Wafer grinding method

By using a chuck table with a specific diameter and a single grinding wheel for both self-grinding and TAIKO grinding, the method addresses thickness variations and enhances wafer rigidity and handling stability.

JP7570780B2Active Publication Date: 2024-10-22DISCO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021010002
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-26
Publication Date
2024-10-22
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Existing wafer grinding methods result in variations in thickness due to the use of different diameter grinding wheels for TAIKO and self-grinding, leading to reduced wafer rigidity and handling difficulties.

Method used

A method involving a chuck table with a larger diameter than the device region and smaller than the wafer, using a single grinding wheel for both self-grinding and TAIKO grinding to shape the holding surface and form a recess with a reinforcing portion, ensuring consistent thickness across the device region.

Benefits of technology

This approach reduces thickness variations by aligning the holding surface and device region shapes, enhancing wafer rigidity and handling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570780000001
    Figure 0007570780000001
  • Figure 0007570780000002
    Figure 0007570780000002
  • Figure 0007570780000003
    Figure 0007570780000003
Patent Text Reader

Abstract

To reduce a variation in the thickness of a portion (portion overlapping a recess) that includes the device region of a wafer obtained by performing TAIKO grinding on the reverse side of the wafer, the surface side of which is held to a holding plane which is curved by self-grind.SOLUTION: The diameter of holding plane of a chuck table is made to be larger than the diameter of a device region and smaller than the diameter of a wafer. In this case, the diameter of a grinding wheel used for self-grind can be made to be the same as the diameter of a grinding wheel used for TAIKO grinding. The holding plane of the chuck table and a region on the reverse side of the wafer obtained by applying TAIKO grinding that is equivalent to the device region can thereby be made to be of a similar shape. As a result of this, a variation in the thickness of a portion (portion overlapping a recess) that includes the device region can be reduced.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for grinding a wafer, the back surface of which has, on its front surface, a device region in which a plurality of devices are formed and a peripheral excess region surrounding the device region, is ground with a grinding wheel. [Background technology]

[0002] Device chips such as ICs (Integrated Circuits) and LSIs (Large Scale Integration) are essential components in various electronic devices such as mobile phones, personal computers, etc. Such chips are manufactured, for example, by thinning a wafer having a device region on its surface on which multiple devices are formed, and then dividing the wafer into regions each including an individual device.

[0003] As a method for thinning the wafer, for example, grinding is performed by a grinding device having a chuck table that holds the front side of the wafer with a circular upper surface (holding surface) and an annular grinding wheel that is provided above the chuck table and has a plurality of grinding stones that are arranged in a circular ring shape. In this grinding device, the back side of the wafer is ground by bringing the bottom surface of the grinding stone into contact with the back side of the wafer while rotating both the chuck table and the grinding wheel.

[0004] However, thinning the wafer reduces its rigidity, which may make it difficult to handle the wafer in subsequent processes. In view of this, a grinding method has been proposed in which a recess is formed in an area of ​​the back surface of the wafer that corresponds to the device area, and an annular reinforcing part is formed outside the outer periphery of the recess (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-19461 A Summary of the Invention [Problem to be solved by the invention]

[0006] Grinding to form recesses and reinforcing parts on the back surface of the wafer is also called TAIKO grinding, and is generally performed using a grinding wheel having a diameter approximately half that of the wafer. That is, in TAIKO grinding, a grinding wheel is used that is sized so that, when viewed from above, a point (first point) on the trajectory of the grinding wheel when the grinding wheel is rotated is positioned near the center of the wafer, and the point furthest from the first point on the trajectory of the grinding wheel (a point (second point) where the trajectory intersects with a straight line passing through the first point and the center of the trajectory) is positioned slightly inside the outer circumference of the wafer.

[0007] In addition, in a grinding device, the entire holding surface of the chuck table may be ground so that the area from the rotation center of the holding surface of the chuck table to the outer periphery is curved. This type of grinding is also called self-grinding, and is performed when the chuck table is replaced or periodically.

[0008] Self-grinding is generally performed using a grinding wheel having a diameter larger than half the diameter of the holding surface. That is, in self-grinding, a grinding wheel of a size is used such that, when viewed from above, a point (third point) on the trajectory of the grinding wheel when the grinding wheel is rotated is positioned near the center of rotation of the holding surface, and the point on the trajectory of the grinding wheel farthest from the third point (a point (fourth point) where the trajectory intersects with a straight line passing through the third point and the center of the trajectory) is positioned outside the outer circumference of the holding surface.

[0009] The shape of the holding surface curved by self-grinding varies depending on the diameter of the grinding wheel used. For example, if the diameter of the grinding wheel is slightly larger than half the diameter of the holding surface, the center of rotation and the outer periphery are at almost the same height, and the holding surface is curved so that the point located near the middle between the center of rotation and the outer periphery is the lowest. If the diameter of the grinding wheel is about 1.2 times half the diameter of the holding surface, the center of rotation is higher than the outer periphery, and the holding surface is curved so that the point closer to the outer periphery than the center of rotation is the lowest.

[0010] Furthermore, if TAIKO grinding is performed so that the area corresponding to the device area on the back surface of the wafer held on a curved holding surface is flat, the thickness of the part including the device area (the part overlapping the recess) of the resulting wafer will vary. For example, the thickness of the area of ​​the wafer held on the higher part of the holding surface (e.g., the center of the wafer) will be thinner than the thickness of the other areas.

[0011] To reduce such variations, it is necessary to grind the back surface of the wafer so that it curves in the same way as the holding surface. To do this, it is necessary to make the diameter of the grinding wheel used in TAIKO grinding approximately the same as the diameter of the grinding wheel used in self-grinding.

[0012] However, in a grinding apparatus, the wafer is generally ground in a state where the entire area of ​​the front surface side of the wafer is held on a chuck table. In other words, the holding surface of the chuck table is generally larger than the front surface of the wafer. Therefore, the diameter of the grinding wheel used in self-grinding is larger than half the diameter of the wafer.

[0013] As described above, TAIKO grinding is performed using a grinding wheel having a diameter approximately half the diameter of the wafer, so the grinding wheel used in TAIKO grinding must be smaller than the grinding wheel used in self-grinding.

[0014] In view of this, an object of the present invention is to reduce the variation in thickness of the portion including the device region of the wafer (the portion overlapping the recess) obtained by performing TAIKO grinding on the back surface of a wafer whose front surface side is held on a curved holding surface by self-grinding. [Means for solving the problem]

[0015] According to one aspect of the present invention, there is provided a wafer grinding method for grinding a back surface of a wafer having, on its surface, a circular device region in which a plurality of devices are formed and a circular outer peripheral excess region surrounding the device region, the method comprising: a holding surface shaping step of grinding the holding surface of a chuck table having a circular holding surface with a diameter larger than a diameter of the device region and smaller than a diameter of the wafer, the holding surface being rotated in a circumferential direction of the holding surface, with the grinding wheel of a first grinding wheel which is circular, to curve the region from the center of rotation of the holding surface to the outer periphery; a holding step, after the holding surface shaping step, in which the holding surface is held by the holding surface; and a grinding step, after the holding step, of grinding the back surface of the wafer corresponding to the device region with the grinding wheel of a second grinding wheel which is circular and has the same outer diameter as the first grinding wheel, to form a circular recess and a circular reinforcing portion surrounding the recess, and to curve the region from the center of rotation of the bottom of the recess to the outer periphery.

[0016] According to another aspect of the present invention, there is provided a wafer grinding method for grinding a back surface of a wafer having, on its surface, a circular device region in which a plurality of devices are formed and a circular outer peripheral excess region surrounding the device region, the method comprising: a holding step of: having a circular holding surface having a diameter larger than a diameter of the device region and smaller than a diameter of the wafer, and grinding the holding surface of a chuck table that rotates in the circumferential direction of the holding surface with the grinding wheel of a first grinding wheel that is circular, thereby holding the front side of the wafer on the holding surface having a curved region from the center of rotation of the holding surface to the outer periphery; and a grinding step of, after the holding step, grinding the back surface of the wafer corresponding to the device region with the grinding wheel of a second grinding wheel that is circular and has the same outer diameter as the first grinding wheel, to form a circular recess and a circular reinforcing portion surrounding the recess, and curving the region from the center of rotation of the bottom of the recess to the outer periphery.

[0017] Furthermore, in the present invention, it is preferable that the first grinding wheel and the second grinding wheel are the same grinding wheel. Effect of the Invention

[0018] In the present invention, the diameter of the holding surface of the chuck table is larger than the diameter of the device region and smaller than the diameter of the wafer. In this case, the diameter of the grinding wheel used in the self grinding can be the same as the diameter of the grinding wheel used in the TAIKO grinding.

[0019] This allows the holding surface of the chuck table and the area of ​​the back surface of the wafer obtained by TAIKO grinding that corresponds to the device area to have the same shape, which reduces the variation in thickness of the area including the device area (the area overlapping the recess). [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a perspective view that illustrates an example of a grinding device. [Diagram 2]FIG. 2 is a partial cross-sectional side view that shows a schematic view of some of the components of the grinding device. [Diagram 3] FIG. 3 is a perspective view illustrating an example of a wafer. [Figure 4] FIG. 4 is a flow chart that illustrates a schematic example of a wafer grinding method. [Diagram 5] FIG. 5 is a top view that typically illustrates the holding surface of the chuck table during self-grinding. [Figure 6] FIG. 6 is a diagram showing a schematic view of the holding surface of the chuck table being ground by a grinding wheel. [Figure 7] FIG. 7 is a top view diagrammatically showing the holding surface of the chuck table during TAIKO grinding. [Figure 8] FIG. 8 is a schematic diagram showing how the back surface of the wafer is ground with a grinding wheel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] An embodiment of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a perspective view showing an example of a grinding device. Note that the X-axis direction (front-back direction) and the Y-axis direction (left-right direction) shown in Fig. 1 are directions perpendicular to each other on a horizontal plane, and the Z-axis direction (up-down direction) is a direction (vertical direction) perpendicular to the X-axis direction and the Y-axis direction.

[0022] The grinding device 2 shown in Fig. 1 has a base 4 that supports each of the components. An opening 4a having a longitudinal portion extending along the X-axis direction is formed on the upper surface of the base 4. A ball screw type X-axis direction moving mechanism (not shown) is disposed inside the opening 4a. The X-axis direction moving mechanism has a pair of guide rails (not shown) that extend along the X-axis direction.

[0023] An X-axis moving plate (not shown) is connected to the top of the pair of guide rails in a manner that allows it to slide along the pair of guide rails. A screw shaft (not shown) extending along the X-axis direction is disposed between the pair of guide rails. A motor (not shown) for rotating the screw shaft is connected to one end of the screw shaft.

[0024] A nut portion (not shown) that houses balls that roll on the surface of the rotating screw shaft is provided on the surface of the screw shaft where the helical groove is formed, forming a ball screw. That is, when the screw shaft rotates, the balls circulate inside the nut portion, and the nut portion moves along the X-axis direction.

[0025] This nut is fixed to the underside of the X-axis moving plate (not shown). Therefore, when the screw shaft is rotated by a motor, the X-axis moving plate moves along the X-axis direction together with the nut.

[0026] A table cover 6 is provided on the X-axis moving table. A chuck table 8 that moves along the X-axis direction together with the X-axis moving table is provided on the table cover 6. The chuck table 8 and other components will now be described with reference to Fig. 2. Fig. 2 is a partially sectional side view that diagrammatically shows some of the components of the grinding device 2, such as the chuck table 8.

[0027] The chuck table 8 has a frame 10 made of a metal material such as stainless steel or ceramics. The frame 10 has a disk-shaped bottom wall and an annular side wall extending upward from the outer periphery of the bottom wall, and a recess is defined by the side wall. A suction path (not shown) is formed in the bottom of the recess. One end of the suction path is exposed at the bottom surface of the recess, and the other end of the suction path is connected to a suction source (not shown) such as an ejector.

[0028] A porous plate 12 is fixed in a recess of the frame 10. The bottom surface of the porous plate 12 is generally flat, and the top surface has a shape in which the center part protrudes slightly compared to the outer periphery, that is, a shape corresponding to the side of a cone. When the suction source is operated, negative pressure is generated on the top surface of the porous plate 12 (the holding surface 8a of the chuck table 8).

[0029] The upper part of a cylindrical spindle 14 is connected to the lower part of the chuck table 8. The chuck table 8 is removable from the spindle 14. The lower part of the spindle 14 is connected to a rotation drive source (not shown) such as a motor. When this rotation drive source is operated, the chuck table 8 rotates about a rotation axis 16 that passes through the center of the holding surface 8a. In other words, the chuck table 8 rotates in the circumferential direction of the holding surface 8a.

[0030] An annular bearing 18 is provided below the chuck table 8 to support the chuck table 8 in a rotatable manner. An annular support plate 20 is fixed below the bearing 18. An annular table base 22 is provided below the support plate 20. The spindle 14 is located in an opening provided in the center of each of the bearing 18, the support plate 20, and the table base 22.

[0031] Three support mechanisms (a fixed support mechanism 26a, a first movable support mechanism 26b, and a second movable support mechanism 26c) are provided on the lower surface side of the table base 22 so as to be spaced apart from each other along the circumferential direction of the lower surface of the table base 22. In this specification, these three support mechanisms are collectively referred to as the tilt adjustment unit 26.

[0032] The table base 22 is supported by a fixed support mechanism 26a, a first movable support mechanism 26b, and a second movable support mechanism 26c. The fixed support mechanism 26a has a pillar (fixed shaft) of a predetermined length. The upper part of this pillar supports an upper support body fixed to the lower surface of the table base 22, and the lower part of this pillar is fixed to the support base.

[0033] Each of the first movable support mechanism 26b and the second movable support mechanism 26c has a pillar (movable shaft) 28 having a male screw formed at its tip. The tip (upper part) of the pillar 28 is rotatably connected to an upper support 30 fixed to the lower surface of the table base 22. More specifically, the upper support 30 is a metallic columnar member such as a rod having a female screw, and the male screw of the pillar 28 is rotatably connected to the female screw of the upper support 30.

[0034] An annular bearing 32 having a predetermined outer diameter is fixed to the outer periphery of the support column 28 of the first movable support mechanism 26b and the second movable support mechanism 26c. A portion of the bearing 32 is supported by a stepped support plate 34. In other words, the first movable support mechanism 26b and the second movable support mechanism 26c are supported by the support plate 34.

[0035] A motor 36 that rotates the support pillar 28 is connected to the lower part of the support pillar 28. By operating the motor 36 to rotate the support pillar 28 in one direction, the upper support 30 rises. By operating the motor 36 to rotate the support pillar 28 in the other direction, the upper support 30 falls. In this manner, the upper supports 30 of the first movable support mechanism 26b and the second movable support mechanism 26c rise and fall, thereby adjusting the inclination of the table base 22 (i.e., the chuck table 8).

[0036] 1 again, other components of the grinding device 2 will be described. A bellows-shaped dustproof and drip-proof cover 38 that is expandable and contractible in the X-axis direction is provided in the opening 4a so as to sandwich the table cover 6. An operation panel 40 for inputting grinding conditions and the like is provided near the front end of the opening 4a.

[0037] Further, near the rear end of the opening 4a, a rectangular parallelepiped support structure 42 extending upward is provided. A Z-axis direction movement mechanism 44 is provided on the front side (i.e., the operation panel 40 side) of the support structure 42. The Z-axis direction movement mechanism 44 includes a pair of Z-axis guide rails 46 extending along the Z-axis direction.

[0038] A Z-axis moving plate 48 is connected to the front side of the pair of Z-axis guide rails 46 in a manner that allows it to slide along the pair of Z-axis guide rails 46. A screw shaft 50 extending along the Z-axis direction is disposed between the pair of Z-axis guide rails 46. A motor 52 for rotating the screw shaft 50 is connected to one end of the screw shaft 50.

[0039] A nut portion (not shown) that accommodates balls that roll on the surface of the rotating screw shaft 50 is provided on the surface of the screw shaft 50 on which the helical groove is formed, thereby forming a ball screw. That is, when the screw shaft 50 rotates, the balls circulate inside the nut portion, and the nut portion moves along the Z-axis direction.

[0040] Moreover, this nut portion is fixed to the rear surface side of the Z-axis moving plate 48. Therefore, when the screw shaft 50 is rotated by the motor 52, the Z-axis moving plate 48 moves along the Z-axis direction together with the nut portion.

[0041] A support 54 is provided on the front side of the Z-axis moving plate 48. The support 54 supports a grinding unit 56. The grinding unit 56 has a cylindrical spindle housing 58 fixed to the support 54. A part of a columnar spindle 60 extending along the Z-axis direction is housed in the spindle housing 58 in a rotatable state.

[0042] A motor 62 for rotating the spindle 60 is connected to the upper end of the spindle 60. The lower end of the spindle 60 is exposed from the spindle housing 58, and the upper surface of a disk-shaped wheel mount 64 made of a metal material such as stainless steel is fixed to this lower end.

[0043] An annular grinding wheel 66 having approximately the same diameter as the wheel mount 64 is attached to the lower part of the wheel mount 64. The grinding wheel 66 is removably connected to the lower part of the wheel mount 64, and has a diameter approximately half the diameter of the holding surface 8a of the chuck table 8.

[0044] 2, the grinding wheel 66 has an annular wheel base 68. The wheel base 68 is made of a metal material such as stainless steel, and a plurality of grinding wheels 70 are discretely arranged on the underside of the wheel base 68 along the circumferential direction of the underside. The undersides of the plurality of grinding wheels 70 are arranged at approximately the same height in the Z-axis direction, and a grinding surface 72 for grinding the workpiece is defined by the underside.

[0045] When the motor 62 operates to rotate the spindle 60, the grinding wheel 66 rotates about a rotation axis 74 that passes through the center of the grinding surface 72. Furthermore, a nozzle (not shown) is provided near or inside the grinding wheel 66 for supplying a grinding fluid such as water to the grinding surface 72 when performing the desired grinding (for example, TAIKO grinding or self grinding).

[0046] Fig. 3 is a perspective view showing a schematic example of a wafer ground by the grinding apparatus 2. The wafer 11 shown in Fig. 3 is made of a semiconductor material such as silicon (Si). The wafer 11 is divided into a plurality of regions by a plurality of planned dividing lines 13 that intersect with each other.

[0047] The front surface 11a of the wafer 11 has a circular device region 15a (the region inside the dotted line shown in FIG. 3) having a smaller diameter than the holding surface 8a (see FIGS. 1 and 2) of the chuck table 8. Devices 17 such as ICs or LSIs are formed in each of a plurality of regions defined by the planned division lines 13 in the device region 15a.

[0048] Furthermore, the surface 11a of the wafer 11 has an annular outer peripheral excess region 15b (the region outside the dotted line shown in FIG. 3) that surrounds the device region 15a and has an outer diameter larger than the diameter of the holding surface 8a. That is, the diameter of the surface 11a of the wafer 11 is larger than the diameter of the holding surface 8a.

[0049] There are no limitations on the material, shape, structure, size, etc. of the wafer 11. For example, the wafer 11 may be a substrate made of a semiconductor material other than silicon, ceramics, resin, metal, etc. Similarly, there are no limitations on the type, number, shape, structure, size, arrangement, etc. of the devices 17.

[0050] In addition, a film-like protective member 19 having a diameter approximately equal to that of the wafer 11 is attached to the front surface 11a of the wafer 11. The protective member 19 is made of, for example, resin, and protects the device 17 by absorbing the impact applied to the front surface 11a when the back surface 11b of the wafer 11 is ground.

[0051] The protective member 19 has, for example, a base material layer and a glue layer (adhesive layer) provided on one surface of the base material layer, and this glue layer is attached to the front surface 11a of the wafer 11. Alternatively, the protective member 19 may be composed of only the base material layer, and may be attached to the front surface 11a side by thermocompression bonding or the like.

[0052] 4 is a flow chart that illustrates an example of a wafer grinding method for grinding the back surface 11b of the wafer 11 using the grinding device 2. In this method, first, the holding surface 8a of the chuck table 8 is ground with a grinding wheel of a self-grinding grinding wheel (first grinding wheel) so that the region from the rotation center of the holding surface 8a of the chuck table 8 to the outer periphery is curved (holding surface shaping step: S1).

[0053] A specific example of the holding surface shaping step (S1) will be described with reference to Fig. 5 and Fig. 6. Fig. 5 is a top view showing the holding surface 8a of the chuck table 8 during self-grinding. Fig. 6 is a view showing the holding surface 8a being ground by a grinding wheel 70a arranged on the lower surface side of a wheel base 68a of a grinding wheel 66a for self-grinding. Furthermore, in Fig. 5, a trajectory 76 of the rotating grinding wheel 70a is shown by a dotted line.

[0054] In the holding surface shaping step (S1), first, an X-axis movement mechanism provided inside opening 4a (see FIG. 1) is operated to move chuck table 8 along the X-axis direction so that, in a top view, a point (first point) on locus 76 is positioned near the center of rotation of holding surface 8a, and the point on locus 76 farthest from the first point (the point (second point) where the straight line passing through the first point and the center of locus 76 intersects with locus 76) is positioned outside the outer periphery of holding surface 8a (see FIG. 5).

[0055] Next, the inclination of the rotation axis 16 of the chuck table 8 is adjusted by the inclination adjustment unit 26. This point will be described in detail below. If the generating line 8b of the holding surface 8a, which overlaps with the line extending from one end to the other end of the trajectory 76, is parallel to the grinding surface 72, the generating line 8b becomes the part of the holding surface 8a that is closest to the grinding surface 72. That is, in this case, the rotation center of the holding surface 8a located at one end of the generating line 8b and the point on the outer periphery of the holding surface 8a located at the other end of the generating line 8b become the points on the holding surface 8a that are closest to the grinding wheel 70.

[0056] In this state, if the first movable support mechanism 26b operates to raise the chuck table 8, the inclination of the rotation axis 16 of the holding surface 8a changes so that the area of ​​the holding surface 8a shown in Fig. 5 close to the first movable support mechanism 26b becomes closer to the grinding surface 72 than the remaining area. That is, the inclination of the rotation axis 16 of the chuck table 8 is adjusted by the inclination adjustment unit 26.

[0057] As a result, for example, the distance between the grinding wheel 70 adjacent to the first movable support mechanism 26b and the holding surface 8a can be made shorter than the distance between one end and the other end of the generatrix 8b and the grinding wheel 70. If self-grinding is performed as shown in Fig. 6 while maintaining this inclination of the rotating shaft 16, the amount of grinding in the region located midway between the rotation center and the outer periphery of the holding surface 8a will be greater than the amount of grinding in the remaining region. As a result, the region from the rotation center to the outer periphery of the holding surface 8a will be curved.

[0058] 4, after the holding surface shaping step (S1), the front surface 11a side of the wafer 11 is held on the holding surface 8a of the chuck table 8 (holding step: S2). Specifically, first, the X-axis direction moving mechanism provided inside the opening 4a is operated to move the chuck table 8 forward along the X-axis direction to a position where the wafer 11 can be loaded (see FIG. 1).

[0059] Next, the wafer 11 is placed on the holding surface 8a via the protective member 19 so that the center of the wafer 11 is positioned directly above the center of rotation of the holding surface 8a. At this time, since the diameter of the surface 11a of the wafer 11 is larger than the diameter of the holding surface 8a, the outer periphery of the wafer 11 is positioned outside the outer periphery of the holding surface 8a. In other words, the vicinity of the outer periphery of the wafer 11 does not come into contact with the holding surface 8a.

[0060] Next, a suction source connected to the chuck table 8 is operated to generate a negative pressure on the holding surface 8a. As a result, the front surface 11a side of the wafer 11 is suction-held on the holding surface 8a of the chuck table 8 via the protective member 19.

[0061] In the wafer grinding method shown in FIG. 4, after the holding step (S2), the back surface 11b of the wafer 11 corresponding to the device region 15a is ground with a grinding wheel of a grinding wheel (second grinding wheel) for TAIKO grinding having the same outer diameter as the grinding wheel 66a for self-grinding (grinding step: S3).

[0062] A specific example of the grinding step (S3) will be described with reference to Fig. 7 and Fig. 8. Fig. 7 is a top view that typically shows the holding surface 8a of the chuck table 8 during TAIKO grinding. Fig. 8 is a view that typically shows how the back surface 11b of the wafer 11 is ground by a grinding wheel 70b arranged on the lower surface side of a wheel base 68b of a grinding wheel 66b for TAIKO grinding. Furthermore, in Fig. 7, the wafer 11 held on the holding surface 8a and the trajectory 78 of the rotating grinding wheel 70b are shown by dotted lines.

[0063] In the grinding step (S3), the grinding wheel 66a for self-grinding attached to the wheel mount 64 is first replaced with a grinding wheel 66b for TAIKO grinding having the same outer diameter as the grinding wheel 66a. Therefore, the outer diameter of the trajectory 76 of the grinding wheel 70a when the grinding wheel 66a for self-grinding rotates is approximately equal to the outer diameter of the trajectory 78 of the grinding wheel 70b when the grinding wheel 66b for TAIKO grinding rotates. The grinding wheel 66a and the grinding wheel 66b may be the same grinding wheel. In this case, it is preferable because there is no need to replace the grinding wheel.

[0064] Next, the X-axis direction moving mechanism provided inside the opening 4a (see FIG. 1) is operated to move the chuck table 8 backward along the X-axis direction so that, in a top view, a point (third point) on the locus 78 is positioned near the center of the wafer 11 (i.e., the rotation center of the holding surface 8a) and the point on the locus 78 farthest from the third point (the point (fourth point) where the line passing through the third point and the center of the locus 78 intersects with the locus 78) is positioned slightly inside the outer periphery of the holding surface 8a (see FIG. 7).

[0065] Next, in TAIKO grinding, the inclination of the rotation axis 16 of the chuck table 8 is adjusted by the inclination adjustment unit 26 so that the area of ​​the back surface 11b of the wafer 11 corresponding to the device area 15a is curved in the same manner as the holding surface 8a. If the inclination of the rotation axis 16 adjusted in the holding surface shaping step (S1) has not been changed, it is not necessary to adjust the inclination of the rotation axis 16 again.

[0066] Then, if TAIKO grinding is performed as shown in Figure 8 while maintaining this inclination of the rotation axis 16, a circular recess 11c and an annular reinforcing portion 11d surrounding the recess 11c are formed on the back surface 11b of the wafer 11, and the area from the center of rotation of the bottom surface of the recess 11c to the outer periphery is curved.

[0067] 4, the diameter of the holding surface 8a of the chuck table 8 where self-grinding is performed is larger than the diameter of the device region 15a and smaller than the diameter of the wafer 11. In this case, the diameter of the grinding wheel 66a used for self-grinding can be the same as the diameter of the grinding wheel 66b used for TAIKO grinding.

[0068] This allows the holding surface 8a of the chuck table 8 and the area corresponding to the device region 15a on the back surface 11b of the wafer 11 obtained by TAIKO grinding to have the same shape. As a result, it is possible to reduce the variation in thickness of the portion including the device region 15a (the portion overlapping the recess 11c).

[0069] It should be noted that the wafer grinding method shown in Fig. 4 is merely one aspect of the present invention, and the wafer grinding method of the present invention is not limited to the wafer grinding method shown in Fig. 4. For example, in the present invention, it is not always necessary to perform the holding surface shaping step (S1) prior to the above-mentioned holding step (S2) and grinding step (S3).

[0070] In other words, when TAIKO grinding is performed on multiple wafers, it is sufficient to perform the holding surface shaping step (S1) prior to processing the first wafer, and it is not necessary to perform the holding surface shaping step (S1) prior to processing each wafer.

[0071] In addition, the existing chuck table connected to the upper part of the spindle 14 may be replaced with a chuck table in which the area from the rotation center to the outer periphery of the holding surface is curved, for example by performing a holding surface shaping step (S1) in advance, and then the above-mentioned holding step (S2) and grinding step (S3) may be performed.

[0072] In addition, the structures and methods according to the above-described embodiments and modifications can be modified as appropriate without departing from the scope of the present invention. [Explanation of symbols]

[0073] 2: Grinding equipment 4: Base (4a: opening) 6: Table cover 8: Chuck table (8a: holding surface) 10:Frame body 12: Porous plate 14: Spindle 16: Rotation axis 18: Bearings 20: Support plate 22: Table base 26: Adjustment unit (26a: fixed support mechanism, 26b, 26c: movable support mechanisms) 28: Post 30: Upper support 32: Bearing 34: Support plate 36: Motor 38: Dust-proof and water-resistant cover 40: Operation panel 42:Support structure 44:Z-axis direction movement mechanism 46: Z-axis guide rail 48: Z-axis moving plate 50: Screw shaft 52: Motor 54: Support 56: Grinding unit 58: Spindle housing 60:Spindle 62: Motor 64: Wheel mount 66(66a, 66b): Grinding wheel 68(68a, 68b): Wheel base 70(70a,70b): Grinding wheel 72: Grinding surface 74: Rotation axis 76,78:Trajectory 11: Wafer (11a: front surface, 11b: back surface) 13: Planned division line 15a: Device area 15b: Surplus outer area 17: Device 19: Protective material

Claims

1. A wafer grinding method for grinding a back surface of a wafer having a front surface including a circular device region in which a plurality of devices are formed and an annular peripheral excess region surrounding the device region, the method comprising the steps of: a holding surface shaping step of grinding the holding surface of a chuck table which has a circular holding surface having a diameter larger than a diameter of the device region and smaller than a diameter of the wafer and rotates in a circumferential direction of the holding surface with a grinding stone of a first grinding wheel which is an annular shape, thereby curving a region from a rotation center of the holding surface to an outer periphery; a holding step of holding the front surface side of the wafer on the holding surface after the holding surface shaping step; and a grinding step of grinding the back surface of the wafer corresponding to the device region with a grinding stone of a second grinding wheel having an annular shape and an outer diameter equal to that of the first grinding wheel, thereby forming a circular recess and an annular reinforcing portion surrounding the recess, and curving a region from a rotation center of the bottom surface of the recess to an outer periphery.

1. A method for grinding a wafer, comprising the steps of:

2. A wafer grinding method for grinding a back surface of a wafer having a front surface including a circular device region in which a plurality of devices are formed and an annular peripheral excess region surrounding the device region, the method comprising the steps of: a holding step in which a holding surface of a chuck table having a circular holding surface with a diameter larger than a diameter of the device region and smaller than a diameter of the wafer, the holding surface being ground by a grinding wheel of a first grinding wheel having an annular shape, the holding surface rotating in a circumferential direction of the holding surface, thereby holding the front side of the wafer on the holding surface having a curved region from a rotation center of the holding surface to an outer periphery; and a grinding step of grinding the back surface of the wafer corresponding to the device region with a grinding stone of a second grinding wheel having an annular shape and an outer diameter equal to that of the first grinding wheel, thereby forming a circular recess and an annular reinforcing portion surrounding the recess, and curving a region from a rotation center of the bottom surface of the recess to an outer periphery.

1. A method for grinding a wafer, comprising the steps of:

3. 3. The method for grinding a wafer according to claim 1, wherein the first grinding wheel and the second grinding wheel are the same grinding wheel.

Citation Information

Patent Citations

  • Method for processing wafer and wafer

    JP2007019461A

  • Working method for wafer

    JP2008060470A

  • Semiconductor device, method of manufacturing semiconductor device, and manufacturing device for semiconductor device

    JP2009279661A

  • Table shaping method

    JP2015072972A

  • Electrostatic chuck device and method of manufacturing electrostatic chuck device

    WO2020044843A1