Martensitic stainless steel sheet and method for producing same

By controlling carbonitride content and optimizing the annealing process, the martensitic stainless steel sheet achieves improved bendability and delayed fracture resistance, addressing the limitations of existing martensitic stainless steel sheets.

JP7570858B2Active Publication Date: 2024-10-22NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020153203
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-11
Publication Date
2024-10-22
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Martensitic stainless steel sheets exhibit poor bendability and insufficient delayed fracture resistance, limiting their application in corrosive environments.

Method used

A martensitic stainless steel sheet composition with controlled carbonitride content and a manufacturing process involving specific annealing temperatures and cooling rates to achieve a martensitic phase structure, reducing undissolved carbonitrides to less than 1.0% area ratio.

Benefits of technology

The solution results in a martensitic stainless steel sheet with improved bendability and enhanced delayed fracture resistance, achieving a 0.2% proof stress of 1300 N/mm and excellent stress corrosion cracking resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570858000003
    Figure 0007570858000003
  • Figure 0007570858000004
    Figure 0007570858000004
  • Figure 0007570858000001
    Figure 0007570858000001
Patent Text Reader

Abstract

To provide a martensitic stainless steel sheet that has excellent bendability and has excellent resistance to delayed fracture.SOLUTION: A martensitic stainless steel sheet contains, in mass%, C: 0.10% or more and 0.15% or less, Si: 0.05% or more and 0.80% or less, Mn: 0.05% or more and 2.00%, P: 0.04% or less, S: 0.003% or less, Ni: 0.50% or less, Cr: 11.0% or more and 15.0% or less, Cu: 0.50% or less, N: 0.005% or more and 0.06% or less, Al: 0.20% or less with the balance being Fe, carbonitrides and inevitable impurities. The M value determined by the following formula (1) is 95.0 or more. The matrix is a martensite phase. In a cross section parallel with a rolling direction and a thickness direction, the carbonitrides have an area ratio of 1.00% or less. Formula (1): M value=420C-11.5Si+7Mn+23Ni-11.5Cr-12Mo-10V+9Cu-52Al+470N+189.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a martensitic stainless steel sheet and a method for producing a martensitic stainless steel sheet. [Background technology]

[0002] Metastable austenitic stainless steel is known as a stainless steel grade suitable for spring materials such as gasket materials, such as cylinder head gaskets for automobiles and motorcycles, retractor spiral springs for automobile seat belts, and springs for electronic equipment parts. However, metastable austenitic stainless steel is expensive because of its high Ni content. Therefore, martensitic stainless steel has attracted attention as a stainless steel grade that can be used for spring materials and is less expensive than metastable austenitic stainless steel.

[0003] However, martensitic stainless steels generally have poor bendability. In addition, because spring members are used in various corrosive environments, it is necessary to improve resistance to delayed fracture in order to use martensitic stainless steels as spring members. Various studies have been conducted to overcome these issues. For example, Patent Document 1 describes a martensitic stainless steel that has good bendability and a 0.2% proof stress in the rolling direction of 1100 N / mm 2 The above discloses a martensitic stainless steel sheet that is also excellent in resistance to delayed fracture.

[0004] Here, delayed fracture is a phenomenon in which a martensitic stainless steel sheet undergoes sudden brittle fracture without any apparent plastic deformation after a certain period of time has elapsed while the martensitic stainless steel sheet is subjected to a static load stress. Stress corrosion cracking is an example of a phenomenon that is a precursor to delayed fracture. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-157229 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, it has been found that although the martensitic stainless steel sheet disclosed in Patent Document 1 has good bendability, its delayed fracture resistance is not necessarily sufficient.

[0007] An object of one aspect of the present invention is to provide a martensitic stainless steel sheet or the like having good bendability and excellent resistance to delayed fracture. [Means for solving the problem]

[0008] In order to solve the above problems, a martensitic stainless steel sheet according to one embodiment of the present invention contains, by mass%, C: 0.10% or more and 0.15% or less, Si: 0.05% or more and 0.80% or less, Mn: 0.05% or more and 2.0% or less, P: 0.04% or less, S: 0.003% or less, Ni: 0.50% or less, Cr: 11.0% or more and 15.0% or less, Cu: 0.50% or less, N: 0.005% or more and 0.06% or less, Al: 0.20% or less, with the balance being Fe, carbonitrides, and unavoidable impurities; The M value determined by the following formula (1) is 95.0 or more, The matrix is ​​a martensite phase, The area ratio of the carbonitrides in a cross section parallel to the rolling direction and the sheet thickness direction is 1.0% or less: M value = 420C-11.5Si+7Mn+23Ni-11.5Cr-12Mo-10V+9Cu-52Al+470N+189 (1) In the above formula (1), the content (mass%) of each element contained in the martensitic stainless steel sheet is substituted for the element symbol, and 0 (zero) is substituted for elements that are not added.

[0009] The martensitic stainless steel sheet according to one embodiment of the present invention may further contain, by mass%, one or more selected from Mo: 1.00% or less, V: 0.50% or less, and B: 0.0001% or more and 0.01% or less.

[0010] In order to solve the above problems, a method for producing a martensitic stainless steel sheet according to one embodiment of the present invention includes a finish annealing step in which finish annealing is performed by holding the temperature range of 1040°C or higher and 1150°C or lower for 30 seconds or more.

[0011] In one embodiment of the manufacturing method for a martensitic stainless steel sheet according to the present invention, in the finish annealing step, the above temperature range may be maintained for 30 seconds or more, and then the temperature may be cooled to 100°C at a cooling rate of 2.0°C / sec or more and 20.0°C / sec or less. Effect of the Invention

[0012] According to one aspect of the present invention, a steel sheet having good bendability and a 0.2% proof stress in the rolling direction of 1300 N / mm 2 Thus, a martensitic stainless steel sheet or the like having excellent resistance to delayed fracture can be realized. [Brief description of the drawings]

[0013] [Figure 1] Reference numeral 101 denotes an SEM photograph showing the observation surface of a martensitic stainless steel sheet according to one embodiment of the present invention. Reference numeral 102 denotes an SEM photograph showing the observation surface of a martensitic stainless steel sheet according to another embodiment of the present invention. Reference numeral 103 denotes an SEM photograph showing the observation surface of a martensitic stainless steel sheet according to a comparative example of the present invention. [Diagram 2] Reference numeral 201 is a perspective view showing the surface shape of a sample of a martensitic stainless steel sheet according to an embodiment of the present invention, and reference numeral 202 is a perspective view showing the surface shape of a sample of a martensitic stainless steel sheet according to a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, a martensitic stainless steel sheet according to one embodiment of the present invention will be described in detail. The following description is intended to provide a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."

[0015] [Mechanism for improving delayed fracture resistance] In the manufacturing process of martensitic stainless steel sheets, hot-rolled steel sheets are usually annealed for a long time at a temperature below the Ac1 point to decompose the martensite phase in the hot-rolled steel sheet into ferrite phase and carbonitrides. Carbonitrides are particles consisting of a compound phase in which either C or N or both C and N are bonded to a metal element. Carbide particles that contain almost no N and nitride particles that contain almost no C are also classified as carbonitrides.

[0016] By annealing the hot-rolled sheet, the hard martensite phase is eliminated as much as possible and the hot-rolled steel sheet is softened, which makes it easier to adjust the sheet thickness in the subsequent cold rolling. The thin sheet material adjusted to the target sheet thickness by cold rolling is heated to a specified temperature in the austenite single phase temperature range, held in the austenite single phase temperature range for a specified time, and then cooled to near room temperature to obtain a high-strength martensite structure. This series of heat treatments is called "finish annealing."

[0017] In this specification, the process of the finish annealing in which the temperature of the thin plate material is raised to a predetermined temperature in the austenite single-phase temperature range is referred to as the "heating process", and the predetermined temperature is referred to as the "maximum material temperature reached". In addition, the process of holding the thin plate material that has been subjected to the heating process in the austenite single-phase temperature range for a predetermined time is referred to as the "temperature holding process", and the austenite single-phase temperature range that is the temperature range of the thin plate material in the temperature holding process is referred to as the "holding temperature range". In addition, the process of cooling the thin plate material that has been subjected to the temperature holding process to near room temperature is referred to as the "cooling process".

[0018] Although the solid solution reaction of the carbonitrides in the thin plate material progresses by performing the finish annealing, some of the carbonitrides remain even after the finish annealing. That is, in the finish annealing, holding the thin plate material at a high temperature for a long time at which the carbonitrides completely dissolve and disappear is a factor that leads to a decrease in productivity. In addition, in general, there is no need to make the structure of the thin plate material a state in which the carbonitrides completely disappear. For these reasons, the matrix (metal base) of the martensitic stainless steel plate usually contains carbonitrides that remain undissolved and are dispersed. In this specification, the carbonitrides that remain undissolved are referred to as "undissolved carbonitrides".

[0019] The C that constitutes the undissolved carbonitride is mainly M 23 It is believed to be bound to a metal element in the form of C6. 23 "M" in C6 is a metal element that composes the matrix, such as Cr or Fe. The fact that the granular phase dispersed in the matrix is ​​undissolved carbonitride can be confirmed by analysis using an EPMA (electron probe microanalyzer). Alternatively, it can be confirmed by analysis methods such as EDX (energy dispersive X-ray analysis).

[0020] As a result of detailed research, the inventors have found that the occurrence of the above-mentioned delayed fracture, which is a problem in martensitic stainless steel sheets, can be reduced by limiting the amount of undissolved carbonitrides present. In other words, they have found that the delayed fracture resistance of martensitic stainless steel sheets can be improved by limiting the amount of undissolved carbonitrides present. This finding is based on the assumption that undissolved carbonitrides function as trap sites for H2, and the increased hydrogen concentration in the martensitic stainless steel sheets induces stress corrosion cracking, which leads to delayed fracture.

[0021] There are several methods for limiting the amount of undissolved carbonitrides present in order to improve delayed fracture resistance, such as limiting the number of undissolved carbonitrides with a large particle size, for example, a circle equivalent diameter of 1.00 μm or more. Among these, the 0.2% proof stress in the rolling direction is 1300 N / mm 2The inventors have found through extensive research that for martensitic stainless steel sheets with the above strength levels, the delayed fracture resistance can be improved by setting the area ratio of undissolved carbonitrides to 1.0% or less. Specifically, the "area ratio of undissolved carbonitrides" is the ratio, expressed in percentage (%), of the total area of ​​undissolved carbonitride regions present in a cross section (L cross section) parallel to the rolling direction and the sheet thickness direction of the martensitic stainless steel sheet. Here, the "rolling direction" refers to the direction in which the steel sheet is passed through the equipment when the steel sheet is hot-rolled and cold-rolled. The cross section may be arbitrarily selected, and it has been found that the delayed fracture resistance can be improved by adjusting the area ratio of undissolved carbonitrides to 1.0% or less in the arbitrarily selected cross section.

[0022] It is believed that some of the precipitated particles in the martensitic stainless steel sheet have a strong bond with trapped H2 and are beneficial in suppressing the diffusion of H2. However, undissolved carbonitrides have a weak bond with H2 and do not exhibit the function of suppressing the diffusion of H2. The present invention was completed based on the above findings, and undissolved carbonitrides are one example of the carbonitrides according to the present invention.

[0023] [Component composition] The martensitic stainless steel sheet according to one embodiment of the present invention has a martensite phase matrix, and contains, by mass%, C: 0.10-0.15%, Si: 0.05-0.80%, Mn: 0.05-2.00%, P: 0.04% or less, S: 0.003% or less, Ni: 0.50% or less, Cr: 11.0-15.0%, Cu: 0.50% or less, N: 0.005-0.06%, Al: 0.20% or less, Mo: 1.00% or less, V: 0.50% or less, and B: 0.0001-0.01%. In the following description, the martensitic stainless steel sheet according to one embodiment of the present invention is abbreviated to "the present stainless steel sheet". In addition, unless otherwise specified, "%" indicating the content ratio of each element means mass%.

[0024] The balance of the stainless steel sheet consists of Fe, undissolved carbonitrides, and unavoidable impurities. Note that Mo, V, and B are not essential elements of the stainless steel sheet, but are optional elements that may contain at least one of these elements as necessary. Each element contained in the stainless steel sheet is described below.

[0025] <c> Carbon (C) is an austenite-forming element that makes it easier to form the austenite phase, and is effective in strengthening the martensite phase. If the C content is too low, not only will the martensite phase not be strengthened sufficiently, but it will also be difficult to adjust the composition (adjust the M value, described below) to obtain the austenite phase by the temperature holding treatment in the final annealing. For these reasons, the C content is set to 0.10% or more.

[0026] On the other hand, if the C content is too high, the amount of undissolved carbonitrides increases more than necessary, making it difficult to adjust the area ratio of undissolved carbonitrides to 1.0% or less. In addition, new Cr carbides precipitate at grain boundaries during the cooling treatment in the finish annealing, which is a factor in reducing the corrosion resistance of this stainless steel sheet. For these reasons, the C content is set to 0.15% or less.

[0027] <si> Silicon (Si) is effective as a deoxidizer and also hardens the martensite phase, contributing to high strength of steel. To bring out these properties, the Si content is set to 0.05% or more. To bring out these properties even more, it is preferable to make the Si content 0.20% or more.

[0028] However, if the Si content is too high, it will cause a decrease in the workability and toughness of the present stainless steel sheet. Also, it will be difficult to achieve a predetermined value or more of the M value described below. For these reasons, the Si content is set to 0.80% or less. In order to ensure the workability and toughness of the present stainless steel sheet, or to easily adjust the M value to a predetermined value or more, it is preferable that the Si content be set to 0.60% or less.

[0029] Mn (manganese) is an austenite-forming element. In order to make the M value equal to or greater than a predetermined value, the Mn content is set to 0.05% or more. In order to easily adjust the M value to equal to or greater than a predetermined value, the Mn content is preferably set to 0.10% or more. However, if the Mn content is too high, the stability of the austenite phase increases. Therefore, there is a risk that the austenite phase will remain after finish annealing, reducing the strength of this stainless steel sheet. In order to avoid this disadvantage, the Mn content is set to 2.00% or less. In order to ensure the strength of this stainless steel sheet, the Mn content is preferably set to 1.0% or less.

[0030] <ni> Ni (nickel) is an austenite-forming element. If the Ni content is too high, the austenite phase becomes more stable. As a result, there is a risk that the austenite phase will remain after finish annealing, reducing the strength of the stainless steel sheet. In addition, since Ni is an expensive element, if the Ni content is too high, it will lead to an increase in manufacturing costs. For these reasons, the Ni content is set to 0.50% or less.

[0031] <cr> Cr (chromium) is an essential element for ensuring corrosion resistance. However, since Cr is a ferrite-forming element, if the Cr content is too high, the contents of austenite-forming elements such as C, Ni, and Mn must be increased to obtain a martensite structure, which leads to an increase in manufacturing costs. In addition, if the Cr content is too high, it can also cause a decrease in the toughness of the stainless steel sheet. For these reasons, the Cr content is set to 11.0 to 15.0%. From the viewpoints of ensuring corrosion resistance and toughness and reducing costs, the Cr content is preferably set to 11.5 to 13.5%.

[0032] <cu> Cu (copper) is an austenite forming element and is effective in increasing the M value to a specified value or higher. When added in trace amounts, it can improve the corrosion resistance of this stainless steel sheet, but if the Cu content is too high, it can actually decrease the corrosion resistance. For these reasons, the Cu content is set to 0.50% or less.

[0033] <n> N (nitrogen) is an austenite forming element, and like C, is effective in strengthening the martensite phase. N is more likely to exist in a solid solution state in the matrix than C, even if the cooling rate during the cooling treatment in the final annealing is relatively slow. On the other hand, its effect of strengthening the martensite phase is weaker than that of C. For these reasons, the N content is set to 0.005 to 0.06%.

[0034] <al> Al (aluminum) is an element with a strong deoxidizing effect. However, deoxidizing the present stainless steel sheet mainly with Si is more advantageous than deoxidizing with Al alone in that it softens oxide-based inclusions to ensure workability and reduces the anisotropy of fatigue resistance properties. If the Al content is too high, it may have a negative effect on the toughness of the present stainless steel sheet. Furthermore, since Al is a ferrite-forming element, if the Al content is too high, it becomes difficult to adjust the composition of other elements to obtain a martensite structure, and the manufacturing cost also increases. For these reasons, the Al content is set to 0.20% or less.

[0035] Mo (molybdenum) is an element that is effective in improving corrosion resistance. However, since Mo is an expensive element, if the Mo content is too high, it will lead to an increase in manufacturing costs. In addition, since Mo is a ferrite forming element, if the Mo content is too high, it will be difficult to adjust the composition of other elements to obtain a martensite structure. For these reasons, the Mo content is set to 1.00% or less.

[0036] <V、B> V (vanadium) and B (boron) are elements effective in improving strength and fatigue resistance. V is also an effective element in improving corrosion resistance. Furthermore, B is also an effective element in improving hot workability. Since V is an expensive element, if the V content is too high, the manufacturing cost will increase. If the B content is too high, the precipitation of Cr2B will lead to a decrease in corrosion resistance. For these reasons, in this stainless steel sheet, the V content is set to 0.50% or less, and the B content is set to 0.010% or less.

[0037] <P、S> P (phosphorus) and S (sulfur) are elements that are mixed in as unavoidable impurities. P is an element that reduces toughness, and S is an element that forms MnS and reduces corrosion resistance, so the lower the content of these elements, the better. As a result of investigation, it has been found that if the P content is 0.040% or less and the S content is 0.003% or less, these contents are within the allowable range. However, excessively low P and S content is difficult in steelmaking, so it is usually sufficient to adjust the P content to 0.001% or more and the S content to 0.0003% or more, respectively.

[0038] <Other> The remainder of this stainless steel plate contains unavoidable impurities other than P and S. These unavoidable impurities are impurities that originate from the raw materials and manufacturing process, and are present to a degree that does not affect the properties of the above elements.

[0039] [Adjusting the content of each element using M value] In this stainless steel sheet, the content of each element is adjusted so that the M value, determined by the following formula (1), is 95.0 or more.

[0040] M value = 420C-11.5Si+7Mn+23Ni-11.5Cr-12Mo-10V+ 9Cu-52Al+470N+189 …(1) Here, the content (mass%) of each element is substituted for the element symbol in formula (1), and 0 (zero) is substituted for elements that are not added.

[0041] The M value is an index representing the amount (volume %) of martensite phase generated by the cooling treatment in the final annealing. In this way, by adjusting the composition of the stainless steel sheet so that the M value is 95.0 or more, the matrix becomes a substantially 100% austenite single phase structure by the temperature holding treatment in the final annealing. Therefore, the matrix can be made into a martensite structure by the cooling treatment after the temperature holding treatment.

[0042] [Area ratio of undissolved carbonitride] As mentioned above, for martensitic stainless steel sheets, the 0.2% yield strength in the rolling direction is 1300N / mm 2 It was found that reducing the area fraction of undissolved carbonitrides is an extremely effective method for improving delayed fracture resistance at the above strength levels. As a result of detailed investigation, it was found that delayed fracture resistance can be improved by setting the ratio (area fraction) of the total area of ​​undissolved carbonitride regions in a cross section parallel to the rolling direction and plate thickness direction of the stainless steel plate to 1.0% or less. It was also found that the bendability of the stainless steel plate can be improved by setting the area fraction of undissolved carbonitrides to 1.0% or less.

[0043] Furthermore, as a result of extensive investigations by the inventors, it was found that in order to make the area ratio of undissolved carbonitrides 1.0% or less in a martensitic stainless steel sheet whose composition has been adjusted so that the M value is 95.0 or more, it is important to satisfy the following three conditions: (i) the content of each element (excluding Mo, V and B) should be within the above-mentioned range, (ii) the heating temperature in the hot-rolled sheet annealing should not be too high to prevent the carbonitrides from coarsening, and (iii) the holding temperature range should be 1040°C or higher to promote the dissolution of the carbonitrides.

[0044] [0.2% yield strength] This stainless steel sheet is expected to be used for spring components such as retractor spiral springs and springs for electronic equipment parts, and is intended to improve delayed fracture resistance at a higher strength level than conventional martensitic stainless steel sheets. For this reason, the scope of application of the present invention is limited to stainless steel sheets with a 0.2% proof stress in the rolling direction of 1300 N / mm 2 In order to obtain a martensitic stainless steel sheet having such a strength level, it is important to satisfy the above condition (i) and the above condition (iii).

[0045] [Manufacturing method] This stainless steel sheet can be manufactured by a general manufacturing process in which the steps of hot rolling, hot-rolled sheet annealing, cold rolling, [intermediate annealing, cold rolling], and finish annealing are carried out in the above order. Note that the intermediate annealing and cold rolling steps in the above [ ] are optional steps, meaning that these steps may be carried out one or more times. Also, the cold rolling step in the above [ ] is the same treatment as the cold rolling step carried out after the hot-rolled sheet annealing step. Each step will be explained below, but the manufacturing method of this stainless steel sheet is not limited to this.

[0046] <Hot rolling process> First, a cast piece such as a slab produced by continuous casting is heated to 1100 to 1300°C, and then hot-rolled by a known method to obtain a hot-rolled steel sheet. The thickness of the hot-rolled steel sheet may be, for example, 3.0 to 6.0 mm. The coiling temperature for coiling the hot-rolled steel sheet may be, for example, 650 to 800°C.

[0047] <Hot-rolled sheet annealing process> Since the hot-rolled steel sheet obtained by hot rolling has a hard martensite phase in addition to the ferrite phase and carbonitrides, it is difficult to cold-roll the hot-rolled steel sheet as it is. Therefore, the hot-rolled steel sheet is subjected to hot-rolled plate annealing to soften the hot-rolled steel sheet. Specifically, the hot-rolled steel sheet is batch-annealed at a heating temperature of 600°C to Ac1 point using a batch-type heat treatment furnace. Specifically, the hot-rolled steel sheet is batch-annealed by holding the temperature range of 600°C to Ac1 point for 6 to 12 hours.

[0048] In addition, when manufacturing the present stainless steel sheet, the annealing performed in the hot-rolled sheet annealing process does not have to be batch annealing. This is because the hot-rolled sheet annealing process aims to soften the hot-rolled steel sheet to a level that does not interfere with the processing in the next process, and therefore it is not necessarily necessary to perform batch annealing in the hot-rolled sheet annealing process to soften the hot-rolled steel sheet to a high level. "High level" softening refers to softening the hot-rolled steel sheet beyond the minimum level that does not interfere with the processing in the next process after the hot-rolled sheet annealing process.

[0049] However, when batch annealing is not performed, short-time continuous annealing is performed instead. In this continuous annealing, the hot-rolled steel sheet is held at a temperature range of 700 to 900°C for 30 to 300 seconds. By performing short-time continuous annealing instead of batch annealing, the processing time of the hot-rolled steel sheet annealing process can be shortened, and the productivity of the present stainless steel sheet can be improved. After the hot-rolled steel sheet is held at the above temperature range, it may be air-cooled.

[0050] <Cold rolling process, intermediate annealing process> Next, the steel sheet that has undergone the hot-rolled sheet annealing process is pickled and then cold-rolled. The cold rolling process is carried out once or multiple times depending on the final target sheet thickness. When the cold rolling process is carried out multiple times, intermediate annealing is carried out between each cold rolling process. The intermediate annealing can be performed under the condition that the temperature range of 750 to 850°C is held for 0 to 2 minutes, for example. Note that the holding time of 0 minutes is a heat pattern in which cooling is started immediately after the steel sheet that has undergone the cold rolling process reaches a predetermined heating temperature.

[0051] The reduction ratio of the cold rolling (when cold rolling is performed multiple times, the reduction ratio in each cold rolling step) is preferably set in the range of 30 to 70%. The reduction ratio R (%) is determined by the following formula (2).

[0052] R = (h0-h1) / h0 × 100 … (2) Here, h0 is the initial thickness (mm) of the stainless steel sheet before cold rolling, and h1 is the final thickness (mm) of the stainless steel sheet after the final pass of cold rolling. The final thickness h1 can be, for example, 0.15 to 2.0 mm.

[0053] <Finish annealing> Next, the steel sheet that has been through the cold rolling process (and possibly an intermediate annealing process) is finish annealed. That is, the steel sheet that has been through the cold rolling process is heated to the maximum material temperature (heating process), held in the holding temperature range for a specified time (temperature holding process), and then cooled to near room temperature (cooling process). This finish annealing finally gives a martensite structure. In addition, the solid solution of carbonitrides also progresses, which can increase the strength of the stainless steel sheet.

[0054] (Temperature retention treatment) A martensitic stainless steel sheet having the above-mentioned composition and adjusted so that the M value is 95.0 or more has a temperature range above the Ac1 point where it becomes an austenite single phase. Therefore, if a steel sheet that has been subjected to a cold rolling process is held in the austenite single phase temperature range, which is the holding temperature range, for a specified time and then cooled to around room temperature, it is possible to obtain a martensite structure. In addition, the longer the holding time in the holding temperature range in the temperature holding treatment, the more the solid solution of carbonitrides progresses, so if a steel sheet after the heating treatment is held in the holding temperature range for a sufficient time, the 0.2% proof stress in the rolling direction can be increased to 1300 N / mm 2 It is entirely possible to achieve these strength levels.

[0055] However, through intensive research by the inventors, it was found that in order to control the amount of undissolved carbonitrides to be small so that the area ratio of undissolved carbonitrides is 1.0% or less, for example, holding the temperature at 1000°C for about 60 seconds in the temperature holding treatment is insufficient, and it was found that holding at a higher temperature range is necessary.

[0056] Specifically, it is necessary to hold the steel sheet in a holding temperature range of 1040 to 1150°C for 30 seconds or more. More specifically, the steel sheet that has been subjected to the cold rolling process is heated until the maximum material temperature reaches 1040 to 1150°C, and then the holding temperature range is set to a temperature range of 1040 to 1150°C and a temperature holding process is performed for 30 seconds or more. Hereinafter, the time during which the steel sheet after the heating process is held in the holding temperature range of 1040 to 1150°C in the temperature holding process is referred to as "holding time at 1040°C or higher". In this embodiment, the holding time at 1040°C or higher is 30 seconds or more.

[0057] Whether or not the temperature is maintained within the temperature range (1040 to 1150°C) during the temperature holding treatment is determined by measuring the temperature at the center in the thickness direction. The temperature at the center in the thickness direction can be measured based on the furnace temperature, plate thickness, residence time of the steel plate in the furnace, and the measured surface temperature of the steel plate.

[0058] In actual operation, the finish annealing process can be carried out using a continuous annealing furnace. When using a continuous annealing furnace, the maximum material temperature and the holding time at 1040°C or higher can be controlled based on the heat pattern (time-material temperature curve) derived from data on the heating conditions, plate thickness, and line speed in each zone in the furnace.

[0059] Here, the reason why the maximum material temperature and the upper limit of the holding temperature range are set to 1150°C is that if the maximum material temperature is too high, the oxide scale becomes thick and descaling after finish annealing becomes difficult. Note that if the holding time at 1040°C or higher is too long, the decrease in productivity exceeds the allowable range, so the holding time at 1040°C or higher is preferably 180 seconds or less.

[0060] (Cooling process) In the cooling treatment after the temperature holding treatment, either water cooling or air cooling may be used. However, the first average cooling rate at which the temperature of the steel sheet after the temperature holding treatment is reduced from the temperature at the start of the cooling treatment to 100°C is 2.0 to 20.0°C / sec. The first average cooling rate is one example of the cooling rate according to the present invention. There is no particular limitation on the second average cooling rate at which the temperature of the steel sheet after the temperature holding treatment is reduced from 100°C to around room temperature.

[0061] If the first average cooling rate is slower than 2.0°C / sec, the time period during the cooling process in the temperature range in which carbonitrides precipitate tends to be too long, and the amount of undissolved carbonitrides present tends to be greater than necessary. Therefore, in order to make the area ratio of undissolved carbonitrides 1.0% or less, it is preferable to set the lower limit of the first average cooling rate to 2.0°C / sec.

[0062] On the other hand, if the first average cooling rate is faster than 20.0°C / sec, the cooling unevenness occurring in each part of the steel sheet during the cooling treatment increases beyond the allowable range. As a result, the unevenness of the martensitic transformation occurring in each part of the steel sheet also exceeds the allowable range, and the unevenness formed on the surface of the steel sheet after the finish annealing increases and becomes larger than necessary. If the unevenness increases and becomes larger than necessary, a finish processing must be performed to correct the surface shape of the steel sheet after the finish annealing, which leads to a decrease in productivity and an increase in manufacturing costs. Therefore, the upper limit of the first average cooling rate is set to 20.0°C / sec.

[0063] By setting the first average cooling rate to 2.0 to 20.0°C / sec, it becomes easy to set the area ratio of undissolved carbonitrides to 1.0% or less, and also it becomes unnecessary to perform finish processing after the finish annealing, thereby realizing improved productivity and reduced costs.

[0064] Even if the cooling treatment is performed by setting the first average cooling rate to 20.0°C / sec or less, unevenness is formed on the surface of the steel sheet after the finish annealing. Therefore, after the finish annealing, the surface of the steel sheet may be subjected to a finish processing to correct the surface shape. Specifically, for example, the steel sheet after the finish annealing may be passed through a tension leveler or a skin pass mill to improve the flatness of the surface of the steel sheet.

[0065] In addition, in the cooling treatment, it is not essential to set the first average cooling rate to 2.0 to 20.0° C. / sec. Even if the first average cooling rate is outside this range, the steel sheet has good bendability and a 0.2% proof stress in the rolling direction of 1300 N / mm 2 It is possible to manufacture martensitic stainless steel sheets having the above strength levels and good delayed fracture resistance.

[0066] [Additional Notes] The present invention is not limited to the present embodiment, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the present embodiment are also included in the technical scope of the present invention.

[0067] [Example] The results of evaluation of the martensitic stainless steel sheets according to the examples of the present invention and the comparative examples are described below. Hereinafter, the martensitic stainless steel sheets according to the examples of the present invention are referred to as "invention steels," and the martensitic stainless steel sheets according to the comparative examples of the present invention are referred to as "comparative steels."

[0068] <Component composition and manufacturing method> First, steels having the respective component compositions shown in Table 1 below were melted and cast slabs were obtained. Next, the resulting cast slabs were heated at 1150 to 1250°C for 60 minutes, and then hot-rolled. The hot-rolled steel sheets were coiled at a coiling temperature of 680 to 800°C to obtain hot-rolled steel sheets having a thickness of 4.5 mm.

[0069] Next, the coil of hot-rolled steel sheet was loaded into a bell-type annealing furnace (batch-type heat treatment furnace) and hot-rolled steel sheet annealing was performed. After being held at a predetermined temperature range during hot-rolled steel sheet annealing, the steel sheet was air-cooled in the furnace. Next, the steel sheet after hot-rolled steel sheet annealing was pickled and then cold-rolled two or three times. Between each cold rolling, intermediate annealing (holding time 0 seconds) and pickling were performed at a predetermined temperature. Through the above processes, cold-rolled steel sheets A1 to A8 and B1 were obtained.

[0070] Next, each of the cold-rolled steel sheets A1 to A8 and B1 was subjected to finish annealing using a continuous annealing furnace under the conditions shown in Table 2 below. In the cooling treatment of the finish annealing step, the first average cooling rate was set in the range of 1.5 to 25.0°C / sec, and then the steel sheets were cooled to a temperature near room temperature at a second average cooling rate. The cooling method in the cooling treatment was air cooling. Finally, the steel sheets after the finish annealing were pickled to obtain the inventive steels and the comparative steels.

[0071] In Table 2 below, "Example of the invention" corresponds to the steel of the invention, and "Comparative example" corresponds to the comparative steel. In Table 2 below, "○" in the "Evaluation (72 hours or more)" column indicates that the fracture time of the U-shaped bending test specimen described below was 72 hours or more and the delayed fracture resistance was good, and "×" in the same column indicates that the fracture time was shorter than 72 hours and the delayed fracture resistance was poor. In Table 2 below, "○" in the "Shape (wave height 2 mm or less)" column indicates that there was no part where the target length described below exceeded 2.0 mm and the surface properties were good, and "×" in the same column indicates that there was a part where the target length exceeded 2.0 mm and the surface properties were poor. Furthermore, in the "Overall Evaluation" column in Table 2 below, "○" indicates that all of the strength, bendability, delayed fracture resistance, and surface properties are good. "△" in the same column indicates that all of the strength, bendability, and delayed fracture resistance are good, but the surface properties are poor. "×" in the same column indicates that at least one of the strength, bendability, and delayed fracture resistance is poor.

[0072] [Table 1]

[0073] [Table 2]

[0074] As shown in Table 1 above, cold-rolled steel sheet A6 contained 0.3% of optional element Mo, cold-rolled steel sheet A7 contained 0.3% of optional element V, and cold-rolled steel sheet A8 contained 0.0025% of optional element B. In addition, cold-rolled steel sheet B1 had an M value of 87.0, which is outside the numerical range of the M value according to the present invention (95.0 or more), and therefore the steel sheet obtained by finish annealing and pickling the cold-rolled steel sheet B1 is comparative steel ("Comparative Example" in Table 2 above) B1.

[0075] The inventive steels and comparative steels obtained by the above-mentioned manufacturing method were subjected to the following tests to evaluate the mechanical properties, etc.

[0076] <Area ratio of undissolved carbonitride> For each of the inventive steels and the comparative steels, a cross section (L cross section) parallel to the rolling direction and the plate thickness direction was mirror-polished, and then electrolytically etched with oxalic acid to prepare an observation surface. The prepared observation surface was then observed with a SEM (scanning electron microscope). 2 The area was observed by randomly selecting multiple non-overlapping fields.

[0077] Next, the area of ​​the undissolved carbonitride particles observed in each randomly selected field of view was measured using image processing software, and the total value of the measured areas was calculated. The calculated total value was then divided by 0.2 mm to calculate the area ratio of the undissolved carbonitride. Note that, for undissolved carbonitride particles that were partially outside the field of view during observation in each field of view, the area of ​​the part that was present within the field of view was added.

[0078] Reference numeral 101 in FIG. 1 shows an SEM photograph of the observation surface of the inventive steel A1-2 (see Table 2). The area ratio of undissolved carbonitrides in the inventive steel A1-2 was 0.3%. Reference numeral 102 in FIG. 1 shows an SEM photograph of the observation surface of the inventive steel A1-1 (see Table 2). The area ratio of undissolved carbonitrides in the inventive steel A1-1 was 1.0%. Reference numeral 103 in FIG. 1 shows an SEM photograph of the observation surface of the comparative steel A3-5 (see Table 2). The area ratio of undissolved carbonitrides in the comparative steel A3-5 was 1.7%. In all of the above SEM photographs, the black dots in the photographs correspond to undissolved carbonitrides.

[0079] The above-mentioned differences between the area ratios indicated by symbols 101 to 103 in FIG. 1 are due to the different holding times in the holding temperature range in the temperature holding treatment of the final annealing (see the "Holding time (s)" column in Table 2).

[0080] <Tensile properties> For each of the inventive steels and the comparative steels, JIS No. 13B test pieces were prepared and subjected to tensile tests in the rolling direction according to the specified JIS standard (JIS Z2241:2011). Then, the 0.2% proof stress (N / mm 2 The test results are shown in Table 2 above.

[0081] As shown in Table 2 above, the comparative steel A1-5 has a strength level of 1280N / mm 2 This gives 1300N / mm 2 This is presumably because the maximum material temperature reached during final annealing was only 1030°C, and the martensite structure that contributes to high strength could not be obtained sufficiently. In addition, the strength level of the 0.2% proof stress of comparative steel B1 was also 1250N / mm 2 This gives 1300N / mm 2 This is presumably because, as the M value remained at 87.0, it was not possible to obtain a 100% austenite single phase structure during the temperature holding treatment in the final annealing process, and as a result, it was not possible to obtain a sufficient martensite structure during the subsequent cooling treatment.

[0082] The fracture elongation of each of the inventive steels was in the range of 6.7 to 8.3%. Here, the conventional 0.2% yield strength level is 1100N / mm 2 The martensitic stainless steel sheets of the invention have good fracture elongation values ​​in the range of about 6.4 to about 8.1%. Therefore, from these test results, it was found that the inventive steels have good bendability while being stronger than the conventional martensitic stainless steel sheets.

[0083] <Hardness> The Vickers hardness (HV) of each surface of each of the inventive steels and each of the comparative steels was measured in accordance with the specified JIS standard (JIS Z2244:2009). As a result of the measurement, the Vickers hardness (HV) of each of the inventive steels (Hardness in Table 2 above) was in the range of 463 to 520. Here, the conventional 0.2% proof stress strength level is 1100 N / mm 2 The martensitic stainless steel sheets of the present invention have good Vickers hardness values ​​in the range of 446 to 519. Therefore, from the measurement results, it can be seen that each of the inventive steels has a 0.2% yield strength of 1300 N / mm 2 It was found that the hardness of the above-mentioned martensitic stainless steel sheet was as good as that of the above-mentioned conventional martensitic stainless steel sheet even at the strength level of the above-mentioned.

[0084] <Resistance to delayed fracture> A stress corrosion cracking test was carried out for each of the inventive steels and the comparative steels according to the method of the JIS standard (JIS G0576:2001, Method B). Specifically, a test piece with a width of 15 mm and a length of 80 mm, with the longitudinal direction being the rolling direction, was first prepared, and a U-shaped bending test piece was prepared using this test piece. The U-shaped bending test piece was then simply immersed in a 30% calcium chloride aqueous solution (pH 3.5±0.1, 80±1°C), and the time until the U-shaped bending test piece broke was measured.

[0085] The presence or absence of breakage of the U-shaped bend test specimen was checked every hour for the first 8 hours from the start of immersion, and then every 24 hours thereafter. The time elapsed from the start of immersion to when breakage was first confirmed was taken as the breakage time of the U-shaped bend test specimen. For example, a U-shaped bend test specimen with a breakage time of 96 hours is evaluated as having the performance of not breaking until at least 72 hours have passed.

[0086] The inventive steel and comparative steel were tested three times, and the shortest rupture time among the three tests was adopted as the rupture time of the U-shaped bend test specimen. The rupture time of metastable austenitic stainless steel SUS301-CSP / H, which is widely used as a spring material, was used as the standard, and specimens with a rupture time of 72 hours or more were judged to pass (stress corrosion cracking resistance: good). In addition, stress corrosion cracking resistance and delayed fracture resistance are closely related, and if stress corrosion cracking resistance is good, delayed fracture resistance is also good (and vice versa), so the quality of stress corrosion cracking resistance was regarded as the quality of delayed fracture resistance.

[0087] The inventive steels A1-1 to A1-4 and the comparative steels A1-5 to A1-7 and A1-9 have the same chemical composition and were treated under the same conditions except for the final annealing. Nevertheless, as shown in Table 2 above, the inventive steels A1-1 to A1-4 had good delayed fracture resistance with the area ratio of undissolved carbonitrides being 1.0% or less. On the other hand, the comparative steels A1-5 to A1-7 and A1-9 had poor delayed fracture resistance with the area ratio exceeding 1.0%.

[0088] This is presumably because, for comparative steel A1-5, the maximum material temperature reached in the final annealing was only 1030°C, and therefore the amount of undissolved carbonitrides could not be controlled so that the area ratio of undissolved carbonitrides was 1.0% or less. For comparative steels A1-6 and A1-7, the holding time in the holding temperature range in the final annealing was only 5 seconds in both cases, and therefore the amount of undissolved carbonitrides could not be controlled so that the area ratio was 1.0% or less. For comparative steel A1-9, the first average cooling rate in the final annealing was 1.5°C / sec, and therefore, more carbonitrides than necessary were precipitated during the cooling treatment in the final annealing.

[0089] Moreover, the inventive steels A3-1 to A3-4 and the comparative steels A3-5 to A3-8 have the same chemical composition and are treated under the same conditions except for the final annealing. Nevertheless, as shown in Table 2 above, the inventive steels A3-1 to A3-4 have an area ratio of undissolved carbonitrides of 1.0% or less and have good delayed fracture resistance. On the other hand, the comparative steels A3-5 to A3-8 have an area ratio of more than 1.0% and have poor delayed fracture resistance. This is presumably because, for all of the comparative steels A3-5 to A3-8, the holding time in the holding temperature range in the final annealing was shorter than 30 seconds, and therefore it was not possible to control the amount of undissolved carbonitrides present so that the area ratio of undissolved carbonitrides was 1.0% or less.

[0090] <Surface texture> For each of the inventive steels and the comparative steels, the surface shape of the sample was measured by three-dimensional shape measurement, and the measurement results were illustrated as shown in FIG. 2. Specifically, first, a sample with a width of 900 mm and a length of 950 mm was cut out from each coil of each of the inventive steels and the comparative steels. Next, the thickness of each sample was measured on a surface plate in the width direction of the sample at a measurement pitch of 10 mm. Also, on the same surface plate, the thickness of each sample was measured in the length direction of the sample (the sheet threading direction of the coil) at a measurement pitch of 10 mm. Next, based on the measurement results of the thickness in the width direction and length direction of each sample, the relative thickness of each sample was reduced to 0.5 mm intervals and illustrated two-dimensionally. Note that the above samples were cut out from the parts formed in the same place for each of the inventive steels and the comparative steels.

[0091] Next, for each of the inventive steels and each of the comparative steels, the surface forming the reference thickness of each sample (hereinafter, the "reference surface") was set to 0.0 mm, and the two-dimensional distribution of the length from the reference surface to the top of the convex part formed on the reference surface (hereinafter, the "target length") was shown by the shade of color of each convex part as shown in Figure 2. The "reference thickness" is the thickness of the sample when it is assumed that no convex part is formed on the surface. Specifically, as shown in Figure 2, the target length was divided into each of the categories of "longer than 0.0 mm and 0.5 mm or less", "longer than 0.5 mm and 1.0 mm or less", "longer than 1.0 mm and 1.5 mm or less", "longer than 1.5 mm and 2.0 mm or less", and "longer than 2.0 mm and 2.5 mm or less". The convex part is illustrated so that the color of the convex part becomes darker as the target length falls in the category with the larger numerical values ​​of the upper limit value and the lower limit value.

[0092] If there were no protrusions in the target length category of "more than 2.0 mm and 2.5 mm or less", the surface quality of the sample was deemed to pass (surface quality: good). This standard was adopted because, if the target length is longer than 2.0 mm, it becomes impossible to pass the steel sheet after finish annealing through a tension leveler or skin pass mill, for example. In Figure 2, "longer than A and equal to or less than B" is expressed as "AB".

[0093] Reference numeral 201 in FIG. 2 shows a two-dimensional diagram of the relative thickness of the sample of the invention steel A1-3 at 0.5 mm intervals. For the invention steel A1-3, the cooling rate in the final annealing was 2.0° C. / sec. Reference numeral 202 in FIG. 2 shows a two-dimensional diagram of the relative thickness of the sample of the comparative steel A1-8 at 0.5 mm intervals. For the comparative steel A1-8, the cooling rate in the final annealing was 25.0° C. / sec. In each of the reference numerals 201 and 202 in FIG. 2, the axis extending diagonally upward to the left of the paper surface is the axis of the width of the sample, and the axis extending diagonally upward to the right of the paper surface is the axis of the length of the sample (both axes are in mm).

[0094] For the invention steel A1-3, as shown by reference numeral 201 in FIG. 2, there were no convex parts belonging to the category of "longer than 2.0 mm and equal to or less than 2.5 mm" in the target length, and therefore the overall evaluation was "○" as shown in Table 2 above. On the other hand, for the comparative steel A1-8, as shown by reference numeral 202 in Table 2 and FIG. 2 above, there were convex parts belonging to the category of "longer than 2.0 mm and equal to or less than 2.5 mm" in the target length. Therefore, as shown in Table 2 above, although the evaluation of the stress corrosion resistance test was "○", the evaluation of the shape (surface property) was "×", and therefore the overall evaluation was also "△". < / al> < / n> < / cu> < / cr> < / ni> < / si> < / c>

Claims

1. The steel contains, in mass %, C: 0.10% or more and 0.15% or less, Si: 0.05% or more and 0.80% or less, Mn: 0.05% or more and 2.00% or less, P: 0.04% or less, S: 0.003% or less, Ni: 0.50% or less, Cr: 11.0% or more and 15.0% or less, Cu: 0.50% or less, N: 0.005% or more and 0.06% or less, Al: 0.20% or less, and the balance being Fe, carbonitrides, and unavoidable impurities, The M value determined by the following formula (1) is 95.0 or more, The matrix is ​​a martensite phase, The area ratio of the carbonitride in a cross section parallel to the rolling direction and the plate thickness direction is 1.0% or less, A martensitic stainless steel plate having a 0.2% yield strength in the rolling direction of 1300 N / mm 2 or more, measured on a JIS No. 13B test piece in accordance with JIS Z2241:2011: M value = 420C-11.5Si + 7Mn + 23Ni-11.5Cr-12Mo-10V + 9Cu-52Al + 470N + 189 (1) In the above formula (1), the content (mass%) of each element contained in the martensitic stainless steel sheet is substituted for the element symbol, and 0 (zero) is substituted for elements that are not added.

2. The martensitic stainless steel sheet according to claim 1, further containing, by mass%, one or more selected from Mo: 1.00% or less, V: 0.50% or less, and B: 0.001% or more and 0.01% or less.

3. A method for producing a martensitic stainless steel sheet according to claim 1, A method for producing martensitic stainless steel sheet, comprising a finish annealing step in which a steel sheet that has been through a hot rolling step, a hot-rolled sheet annealing step, and a cold rolling step, in that order, is held at a temperature range of 1040°C or higher and 1150°C or lower for 30 seconds or more to perform finish annealing.

4. 4. The method for producing a martensitic stainless steel sheet according to claim 3, wherein in the finish annealing step, the temperature range is maintained for 30 seconds or more, and then the temperature is cooled to 100°C at a cooling rate of 2.0°C / sec or more and 20.0°C / sec or less.

Citation Information

Patent Citations

  • Martensitic stainless steel excellent in corrosion resistance

    JP2008163452A

  • Stainless steel for surface modified spring and production method therefor

    JP2016166385A

  • Martensitic stainless steel sheet and metal gasket manufacturing method

    JP2017171990A

  • Martensitic stainless steel sheet and method of producing the same, and spring member

    JP2019157229A

  • Stainless steel sheet for springs, and production method therefor

    WO2017203695A1