Polishing Pad

The polishing pad with lattice grooves and varying contact areas addresses uneven polishing and durability issues, ensuring consistent and long-lasting surface quality.

JP7570903B2Active Publication Date: 2024-10-22FUJIBO HLDG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020199738
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2024-10-22
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Conventional polishing pads face issues with uneven polishing distribution leading to surface roughness and poor durability due to increased groove density, which can degrade the quality of polished surfaces.

Method used

A polishing pad design featuring lattice grooves and spiral or through holes on the polishing surface, with varying contact area ratios in different regions, to enhance polishing uniformity and durability.

Benefits of technology

The design achieves improved polishing uniformity and extended durability by minimizing surface deformation and over-polishing, maintaining high polishing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570903000002
    Figure 0007570903000002
  • Figure 0007570903000003
    Figure 0007570903000003
  • Figure 0007570903000001
    Figure 0007570903000001
Patent Text Reader

Abstract

To provide a polishing pad having excellent polishing homogeneity and high durability.SOLUTION: A polishing pad 1A comprises a polishing layer having a polishing face P for polishing a material to be polished, and grid-like grooves 11 formed like a grid on the polishing face. The polishing pad has on the polishing face: a first area from a circle of 1 / 4 of a radius of the polishing face to that of 1 / 2 of the radius in a direction heading for an outer peripheral edge from the center of the face; and a second area from the circle of 1 / 2 of the radius of the polishing face to the outer peripheral edge. The polishing pad is characterized in that an area of non-contact with the material to be polished is provided in addition to the grid-like groove so that a first contact area rate per unit area capable of coming into contact with the material to be polished in the first area is lower than a second contact area rate per unit area capable of coming into contact the material in the second area.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing pad. [Background technology]

[0002] Conventionally, when performing precision flat surface polishing of objects to be polished such as semiconductor wafers, silicon wafers for semiconductor devices, substrates for various recording disks, glass substrates for liquid crystal displays, etc., polishing processing is performed using a polishing pad. In order to obtain better polishing performance, various studies have been made on the polishing pad.

[0003] For example, Patent Document 1 discloses a polishing pad in which groove groups having different density distributions at least between adjacent regions on the surface are formed in each of a number of regions, for the purpose of correcting the uneven distribution of polishing amounts caused by the planarization of the polishing pad surface during chemical mechanical polishing. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-94303 A Summary of the Invention [Problem to be solved by the invention]

[0005] Here, in the polishing pad described in Patent Document 1, the distribution of the polishing amount on the polishing surface can be made uniform by adjusting the density distribution of a single type of groove. However, if the density of the grooves is increased to a level that can correct the uneven distribution of the polishing amount on the polishing surface, the polishing surface is deformed due to the portion of the polishing surface that contacts the workpiece being polished being fragmented, and the durability of the polishing pad is deteriorated. In addition, if the polishing surface is deformed, the surface quality of the workpiece may also deteriorate.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a polishing pad which is excellent in polishing uniformity and has high durability. [Means for solving the problem]

[0007] As a result of intensive research by the inventors to solve the problems of the above-mentioned conventional technology, they discovered that excellent polishing uniformity and high durability can be obtained by using a polishing pad which is provided with a polishing sheet having a polishing surface for polishing an object to be polished, and which is provided with lattice grooves formed in a lattice pattern on the polishing surface, and through holes which penetrate the polishing sheet in a direction perpendicular to the polishing surface, or a spiral groove which is formed in a spiral pattern in a direction from the center toward the outer edge, and which has a polishing surface having predetermined first and second regions with different contact area rates that can come into contact with the object to be polished by the through holes or spiral grooves, and which has thus completed the present invention.

[0008] That is, the present invention is as follows. [1] A polishing pad comprising a polishing layer having a polishing surface for polishing an object to be polished, the polishing surface being provided with lattice grooves formed in a lattice pattern, The polishing surface has a first region extending from a center of the polishing surface toward an outer periphery thereof to a circle having a radius of 1 / 4 to a circle having a radius of 1 / 2 of the polishing surface, and a second region extending from the circle having a radius of 1 / 2 of the polishing surface to the outer periphery thereof, A polishing pad characterized in that a first contact area ratio per unit area in the first region that can contact the workpiece is smaller than a second contact area ratio per unit area in the second region that can contact the workpiece, the second region having a non-contact area with the workpiece, the first contact area ratio being separate from the grating grooves. [2] The polishing pad described in [1], characterized in that the area that is separate from the grating groove and does not come into contact with the workpiece is a spiral groove that is formed in a spiral shape in a direction from the center toward the outer periphery. [3] The polishing pad according to claim 2, wherein the groove width of the spiral groove in the first region is greater than the groove width of the spiral groove in the second region. [4] The polishing pad described in [2] or [3], wherein the spiral groove arranged in a direction from the center of the polishing surface toward the outer peripheral edge has no grooves other than the lattice grooves at the point where the spiral groove intersects with a circle with a radius of 1 / 3 of the polishing surface. [5] The polishing pad according to claim 1, characterized in that an area separate from the grating grooves and not in contact with the workpiece is a through hole penetrating the polishing layer in a direction perpendicular to the polishing surface. [6] The polishing pad according to claim 5, wherein the through holes are arranged in a spiral pattern, a concentric pattern, or a radial pattern drawn in a direction from the center of the polishing surface toward the outer peripheral edge. [Brief description of the drawings]

[0009] [Figure 1] 3A to 3C are schematic diagrams showing examples of patterns of lattice grooves and spiral grooves in a polishing pad according to an embodiment of the present invention. [Diagram 2] 3A to 3C are schematic diagrams showing examples of patterns of lattice grooves and through holes in a polishing pad according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a form for carrying out the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary, but the present invention is not limited to the present embodiment described below. The present invention can be modified in various ways without departing from the gist of the invention. In addition, the same elements in the drawings will be given the same reference numerals, and duplicated explanations will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right will be based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.

[0011] Polishing Pad The polishing pad of this embodiment includes a polishing sheet having a polishing surface for polishing an object to be polished, and the polishing surface is provided with lattice grooves formed in a lattice pattern. In addition, the polishing surface of the polishing pad has, in a direction from the center toward the outer peripheral edge, a first region extending from a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 of the polishing surface, and a second region extending from the circle with a radius of 1 / 2 of the polishing surface to the outer peripheral edge. Furthermore, a first contact area ratio per unit area that can come into contact with the workpiece in the first region is smaller than a second contact area ratio per unit area that can come into contact with the workpiece in the second region.

[0012] Conventionally, for example, in the polishing pad described in Patent Document 1, the distribution of the polishing amount on the polishing surface can be made uniform by adjusting the density distribution of a single type of groove. However, if the density of the grooves is increased to a level that can correct the uneven distribution of the polishing amount on the polishing surface, the polishing surface is deformed due to the fact that the part of the polishing surface that contacts the polished object is subdivided, and the durability of the polishing pad is deteriorated. In addition, if the polishing surface is deformed, the surface quality of the polished object may also deteriorate. Here, the inventors have focused on the fact that the polishing degree of the wafer or the like, which is the polishing object, is easily different between the wafer center and the periphery, and the difference in the polishing degree from the wafer center is particularly noticeable at the wafer periphery, which is in contact with the part close to the circle with a radius of 1 / 3 from the center of the polishing pad. First, according to the polishing pad of this embodiment, the polishing surface is provided with a lattice groove formed in a lattice shape, so that high slurry fluidity can be obtained, deformation due to shear stress can be suppressed, and high durability can be obtained. Next, according to the polishing pad of this embodiment, the polishing surface of the polishing pad has a first region from a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 of the polishing surface in the direction from the center to the outer periphery, and a second region from a circle with a radius of 1 / 2 of the polishing surface to the outer periphery, and the first contact area ratio per unit area that can contact the polished object in the first region is smaller than the second contact area ratio per unit area that can contact the polished object in the second region, thereby suppressing over-polishing around the wafer and providing excellent polishing uniformity. However, the factors that cause the polishing pad of this embodiment to have the above-mentioned effects are not limited to this.

[0013] FIG. 1 is a schematic diagram showing an example of a pattern of a lattice groove and a spiral groove in a polishing pad according to this embodiment. The polishing pad 1A includes a polishing layer 10 having a polishing surface P. The polishing surface P of the polishing pad 1A is provided with a lattice groove 11 formed in a lattice shape. The polishing surface P of the polishing pad 1A is provided with a spiral groove formed in a spiral shape in a direction from the center C toward the outer periphery O as a groove other than the lattice groove 11. The spiral groove is provided with a spiral groove 21a and a spiral groove 21b on one spiral pattern from the center C toward the outer periphery O. In addition, a spiral groove 22a and a spiral groove 22b similar to the spiral groove 21a and the spiral groove 21b are provided on a spiral pattern that faces in a direction different from the above spiral pattern. Here, the spiral grooves may be grooves that do not come into contact with the object to be polished, and there is no limitation on the depth of the grooves in the polishing layer 10. The spiral grooves are not limited to those provided in two spiral patterns as described above, and may be provided in, for example, 2 to 12 spiral patterns.

[0014] The spiral grooves 21a and 21b provided in the direction from the center C of the polishing surface P toward the outer peripheral edge O are not formed with a spiral groove at the point where they intersect with a circle of 1 / 3 radius of the polishing surface P, and are divided. The same is true for the spiral grooves 22a and 22b. By having such a portion, the polishing pad can obtain a higher durability. In addition, the spiral grooves 21a and 21b have a smoothly rounded shape at the point where they intersect with the circle of 1 / 3 radius that is divided from the spiral pattern, in order to suppress the application of a sudden high load to the wafer. Spiral groove 21a is provided at a position rotated 90° with respect to center C, independent of spiral groove 21b. Similarly, spiral groove 22a is provided at a position rotated 90° with respect to center C, independent of spiral groove 22b. This angle can be arbitrarily adjusted within a range of 0 to 360°.

[0015] The width of the spiral groove is adjusted so that the closer it is to the intersection point of the spiral pattern with a circle having a radius of 1 / 3 of the polishing surface P, the larger the width of the spiral groove. As a result, the first contact area ratio is smaller than the second contact area ratio. The width of the spiral groove is determined by a perpendicular line drawn from the intersection point of the spiral pattern from the center C toward the outer peripheral edge O with the circle from the center C to a concentric circle. Three to fifteen of the concentric circles can be set at equal intervals from the center C toward the outer peripheral edge O.

[0016] FIG. 2 is a schematic diagram showing an example of a pattern of lattice grooves and through holes in the polishing pad according to this embodiment. The polishing pad 1B includes a polishing layer 10 having a polishing surface P. The polishing surface P of the polishing pad 1B is provided with lattice grooves 11 formed in a lattice shape. The polishing surface P of the polishing pad 1B is provided with through holes 31 that penetrate the polishing layer 10 in a direction perpendicular to the polishing surface P. A plurality of through holes 31 are provided on one spiral pattern drawn in a direction from the center C of the polishing surface P toward the outer periphery O. Note that although the spiral patterns are shown in FIG. 2 with solid lines, these spiral patterns are merely guide lines for determining the positions of the through holes for convenience, and are not grooves provided on the polishing pad.

[0017] The through holes are provided at regular intervals on the spiral pattern, but are adjusted so that the intervals between the through holes become smaller as they approach the point where the spiral pattern intersects with a circle with a radius of 1 / 3 of the polishing surface P. This makes the first contact area ratio smaller than the second contact area ratio. However, the first contact area ratio may be arranged randomly rather than at regular intervals, as long as it can be adjusted to be smaller than the second contact area ratio. Furthermore, the method for spacing the through holes at regular intervals on the spiral pattern is not particularly limited, but an example thereof is a method in which 3 to 15 concentric circles are set at equal intervals from the center C toward the outer peripheral edge O, and the through holes are provided at the intersections of the spiral pattern and the concentric circles.

[0018] The through holes may be provided on a spiral pattern, a concentric pattern, or a radial pattern instead of the above-mentioned spiral pattern. The spiral of the spiral pattern may be, for example, a logarithmic spiral, an involute curve, or a hyperbolic spiral, other than the spiral of the above-mentioned spiral pattern, and is preferably a logarithmic spiral. The number of spirals is not particularly limited, but is, for example, 2 to 12. By providing the through holes on the spiral pattern, the slurry is discharged from the periphery of the polishing pad in a spiral on the polishing pad P where the slurry rotates, and therefore the slurry has excellent fluidity.

[0019] For example, the through hole 31 has a diameter of 1.5 to 4.0 cm for a polishing pad having a diameter of 35 to 70 cm. A diameter of 1.5 cm or more tends to suppress edge effects and overpolishing, and a diameter of 4.0 cm or less makes it possible to obtain excellent polishing uniformity. The number of through holes is not particularly limited as long as the first contact area ratio is smaller than the second contact area ratio.

[0020] The spiral grooves and through holes are provided to adjust the contact area with the workpiece, and the non-contact area ratio due to the spiral grooves and through holes varies depending on each region. The first non-contact area ratio in the first region from a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 of the polishing surface is preferably in the range of 5 to 20%, more preferably in the range of 6 to 18%. When the first non-contact area ratio is 6% or more, over-polishing of the circumference of the wafer tends to be suppressed, and when the first non-contact area ratio is 18% or less, the polishing difference between the first region and other regions is suppressed from becoming large, and excellent polishing uniformity can be obtained.

[0021] The second non-contact area ratio in the second region from the circle with a radius of 1 / 2 of the polishing surface to the outer periphery is preferably 10% or less, more preferably 9.5% or less. By having the second non-contact area ratio of 9.5% or less, the polishing rate of the polishing pad can be maintained high. The difference between the first non-contact area ratio and the second non-contact area ratio is preferably in the range of 0.5 to 15%, more preferably in the range of 1 to 13%. When the difference in the non-contact area ratio is 1% or more, over-polishing of the circumference of the wafer tends to be suppressed, and when the difference in the non-contact area ratio is 13% or less, the polishing difference between the first region and the other regions is suppressed from becoming large, and excellent polishing uniformity can be obtained.

[0022] Also, as shown in the examples described later, instead of the second region described above, a first region from a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 of the polishing surface in a direction from the center to the outer periphery of the polishing surface of the polishing pad and a third region which is the entire region other than the first region may be used. The third region is a region of the polishing surface of the polishing pad, which is a region from the center to the circle with a radius of 1 / 4 of the polishing surface in a direction from the center to the outer periphery of the polishing surface of the polishing pad, combined with the second region. That is, the first contact area ratio per unit area that can contact the polished object in the first region is smaller than the third contact area ratio per unit area that can contact the polished object in the third region. The above description of the second region and the second region is similarly applied to the third region and the third contact area ratio.

[0023] The polishing pad may or may not be circular. If the pad is not circular, the outer periphery is regarded as the outermost periphery of the polishing pad through which the workpiece passes.

[0024] Details of the polishing pad common to the polishing pads shown in FIG. 1 and FIG. 2 will be described below.

[0025] The polishing pad is a polishing pad with an abrasive layer having a nonwoven fabric and a resin impregnated in the nonwoven fabric, and includes the polishing layer having an abrasive surface and a double-sided tape for fixing the polishing pad to the polishing platen of a polishing machine, laminated in this order. In this example, the polishing layer is laminated on one adhesive surface of the double-sided tape, and release paper is laminated on the other adhesive surface. Between the polishing layer and the double-sided tape, there may be a layer (lower layer, support layer) other than the polishing layer and the double-sided tape. By providing a layer other than the polishing layer and the double-sided tape, the profile (surface and end shape) of the wafer can be adjusted. Examples of the support layer include nonwoven fabric, plastic sheet, rubber, sponge, etc. The thickness of the support layer is not particularly limited, but is preferably 0.1 to 3.0 mm, more preferably 0.15 to 2.5 mm, and even more preferably 0.35 to 2.0 mm.

[0026] The thickness of the polishing layer in this embodiment is not particularly limited, but is preferably 0.5 mm to 7 mm, and more preferably 1 mm to 5 mm. The thickness of the polishing sheet is measured in accordance with the measurement method described in the Japanese Industrial Standards (JIS K 6550 (1994)). In other words, the thickness of the polishing sheet is measured in accordance with the measurement method described in the Japanese Industrial Standards (JIS K 6550 (1994)). 2 This is the thickness when a load of 480g is applied (stressed).

[0027] The nonwoven fabric constituting the polishing layer is not particularly limited as long as it is used in the polishing layer of the polishing pad, and various known nonwoven fabrics can be used. Such nonwoven fabrics are not particularly limited, but may be manufactured by a conventional method known in the art, for example, a spunbond method, a meltblown method, a dry method, or a wet method. In addition, a commercially available nonwoven fabric may be used as the nonwoven fabric contained in the polishing layer of this embodiment. Examples of the nonwoven fabric include polyamide-based and polyester-based nonwoven fabrics. In addition, the method of entangling fibers when obtaining the nonwoven fabric is not particularly limited, and may be, for example, needle punching or water flow entanglement. The nonwoven fabric may be one type alone from the above-mentioned nonwoven fabrics, or two or more types may be used in combination.

[0028] The fineness of the nonwoven fabric in this embodiment is not particularly limited, but is preferably 2 to 6 d from the viewpoint of reducing the occurrence of scratches during polishing.

[0029] The basis weight of the nonwoven fabric in this embodiment is not particularly limited, but is preferably 150 to 1000 g / m from the viewpoint of the polishing pad density and the ratio of the nonwoven fabric to the resin. 2 It is preferable that:

[0030] The nonwoven fabric of the polishing layer may be made of one type of fiber alone, or may contain two or more types of fibers.

[0031] The resin in this embodiment is not particularly limited as long as it can be provided in the polishing pad, and may be a conventionally known resin. Examples of such resins include resins that can be impregnated into nonwoven fabric by wet impregnation and resins that can be impregnated into nonwoven fabric by dry impregnation. As the resin impregnated into the polishing layer of this embodiment, one type of resin can be used alone, or two or more types of resins can be used. In this embodiment, it is preferable that the resin includes a first resin and a second resin different from the first resin.

[0032] The first resin is not particularly limited as long as it can be impregnated into the nonwoven fabric by so-called wet impregnation, and various known resins can be applied. Examples of such resins (hereinafter simply referred to as "wet resins") include, but are not limited to, polyurethane-based resins such as polyurethane and polyurethane polyurea, acrylic resins such as polyacrylate and polyacrylonitrile, vinyl resins such as polyvinyl chloride, polyvinyl acetate and polyvinylidene fluoride, polysulfone-based resins such as polysulfone and polyethersulfone, acylated cellulose resins such as acetylated cellulose and butyrylated cellulose, polyamide resins and polystyrene resins. Examples of polyurethane resins include, but are not limited to, polyester-based polyurethane resins, polyether-based polyurethane resins, and polycarbonate-based polyurethane resins. The 100% modulus of the resin is preferably 5 MPa to 30 MPa, and more preferably 10 MPa to 20 MPa. The 100% modulus of a resin is the value obtained by dividing the load applied when a sheet made of that resin is stretched 100%, that is, when it is stretched to twice its original length, by the unit area.

[0033] The second resin is not particularly limited as long as it can be impregnated into the nonwoven fabric by so-called dry impregnation, and various known resins can be applied. The second resin (hereinafter also simply referred to as "dry resin") can be obtained by a dry method using a solution containing a urethane prepolymer having an isocyanate group at the end, an amine compound and / or a polyhydric alcohol compound as a curing agent, and a solvent capable of dissolving them. Here, the urethane prepolymer is not particularly limited, and examples thereof include an adduct of hexamethylene diisocyanate and hexanetriol, an adduct of 2,4-tolylene diisocyanate and prenzcatechol, an adduct of tolylene diisocyanate and hexanetriol, an adduct of tolylene diisocyanate and trimethylolpropane, an adduct of xylylene diisocyanate and trimethylolpropane, an adduct of hexamethylene diisocyanate and trimethylolpropane, and an adduct of isocyanuric acid and hexamethylene diisocyanate. Among the curing agents, examples of the amine compounds include 3,3'-dichloro-4,4'-diaminodiphenylmethane, 4-methyl-2,6-bis(methylthio)-1,3-benzenediamine, 2-methyl-4,6-bis(methylthio)-1,3-benzenediamine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis[3-(isopropylamino)-4-hydroxyphenyl]propane, 2,2-bis[3-(1-methylpropylamino)-4-hydroxyphenyl]propane, 2,2-bis[3-(1-methylpentylamino)-4-hydroxyphenyl]propane, 2,2-bis(3,5-diamino-4-hydroxyphenyl)propane, 2,6-diamino-4-methylphenol, trimethylethylenebis-4-aminobenzoate, and polytetramethyleneoxide-di-p-aminobenzoate.Examples of polyhydric alcohol compounds include ethylene glycol, propylene glycol, diethylene glycol, trimethylene glycol, tetraethylene glycol, triethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,2-butanediol, 3-methyl-1,2-butanediol, 1,2-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 2,3-dimethyltetrahydrofuran, and the like. Examples of the urethane prepolymer and the curing agent include, but are not limited to, N,N-dimethylformamide and N,N-dimethylacetamide. Examples of the solvent include, but are not limited to, N,N-dimethylformamide and N,N-dimethylacetamide. Examples of the solvent include, but are not limited to, N,N-dimethylformamide, ...

[0034] In the polishing pad of this embodiment, from the viewpoint of maintaining tensile strength during polishing, it is preferable that the content of the nonwoven fabric is 10 to 50 mass%, the content of the first resin is 10 to 60 mass%, and the content of the second resin is 10 to 70 mass% relative to the total of the nonwoven fabric, the first resin, and the second resin. From the same viewpoint, it is more preferable that the content of the nonwoven fabric is 20 to 40 mass%, the content of the first resin is 20 to 50 mass%, and the content of the second resin is 20 to 60 mass%. The contents of the nonwoven fabric, the first resin, and the second resin in the polishing pad can be determined from the mass of the eluted component or the mass of the residue by utilizing the difference in solubility (polarity) in a polar solvent or the difference in amine decomposition. In addition, the density of the polishing pad after the first impregnation step described later, the density of the polishing pad after the immersion step described later, and the density of the polishing pad after the second impregnation step described later are measured, and the density can be calculated from the density difference. The density can be measured in the same manner as above.

[0035] In addition to the nonwoven fabric and resin described above, the polishing pad of this embodiment may contain various additives that can be contained in a normal polishing pad, as long as the desired effect of this embodiment is not impaired. Examples of such additives include, but are not limited to, pigments such as carbon black, hydrophilic active agents, and hydrophobic active agents.

[0036] The thickness of the polishing pad of this embodiment is not particularly limited, but is preferably 0.8 to 10 mm, more preferably 1.2 to 6 mm, from the viewpoint of sufficiently securing a flat contact surface with the workpiece, securing flatness, and storing slurry. The thickness is measured in accordance with the Japanese Industrial Standards (JIS K 6505). Specifically, three sample pieces obtained by cutting the polishing pad into 10 cm x 10 cm squares are prepared, and each sample piece is set at a predetermined position in a thickness measuring device, and then a pressure surface with a load of 480 g / cm2 is placed on the surface of the sample piece, and the thickness is measured after 5 seconds. For each sample piece, the thickness is measured at five points and the arithmetic average is calculated, and the arithmetic average of the three sample pieces is further calculated.

[0037] The density (bulk density) of the polishing layer in this embodiment is not particularly limited, but is preferably 0.30 g / cm at 25° C. from the viewpoints of suppressing permanent deformation of the polishing pad, suppressing a pressure drop at the point of application due to an increase in the contact area with the workpiece, and improving slurry retention. 3 More than 0.60g / cm 3 It is preferable that the g / cm3 is 0.35 g / cm3 or less. 3 More than 0.55g / cm 3 More preferably, it is 0.35 g / cm or less. 3 More than 0.50g / cm 3 The density is measured in accordance with the Japanese Industrial Standards (JIS K 6505). Specifically, the mass of a sample piece similar to that used in the thickness measurement is measured using an automatic balance, and then the mass is calculated using the following formula: Density (g / cm 3 ) = mass (g) / (10 (cm) x 10 (cm) x thickness of sample piece (cm)) The density is calculated by the above method, and the arithmetic average of the three sample pieces is obtained.

[0038] The A hardness of the polishing layer of this embodiment is not particularly limited, but is preferably 50 degrees or more and 95 degrees or less, more preferably 60 degrees or more and 90 degrees or less, from the viewpoint of ensuring good adhesion with the workpiece and preventing deformation of the polishing pad. The A hardness is measured at 25°C in accordance with the Japanese Industrial Standards (JIS K 6253). More specifically, the A hardness is measured using a Shore A durometer according to JIS K 7311 for a sample with dimensions of 30 mm x 30 mm.

[0039] The compression ratio of the polishing layer in this embodiment is not particularly limited, but is preferably 0.5% to 20%, and more preferably 1% to 10%. When the compression ratio is within the above range, the polishing pad 300 tends to be able to wipe off and remove the polishing debris and the like present on the polished object during polishing. Therefore, it tends to be possible to suppress microdefects caused by the agglomerates of the slurry in particular. The compression ratio can be controlled, for example, by adjusting the size and number of the openings in the polishing sheet that communicate with the polishing surface S. The compression ratio of the polishing layer can be determined using a Shopper-type thickness measuring device (pressure surface: circular with a diameter of 1 cm) in accordance with the Japanese Industrial Standards (JIS L 1021). Specifically, the thickness t0 is measured after applying an initial load for 30 seconds from a no-load state at room temperature, and then the final load is applied from the thickness t0 state, and the thickness t1 is measured after leaving it as it is for 5 minutes. From these, the compression ratio is calculated using the following formula: Compression ratio (%) = (t0-t1) / t0 x 100 In this case, the initial load is 100g / cm 2 , final load is 1120g / cm 2 and do.

[0040] The compressive elastic modulus of the polishing pad is preferably 50 to 98%, more preferably 60 to 95%, from the viewpoint of ensuring good adhesion to the workpiece and preventing deformation of the polishing pad. The compressive elastic modulus can be determined using a Shopper-type thickness measuring device (pressure surface: circular with a diameter of 1 cm) in accordance with the Japanese Industrial Standards (JIS L 1021). Specifically, at room temperature, a thickness t0 is measured after applying an initial load for 30 seconds from a no-load state, and then a thickness t1 is measured after applying a final load for 30 seconds from a thickness t0 state. Next, all loads are removed from the thickness t1 state, and the pad is left for 5 minutes (to be in a no-load state), after which a thickness t0' is measured after applying an initial load for 30 seconds again. From these, the compressive elastic modulus is calculated using the following formula: Compressive elastic modulus (%) = (t0'-t1) / (t0-t1) x 100 In this case, the initial load is 100g / cm 2 , final load is 1120g / cm 2Let us assume that.

[0041] Method for manufacturing polishing pad Next, an example of a method for manufacturing the polishing pad of this embodiment will be described. The method for producing a polishing pad of this embodiment includes a first impregnation step of impregnating a nonwoven fabric with a resin solution containing a first resin and performing wet coagulation to obtain a resin-impregnated nonwoven fabric, an immersion step of immersing the resin-impregnated nonwoven fabric in a solvent in which the first resin is soluble, and a second impregnation step of impregnating the resin-impregnated nonwoven fabric after the immersion step in a resin solution containing a second resin. Since the method for producing a polishing pad of this embodiment is configured as described above, it is possible to obtain a polishing pad that has excellent chemical resistance and can ensure a sufficient life even when subjected to polishing using a strong oxidizing agent.

[0042] In the above-mentioned first impregnation step, the nonwoven fabric is impregnated with a resin solution, and then a wet coagulation method is used to obtain a resin-impregnated nonwoven fabric. The wet coagulation method is a method in which the resin solution is immersed in a coagulation liquid, which is a poor solvent for the resin, at room temperature to coagulate and regenerate the resin. When the wet coagulation method is used after the nonwoven fabric is impregnated with the resin solution as in this embodiment, the resin is coagulated and regenerated on the surface of the fibers in the coagulation liquid as the solvent of the resin solution and the coagulation liquid are replaced on the surface of the resin solution adhering to the fibers of the nonwoven fabric.

[0043] A specific example of the first impregnation step is as follows. First, the wet resin as described above is mixed with a solvent capable of dissolving the wet resin and miscible with the coagulation liquid described below, and other additives to be mixed into the polishing pad as necessary, and the mixture is degassed under reduced pressure as necessary to prepare a resin solution. The solvent is not particularly limited, but examples thereof include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), methyl ethyl ketone (MEK) and dimethyl sulfoxide. From the viewpoint of selecting a good solvent for the resin and further from the viewpoint of uniformly mixing the resin in the coagulation bath to facilitate wet coagulation, it is preferable that the first resin is soluble in one or more solvents selected from the group consisting of N,N-dimethylformaldehyde, dimethylacetamide and dimethylsulfoxide. Similarly, it is preferable that the solvent contains one or more solvents selected from the group consisting of N,N-dimethylformaldehyde, dimethylacetamide and dimethylsulfoxide.

[0044] From the viewpoint of impregnating the entire nonwoven fabric with the resin and from the viewpoint of ensuring a sufficient amount of impregnation of the resin, the viscosity of the resin solution measured at 20°C using a B-type rotational viscometer is preferably 8000 cp or less, more preferably 100 cp to 5000 cp, and even more preferably 400 cp to 3000 cp. From the viewpoint of obtaining a resin solution having such a numerical viscosity range, for example, polyurethane resin may be dissolved in a solvent in a range of 5 to 25 mass % relative to the total amount of the resin solution, more preferably in a range of 8 to 15 mass %. Since the viscosity of the resin solution also depends on the type and molecular weight of the resin used, it is preferable to select the resin, set the concentration, etc., by comprehensively considering these factors.

[0045] Next, the nonwoven fabric is sufficiently immersed in the resin solution, and then the resin solution is squeezed out of the nonwoven fabric with the resin solution attached thereto using a mangle roller capable of applying pressure between a pair of rollers, thereby adjusting the amount of the resin solution attached to the nonwoven fabric to a desired amount, and the nonwoven fabric is uniformly or approximately uniformly impregnated with the resin solution. Next, the nonwoven fabric impregnated with the resin solution is immersed in a coagulation liquid mainly composed of a poor solvent for the resin, such as water, to coagulate and regenerate the wet resin. In order to adjust the regeneration speed of the resin, an organic solvent such as a polar solvent other than the solvent in the resin solution may be added to the coagulation liquid. The temperature of the coagulation liquid is not particularly limited as long as it is a temperature at which the resin can be coagulated, and may be, for example, 15 to 60°C.

[0046] In this embodiment, after the above-mentioned wet coagulation, it is preferable to subject the nonwoven fabric to the following washing and drying steps. First, the nonwoven fabric in which the wet resin has been coagulated and regenerated is washed in a washing liquid such as water to remove the solvent such as DMF remaining in the nonwoven fabric. After washing, the nonwoven fabric is lifted from the washing liquid, and excess washing liquid is squeezed off using a mangle roller or the like. Thereafter, the nonwoven fabric substrate may be dried in a dryer at 100°C to 150°C. In addition, after the above drying, it is preferable to further slice, process the obtained resin-impregnated nonwoven fabric with a buff, or the like, remove the surface skin layer, and make it into a predetermined thickness from the viewpoint of improving the uniformity of the next immersion step.

[0047] The immersion step in this embodiment is a step of immersing the above-mentioned resin-impregnated nonwoven fabric in a solvent in which the above-mentioned wet resin is soluble, thereby re-dissolving the wet resin in the solvent. It is considered that the immersion step reduces bubbles (e.g., closed pores and open pores with small openings) inside the resin-impregnated nonwoven fabric, improving the adhesion between the nonwoven fabric and the wet resin. The solvent used in the immersion step is not particularly limited, and examples thereof include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), methyl ethyl ketone (MEK), and dimethyl sulfoxide. In addition, the temperature condition during immersion is preferably 15.0 to 25.0°C from the viewpoint of reducing bubbles in the first resin and preventing the resin from dissolving into the solvent, and the immersion time is preferably 5 to 30 seconds from the same viewpoint. In addition, it is preferable to provide a drying step after the above-mentioned immersion step.

[0048] In the present embodiment, the secondary impregnation step is a step of immersing the resin-impregnated nonwoven fabric after the immersion step in a solution containing a urethane prepolymer and a curing agent. It is presumed that the secondary impregnation step forms a dry resin on the surface of the above-mentioned wet resin.

[0049] As a specific example of the secondary impregnation step, first, a solution containing a prepolymer, a curing agent, and a solvent capable of dissolving them is prepared. Next, after the resin-impregnated nonwoven fabric after the immersion step is immersed in the solution, the solution is squeezed out of the resin-impregnated nonwoven fabric to which the solution has been attached using a mangle roller capable of applying pressure between a pair of rollers, thereby adjusting the amount of the solution attached to the resin-impregnated nonwoven fabric to a desired amount, and the resin-impregnated nonwoven fabric is uniformly or approximately uniformly impregnated with the solution. Next, the resin-impregnated nonwoven fabric impregnated with the solution is dried in a dryer. As a result, the polishing pad of this embodiment in which the resin-impregnated nonwoven fabric is impregnated with the dry resin by polymerization of the urethane prepolymer and the curing agent is obtained. The drying temperature may be, for example, 100°C to 140°C.

[0050] By going through the above-mentioned first impregnation step, immersion step, and second impregnation step, a polishing pad having the desired configuration of this embodiment is obtained. This polishing pad is presumed to have the following configuration, although it is not intended to be limited to the contents described below. That is, by going through the first impregnation step, a wet resin is formed on the surface of the nonwoven fabric. In particular, by adopting wet coagulation in the first impregnation step, the wet resin is uniformly attached within the nonwoven fabric. However, at this stage, there are many fine bubbles derived from the wet coagulation method in the resin inside the resin-impregnated nonwoven fabric obtained, and the adhesion and strength between the nonwoven fabric and the wet resin are not sufficient. Next, by going through the immersion process, the immersion solution fills the fine bubbles of the wet resin, and the wet resin is redissolved by heating due to drying, and the fine bubbles (e.g. closed pores and small open pores) inside the resin-impregnated nonwoven fabric are reduced, and the resin (wet resin) impregnated in the nonwoven fabric is densified around the fibers, so that the adhesion between the fibers of the nonwoven fabric and the wet resin is improved and the strength is improved. In addition, the reduction in the fine bubbles leads to uniform impregnation of the dry resin in the secondary impregnation process and improved strength. Furthermore, by going through the secondary impregnation process, a layer of dry resin is formed on the surface of the layer of wet resin on the nonwoven fabric fibers. If the secondary impregnation process is performed without going through the immersion process, it becomes difficult for the dry resin to penetrate into the spaces in the bubbles inside the resin-impregnated nonwoven fabric, and the adhesion of the dry resin becomes uneven. In this case, the wet resin and the dry resin are unevenly attached, and the elasticity and rigidity properties are partially uneven, so that the resin in the polishing pad peels off during polishing, and the lifespan is shortened. In addition, the strong oxidizing agent is easily infiltrated into the air bubbles where the dry resin, which has excellent resistance to the strong oxidizing agent, does not exist, so that the chemical resistance is poor and the lifespan is shortened. On the other hand, according to this embodiment, the air bubbles are reduced in the immersion process, so that the voids that can be impregnated in the secondary impregnation process are secured and the air permeability is improved, so that the number of places where the dry resin is difficult to infiltrate is reduced, and the area where the dry resin exists is increased. Therefore, the intrusion of the strong oxidizing agent into the area where the dry resin does not exist is suppressed, the chemical resistance is improved, and the lifespan can be extended. In addition, the wet resin in the part that is not directly attached to the nonwoven fabric is reduced, so that the peeling of the resin in the polishing pad is suppressed during polishing, and the lifespan can be extended.Thus, in the polishing pad of this embodiment, it is presumed that a nonwoven fabric is used as a base material, a wet resin layer is formed on the nonwoven fabric, and a dry resin layer is formed on the wet resin layer. In addition, as a whole of the polishing pad, the adhesion between the nonwoven fabric and the wet resin layer and the adhesion between the wet resin layer and the dry resin layer are both considered to be good. In addition, if the first impregnation process and the soaking process are omitted and the dry resin is impregnated into the nonwoven fabric by the second impregnation process, the compatibility between the nonwoven fabric and the dry resin is poor, problems occur in the adhesion between the fibers and the resin, and structural stability is impaired. In addition, if only dry resin is attached to the nonwoven fabric without wet resin, the polishing pad will have high hardness and low elasticity, and will not conform well to the workpiece during polishing, which will interfere with polishing. Furthermore, dry resin has poor moisture retention compared to wet resin, so it is difficult to sufficiently retain the polishing liquid with only dry resin.

[0051] The fact that the polishing pad of this embodiment has the configuration inferred as described above can be confirmed, for example, from, but not limited to, the tensile strength retention value of the polishing pad, as well as the above-mentioned air permeability value and the respective contents of the nonwoven fabric, first resin and second resin in the polishing pad.

[0052] The polishing pad obtained as described above may then be cut to the desired shape and dimensions, such as a circle, as necessary, and may be inspected to ensure that there is no dirt or foreign matter attached thereto.

[0053] The surface of the obtained polishing pad becomes the polishing surface, but when the polishing pad is used to polish a workpiece, a layer other than the polishing layer (e.g., a lower layer, a support layer) such as a nonwoven fabric, a plastic sheet, rubber, or sponge may be attached in advance to the surface of the polishing pad opposite the polishing surface. In addition, a double-sided tape (having an adhesive layer and a release paper) for attaching the polishing pad to the polishing platen of a polishing machine may be attached to the surface of the layer other than the polishing layer that is not bonded to the polishing layer.

[0054] The polishing pad of this embodiment has a processing step in which groove processing is performed to provide a lattice groove or a spiral groove on the polishing surface, and hole processing (punching processing) is performed to provide a through hole as necessary. As a groove processing method, a known method can be appropriately used, and for example, a spiral groove can be provided by a CNC (Computer Numerical Control) router machine with a programmed shape.

[0055] The depth of the groove is preferably 0.1 mm to 0.8 mm. When a groove having a depth within the above range is formed, the fluidity of the slurry on the polishing surface during polishing is further improved, and the polishing rate is further improved.

[0056] Although the present embodiment has been described in detail above, the present invention is not limited to the above embodiment. For example, the polishing sheet may have a light transmitting portion for optically detecting the polishing state. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. It is not something that is done.

[0058] Example 1 A 2.2d polyethylene terephthalate fiber and a 3.3d polyethylene terephthalate fiber were blended in the above order in a blending ratio of 2:1 to obtain a nonwoven fabric with a thickness of 3.5 mm. A resin solution was prepared by mixing 55 parts by mass of polyurethane resin (manufactured by DIC Corporation, product name "Crisbon", 100% modulus 12 MPa at 23±2°C) and 45 parts by mass of N,N-dimethylformamide (DMF). The nonwoven fabric was immersed in the resin solution at room temperature, and then the resin solution was impregnated into the nonwoven fabric approximately uniformly using a mangle roller capable of applying pressure between a pair of rollers. Next, the nonwoven fabric was immersed in a coagulation liquid consisting of water at room temperature to coagulate and regenerate the resin, thereby obtaining a nonwoven fabric impregnated with the first resin.

[0059] The nonwoven fabric impregnated with the first resin was taken out of the coagulation liquid, and was further immersed in a washing liquid consisting of water for washing, and then dried. Next, the nonwoven fabric impregnated with the first resin obtained above was immersed in a solvent in which DMF and pure water were mixed in this order at a mixing ratio of 65:35. Thereafter, washing and drying were performed in the same manner as above.

[0060] A prepolymer solution was prepared by mixing 426 parts by mass of urethane prepolymer with 74 parts by mass of crosslinking agent, 150 parts by mass of DMF as an organic solvent, and 350 parts by mass of methyl ethyl ketone. The nonwoven fabric impregnated with the first resin after the above immersion was immersed in the prepolymer solution at room temperature, and then the nonwoven fabric was impregnated with the prepolymer solution approximately uniformly using a mangle roller capable of applying pressure between a pair of rollers. The nonwoven fabric was dried to obtain a resin-impregnated nonwoven fabric impregnated with the first resin and the second resin.

[0061] The surface of the resin-impregnated nonwoven fabric was buffed and the surface skin layer was removed to obtain an abrasive layer. The abrasive layer was cut into a circle with a diameter of 500 mm, and a grid groove with a pitch of 15 mm and a width of 3 mm was provided on the buffed abrasive surface. In addition, a through hole with a diameter of 25 mm was punched to obtain the abrasive pad shown in Figure 2.

[0062] Comparative Example 1 A polishing pad was obtained in the same manner as in Example 1, except that no through holes were provided.

[0063] Abrasion test The polishing pad was polished under the following polishing conditions, and a polishing measurement test was performed. In the measurement, the polishing pad was attached to a predetermined position of a polishing machine, and a silicon wafer was used as a work (object to be polished). The surface of the polishing pad was previously dressed using a diamond dresser under the dressing conditions of a pressure of 1.5 kpa, a polishing head and polishing platen rotation speed of 60 rpm, ultrapure water supply rate of 1000 mL / min, and a dressing time of 10 minutes, before being used for polishing evaluation.

[0064] Polishing conditions Polishing machine used: Fujikoshi Machinery Co., Ltd., product name "MCP-150" Polishing speed (platen rotation speed): 60 rpm Processing pressure: 17kpa Slurry: Fujimi Incorporated, product name "COMPOL 80" (original solution: water = 1:7) Slurry flow rate: 780mL / min Polishing time: 60 minutes Workpiece: Silicon wafer

[0065] After polishing under the above conditions, the thickness of the silicon wafer was measured from the center to the circumference, and the difference in thickness from the center of the wafer was calculated. A difference in thickness of 8 μm or less was evaluated as "Good", and a difference exceeding 8 μm was evaluated as "Poor".

[0066] The diameter of the through holes of each polishing pad is shown in Table 1. The area and area ratio were calculated assuming that the portion in which the through holes were formed was a non-contact portion that did not contact the workpiece.

[0067] [Table 1]

[0068] An explanation of each item in the table is given below. "Diameter of through hole": Diameter of the through hole provided to adjust the contact area with the workpiece (cm) Non-contact area (cm2) in the range of 1 / 4 to 1 / 2 2 )": Non-contact area created by adjusting the contact area using through holes in the range from 1 / 4 radius to 1 / 2 radius from the center of the polishing surface (total area of ​​through holes provided in the range from 1 / 4 radius to 1 / 2 radius) 1 / 4 to 1 / 2 range of reference area (cm 2 )": The reference contact area (area of ​​the polishing pad in the range from 1 / 4 radius to 1 / 2 radius from the center of the polishing surface) when the contact area adjustment by through holes is not performed. "Non-contact area ratio in the range of 1 / 4 to 1 / 2": The ratio of the non-contact area to the reference area in the range from the center of the polishing surface to a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 (area of ​​through holes / area of ​​polishing pad x 100) "Outside range non-contact area (cm 2 )": The non-contact area outside the range from the center of the polishing surface with a radius of 1 / 4 to 1 / 2 (hereinafter simply referred to as "outside the range"), which is the non-contact area created by adjusting the contact area with through holes (the total area of ​​the through holes provided outside the range) "Out-of-range reference area (cm 2 )": The reference contact area (area of ​​the polishing pad outside the range) when the contact area adjustment by the through holes outside the range is not performed "Ratio of non-contact area outside the range": The ratio of non-contact area outside the range to the reference area (area of ​​through holes / area of ​​polishing pad x 100) "Difference in non-contact area ratio": The difference between the non-contact area ratio in the range from a circle with a radius of 1 / 4 to a circle with a radius of 1 / 2 from the center of the polished surface and the non-contact area ratio outside the range ("Non-contact area ratio in the range of 1 / 4 to 1 / 2" - "Non-contact area ratio outside the range") 1 / 2 - Non-contact area of ​​circumference (cm 2 )": Non-contact area created by adjusting the contact area using through holes in the range from the center of the polishing surface to the periphery of the circle with a radius of 1 / 2 (total area of ​​through holes in the range from the periphery of the circle with a radius of 1 / 2) 1 / 2 Circumference Reference Area (cm 2 )": The reference contact area (area of ​​the polishing pad within the range from the center of the polishing surface to the outer edge of the circle with a radius of 1 / 2 from the center of the polishing surface) when the contact area adjustment by the through holes is not performed. "Non-contact area ratio from 1 / 2 to the circumference": The ratio of the non-contact area to the reference area in the range from the center of the polishing surface to the circle with a radius of 1 / 2 to the outer edge (area of ​​the through hole / area of ​​the polishing pad x 100) "Difference in non-contact area ratio": The difference between the non-contact area ratio in the range from the center of the polished surface to the circle with a radius of 1 / 4 to the circle with a radius of 1 / 2, and the non-contact area ratio in the range from the center of the polished surface to the circle with a radius of 1 / 2 to the outer edge ("Non-contact area ratio in the range of 1 / 4 to 1 / 2" - "Non-contact area ratio in the range of 1 / 2 to the circumference") "Polishing test": Evaluation result of polishing test using a polishing pad (if the difference in thickness between the center and the circumference of the wafer is 8 μm or less, it is ◯; if it exceeds 8 μm, it is ×) [Industrial Applicability]

[0069] The polishing pad of the present invention is suitable for use in polishing semiconductors, silicon wafers for semiconductor devices, substrates for various recording disks, glass substrates for liquid crystal displays, and the like, and is therefore industrially applicable for these applications. [Explanation of symbols]

[0070] 1A, 1B...Polishing pad P…Polished surface 10...polishing layer 11...Lattice groove C…center O...Outer edge 21a, b, 22a, b...Spiral groove 31...Through hole

Claims

1. A polishing pad comprising a polishing layer having a polishing surface for polishing an object to be polished, the polishing surface being provided with lattice grooves formed in a lattice pattern, The polishing surface has a first region extending from a center of the polishing surface toward an outer periphery thereof to a circle having a radius of ¼ to a circle having a radius of ½ of the polishing surface, and a second region extending from the circle having a radius of ½ to the outer periphery of the polishing surface, providing a region that is not in contact with the workpiece, separate from the grating grooves, so that a first contact area ratio per unit area in the first region that can come into contact with the workpiece is smaller than a second contact area ratio per unit area in the second region that can come into contact with the workpiece; 13. A polishing pad according to claim 12, wherein the non-contact area is a spiral groove formed in a spiral shape extending from the center to the outer periphery.

2. The polishing pad of claim 1 , wherein a groove width of the spiral groove in the first region is greater than a groove width of the spiral groove in the second region.

3. A polishing pad comprising a polishing layer having a polishing surface for polishing an object to be polished, the polishing surface being provided with lattice grooves formed in a lattice pattern, The polishing surface has a first region extending from a center of the polishing surface toward an outer periphery thereof to a circle having a radius of ¼ to a circle having a radius of ½ of the polishing surface, and a second region extending from the circle having a radius of ½ to the outer periphery of the polishing surface, providing a region that is not in contact with the workpiece, separate from the grating grooves, so that a first contact area ratio per unit area in the first region that can come into contact with the workpiece is smaller than a second contact area ratio per unit area in the second region that can come into contact with the workpiece; A polishing pad, characterized in that the non-contact area is a through hole that penetrates the polishing layer in a direction perpendicular to the polishing surface.

4. 4. The polishing pad of claim 3, wherein the through holes are arranged in a spiral pattern, a concentric pattern, or a radial pattern drawn in a direction from the center of the polishing surface toward the outer periphery.

Citation Information

Patent Citations

  • Grinding method and grinding device

    JP2000094303A

  • Polishing pad

    JP2004327567A

  • Abrasive pad and chemical mechanical polishing device

    JP2015018835A

  • Polishing pad

    JP2018167370A

  • Polishing pad

    JP2019123031A