Cap liner material

A liner material with ethylene vinyl acetate copolymer, paraffin wax, and tackifier addresses cracking and abrasion issues in hot melt compositions, ensuring long-term sealing and opening performance and moisture resistance for caps.

JP7570948B2Active Publication Date: 2024-10-22NIPPON CLOSURES +2
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021038915
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-11
Publication Date
2024-10-22
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

Conventional hot melt composition-based liner materials for caps suffer from issues such as cracking, abrasion, and reduced heat resistance due to high hardness, which affect their sealing and opening properties over time.

Method used

A liner material composed of ethylene vinyl acetate copolymer, paraffin wax, liquid polymer, and tackifier, with specific ratios and properties, is used to form a sealing layer on caps, enhancing viscosity, cohesive force, and durability, allowing spin lining for high productivity.

Benefits of technology

The material effectively prevents cracking and abrasion, maintains excellent sealing and opening properties over a long period, and ensures high moisture resistance, suitable for chemical containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570948000001
    Figure 0007570948000001
  • Figure 0007570948000002
    Figure 0007570948000002
Patent Text Reader

Abstract

To provide a liner material that can maintain excellent sealability for a long time since the same is properly protected from cracking or scraping due to repeated opening / closing, excessive winding-up and the like and is also prevented from cracking during long-term storage at high temperatures.SOLUTION: A liner material for caps contains, relative to an ethylene vinyl acetate copolymer 100 pts.mass, paraffin wax 62-117 pts.mass, a liquid polymer 1-17 pts.mass, and a tackifier 50-117 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liner material for a cap made of a hot melt composition, and more specifically, to a liner material for a cap capable of maintaining excellent moisture resistance and sealing properties for a long period of time, a cap having a sealing layer using this liner material, and a method for manufacturing the same. [Background technology]

[0002] A resin liner is provided on the inner surface of the top plate of the cap, which is in close contact with the tip of the container mouth to improve the sealing performance of the container. Generally, resin liners include liners made of thermoplastic resins such as polyethylene, liners made of polyvinyl chloride resin, liners made of natural rubber, and liners made of urethane-based elastomers.

[0003] Conventionally, in caps used for containers containing medicines, a liner material made of a water-dispersed latex of natural rubber has been formed on the inner surface of the cap shell from the standpoint of moisture resistance, safety, etc. However, when a liner is formed using a water-dispersed natural rubber latex, problems such as floating of sugar components and blackening derived from the natural rubber component make quality control complicated, and a long drying process is required to dry out the moisture in the material, resulting in problems in terms of productivity. Furthermore, for containers containing pharmaceuticals, it is important that they have high moisture resistance. In addition to undergoing the long drying process mentioned above, traditionally these containers have been packed using a combination of special packaging materials such as tarpaulin paper and rust-proof sheets, which means there is a risk of paper powder becoming mixed in.

[0004] From this perspective, there is a demand for liner materials for pharmaceutical caps that do not use natural rubber, are excellent in safety and productivity, are free of problems such as odor and moisture barrier properties, do not require special equipment, and are excellent in productivity and economy. On the other hand, a liner material made of a hot melt composition has been proposed as a liner material that can be formed by spin lining, is excellent in safety and productivity, and can maintain high moisture resistance (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6038472 [Patent Document 2] JP 2015-27882 A Summary of the Invention [Problem to be solved by the invention]

[0006] The liner material made of the above hot melt composition is generally made of a thermoplastic resin such as an olefin resin or a thermoplastic elastomer such as a styrene-based elastomer, and wax or a plasticizer for adjusting viscosity is blended therein as required. However, since the liner material made of the hot melt composition has a higher hardness and a lower heat resistance than the above-mentioned liner material mainly made of natural rubber, problems have arisen such as wear due to repeated opening and closing, cracks due to over-tightening, or cracks due to long-term storage at high temperatures. SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a liner material made of a hot melt composition which solves the above-mentioned problems and is capable of maintaining excellent sealing properties and opening properties for a long period of time. [Means for solving the problem]

[0007] According to the present invention, there is provided a liner material for caps, characterized by containing 62 to 117 parts by weight of paraffin wax, 1 to 17 parts by weight of a liquid polymer, and 50 to 117 parts by weight of a tackifier relative to 100 parts by weight of ethylene-vinyl acetate copolymer.

[0008] In the liner material for caps of the present invention, 1. The viscosity at 150℃ measured with a B-type viscometer is in the range of 500 to 1500 mPa s. 2. The liquid polymer is polyisobutylene having a viscosity average molecular weight in the range of 40,000 to 70,000; 3. The paraffin wax has a melting point of 65 to 85°C and a needle penetration at 25°C of 5 to 15 dmm; 4. The ethylene-vinyl acetate copolymer has a vinyl acetate content of 25 to 35% by weight and a melt flow rate (hereinafter simply referred to as "MFR") (190°C, 2.16 kg) in the range of 350 to 1200 g / 10 min.; 5. The tackifier is a styrene-based resin having a softening point in the range of 90 to 120°C. 6. The JIS A hardness of the liner after molding is 75 to 95. is preferred.

[0009] The present invention also provides a cap, characterized in that the above-mentioned cap liner material is formed on the inner surface as a sealing layer.

[0010] The present invention further provides a method for manufacturing a cap, in which a sealing layer made of the above-mentioned cap liner material is formed in a cap shell by spin lining, characterized in that the spin lining process is carried out by rotating the cap shell under conditions of 100 to 600 rpm. Effect of the Invention

[0011] The cap liner material of the present invention effectively prevents the occurrence of wear due to repeated opening and closing, cracks due to over-tightening, or cracks due to long-term storage at high temperatures, which are problems associated with liner materials made of conventional hot melt compositions, and can maintain excellent sealing performance for a long period of time. The liner material of the present invention has a viscosity at 150° C. in the range of 500 to 1500 mPa·s as measured by a Brookfield viscometer, and therefore a liner with excellent surface smoothness can be molded by spin lining with good productivity. Furthermore, the liner after molding has a JIS A hardness in the range of 75 to 95, and has excellent sealing properties as well as excellent opening properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (liner material) An important feature of the liner material of the present invention is that it is made of a hot melt composition containing 62 to 117 parts by weight of paraffin wax, 1 to 17 parts by weight of a liquid polymer, and 50 to 117 parts by weight of a tackifier, relative to 100 parts by weight of ethylene-vinyl acetate copolymer. Paraffin wax is blended into liner materials made of hot melt compositions for the purposes of improving wettability to adherends, adjusting viscosity, preventing surface tack, etc. Although the incorporation of paraffin wax improves moisture resistance, liner materials containing paraffin wax are prone to cracking and chipping. In the present invention, it was found that the above-mentioned cracking and chipping caused by paraffin wax can be improved by blending the liquid polymer in the above range. That is, the liquid polymer functions as a binder for the liner material, making it possible to suppress the occurrence of chipping due to repeated opening and closing, cracking due to over-seaming, or cracking due to long-term storage at high temperatures in the liner material made of a hot melt composition containing paraffin wax. In addition, by incorporating the above-mentioned tackifier, the compatibility between the base resin, ethylene-vinyl acetate copolymer, and the paraffin wax is improved, thereby improving the cohesive strength of the liner material and adjusting its hardness, thereby making it possible to improve its durability. Furthermore, the viscosity of the liner material of the present invention at 150° C. as measured with a Brookfield viscometer is adjusted to the range of 500 to 1500 mPa·s, making it possible to form a liner by spin lining, which will be described later.

[0013] [Ethylene vinyl acetate copolymer] In the liner material of the present invention, the ethylene vinyl acetate copolymer (hereinafter sometimes referred to as "EVA") serving as the base resin preferably has a vinyl acetate content in the range of 25 to 35% by weight, particularly 28 to 32% by weight. If the vinyl acetate content is lower than the above range, the liner material will be harder than when it is in the above range, and there is a risk that cracks will easily occur due to over-seaming, and if the vinyl acetate content is higher than the above range, the liner material will be too soft compared to when it is in the above range, and there is a risk that the opening torque will increase and that scraping will occur due to repeated opening and closing. The ethylene-vinyl acetate copolymer preferably has an MFR (190°C, 2.16 kg) in the range of 350 to 1200 g / 10 min, particularly 400 to 1000 g / 10 min. If the MFR is smaller than the above range, it is more difficult to obtain smoothness in the liner material formed by spin lining than when it is in the above range, while if the MFR is larger than the above range, it is more difficult to form a uniform liner by spin lining than when it is in the above range.

[0014] [Paraffin wax] As mentioned above, paraffin wax is blended in an amount of 62 to 117 parts by weight, preferably 80 to 90 parts by weight, per 100 parts by weight of ethylene-vinyl acetate copolymer in order to improve the moisture resistance of the liner material and adjust the viscosity of the liner material. If the amount of paraffin wax is less than the above range, the liner surface may become sticky due to increased tackiness, and the openability may decrease, and the viscosity may increase, resulting in decreased moldability, compared to when the amount is within the above range. On the other hand, if the amount of paraffin wax is more than the above range, cracking and chipping may occur more easily, compared to when the amount is within the above range. The paraffin wax preferably has a melting point in the range of 65 to 85° C., particularly 70 to 80° C. If the melting point is lower than the above range, the heat resistance of the liner material may be reduced compared to when the melting point is within the above range, while if the melting point is higher than the above range, the hardness of the liner material may be higher compared to when the melting point is within the above range, and scraping may occur due to repeated opening and closing. The paraffin wax preferably has a penetration at 25° C. in the range of 4 to 19 dmm, particularly 5 to 15 dmm. With the penetration in the above range, the hardness of the liner material tends to be in the appropriate range, making it possible to suppress abrasion of the liner material.

[0015] [Liquid polymer] As described above, the liquid polymer is blended in an amount of 1 to 17 parts by weight, preferably 5 to 10 parts by weight, per 100 parts by weight of ethylene-vinyl acetate copolymer in order to suppress abrasion during repeated opening and closing of the liner material, cracking during storage at high temperatures, etc. If the amount of liquid polymer is less than the above range, there is a risk that cracking and abrasion will occur more easily than when it is within the above range due to a lack of binder. On the other hand, if the amount of liquid polymer is more than the above range, there is a risk that the liner surface will become sticky due to increased tackiness, compared to when it is within the above range, and the opening property will decrease, and the heat resistance will also decrease. Examples of liquid polymers include liquid polybutene, liquid polyisobutene, liquid polyisoprene, liquid polybutadiene, liquid poly-α-olefin, liquid ethylene-α-olefin copolymer, liquid ethylene propylene copolymer, liquid ethylene butylene copolymer, etc., and among these, liquid polyisobutylene is preferably used. The liquid polymer preferably has a viscosity average molecular weight in the range of 40000 to 70000. When the viscosity average molecular weight of the liquid polymer is in the above range, the above-mentioned effect of suppressing cracking and chipping is more effectively exhibited.

[0016] [Tackifire] As described above, the tackifier is blended in an amount of 50 to 117 parts by weight, preferably 80 to 90 parts by weight, per 100 parts by weight of ethylene-vinyl acetate copolymer in order to improve the compatibility between the base resin ethylene-vinyl acetate copolymer and the paraffin wax, and thereby improve the cohesive strength and durability of the liner material. If the amount of tackifier is less than the above range, the above effect obtained by blending the tackifier cannot be fully obtained compared to when it is within the above range, while if the amount of tackifier is more than the above range, the tackiness increases compared to when it is within the above range, so the liner surface becomes sticky, the opening property decreases, and the liner material may become more likely to crack. As the tackifier, a conventionally known tackifier can be used, and examples thereof include styrene-based resins such as styrene oligomers, copolymers of styrene and α-methylstyrene, copolymers of vinyltoluene and α-methylstyrene, phenoxyethyl acrylate oligomers, petroleum-based saturated hydrocarbons and hydrogenated products thereof, terpene phenols and hydrogenated products thereof, rosin phenols and hydrogenated products thereof, aromatic petroleum resins and hydrogenated products thereof, and the like. Among these, styrene-based resins having a softening temperature in the range of 90 to 120°C can be preferably used.

[0017] [others] In the liner material of the present invention, additives such as plasticizers, lubricants, and fillers which have been used in liner materials made of conventional hot melt compositions can be added as necessary. Examples of the plasticizer include conventionally known plasticizers such as silicone oil and polyethylene glycol, and silicone oil is particularly preferred. The plasticizer is preferably blended in an amount of 0.25 to 6.7 parts by weight per 100 parts by weight of ethylene vinyl acetate copolymer. This makes it possible to improve the slipperiness of the surface of the liner material. Examples of the lubricant include conventionally known lubricants such as erucic acid amide and stearic acid amide, and erucic acid amide is particularly suitable. The lubricant is preferably blended in an amount of 0.25 to 6.7 parts by weight per 100 parts by weight of ethylene-vinyl acetate copolymer. This can suppress an increase in the opening torque of the cap, and good opening properties can be obtained.

[0018] (Cap and its manufacturing method) The liner material made of the hot melt composition of the present invention can be prepared by mixing the above-mentioned ethylene-vinyl acetate copolymer and other components in a mixer heated to a temperature of 100 to 180°C. As mentioned above, the prepared liner material preferably has a viscosity in the range of 500 to 1500 mPa·s at 150°C as measured with a Brookfield viscometer, which makes it possible to form the liner by spin lining. The heated and melted liner material is applied by spin lining to the annular portion of the inner surface of the top plate of the cap shell rotating at 100 to 600 rpm where the tip of the container mouth abuts, and is then allowed to cool naturally and solidify to form an annular liner that serves as a sealing layer. This liner preferably has a JIS A hardness in the range of 75 to 95, which enables it to function as a sealing layer that is excellent in terms of sealing performance, opening properties, durability, and the like.

[0019] The liner material of the present invention does not require high-temperature drying during liner molding, and therefore can be applied not only to metal caps but also to conventionally known resin caps such as polyethylene and polypropylene. Furthermore, the liner material of the present invention is effectively prevented from being worn down due to repeated opening and closing, and from being cracked due to over-tightening, and therefore can be suitably used, particularly for caps having a screw portion. EXAMPLES

[0020] (Evaluation method) [Repeated opening and closing evaluation (wear resistance)] The resulting cap with liner was applied to a glass bottle and wrapped with a force of 200 N·cm, then stored at room temperature of 23°C for one day and opened and closed 100 times, after which the condition of the liner surface was visually inspected. The evaluation criteria in the table are as follows: ○: No chipping occurred. ×: Scraping occurred.

[0021] [High temperature storage evaluation] The resulting cap with liner was applied to a glass bottle, which was then tightened with a force of 200 N·cm and stored in a thermostatic chamber at 55°C for one day. The bottle was then opened and the condition of the liner surface was visually inspected. The evaluation criteria in the table are as follows: ◯: No cracks were observed. ×: Cracks occurred.

[0022] [Overtightening evaluation] The resulting cap with liner was applied to a glass bottle, and the bottle was then tightened with a force of 250 N·cm. The bottle was then opened and the condition of the liner surface was visually inspected. The evaluation criteria in the table are as follows: ◯: No cracks were observed. ×: Cracks occurred.

[0023] [Opening ability] The resulting cap with liner was applied to a glass bottle, which was then sealed with a force of 200 N·cm. The bottle was then stored at room temperature of 23°C for one week, after which the bottle was opened and the ease of opening was evaluated. The evaluation criteria in the table are as follows: ○: The bottle was opened successfully. △: The bottle was opened generally well. ×: Cannot be opened easily.

[0024] [Moisture resistance] The resulting cap with liner was applied to a glass bottle, which was then sealed with a force of 130 N·cm. The bottle was then stored in an environment of 40°C and 90% RH for one month, after which the change in humidity inside the container was measured. The evaluation criteria in the table are as follows: ○: Moisture permeability is 1 mg / day or less. ×: Moisture permeability exceeds 1 mg / day.

[0025] [Moldability] The liner formed within the cap was visually evaluated. A: A smooth liner is uniformly formed inside the cap. ×: A smooth liner is not uniformly molded within the cap.

[0026] (Examples 1 to 3, Comparative Examples 1 to 7) Liner materials were prepared with the compositions shown in Tables 1 and 2 below. The obtained liner materials were applied by spin lining in an amount of 0.6 to 0.7 g onto a metal cap (diameter 40.5 mm) rotated at 350 rpm, and allowed to cool naturally and solidify to form liners. The above-mentioned evaluations were carried out on the obtained cap with liner. The results are shown in Tables 1 and 2.

[0027] [Table 1]

[0028] [Table 2] [Industrial Applicability]

[0029] The liner material of the present invention is effectively prevented from cracking or wear caused by repeated opening and closing, over-tightening, etc., and from cracking when stored at high temperatures for long periods of time, and therefore can maintain good sealing performance for long periods of time. It also has excellent moisture resistance, making it suitable for use as a liner material applied to the caps of pharmaceutical containers.

Claims

1. A liner material for a cap, comprising 62 to 117 parts by weight of paraffin wax, 1 to 17 parts by weight of a liquid polymer, and 50 to 117 parts by weight of a tackifier, relative to 100 parts by weight of an ethylene-vinyl acetate copolymer.

2. 2. The liner material for caps according to claim 1, wherein the viscosity at 150° C. as measured by a Brookfield viscometer is in the range of 500 to 1500 mPa·s.

3. 3. The liner material for caps according to claim 1, wherein the liquid polymer is polyisobutylene having a viscosity average molecular weight in the range of 40,000 to 70,000.

4. 4. The liner material for caps according to claim 1, wherein the paraffin wax has a melting point of 65 to 85°C and a penetration at 25°C of 5 to 15 dmm.

5. The liner material for caps according to any one of claims 1 to 4, wherein the ethylene-vinyl acetate copolymer has a vinyl acetate content of 25 to 35% by weight and an MFR (190°C, 2.16 kg) in the range of 350 to 1200 g / 10 min.

6. 6. The liner material for caps according to claim 1, wherein the tackifier is a styrene-based resin having a softening point in the range of 90 to 120°C.

7. 7. The liner material for caps according to claim 1, wherein the liner after molding has a JIS A hardness of 75 to 95.

8. A cap, characterized in that the cap liner material according to any one of claims 1 to 7 is formed on an inner surface as a sealing layer.

9. A method for manufacturing a cap, comprising forming a sealing layer made of the cap liner material according to any one of claims 1 to 7 in a cap shell by spin lining, A method for manufacturing a cap, wherein the spin lining step is carried out by rotating the cap shell at a speed of 100 to 600 rpm.

Citation Information

Patent Citations

  • Hottmelt adhesive composition

    JP1979127441A

  • Sealing agent composition and sealing method

    JP1982014675A

  • Production of hermetically sealing gasket for container

    JP1984222278A

  • Composite-structure carbon black and production thereof

    JP1985038472A

  • Cap linear having excellent heat resistance

    JP1988120750A