Cubic boron nitride sintered body
A cubic boron nitride sintered body with optimized composition and structural parameters addresses the issues of wear and chipping resistance, enhancing tool life and performance in high-speed machining of sintered metals.
Patent Information
- Application Number
- JP2022137154
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-30
AI Technical Summary
Existing cubic boron nitride sintered bodies do not provide sufficient wear resistance and chipping resistance for high-speed machining of sintered metals, leading to reduced tool life due to weakened bonding strength and increased fracture risk.
A cubic boron nitride sintered body with a specific composition and structural parameters, including a cubic boron nitride content of 85-95% by volume, a binder phase of 5-15% by volume, and controlled X-ray diffraction peak intensities and ratios, enhances bonding strength and resistance to wear and chipping.
The improved cubic boron nitride sintered body exhibits enhanced wear resistance and chipping resistance, extending tool life and maintaining tool integrity during high-speed machining of sintered metals.
Smart Images

Figure 0007570601000001 
Figure 0007570601000002 
Figure 0007570601000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cubic boron nitride sintered body. [Background technology]
[0002] Cubic boron nitride (hereinafter referred to as "cBN") has a hardness second only to diamond and excellent thermal conductivity. Cubic boron nitride also has the characteristic of having a lower affinity with iron than diamond. For this reason, cubic boron nitride sintered bodies consisting of cubic boron nitride and a bonding phase of metal or ceramics are used in cutting tools and wear-resistant tools.
[0003] Sintered metals are highly moldable and often have complex shapes, so when they are processed using tools, the tools are prone to chipping due to thermal shock. In addition, sintered metals may contain hard particles, which makes the tools prone to wear. For this reason, cubic boron nitride is often used to process sintered metals, and in particular, cubic boron nitride sintered bodies with a high cubic boron nitride content have been much studied.
[0004] For example, Patent Document 1 discloses a cubic boron nitride sintered body having 85 volume % or more and less than 100 volume % of cubic boron nitride particles and the remainder being a binder, the binder containing WC, Co and Al compounds, and the binder being WCo 21 B6, and the X-ray diffraction intensity of the (111) face of the cubic boron nitride particle is I A The X-ray diffraction intensity of the (100) plane of WC is I B , the above W2Co 21 The X-ray diffraction intensity of the (420) plane of B6 is I C When expressed as above, I A For the above I C Ratio I C / I A is greater than 0 and less than 0.10, and the above I B For the above I C Ratio I C / I B is greater than 0 and less than 0.40. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2020 / 059756 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, there has been a demand for even higher efficiency in cutting, and so there has been a greater trend toward higher speeds, higher feed rates, and deeper cuts. In response to this trend, there is a demand for cubic boron nitride sintered bodies that are excellent in wear resistance and chipping resistance and can have a long tool life, even in high-speed cutting of sintered metals.
[0007] In this context, the cubic boron nitride sintered body described in Patent Document 1 does not contain a sufficient amount of Co3W3C, and furthermore, W2Co 21 Since the X-ray diffraction intensity of the (420) plane of B6 is much smaller than that of the (100) plane of WC, the WC content is high, which tends to weaken the bonding strength of the cubic boron nitride sintered body, making it easy for the chipping resistance to decrease.
[0008] An object of the present invention is to provide a cubic boron nitride sintered body having excellent wear resistance and chipping resistance, thereby enabling an extension of tool life. [Means for solving the problem]
[0009] The inventors have conducted extensive research into extending tool life and have discovered that by giving a cubic boron nitride sintered body a specific configuration, it is possible to improve its wear resistance and chipping resistance, thereby extending tool life, which has led to the completion of the present invention.
[0010] The gist of the present invention is as follows. [1] A cubic boron nitride sintered body comprising cubic boron nitride and a binder phase, the content of the cubic boron nitride is 85% by volume or more and 95% by volume or less with respect to the total amount of the sintered body, The content of the binder phase is 5% by volume or more and 15% by volume or less with respect to the total amount of the sintered body, The binder phase is Co3W3C, W2Co 21 B6 and Al compounds, The X-ray diffraction peak intensity of the (111) plane of the cubic boron nitride is I A The X-ray diffraction peak intensity of the (400) plane of the Co3W3C is I B , W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C , the X-ray diffraction peak intensity of the (001) plane of WC is I D When I B / I A is 0.02 or more and 0.15 or less, I C / I A is equal to or greater than 0.02 and equal to or less than 1.00, I C ≧I D A sintered cubic boron nitride body. [2] I D / I A The cubic boron nitride sintered body according to [1], wherein [3] I C / I B The cubic boron nitride sintered body according to [1] or [2], wherein is 0.2 or more and 15.0 or less. [4] I C The cubic boron nitride sintered body according to any one of [1] to [3], wherein the half width of is 0.25 or more and 0.60 or less. [5] The cubic boron nitride sintered body according to any one of [1] to [4], wherein the cubic boron nitride has an average grain size of 0.5 μm or more and 4.0 μm or less. Effect of the Invention
[0011] According to the present invention, it is possible to provide a cubic boron nitride sintered body that has excellent wear resistance and chipping resistance, thereby enabling an extension of tool life. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as the present embodiment) will be described in detail, but the present invention is not limited to the present embodiment. The present invention can be modified in various ways without departing from the gist of the present invention.
[0013] [Cubic boron nitride sintered body] The cubic boron nitride sintered body of this embodiment is a cubic boron nitride sintered body containing cubic boron nitride (hereinafter also referred to as "cBN") and a binder phase, the content of cubic boron nitride is 85 volume % or more and 95 volume % or less with respect to the total amount of the sintered body, the content of the binder phase is 5 volume % or more and 15 volume % or less with respect to the total amount of the sintered body, and the binder phase is Co3W3C, W2Co 21 B6, and Al compounds, and the X-ray diffraction peak intensity of the (111) plane of cubic boron nitride is I A , the X-ray diffraction peak intensity of the (400) plane of Co3W3C is I B , W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C , the X-ray diffraction peak intensity of the (001) plane of WC is I D Then, I B / I A is between 0.02 and 0.15, and I C / I A is between 0.02 and 1.00, and I C ≧I D It is.
[0014] By providing the cubic boron nitride sintered body of the present embodiment with the above-mentioned configuration, it is possible to improve the wear resistance and chipping resistance, and as a result, the tool life can be extended. The factors that enable the cubic boron nitride sintered body of this embodiment to improve the wear resistance and fracture resistance of a tool and extend the tool life are not clear in detail, but the present inventors believe that the factors are as follows, although the factors are not limited to these. The cubic boron nitride sintered body of this embodiment has a cubic boron nitride content of 85 volume % or more, and therefore the proportion of the binder phase is relatively small, so that the hardness is improved and the wear resistance is excellent. On the other hand, the cubic boron nitride sintered body of this embodiment has a cubic boron nitride content of 95 volume % or less, so that the falling off of cubic boron nitride particles can be suppressed, and the wear resistance is excellent. Furthermore, in cutting, the surface roughness of the machined surface of the workpiece tends to be small, and the appearance after machining tends to be good. In addition, the cubic boron nitride sintered body of this embodiment has a binder phase content of 5 volume % or more, which can suppress the falling off of cBN particles and has excellent wear resistance. On the other hand, the cubic boron nitride sintered body has a binder phase content of 15 volume % or less, which makes the cBN content relatively high and improves hardness, resulting in excellent wear resistance. The cubic boron nitride sintered body of this embodiment is B / I A When the bond strength of the cBN sintered body is 0.02 or more, the bond strength of the cBN sintered body is improved and the chipping resistance is excellent. B / I A By making the ratio of I to 0.15 or less, the hardness of the cBN sintered body is prevented from decreasing, and the cBN sintered body has excellent wear resistance. C / I A is 0.02 or more, the cubic boron nitride sintered body is W2Co 21 The moderate content of B6 suppresses the propagation of cracks during cutting into cBN, resulting in excellent chipping resistance. C / I A By making the value of I equal to or less than 1.00, the toughness of the binder phase is improved and the fracture resistance is excellent. C ≧I D This improves the bonding strength of the cBN sintered body and provides excellent chipping resistance. As a result of the combined effects described above, the cubic boron nitride sintered body of this embodiment can improve wear resistance and chipping resistance, and extend the tool life.
[0015] The cubic boron nitride sintered body of this embodiment contains cBN and a binder phase. The cBN content is 85% by volume or more and 95% by volume or less with respect to the total amount of the sintered body. The binder phase content is 5% by volume or less with respect to the total amount of the sintered body. End The total content of cBN and the binder phase in the cubic boron nitride sintered body of the present embodiment is 100% by volume.
[0016] [Cubic boron nitride (cBN)] In the cubic boron nitride sintered body of this embodiment, the content of cubic boron nitride is 85% by volume or more, so that the proportion of the binder phase is relatively small, and thus the hardness is improved and the wear resistance is excellent. On the other hand, the content of cubic boron nitride in the cubic boron nitride sintered body of this embodiment is 95% by volume or less, so that the falling off of cubic boron nitride particles can be suppressed, and the wear resistance is excellent. Furthermore, in cutting processing, the surface roughness of the processed surface of the workpiece tends to be small, and the appearance after processing tends to be good. From the same viewpoint, the content of cubic boron nitride is preferably 85% by volume or more and 92% by volume or less, and more preferably 85% by volume or more and 90% by volume or less.
[0017] In the cubic boron nitride sintered body of this embodiment, the average grain size of cubic boron nitride (cBN) is preferably 0.5 μm or more and 4.0 μm or less. The cubic boron nitride sintered body can suppress the falling off of cBN grains by having an average grain size of cBN of 0.5 μm or more, and tends to have improved mechanical strength and excellent chipping resistance by having an average grain size of cBN of 4.0 μm or less. From the same viewpoint, the average grain size of cBN is more preferably 0.5 μm or more and 3.2 μm or less, and even more preferably 0.5 μm or more and 2.4 μm or less.
[0018] In this embodiment, the average grain size of cBN can be determined, for example, as follows. The cross-sectional structure of cubic boron nitride sintered body is photographed by SEM. The photographed structure is analyzed to determine the area of the cBN grains, and the diameter of a circle with the same area as this area is calculated as the grain size of the cBN. The average value of the particle diameters of a plurality of cBN particles is determined as the average particle diameter of cBN. The average particle diameter of cBN can be determined from an image of the cross-sectional structure of the cubic boron nitride sintered body using commercially available image analysis software. More specifically, it can be determined by the method described in the examples below.
[0019] [Binded phase] The cubic boron nitride sintered body of this embodiment has a binder phase content of 5% or more by volume, which can suppress the falling off of cBN particles and has excellent wear resistance. On the other hand, the cubic boron nitride sintered body has a binder phase content of 15% or less by volume, which makes the cBN content relatively high and improves hardness, resulting in excellent wear resistance. From the same viewpoint, the binder phase content is preferably 8% or more and 15% or less by volume, and more preferably 10% or more and 15% or less by volume.
[0020] The cubic boron nitride sintered body of this embodiment has a binder phase of Co3W3C, W2Co 21 B6, and Al compounds, and the X-ray diffraction peak intensity of the (111) plane of cubic boron nitride is I A , the X-ray diffraction peak intensity of the (400) plane of Co3W3C is I B , W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C , the X-ray diffraction peak intensity of the (001) plane of WC is I D Then, I B / I A is between 0.02 and 0.15, and I C / I A is between 0.02 and 1.00, and I C ≧I D It is.
[0021] Compounds that can be included in the bonded phase of this embodiment include Co3W3C, W2Co 21 Other than B6 and Al compounds, there are no particular limitations, and examples of compounds containing W include WC, CoWB, W2C, WB, etc. Furthermore, examples of Al compounds (compounds containing Al element) include CoAl, AlN, AlB2, and Al2O3, as well as composite compounds thereof. Furthermore, examples of Cr compounds (compounds containing Cr element) include CrN, Cr2N, Cr3C2, Cr7C3, Cr 23 Examples of the CrN-based binder include C6, Cr2O3, and CrB2, as well as composite compounds thereof. In this embodiment, the binder phase preferably contains a Cr compound, and more preferably contains CrN. By containing a Cr compound, the W2Co generated during sintering can be easily obtained. 21 The grain growth of B6 tends to be suppressed. Compounds that can be contained in the binder phase of the present embodiment other than those mentioned above include, for example, TiN, TiC, Ti(C,N), TiB2, Co, Co 5.47 N, CoN, etc.
[0022] The cubic boron nitride sintered body of this embodiment has an X-ray diffraction peak intensity of I A , the X-ray diffraction peak intensity of the (400) plane of Co3W3C is I B Then, I B / I A is between 0.02 and 0.15. B / I A By setting the value of I to 0.02 or more, the bonding strength of the cBN sintered body is improved and the chipping resistance is excellent. B / I A By keeping I at 0.15 or less, the hardness of the cBN sintered body is prevented from decreasing, and the body has excellent wear resistance. B / I A is preferably 0.04 or more and 0.14 or less, and more preferably 0.05 or more and 0.13 or less.
[0023] The cubic boron nitride sintered body of this embodiment has an X-ray diffraction peak intensity of I A, W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C Then, I C / I A is between 0.02 and 1.00. C / I A is 0.02 or more, the cubic boron nitride sintered body is W2Co 21 The moderate content of B6 suppresses the propagation of cracks during cutting into the cBN, providing excellent chipping resistance. C / I A By making I equal to or less than 1.00, the toughness of the binder phase is improved and the fracture resistance is excellent. C / I A is preferably 0.02 or more and 0.88 or less, and more preferably 0.06 or more and 0.73 or less.
[0024] The cubic boron nitride sintered body of this embodiment is WCo 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C , the X-ray diffraction peak intensity of the (001) plane of WC is I D Then, I C ≧I D The relationship is satisfied. C ≧I D This improves the bonding strength of the cBN sintered body and provides excellent chipping resistance. D / I C is preferably 0.00 or more and 1.00 or less, more preferably 0.00 or more and 0.60 or less, and even more preferably 0.00 or more and 0.42 or less.
[0025] The cubic boron nitride sintered body of this embodiment has an X-ray diffraction peak intensity of I D , the X-ray diffraction peak intensity of the (111) plane of cubic boron nitride is I A Then, I D / I A is preferably 0.00 or more and 0.20 or less. D / I ABy keeping I at 0.20 or less, the bonding strength of the cubic boron nitride sintered body is improved, and the body tends to have excellent chipping resistance. D / I A is more preferably 0.00 or more and 0.16 or less, even more preferably 0.00 or more and 0.08 or less, and even more preferably 0.00.
[0026] The cubic boron nitride sintered body of this embodiment has an X-ray diffraction peak intensity of I B , W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C Then, I C / I B is preferably 0.2 or more and 15.0 or less. C / I B is 0.2 or more, the cubic boron nitride sintered body is W2Co 21 By containing a specified amount or more of B6, the propagation of cracks during cutting into the cubic boron nitride is suppressed, and chipping resistance and fracture resistance tend to be excellent. C / I B When I is 15.0 or less, the bonding strength of the cubic boron nitride sintered body and / or the toughness of the bonding phase are improved, and the fracture resistance tends to be excellent. C / I B is more preferably 0.6 or more and 13.5 or less, and further preferably 0.6 or more and 12.0 or less.
[0027] In the cubic boron nitride sintered body of this embodiment, the content of Al in the binder phase may be 0.3% by mass or more and 5% by mass or less, based on the total of all elements contained in the sintered body (100% by mass). When the content of Al is 0.3% by mass or more, the Al element reacts with oxygen atoms on the surface of the cBN particles, which tends to suppress the falling off of the cBN particles. When the content of Al is 5.0% by mass or less, the formation of Al nitrides and Al borides is suppressed, and the wear resistance tends to be excellent. From the same viewpoint, the content of Al in the binder phase is preferably 0.4% by mass or more and 2.1% by mass or less, more preferably 0.6% by mass or more and 1.6% by mass or less, based on the total of all elements contained in the sintered body (100% by mass).
[0028] In the cubic boron nitride sintered body of this embodiment, the binder phase is Co3W3C, W2Co 21 The B6 and Al compounds may contain elements other than those constituting the compound. Specific examples include, but are not limited to, Cr, Ti, Zr, Nb, Mo, Hf, Ta, Mn, Fe, Ni, and N, with Cr, Ti, Zr, Nb, Mo, Ta, Mn, Ni, and N being preferred, and Cr, Ti, Zr, Mo, Ta, Ni, and N being more preferred. These elements may be unavoidably contained or may be intentionally added, for example, originating from cylinders and balls for a ball mill, high melting point metal capsules used for filling, etc. The content ratio of the above other elements is not particularly limited, and may be, for example, 0% by mass or more and 10% by mass or less with respect to the total of all elements contained in the sintered body being 100% by mass.
[0029] In the cubic boron nitride sintered body of this embodiment, the content ratio (volume %) of cubic boron nitride and the binder phase can be obtained by analyzing the structure photograph of the cubic boron nitride sintered body taken with a scanning electron microscope (SEM) using commercially available image analysis software. More specifically, the cubic boron nitride sintered body is mirror-polished in a direction perpendicular to its surface. Next, the backscattered electron image of the mirror-polished surface of the cubic boron nitride sintered body that appears after mirror polishing is observed using the SEM. At this time, the backscattered electron image of the mirror-polished surface of the cubic boron nitride sintered body enlarged at a magnification selected so that 100 to 400 cubic boron nitride particles are included is observed using the SEM. By using an energy dispersive X-ray analyzer (EDS) attached to the SEM, the black area can be identified as cubic boron nitride, and the gray area and white area can be identified as binder phase. Then, a structural photograph of the cross section of the cubic boron nitride is taken using an SEM. Using commercially available image analysis software, the areas occupied by the cubic boron nitride and the binder phase are determined from the obtained structural photograph, and the content (volume %) is calculated from the areas.
[0030] In this embodiment, the content (mass%) of each element in the binder phase can be determined by using an energy dispersive X-ray analyzer (EDS) in the same observation field as the structural photograph of the cubic boron nitride sintered body taken with a scanning electron microscope (SEM) to determine the content (volume%) of the cubic boron nitride and binder phase described above. More specifically, EDS analysis is performed in the entire observation field of the enlarged mirror-polished surface described above, and the content (mass%) of each element is calculated when the total of all elements contained in the cubic boron nitride sintered body is 100 mass%.
[0031] Here, the mirror-polished surface of the cubic boron nitride sintered body is a cross-section of the cubic boron nitride sintered body obtained by mirror-polishing the surface or any cross-section of the cubic boron nitride sintered body. A method for obtaining a mirror-polished surface of the cubic boron nitride sintered body can be, for example, a method of polishing with diamond paste.
[0032] The composition of the binder phase can also be identified using a commercially available X-ray diffractometer. For example, the composition of the binder phase can be identified by performing X-ray diffraction measurement of a 2θ / θ focused optical system using Cu-Kα radiation using an X-ray diffractometer (product name "RINT TTRIII") manufactured by Rigaku Corporation. Here, the measurement conditions are preferably, for example, those described in the examples described later. Furthermore, when the measurement range of 2θ is widened for analysis, more peaks tend to be detected, and the material contained in the sintered body can be more reliably identified. From this viewpoint, for example, it is preferable to perform the measurement in the range of 2θ=20 to 140°. In this embodiment, the content ratio of cubic boron nitride and the binder phase, and the composition of the binder phase can also be measured by the method described in the Examples below. Specifically, the composition of the binder phase can be specified by analyzing the results of measurement by an X-ray analyzer and the results of element mapping using EDS.
[0033] The cubic boron nitride sintered body of this embodiment is WCo 21 X-ray diffraction peak intensity of the (420) plane of B6 I C It is preferable that the half width of I is 0.25 or more and 0.60 or less. C When the half-value width of I is 0.25 or more, the toughness of the binder phase is improved and the fracture resistance tends to be excellent. C When the half-value width of I is 0.60 or less, cracks during cutting are inhibited from propagating to the cubic boron nitride, and chipping resistance and fracture resistance tend to be improved. C The half width is more preferably 0.28 or more and 0.60 or less, and further preferably 0.32 or more and 0.48 or less.
[0034] [Method of producing sintered cubic boron nitride] The cubic boron nitride sintered body of this embodiment can be produced, for example, by the following method. As the raw material powders, cBN powder, WC powder, Co powder, Al powder, and Cr powder are prepared. Here, by appropriately adjusting the average particle size of the raw material cBN powder, the average particle size of cBN in the obtained cubic boron nitride sintered body can be controlled within the above-mentioned specific range. In addition, by appropriately adjusting the ratio of each raw material powder, the content ratio of cBN and the binder phase in the obtained cubic boron nitride sintered body can be controlled within the above-mentioned specific range. Next, the prepared raw material powders are mixed in a ball mill cylinder together with cemented carbide balls, a solvent, and paraffin. The raw material powders mixed in the ball mill are filled into a Ta high melting point metal capsule, and vacuum heat treatment is performed with the capsule open to remove moisture and other attached components adsorbed on the surface of the powder. Next, the capsule is sealed, and the raw powder filled in the capsule is sintered under high pressure. When filling the capsule, a base material made of cemented carbide may be placed on the bottom of the capsule. The conditions for high pressure sintering are, for example, pressure: 7.7 to 8.5 GPa, heating rate: 20 to 30°C / sec, temperature: 1800 to 1900°C, and sintering time: 30 to 45 minutes.
[0035] In the bonding phase used in this embodiment, the above-mentioned I B / I A There are no particular limitations on the method for increasing this, but examples of the method include increasing the sintering temperature in the manufacturing process of a cubic boron nitride sintered body, increasing the heating rate during sintering, decreasing the cBN content, increasing the blending ratio of Co powder in the binder phase material, decreasing the blending ratio of Al powder in the binder phase material, and the like.
[0036] In the bonding phase used in this embodiment, the above-mentioned I C / I A There are no particular limitations on the method for increasing the sintering pressure in the manufacturing process of the cubic boron nitride sintered body, a method for decreasing the cBN content, a method for decreasing the average particle size of cBN, a method for increasing the blending ratio of Co powder in the binder phase material, and the like can be mentioned.
[0037] In the bonding phase used in this embodiment, the above-mentioned I D / I A There are no particular limitations on the method for reducing this, but examples include increasing the sintering temperature in the manufacturing process of the cubic boron nitride sintered body, reducing the cBN content, and reducing the blending ratio of WC powder as a binder phase material.
[0038] In the bonding phase used in this embodiment, the above-mentioned I C ≧I D or I D / I C There are no particular limitations on the method for reducing this, but examples of the method include increasing the sintering temperature during sintering in the manufacturing process of a cubic boron nitride sintered body, increasing the temperature rise rate during sintering, increasing the content of cBN, and decreasing the blending ratio of WC powder as a binder phase material.
[0039] In the bonding phase used in this embodiment, the above-mentioned I C / I B There are no particular limitations on the method for increasing this, but examples of the method include lowering the sintering temperature in the manufacturing process of the cubic boron nitride sintered body, slowing down the heating rate during sintering, lowering the sintering pressure, and reducing the proportion of Al powder in the binder phase material.
[0040] In the bonding phase used in this embodiment, the above-mentioned I C The method for increasing the half-value width of is not particularly limited, but examples include a method of increasing the content of cBN in the manufacturing process of the cubic boron nitride sintered body, and a method of making the cubic boron nitride sintered body contain Cr compounds. 21 When the average particle size of B6 becomes smaller, I C The half-width of the peak tends to be large.
[0041] The cubic boron nitride sintered body of this embodiment may be used as a coated cubic boron nitride sintered body having a coating layer on its surface. The coating layer formed on the surface of the cubic boron nitride sintered body further improves the wear resistance. The coating layer is not particularly limited, and may contain, for example, at least one element selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al and Si, and at least one element selected from the group consisting of C, N, O and B. The coating layer may have a single layer structure or a laminated structure including two or more layers. When the coating layer has such a structure, the coated cubic boron nitride sintered body of this embodiment tends to have further improved wear resistance.
[0042] Examples of the compound forming the coating layer include, but are not limited to, TiN, TiC, TiCN, TiAlN, TiSiN, and AlCrN. Among them, TiCN, TiAlN, and AlCrN are preferable. The coating layer may have a structure in which multiple layers having different compositions are laminated.
[0043] The thickness of each layer constituting the coating layer and the thickness of the entire coating layer can be measured from the cross-sectional structure of the coated cubic boron nitride sintered body using an optical microscope, SEM, transmission electron microscope (TEM), etc. The average thickness of each layer in the coated cubic boron nitride sintered body and the average thickness of the entire coating layer can be obtained by measuring the thickness of each layer and the thickness of the entire coating layer from three or more cross sections in the vicinity of a position 50 μm from the cutting edge of the surface facing the metal evaporation source toward the center of the surface, and calculating the average value.
[0044] The composition of each layer constituting the coating layer can be measured from the cross-sectional structure of the coated cubic boron nitride sintered body using EDS, a wavelength dispersive X-ray analyzer (WDS), or the like.
[0045] The method for producing the coating layer is not particularly limited, and examples thereof include chemical vapor deposition, ion plating, arc ion plating, sputtering, ion mixing, and other physical vapor deposition methods. Among these, the arc ion plating method is preferred because it provides better adhesion between the coating layer and the cubic boron nitride sintered body.
[0046] The cubic boron nitride sintered body or coated cubic boron nitride sintered body of this embodiment is excellent in wear resistance and chipping resistance, so it is preferably used as a cutting tool or wear-resistant tool, and is particularly preferably used as a cutting tool. The cubic boron nitride sintered body or coated cubic boron nitride sintered body of this embodiment is more preferably used as a cutting tool for sintered metals or a cutting tool for cast iron. When the cubic boron nitride sintered body or coated cubic boron nitride sintered body of this embodiment is used as a cutting tool or wear-resistant tool, the tool life can be extended more than before. EXAMPLES
[0047] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0048] Example 1 [Preparation of raw powder] WC powder, Co powder, Al powder, and Cr powder were mixed in the ratios (mass%) shown in Table 1 to prepare eight different binder phase materials A to I. The average particle sizes of the WC powder, Co powder, Al powder, and Cr powder were 2.0 μm, 1.5 μm, 1.8 μm, and 2.8 μm, respectively. The average particle sizes of the raw material powders were measured by the Fisher method (Fisher Sub-Sizer, FSSS) according to the American Society for Testing and Materials (ASTM) standard B330. In Table 1, "-" indicates that the raw material corresponding to the column is not included. In addition, cubic boron nitride (cBN) powder was mixed with the binder phase materials in the proportions (volume %) shown in Table 2.
[0049] [Table 1]
[0050] [Table 2]
[0051] [Mixing process] The raw material powder was further mixed in a cylinder for a ball mill together with a hexane solvent, paraffin, and cemented carbide balls.
[0052] [Filling and drying processes] The mixed raw powder was filled into a disk-shaped capsule made of Ta, a high melting point metal. In order to remove moisture and organic components adsorbed on the surface of the filled raw powder, the capsule was left open and subjected to vacuum heat treatment. After removing the moisture and other attached components adsorbed on the surface of the powder, the capsule was sealed.
[0053] [High pressure sintering] The raw material powder packed in the capsule was then sintered under high pressure. The conditions for high pressure sintering are shown in Table 3.
[0054] [Table 3]
[0055] [Measurement / Analysis] The content (volume %) of cubic boron nitride and binder phase of the cubic boron nitride sintered body obtained by high pressure sintering was obtained by analyzing the structure photograph of the cubic boron nitride sintered body taken by a scanning electron microscope (SEM) using commercially available image analysis software. More specifically, the cubic boron nitride sintered body was mirror-polished in a direction perpendicular to its surface. Next, a backscattered electron image of the mirror-polished surface of the cubic boron nitride sintered body that appeared after mirror polishing was observed using an SEM. At this time, the backscattered electron image of the mirror-polished surface of the cubic boron nitride sintered body magnified at a magnification selected so that 100 to 400 cubic boron nitride particles were included was observed using an SEM. By using an energy dispersive X-ray analyzer (EDS) attached to the SEM, the black area was identified as cubic boron nitride, and the gray and white areas as binder phase. Then, a microstructure photograph of the mirror-polished surface of the cubic boron nitride was taken using a SEM. Using commercially available image analysis software, the areas occupied by the cubic boron nitride and the binder phase were determined from the obtained microstructure photograph, and the content (volume %) was calculated from the areas. Here, the mirror-polished surface of the cubic boron nitride sintered body was a cross-section of the cubic boron nitride sintered body obtained by mirror-polishing the surface or any cross-section of the cubic boron nitride sintered body. The mirror-polished surface (hereinafter also referred to as "cross-section") of the cubic boron nitride sintered body was obtained by polishing with diamond paste.
[0056] The area of the cBN grains was calculated by image analysis of the SEM photograph of the cubic boron nitride sintered body, and the diameter of a circle with the same area was taken as the grain size of the cBN. The value that satisfied the following formula was taken as the average grain size of the cBN. (D 50 (area occupied by cBN particles with a particle size below) / (area occupied by all cBN particles)=0.5
[0057] Furthermore, the composition of the binder phase was identified using an X-ray diffractometer (product name "RINT TTRIII") manufactured by Rigaku Corporation. Specifically, the composition of the binder phase was identified by analyzing the results of X-ray diffraction measurement using a 2θ / θ focused optical system with Cu-Kα radiation under the following conditions and the element mapping results using EDS. <Measurement conditions> Output: 50kV, 250mA -Soller slit on entrance side: 5° Divergence vertical slit: 1 / 2° Vertical limit divergence slit: 10mm Scattering slit: 2 / 3° -Solar slit on light receiving side: 5° Receiving slit: 0.15mm BENT Monochromator Receiving monochrome slit: 0.8 mm Sampling width: 0.02° Scan speed: 1° / min 2θ measurement range: 30~90°
[0058] Specifically, the X-ray diffraction measurement by the above-mentioned method identified that the obtained cubic boron nitride sintered body contained the following materials. Co3W3C (excluding comparison products 1 to 3, 7 and 8) ·W2Co 21 B6 WC (excluding invention products 2, 9, 14-16, and comparison products 4-6 and 8) For compounds containing Al, no clear peaks were obtained in X-ray diffraction measurements, so they were identified by element mapping using EDS. For compounds containing Cr, except for CrN, no clear peaks were obtained in X-ray diffraction measurements, so they were identified by element mapping using EDS. As a result, it was found that all of the obtained cubic boron nitride sintered bodies contained compounds containing Al (simply referred to as Al compounds in the table). It was also found that inventive products 8, 9, and 13 and comparative product 12, Cr compounds were contained that were presumed to be composed of multiple Cr compounds, and inventive products 15 and 16 contained CrN. Furthermore, the samples prepared using binder phase materials F to I contained I C The half-width of the Cr-containing binder phase tends to increase. 21 It is presumed that this is due to the suppression of grain growth of B6.
[0059] Furthermore, the content (mass%) of each element in the binder phase was determined by using EDS in the same observation field as the structural photograph of the cubic boron nitride sintered body taken by SEM to determine the above-mentioned content (volume%) of cBN and the binder phase. Specifically, EDS analysis was performed in the entire observation field of the above-mentioned enlarged mirror-polished surface, and the content (mass%) of Al was calculated when the total of all elements contained in the cubic boron nitride sintered body was taken as 100 mass%. The measurement results obtained above are shown in Table 4.
[0060] The X-ray diffraction peak intensity (I A ), and the X-ray diffraction peak intensity of the (400) plane of Co3W3C (I B ), W2Co 21 X-ray diffraction peak intensity of the (420) plane of B6 (I C ), and the X-ray diffraction peak intensity of the (001) plane of WC (I D ) to I B / I A , I C / I A , I D / I A , I C / I B , and I C Calculate the half-width of each, I C ≧I D The X-ray diffraction peaks of each crystal plane were identified based on the information in the following PDF (Powder Diffraction File) card numbers, and had peak tops in the following ranges. The values obtained above are summarized in Table 5. ·cBN (111) surface: PDF card No. 73-0887 Range: 42.7° to 43.9° Co3W3C (400) side: PDF card No. 06-0639 Range: 31.9° to 32.7° ·W2Co 21 B6 (420) side: PDF card No. 19-0372 Range: 37.7° to 38.7° ·WC (001) side: PDF card No. 65-4539 Range: 31.2° to 31.8°
[0061] [Table 4]
[0062] [Table 5]
[0063] [Cutting tool manufacturing] The obtained cubic boron nitride sintered body was cut out using a wire electric discharge machine to match the tool shape of the insert shape defined by ISO standard CNGA120408. The cut cubic boron nitride sintered body was joined by brazing to a base metal made of cemented carbide. The brazed tool was subjected to honing to obtain a cutting tool.
[0064] [Cutting test] Using the obtained cutting tool, a cutting test was carried out under the following conditions. ·Workpiece material: Sintered metal (Material: Old JIS standard SMF4040, Hardness: HRB80) Workpiece shape: Gear shape, φ45mm (tooth height 8mm) x 30mm ·Cutting speed: 200m / min Feed: 0.15mm / rev Cutting depth: 0.20mm Coolant: None (dry cutting) -Evaluation items: The damage form after 10 minutes of machining was observed using an SEM or optical microscope. At this time, if minute defects occurred that allowed machining to continue, the damage form was designated as "chipping" to distinguish it from "normal wear" and "fracture". Even if the tool reached the end of its life before the machining time reached 10 minutes, the damage form is also recorded for reference. Additionally, the machining time until the tool's flank wear width exceeded 0.15 mm or until it was fractured was designated the tool life. The measurement results are shown in Table 6.
[0065] [Table 6]
[0066] From the results shown in Table 6, the cubic boron nitride sintered body contains cubic boron nitride and a binder phase, the content of cubic boron nitride is 85% by volume or more and 95% by volume or less with respect to the total amount of the sintered body, the content of the binder phase is 5% by volume or more and 15% by volume or less with respect to the total amount of the sintered body, and the binder phase is Co3W3C, W2Co 21 B6, and Al compounds, and the X-ray diffraction peak intensity of the (111) plane of cubic boron nitride is I A , the X-ray diffraction peak intensity of the (400) plane of Co3W3C is I B , W2Co 21 The X-ray diffraction peak intensity of the (420) plane of B6 is I C , the X-ray diffraction peak intensity of the (001) plane of WC is I D Then, I B / I A is between 0.02 and 0.15, and I C / I A is between 0.02 and 1.00, and I C ≧I D It was found that the inventive product had better cutting performance and longer tool life than the non-inventive comparison product. [Industrial Applicability]
[0067] The cubic boron nitride sintered body of the present invention has excellent wear resistance and chipping resistance, and therefore can extend the tool life compared to conventional tools, and in that respect has high industrial applicability.
Claims
1. A cubic boron nitride sintered body comprising cubic boron nitride and a binder phase, the content of the cubic boron nitride is 85 volume % or more and 95 volume % or less with respect to the total amount of the sintered body, The content of the binder phase is 5 volume % or more and 15 volume % or less with respect to the total amount of the sintered body, The binder phase is Co 3 W 3 C.W. 2 Co 21 B 6 and an Al compound, The X-ray diffraction peak intensity of the (111) plane of the cubic boron nitride is I A , the Co 3 W 3 The X-ray diffraction peak intensity of the (400) plane of C is I B , the W 2 Co 21 B 6 The X-ray diffraction peak intensity of the (420) plane of C , the X-ray diffraction peak intensity of the (001) plane of WC is I D When I B / I A is equal to or greater than 0.02 and equal to or less than 0.15, I C / I A is 0.02 or more and 1.00 or less, A cubic boron nitride sintered body having an I D / I C ratio of 0.00 or more and 0.60 or less.
2. I D / I A 2. The cubic boron nitride sintered body according to claim 1, wherein is 0.00 or more and 0.20 or less.
3. I C / I B 3. The cubic boron nitride sintered body according to claim 1, wherein the cubic boron nitride sintered body has a crystallinity of 0.2 or more and 15.0 or less.
4. The W 2 Co 21 B 6 X-ray diffraction peak intensity I of the (420) plane C3. The cubic boron nitride sintered body according to claim 1, wherein the half-value width of is 0.25 or more and 0.60 or less.
5. 3. The cubic boron nitride sintered body according to claim 1, wherein the average grain size of the cubic boron nitride is 0.5 μm or more and 4.0 μm or less.
Citation Information
Patent Citations
Coated compound sintered compact, cutting tool and cutting method
JP2008222485A
Tool made of cubic boron nitride sintered body
US20130291446A1
Cubic boron nitride sintered body and cutting tool containing this
WO2020059756A1