the present invention in consideration of the above circumstances and recognition, and it is an object of the present invention to provide a coated tool that has durability over a long period of time even in continuous cutting of stainless steel (particularly austenitic stainless steel). [Means for solving the problem]
[0011] In order to achieve the above object, the present inventors have intensively studied WC-based cemented carbides used as tool substrates of coated tools. As a result, they obtained a new finding that the above object can be achieved when a specific relationship holds for the lattice constants of Co contained in each of the binder phases existing near the surface of the tool substrate and inside the tool substrate.
[0012] The present invention is based on this finding and is as follows. (1) A surface-coated cutting tool having a tool substrate and a coating layer on the surface of the tool substrate, wherein the tool substrate is made of a WC-based cemented carbide, A part of the tool base is at least 200 μm inward along a direction perpendicular to the surface of the tool base. when the lattice constant of Co contained in the internal binder phase is a, From the surface of the tool base to within 50 μm along the perpendicular direction and the lattice constant of Co contained in the binder phase of the surface layer portion of is b, a surface-coated cutting tool, characterized in that a < b, the difference between a and b is 0.002 Å or more, and b is less than 3.575 Å. (2) The surface-coated cutting tool according to (1) above, characterized in that the lattice constant a is less than 3.560 Å. (3) The surface-coated cutting tool according to (1) or (2) above, characterized in that the WC-based cemented carbide contains 4.5 to 12.0% by mass of the Co. (4) The surface-coated cutting tool according to any one of (1) to (3) above, characterized in that the average layer thickness of the coating layer is 1.0 to 20.0 μm.
Effect of the Invention
[0013] According to the present invention, a cutting tool having long-term durability can be obtained even in continuous cutting of stainless steel.
Mode for Carrying Out the Invention
[0014] The present invention will be described in detail below. In this specification and the claims, when a numerical range is expressed as "A to B" (both A and B are numerical values), the range includes the upper limit value (B) and the lower limit value (A), and the units of the upper limit value (B) and the lower limit value (A) are the same. In addition, the composition of a compound not represented by a compositional formula is not limited to a stoichiometric composition, but includes all compositions of conventional known atomic ratios.
[0015] 1. Tool substrate (1) Composition There are no particular restrictions on the composition of the WC-based cemented carbide constituting the tool substrate, and a known composition may be used, but it is more preferable that Co is contained in an amount of 4.5 to 12.0% by mass. The reason is that if it is less than 4.5% by mass, the toughness of the tool substrate may decrease, and chipping may easily occur. Also, if it exceeds 12.0% by mass, welding may easily occur. That is, when the Co content ratio is within this range, the above object can be more surely achieved.
[0016] (2) Shape The shape of the tool substrate is not particularly restricted as long as it is a shape used as a cutting tool, and examples include the shape of an insert and the shape of a drill.
[0017] 2. Lattice constant of Co (1) Magnitude relationship of lattice constants When the lattice constant of Co contained in the binding phase inside the tool substrate (WC-based cemented carbide) is a, and the lattice constant of Co contained in the binding phase in the surface layer part is b, it is preferable that a < b and the difference between a and b is 0.002 Å or more. The reason is that when this relationship is satisfied, it is possible to suppress local plastic deformation near the surface while maintaining the toughness required for the tool substrate. In particular, in continuous cutting of stainless steel, it is possible to suppress defects at the cutting boundary part where intermittent cutting occurs, and to suppress minute plastic deformation near the surface (surface layer part) of the tool substrate that causes peeling of the coating layer.
[0018] (2) Absolute value of lattice constant It is more preferable that the lattice constant a of Co contained in the internal binder phase is less than 3.560 Å, because this makes it possible to more reliably suppress chipping at the notch boundary portion.
[0019] In addition, the lattice constant b of Co contained in the binder phase of the surface layer is preferably less than 3.575 Å, and more preferably 3.562 Å (3.560+0.002 Å) or more. The reason is that it is possible to suppress fine plastic deformation occurring near the substrate surface and to suppress peeling, which is a cause of shortening the life when cutting stainless steel. In other words, if it is 3.562 Å or less, it may be difficult to suppress localized plastic deformation near the surface, and if it is less than 3.575 Å, a brittle carbide phase (η phase) appears, causing chipping.
[0020] (3)Measurement method The lattice constant of the binder phase is measured by X-ray diffraction (XRD) using CuKα radiation (λ=1.5418 Å) as the characteristic X-ray. The lattice constant of the binder phase present in the surface layer is obtained by measuring from the surface of the tool substrate or the surface of the coating layer. The lattice constant of the binder phase present inside is obtained by measuring the polished cross section of the tool substrate.
[0021] The average thickness of the coating layer is determined by observing a cross section perpendicular to the tool base (cross section in the layer thickness direction, longitudinal cross section) using a scanning electron microscope at an appropriate magnification, for example 5000x, measuring the layer thickness at five points within the observation field near the cutting edge ridge, and averaging the measurements.
[0022] In the present invention, the surface layer and the interior of the tool base body are defined as follows.
[0023] First, the surface of the tool base is determined by finding the interface between the tool base and the coating layer in a longitudinal section (in the case of an insert, a section perpendicular to the surface of the tool base when the surface of the tool base is considered to be flat, ignoring any minute irregularities on the surface of the tool base. In the case of an axial tool such as a drill, a section perpendicular to the axis of rotation). The average line of the roughness curve of this interface is then arithmetically determined.
[0024] The surface layer of the tool substrate refers to a region extending from the surface of the tool substrate to a depth of 50 μm along the perpendicular direction, and the interior of the tool substrate refers to a region extending from the surface of the tool substrate to a depth of 200 μm or more along the perpendicular direction.
[0025] 3.Coating layer There are no particular limitations on the coating layer, so long as it is a conventionally known coating layer, such as an oxide layer or nitride layer of Al, a nitride layer, carbide layer, carbonitride layer or carbonate layer of Ti, or a composite nitride layer or composite carbonitride layer of Al and Ti.
[0026] Also, the average layer thickness is more preferably 1.0 to 20.0 μm. The reason is that if the average layer thickness is less than 1.0 μm, the average layer thickness is too thin to ensure sufficient wear resistance over long-term use, while if the average layer thickness exceeds 20.0 μm, the crystal grains of the coating layer tend to become coarse, which may lead to chipping.
[0027] 4. Manufacturing method (1) Tool base Each step from preparation of the raw material powder to sintering can be a well-known step. The sintered tool base is then subjected to a tool base surface decarburization step and a tool base surface carburization step.
[0028] The tool base surface decarburization step is a step in which the tool base surface is decarburized in a hydrogen atmosphere after sintering. An example of this step is as follows.
[0029] Reaction gas atmosphere: H 2 Gas atmosphere Reaction atmosphere temperature: 1000℃~1200℃ Reaction atmosphere pressure: 5kPa~20kPa Reaction time: 30 to 60 minutes
[0030] The tool base surface carburizing step is a treatment step in which the decarburized tool base surface is carburized to obtain a desired Co lattice constant. An example of this is as follows.
[0031] Reactant gas composition (volume %): Hydrocarbon gas (CH 4 Gas, C. 2 H 4 Gas, etc.) 5-20vol%, Ar balance Reaction atmosphere temperature: 1000℃~1200℃ Reaction atmosphere pressure: 5kPa~20kPa Reaction time: 30 to 60 minutes
[0032] (2) Coating layer deposition There are no particular limitations, and well-known PVD and CVD methods can be used. EXAMPLES
[0033] Next, an embodiment will be described. Here, as a specific example of the coated tool of the present invention, an insert cutting tool will be described, but the application to drills and end mills is similar.
[0034] 1. Mix with raw powder First, as powders for sintering, WC powder with an average particle size (d50) of 0.5 to 4.0 μm, and Co powder, Ni powder, and Cr powder, all of which have an average particle size (d50) in the range of 1.0 to 4.0 μm, as shown in Table 1, were used. 3 C 2 Powder, TaC powder, NbC powder, TiC powder, ZrC powder, HfC powder, and VC powder were prepared.
[0035] 2. Preparation of the molded body Next, these powders were mixed to obtain the composition shown in Table 1 to prepare powder for sintering. The powder was wet mixed in a ball mill for 72 hours, dried using a spray dryer, and then pressed at a pressure of 100 MPa to obtain the shape of ANSI designation CNMG432MS to produce a powder compact.
[0036] 3. Sintering Next, the powder compacts were subjected to a main sintering step in which they were held at a predetermined temperature for a predetermined time. In this example, the conditions shown in Table 2 were met, that is, the compacts were heated to a holding temperature range of 1350 to 1450°C in a vacuum atmosphere of 5.0 Pa or less, and held at the holding temperature for 60 to 120 minutes.
[0037] 4. Tool base surface decarburization process Detailed treatment conditions are shown in Table 2, but were generally as follows. Reaction gas atmosphere: H 2 Gas atmosphere Reaction atmosphere temperature: 1000℃~1200℃ Reaction atmosphere pressure: 5.0kPa~20.0kPa Reaction time: 30 to 60 minutes
[0038] 5. Tool base surface carburizing process Detailed treatment conditions are shown in Table 2, but were generally as follows. Reactant gas composition (volume %): Hydrocarbon gas (CH 4 Gas, C. 2 H 4 Gas) 5-20vol%, Ar balance Reaction atmosphere temperature: 1000℃~1200℃ Reaction atmosphere pressure: 5.0kPa~20.0kPa Reaction time: 30 to 60 minutes
[0039] 6. Post-processing Next, machining and grinding were performed to shape the tool into CNMG432MS, and a coating layer was formed on the tool base of the example shown in Table 3 under the film-forming conditions shown in Table 5 to produce example coated tools 1 to 10 (hereinafter referred to as Examples 1 to 10).
[0040] For comparison, comparative example tool base bodies 1' to 8' shown in Table 4 were manufactured. The manufacturing process was such that the tool base surface decarburization treatment process and the tool base surface carburization treatment process were omitted from the manufacturing processes of Examples 1 to 10 (in Table 2, the respective process conditions are marked with "-"), or the tool base surface decarburization treatment process and the tool base surface carburization treatment process shown in Table 2 were performed under manufacturing conditions other than those of the above-mentioned example, and coating layers were formed under the film formation conditions shown in Table 5 to produce comparative example coated tools 1' to 8' (hereinafter referred to as Comparative Examples 1' to 8').
[0041] [Table 1]
[0042] [Table 2]
[0043] [Table 3]
[0044] [Table 4]
[0045] [Table 5]
[0046] Next, cutting tests were carried out on Examples 1 to 10 and Comparative Examples 1' to 8' under the following cutting conditions 1 to 3, and the results are shown in Tables 6 to 8, respectively.
[0047] Cutting conditions 1 Material: SUS304 round bar with outer diameter of 100 mm Cutting speed: 200m / sec Cutting depth: 1.5mm Feed per revolution: 0.3mm Wet cutting
[0048] Cutting conditions 2 Work material: SUS316 round bar with outer diameter of 100 mm Cutting speed: 150m / sec Cutting depth: 2.0mm Feed per revolution: 0.2mm Wet cutting
[0049] Cutting conditions 3 Work material: SUS630 round bar with outer diameter of 100 mm Cutting speed: 120m / sec Cutting depth: 2.0mm Feed per revolution: 0.15mm Wet cutting
[0050] [Table 6]
[0051] [Table 7]
[0052] [Table 8]
[0053] As is clear from Tables 6 to 8, all of the Examples showed excellent cutting performance, with little flank wear and no chipping or peeling due to plastic deformation. In contrast, all of the Comparative Examples showed chipping or peeling due to plastic deformation before the end of the cutting test time (15 minutes), reaching the end of their service life.
Claims
1. A surface-coated cutting tool having a tool substrate and a coating layer on a surface of the tool substrate, The tool base is made of a WC-based cemented carbide, and when the lattice constant of Co contained in an internal binder phase located 200 μm or more inward from the surface of the tool base along a perpendicular line thereto is taken as a, and the lattice constant of Co contained in a surface layer binder phase located up to 50 μm inward from the surface of the tool base along a perpendicular line thereto is taken as b, A surface-coated cutting tool, characterized in that a<b and the difference between a and b is 0.002 Å or more, and b is less than 3.575 Å.
2. 2. The surface coated cutting tool of claim 1, wherein the lattice constant a is less than 3.560 Å.
3. 3. The surface-coated cutting tool according to claim 1, wherein the WC-based cemented carbide contains 4.5 to 12.0 mass % of Co.
4. The surface-coated cutting tool according to any one of claims 1 to 3, characterized in that the coating layer has an average thickness of 1.0 to 20.0 µm.
Citation Information
Patent Citations
Triply coated superhard alloy parts and their preparation
JP1978070905A
Multi-point stress measuring apparatus for rotor
JP1984000800A
Covered super hard alloy end mill
JP1999207515A
Method of cutting heat-resisting cast steel using covered cemented carbide alloy insert
JP2001138108A
Surface coated hard alloy
JP2003129165A