Cold-rolled heat-treated steel sheet and its manufacturing method
A steel composition and manufacturing process with specific elements and microstructure enhance mechanical properties, achieving yield and tensile strengths, uniform elongation, and hole expansion ratio for lightweight automotive components.
Patent Information
- Application Number
- JP2022530217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-12-16
AI Technical Summary
Existing high-strength steels struggle to achieve a combination of yield strength greater than 950 MPa, tensile strength greater than 1180 MPa, uniform elongation greater than 10%, and hole expansion ratio greater than 25%, which are essential for lightweight automotive components without compromising safety and formability.
A steel composition with specific carbon, manganese, silicon, aluminum, boron, niobium, molybdenum, vanadium, and titanium contents, combined with a microstructure of 5%~45% ferrite, 25%~85% distributed martensite, 10%~30% retained austenite, and less than 8% fresh martensite, achieved through a manufacturing process involving hot rolling, annealing, cold rolling, and quenching and partitioning (Q&P) treatment.
The solution results in a steel plate with enhanced mechanical properties, including yield strength greater than 950 MPa, tensile strength greater than 1180 MPa, uniform elongation greater than 10%, and hole expansion ratio greater than 25%, meeting the requirements for lightweight automotive applications.
Smart Images

Figure 0007571137000001 
Figure 0007571137000002 
Figure 0007571137000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cold rolled high strength steel sheet having high ductility and formability and to a method for obtaining such a steel sheet. [Background technology]
[0002] It is known to use steel sheets made from DP (Dual Phase) steels or TRIP (Transformation Induced Plasticity) steels to manufacture various items such as body structural members and body panel parts for automobiles.
[0003] One of the main challenges in the automotive industry is to reduce the weight of vehicles to improve their fuel efficiency in terms of global environmental conservation, without neglecting safety requirements. To meet these requirements, new high-strength steels are continuously developed by the steelmaking industry to have steel plates with improved yield strength and tensile strength, as well as good ductility and formability.
[0004] Publication WO2019123245 describes a method for obtaining a high-strength and high-formability cold-rolled steel sheet having a yield strength YS of 1000 MPa to 1300 MPa, a tensile strength TS of 1200 MPa to 1600 MPa, a uniform elongation UE of at least 10%, and a hole expansion ratio HER of at least 20% by quenching and partitioning treatment. The microstructure of this cold-rolled steel sheet consists of a surface fraction of: 10% to 45% ferrite, with an average grain size of at most 1.3 μm, the product of the surface fraction of ferrite and the average grain size of ferrite being at most 35 μm%, 8% to 30% retained austenite, the retained austenite having a Mn content higher than 1.1*Mn%, where Mn% denotes the Mn content of the steel, with at most 8% fresh martensite, at most 2.5% cementite, and the remainder being partitioned martensite. A surface fraction of at least 8% of retained austenite with a Mn content higher than 1.1*Mn% makes it possible to obtain a combination of high ductility and high strength.
[0005] During annealing of the hot rolled steel sheet, the austenite is enriched with manganese. The annealing after cold rolling according to the present invention homogenizes the microstructure with finer fresh martensite and islands of MA, and therefore does not give the characteristics of publication WO2019123245.
[0006] Publication WO2018220430 relates to a steel sheet that is hot formed to produce a part. The steel part is then cooled before being reheated, held at the post-treatment temperature and cooled to room temperature. Such a hot forming process induces severe local deformation of the steel part due to the geometry of the part and the forming tool, resulting in local modifications of the microstructure. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2019 / 123245 [Patent Document 2] International Publication No. 2018 / 220430 Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to solve the above-mentioned problems and provide a steel sheet having a yield strength greater than 950 MPa, a tensile strength greater than 1180 MPa, a uniform elongation greater than 10%, and a hole expansion ratio HER greater than 25%. [Means for solving the problem]
[0009] The object of the present invention is achieved by providing a steel sheet according to claim 1. The steel sheet may also comprise the features according to any one of claims 2 to 10. Another object is achieved by providing a method according to claim 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The invention will now be described in detail and illustrated by examples without introducing limitations.
[0011] In the following, Ae1 denotes the equilibrium transformation temperature below which austenite becomes completely unstable, Ae3 denotes the equilibrium transformation temperature above which austenite becomes completely stable, and Ms denotes the martensite transformation start temperature, i.e. the temperature at which austenite begins to transform into martensite on cooling. These temperatures can be calculated from the following formulas:
[0012] Ae1 = 670 + 15 * % Si - 13 * % Mn + 18 * % Al Ae3=890-20*√%C+20*%Si-30*%Mn+130*%Al Ms=560-(30*%Mn+13*%Si-15*%Al+12*%Mo)-600*(1-exp(-0,96*C)) The composition of the steel according to the invention comprises, by weight percentage:
[0013] According to the present invention, the carbon content is 0.12%-0.25%. If the addition amount exceeds 0.25%, the weldability of the steel plate may be deteriorated. If the carbon content is less than 0.12%, the residual austenite fraction is not stabilized enough to obtain sufficient elongation and tensile strength. In a preferred embodiment, the carbon content is 0.15%-0.25%.
[0014] According to the invention, the manganese content is between 3.0% and 8.0% in order to obtain sufficient elongation together with the stabilization of austenite. If the addition exceeds 8.0%, the risk of central segregation increases and the yield strength and tensile strength are impaired. Below 3.0%, the final structure contains an insufficient fraction of retained austenite so that the desired combination of ductility and strength is not achieved. In a preferred embodiment, the manganese content is between 3.0% and 5.0%.
[0015] According to the invention, the silicon content is between 0.70% and 1.50%. A silicon addition of at least 0.70% helps to stabilize a sufficient amount of retained austenite. Above 1.50%, silicon oxides form on the surface, which impairs the coatability of the steel. In a preferred embodiment, the silicon content is between 0.80% and 1.30%.
[0016] The aluminum content is between 0.3% and 1.2%, because aluminum is a very effective element for deoxidizing steel in the liquid phase during refining. The aluminum content is below 1.2% to avoid the occurrence of inclusions and to avoid oxidation problems. In a preferred embodiment, the aluminum content is between 0.3% and 0.8%.
[0017] The boron content is 0.0002%-0.004% to increase the hardenability of the steel and improve the weldability of the steel plate. Optionally, several elements can be added to the composition of the steel according to the invention.
[0018] Niobium may optionally be added up to 0.06% to refine the austenite grains during hot rolling and provide precipitation strengthening. Preferably, the minimum amount of niobium added is 0.0010%. Above 0.06%, the yield strength and elongation are not at the desired levels.
[0019] Molybdenum can be added up to 0.5%. It stabilizes the retained austenite and therefore reduces the austenite decomposition during distribution. Above 0.5%, the addition of molybdenum becomes costly and ineffective considering the properties required.
[0020] Vanadium may optionally be added up to 0.2% to provide precipitation strengthening.
[0021] Titanium may be added up to 0.05% to provide precipitation strengthening. At titanium levels above 0.05%, yield strength and elongation are not as good as desired. Preferably, a minimum of 0.01% titanium is added in addition to boron to protect the boron from the formation of BN.
[0022] The balance of the steel composition is iron and impurities resulting from smelting. In this respect, at least P, S and N are considered as residual elements, which are unavoidable impurities. Their contents are less than 0.010% for S, less than 0.020% for P and less than 0.008% for N.
[0023] Next, the microstructure of the cold-rolled heat-treated steel sheet according to the present invention will be described. The cold-rolled heat-treated steel sheet has a surface fraction of 5% to 45% ferrite and 25% to 85% distributed martensite, and is strictly 2x10 6 / mm 2 The microstructure comprises said partitioned martensite having a carbide density of less than 10%, 10% to 30% retained austenite, and less than 8% fresh martensite. A portion of the fresh martensite combines with the retained austenite to form martensite-austenite (MA) islands with a total surface fraction of less than 10%. In a preferred embodiment, these MA islands have a shape factor of 2 or less.
[0024] Ferrite is formed during annealing at a temperature between (Ae1+Ae3) / 2 and Ae3. If the ferrite fraction is less than 5%, the uniform elongation does not reach 10%. If the ferrite fraction is higher than 45%, the tensile strength of 1180 MPa and the yield strength of 950 MPa are not achieved.
[0025] The microstructure of the cold rolled heat treated steel sheet contains 25% to 85% of distributed martensite to ensure high ductility of the steel, and the distributed martensite is strictly 2x10 6 / mm 2The microstructure has a carbide density of less than 100%. Partitioned martensite is martensite that is formed upon cooling after annealing and then partitioned during the partitioning step. Preferably, the microstructure contains 40% to 80% partitioned martensite.
[0026] The microstructure of the cold rolled heat treated steel sheet contains 10% to 30% retained austenite and less than 8% fresh martensite to ensure high ductility of the steel. Preferably, the microstructure contains a maximum of 6% fresh martensite. Fresh martensite is formed during cooling of the cold rolled heat treated steel sheet at room temperature. The size of the fresh martensite and martensite-austenite islands is less than 0.7 μm.
[0027] The steel sheet according to the invention can be manufactured by any suitable manufacturing method, which the person skilled in the art can define, however it is preferable to use a method according to the invention comprising the following steps:
[0028] Further, the above-mentioned steel composition is provided for semi-finished products that can be hot rolled. The semi-finished products are then heated to a temperature T of 1150°C to 1300°C to facilitate hot rolling. reheat The steel sheet is heated to a final hot rolling temperature FRT of 800°C to 950°C to obtain a hot rolled steel sheet. The maximum value of FRT is selected to avoid coarsening of austenite grains. Preferably, FRT is 800°C to 910°C.
[0029] The hot-rolled steel is then cooled to a temperature T coil The winding temperature is preferably (Ms-100°C) to 550°C.
[0030] After coiling, the steel sheet may be pickled to remove oxidation.
[0031] Then, in order to improve the cold rollability and toughness of the hot rolled steel sheet, the hot rolled steel sheet is annealed at a first annealing temperature TA1 of 550°C to 700°C, and maintained at the annealing temperature for a holding time tA1 of 30 seconds to 50 hours.
[0032] The hot rolled annealed steel sheet is then cold rolled to obtain a cold rolled steel sheet having a thickness which may range, for example, from 0.7 mm to 3 mm, or even better from 0.8 mm to 2 mm. The cold rolling reduction is preferably between 20% and 80%. Below 20%, recrystallization during the subsequent heat treatment is unfavorable and may impair the ductility of the cold rolled heat treated steel sheet. Above 80%, there is a risk of edge cracking during cold rolling.
[0033] The cold rolled steel sheet is then reheated to a second annealing temperature TA2 above Ae3-10°C and maintained at said TA2 temperature for a holding time tA2 between 1 second and 1000 seconds to obtain, as annealed, a microstructure comprising martensite and bainite, the sum of which is greater than 80%, strictly less than 20% ferrite and strictly less than 20% islands of martensite-austenite (MA) and carbides.
[0034] Martensite in the martensite-austenite islands is fresh martensite. Martensite that is greater than 80% of the total of martensite and bainite is self-tempered martensite. Determination of the type of martensite can be done and quantified by scanning electron microscopy with a field emission gun ("FEG-SEM").
[0035] The cold rolled steel sheet then undergoes a quenching and distribution process (Q&P), which includes the following steps:
[0036] reheating the cold-rolled steel sheet to a temperature TA3 strictly below Ae3 and above (Ae1+Ae3) / 2, in order to obtain an austenitic and ferritic structure, and maintaining it at said annealing temperature TA3 for a holding time tA3 ranging from 3 seconds to 1000 seconds.
[0037] - A process of quenching a cold rolled steel sheet at a quenching temperature TQ below (Ms-50°C) to obtain a quenched steel sheet. During this quenching process, the austenite is partially transformed into martensite. If the quenching temperature is higher than (Ms-50°C), the fraction of tempered martensite in the final structure will be too low, resulting in a fraction of fresh martensite exceeding 8%, which is detrimental to the total elongation of the steel.
[0038] - reheating the hardened steel to a distribution temperature TP between 350°C and 550°C and maintaining it at said distribution temperature for a distribution time between 1 s and 1000 s before being cooled to room temperature.
[0039] The cold rolled heat treated steel sheet according to the present invention has a yield strength YS greater than 950 MPa, a tensile strength TS greater than 1180 MPa, a uniform elongation UE greater than 10%, and a hole expansion ratio HER greater than 25%.
[0040] Preferably, the cold rolled heat treated steel sheet according to the present invention has YS and TS expressed in MPa, UE expressed in %, total elongation TE and HER, and silicon content %Si expressed in weight percent, satisfying the following formula: (YS*UE+TS*TE+TS*HER) / %Si>65000.
[0041] This formula gives the level of mechanical properties for a given silicon content.
[0042] Preferably, the total elongation TE is greater than 14%.
[0043] YS, TS, UE and TE are measured according to ISO standard ISO 6892-1. HER is measured according to ISO standard ISO 16630.
[0044] The present invention will now be illustrated by the following examples, which are not intended to be limiting in any way. EXAMPLES
[0045] The three grades, whose compositions are summarized in Table 1, were cast into semi-finished products and processed into steel sheets according to the processing parameters summarized in Table 2.
[0046] Table 1 - Composition The compositions tested are summarized in the following table, with elemental contents expressed as weight percent.
[0047] [Table 1]
[0048] Table 2 - Processing parameters The as-cast steel semi-finished product was reheated at 1200°C, hot rolled at a finishing rolling temperature FRT, coiled and first heat treated at a temperature TA1 and maintained at said TA1 temperature for a holding time ta1 before cold rolling. A second annealing was performed at a temperature TA2 and the cold rolled steel was maintained at said TA2 temperature for a holding time ta2 before quenching and distribution treatment (Q&P) and subsequent cooling at room temperature. The following specific conditions were applied:
[0049] [Table 2]
[0050] The annealed steel sheets were then analyzed, and the corresponding microstructural elements before and after Q&P and mechanical properties after Q&P were summarized in Tables 3, 4, and 5, respectively.
[0051] Table 3-Microstructure of steel sheet before Q&P treatment The microstructures of the samples tested were determined and are summarized in the following table.
[0052] [Table 3]
[0053] B: represents the bainite surface fraction F: Ferrite surface fraction M: represents the martensite surface fraction MA: represents the surface fraction of martensite-austenite islands The surface fraction is determined by the following method: a test piece is cut from a cold-rolled heat-treated steel sheet, polished and etched with reagents known per se to reveal the microstructure. The section is then examined at a magnification of more than 5000 times using an optical microscope or a scanning electron microscope, for example a scanning electron microscope equipped with a field emission gun coupled to a BSE (backscattered electrons) device ("FEG-SEM").
[0054] The determination of the surface fraction of each component is carried out by means of image analysis in a manner known per se. The retained austenite fraction is determined, for example, by X-ray diffraction (XRD).
[0055] For tests 6 and 7, which were not annealed at temperature TA2 during tA2, the microstructure before Q&P is that of the cold-rolled steel sheet. For tests 1 to 5, the microstructure given before Q&P is the microstructure obtained after the second annealing.
[0056] Table 4-Microstructure of steel sheets after Q&P treatment The microstructures of the samples tested were determined and are summarized in the following table.
[0057] [Table 4]
[0058] γ: Represents the surface fraction of retained austenite PM: represents the surface fraction of partitioned martensite FM: represents the surface fraction of fresh martensite F: Ferrite surface fraction MA: represents the surface fraction of martensite-austenite islands Due to the second annealing, there is a more homogeneous microstructure with fine fresh martensite and MA islands with sizes less than 0.7 μm, whereas in Tests 6 and 7, there is no second annealing and therefore there is a more significant enrichment of Mn in the austenite, forming more than 10% larger fresh martensite and MA islands with a more heterogeneous size distribution.
[0059] Table 5-Mechanical properties of cold-rolled heat-treated steel sheets after Q&P treatment The mechanical properties of the tested samples were determined and are summarized in the following table.
[0060] [Table 5]
[0061] These examples show that the steel sheets according to the invention, ie, Examples 1 to 4, are unique in that they exhibit all the targeted properties due to their specific composition and microstructure.
[0062] In test 5, steel A is hot rolled, coiled, annealed a first time and cold rolled before annealing a second time according to the invention. During the quenching and distribution process, the steel is heated to a low temperature TA3, limiting the austenite and thus favoring ferrite during cooling. The yield strength of the final steel sheet is less than 950 MPa and the formula (YS*UE+TS*TE+TS*HER) / %Si does not reach 65000.
[0063] In Tests 6 and 7, Steels C and A, respectively, were not reheated before quenching and partitioning treatment. The microstructure before Q&P was 97% ferritic, which resulted in a high content of fresh martensite after Q&P. This high fraction of large size fresh martensite resulted in a hole expansion ratio of less than 25%, with the formula (YS*UE+TS*TE+TS*HER) / %Si being less than 65000.
Claims
1. Cold-rolled heat-treated steel sheet, C: 0.12-0.25% Mn: 3.0-8.0% Si: 0.70~1.50% Al: 0.3-1.2% B: 0.0002-0.004% S≦0.010% P≦0.020% N≦0.008% 0.2%≦Mo≦0.5% Including, Optionally, one or more of the following elements, in weight percent: V≦0.2% Nb≦0.06% Ti≦0.05% Including, The remainder of the composition is made of steel having a composition of iron and inevitable impurities resulting from smelting, The steel plate has a surface fraction of -5% to 45% ferrite; -25% to 85% distributed martensite, 2x10 6 / mm 2 the partitioned martensite having a carbide density of less than -10% to 30% retained austenite; -8% or less fresh martensite; a portion of the fresh martensite is combined with retained austenite in the form of martensite-austenite (MA) islands with a total surface fraction of less than 10%; having a microstructure consisting of The size of fresh martensite and martensite-austenite islands is less than 0.7 μm; The yield strength YS, expressed in MPa, the tensile strength TS, expressed in MPa, the uniform elongation UE, expressed in %, the total elongation TE, expressed in %, the hole expansion ratio HER, expressed in %, and the silicon content, expressed in weight percent, are determined by the following formula: (YS*UE+TS*TE+TS*HER) / %Si>65000 Fulfilling Cold rolled heat treated steel sheet.
2. 2. The cold rolled heat treated steel sheet according to claim 1, wherein the manganese content is 3.0% to 5.0%.
3. The cold rolled heat treated steel sheet according to any one of claims 1 to 2, having a silicon content of 0.80% to 1.30%.
4. The cold rolled heat treated steel sheet according to any one of claims 1 to 3, wherein the microstructure contains up to 6% fresh martensite.
5. The cold-rolled heat-treated steel sheet according to any one of claims 1 to 4, having a yield strength YS of more than 950 MPa.
6. The cold-rolled heat-treated steel sheet according to any one of claims 1 to 5, having a tensile strength TS of more than 1180 MPa.
7. The cold rolled heat treated steel sheet according to any one of claims 1 to 6, having a uniform elongation of greater than 10%.
8. The cold rolled heat treated steel sheet according to any one of claims 1 to 7, wherein the hole expansion ratio is greater than 25%.
9. The method for producing a cold-rolled heat-treated steel sheet according to claim 1, comprising the steps of: - casting a steel to obtain a semi-finished product, said semi-finished product having a composition according to claim 1; - The slab is heated to a temperature T reheat and reheating the mixture with - hot rolling the reheated slab at a finishing rolling temperature FRT between 800 ° C. and 950 ° C. to obtain a hot rolled steel sheet; - hot-rolled steel sheet is wound at a coiling temperature T of 200 ° C to 700 ° C. coil and winding the wire by annealing the hot-rolled steel sheet at a first annealing temperature TA1 between 550 ° C. and 700 ° C. and maintaining said steel sheet at said TA1 temperature for a holding time tA1 between 30 seconds and 50 hours; - cold rolling the hot rolled steel sheet to obtain a cold rolled steel sheet; reheating the cold rolled steel sheet to a second annealing temperature TA2 above Ae3-10°C and maintaining the steel sheet at said TA2 temperature for a holding time tA2 between 1 s and 1000 s to obtain, as annealed, a microstructure comprising martensite and bainite, the sum of which is more than 80%, less than 20% ferrite, and less than 20% sum of martensite-austenite islands (MA) and carbides, wherein the martensite of the martensite-austenite islands (MA) is fresh martensite and Ae3 is represented by the formula: Ae3=890-20*√%C+20*%Si-30*%Mn+130*%Al and reheating the cold-rolled steel sheet to a temperature TA3 lower than Ae3 and higher than (Ae1+Ae3) / 2 and maintaining said sheet at said annealing temperature TA3 for a holding time tA3 ranging from 3 seconds to 1000 seconds, Ae1 being defined by the formula: Ae1=670+15*%Si-13*%Mn+18*%Al and - quenching a cold-rolled steel sheet at a quenching temperature TQ below (Ms-50 ° C) to obtain a quenched steel sheet, where Ms is determined by the formula: Ms=560-(30*%Mn+13*%Si-15*%Al+12*%Mo)-600*(1-exp(-0,96*%C)) and - reheating the hardened steel plate to a distribution temperature TP, which is between 350°C and 550°C, and maintaining the hardened steel plate at the distribution temperature for a distribution time, which is between 1 second and 1000 seconds; - cooling the steel sheet to room temperature to obtain a cold-rolled heat-treated steel sheet; A manufacturing method comprising:
Citation Information
Patent Citations
High strength cold rolled steel sheet having excellent coating film adhesion and ductility, and automobile steel component
JP2006283130A
Steel sheet for manufacturing press hardened parts, press hardened part having a combination of high strength and crash ductility, and manufacturing methods thereof
WO2018220430A1
Steel sheet for manufacturing press hardened parts, press hardened part having a combination of high strength and crash ductility, and manufacturing methods thereof
WO2018220598A1
Cold rolled and annealed steel sheet and method of manufacturing the same
WO2019111084A1
High strength and high formability steel sheet and manufacturing method
WO2019123245A1