Composition for sintered compact and sintered compact
A combination of polyacetal and polyolefin resins with specific melt flow indices addresses moldability issues, ensuring high fluidity and preventing defects in sintered compact production, allowing for efficient and robust thin part manufacturing.
Patent Information
- Application Number
- JP2023512897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-07
- Filing Date
- 2022-03-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-16
AI Technical Summary
Existing methods using polyacetal resin as a binder for sintered compact production face issues with low fluidity leading to poor moldability, especially for thin parts, and adding flow aids can cause cracking and blistering during degreasing.
A composition for sintered bodies using a combination of polyacetal resin and polyolefin resin with specific melt flow indices, along with optional additives like nitrogen-containing compounds and fatty acid metal salts, to enhance fluidity and maintain shape retention during degreasing.
The composition allows for high fluidity and prevents cracking or blistering during degreasing, enabling the production of thin sintered compacts with improved yield and strength.
Smart Images

Figure 0007571285000001 
Figure 0007571285000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a molding material used in producing a sintered compact. [Background technology]
[0002] Particularly precise sintered compacts and sintered compacts of complex shapes that utilize sinterable powders of metals, ceramics, cermets, etc. are formed by injection molding a raw material for sintered compacts, which is prepared by heating and kneading a composition for producing sintered compacts that contains a sinterable powder and a binder, and then subjecting the green compact to a debinding process and sintering it.
[0003] In the above-mentioned method for forming a sintered compact, the most important step for obtaining a good quality compact without defects such as cracks, swelling, and deformation is the debinding step. This debinding step is a step for removing the binder from the green compact made of the injection molded body, and the method of heating the green compact to thermally decompose and gasify the binder, or the method of treating the green compact with a solvent to elute and remove the soluble binder components in the green compact, and then thermally decomposing and gasifying the remaining binder, is used. However, in the thermal debinding method in which the green compact is heated for debinding, if the thermal decomposition and gasification of the binder in the green compact occurs intensively in a short period of time, the compact during the debinding step may develop cracks or swelling, so the debinding must be performed by heating for a long period of time.
[0004] It is already known that the use of polyacetal resin, which is a depolymerizable polymer, as a binder, either alone or together with other polymers, provides the following effects: excellent shape retention of green molded bodies due to the rigidity of the polyacetal resin, and excellent shape retention of molded bodies during a debinding step by heating; no residue remains after debinding by heating; and the debinding step by heating is quick, thereby improving production efficiency (e.g., JP-A-4-247802, JP-A-5-98306, etc.). Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the methods described in JP-A-4-247802 and JP-A-5-98306, the fluidity of commercially available high-fluidity polyacetal resin is about 45 g / 10 min in melt flow index, and when a binder containing a large amount of polyacetal resin is used, the fluidity of the feedstock decreases, and moldability becomes poor, especially for products having thin parts. In addition, when trying to increase the fluidity of a binder using polyacetal resin, it is possible to add a large amount of a flow aid such as wax, but adding a large amount of one component leads to rapid volatilization during degreasing, which causes problems such as cracking and swelling.
[0006] Furthermore, for example, in the acid degreasing method described in Japanese Patent No. 5249213, in which a green molded body is degreased using an acid such as nitric acid, a binder composition with improved fluidity is proposed, which is composed of a polyacetal resin containing 2 mol % of 1,3-dioxepane, polyethylene, and poly-1,3-dioxepane. However, there is no description regarding the fluidity of the polyacetal resin, and it is assumed that the fluidity of the polyacetal resin described in the examples is low, and it is difficult to obtain a thin molded body with a thickness of 1 to 2 mm when compounded with metal powder.
[0007] Furthermore, if the concentration of 1,3-dioxepane is increased in order to increase the fluidity of the polyacetal resin, the strength of the polyacetal resin decreases, resulting in a problem that the strength of the molded body obtained by preparing a compound with metal powder and injection molding the compound decreases.
[0008] Therefore, an object of the present invention is to provide a composition for sintered molded bodies that does not impair the shape retention of green molded bodies based on the rigidity of polyacetal resin, has high fluidity, and does not cause cracks or blistering during degreasing. [Means for solving the problem]
[0009] Means for Solving the Problems The present inventors conducted intensive research to solve the above-mentioned problems, and as a result, discovered that a composition for sintered molded bodies containing an organic binder containing a polyacetal resin and a polyolefin resin having a predetermined melt flow index can solve the above-mentioned problems, thereby arriving at the present invention.
[0010] That is, the present invention is as follows. [1] A sinterable inorganic powder and an organic binder are included, the organic binder contains at least a polyacetal resin and a polyolefin resin, Melt flow index of the polyacetal resin (190℃, 2.16kg) but 90 The composition for sintered compacts has a viscosity of about 200 g / 10 min. or less. [2] 2. The composition for sintered molded bodies according to claim 1, wherein the polyolefin resin has a melt flow index (190° C., 2.16 kg) of 40 g / min or more. [3] The composition for sintered molded bodies according to [1] or [2], wherein the organic binder contains 5 to 95 mass % of the polyacetal resin and 5 to 95 mass % of the polyolefin resin, based on the mass of the organic binder. [4] The composition for sintered compacts according to any one of [1] to [3], wherein the composition for sintered compacts contains 70 to 95 parts by mass of the sinterable inorganic powder per 100 parts by mass of the composition for sintered compacts. [5] The composition for sintered compacts according to any one of [1] to [4], wherein the organic binder contains 5 to 60 mass % of a fluidity imparting agent based on the mass of the organic binder. [6] The composition for sintered compacts according to any one of [1] to [5], wherein the polyacetal resin contains an oxymethylene unit and an oxyethylene unit. [7] The composition for sintered molded bodies according to any one of [1] to [6], comprising 5 to 50 mass % of the polyacetal resin based on the mass of the organic binder. [8] The composition for sintered compacts according to any one of [1] to [7], wherein the organic binder contains a nitrogen-containing compound and a fatty acid metal salt. [9] A green compact obtained by compacting the composition for sintered compacts according to any one of [1] to [8].
[10] The green molded body according to [9], having a portion having a thickness of 1 mm or less present at 100 mm2 or more.
[11] A sinterable inorganic powder and an organic binder are included, the organic binder contains at least a polyacetal resin and a polyolefin resin, The polyacetal resin has a melt flow index (190° C., 2.16 kg) of 70 to 200 g / 10 min; The organic binder contains a nitrogen-containing compound and a fatty acid metal salt. A composition for sintered compacts comprising: Effect of the Invention
[0011] According to the present invention, it is possible to provide a composition for sintered molded bodies that does not impair the shape retention of green molded bodies based on the rigidity of polyacetal resin, has high fluidity, and does not cause cracks or blistering during degreasing. Furthermore, by using the composition for sintered compacts of the present invention, thin compacts can be easily formed, and since the composition has good degreasing properties, sintered compacts can be obtained with good yield. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following description, and can be modified in various ways within the scope of the present invention.
[0013] [Composition for sintered compacts] In this embodiment, the composition for sintered compacts contains a sinterable inorganic powder and an organic binder, and preferably consists of the inorganic powder and the organic binder. The composition for sintered compacts may further contain other additives in addition to the inorganic powder and the organic binder.
[0014] <Organic binder> The organic binder contains a polyacetal resin and a polyolefin resin. Since polyacetal resin and polyolefin resin have different thermal decomposition starting points, it is possible to gradually remove the organic binder from the green molded body during the temperature rise process during thermal degreasing. In acid degreasing, polyacetal resin is decomposed by an acid such as nitric acid and removed from the green molded body, but by blending a polyolefin resin that is not decomposed by acid, it is possible to maintain the shape of the green molded body from which the polyacetal resin has been removed.
[0015] The resin components contained in the organic binder are preferably only the polyacetal resin, the polyolefin resin, a fluidity imparting agent described below, and a nitrogen-containing compound (for example, a polyamide resin) described below.
[0016] The mass proportion of the organic binder in the composition for sintered compacts is preferably 5 to 30 parts by mass, more preferably 5 to 20 parts by mass, and even more preferably 5 to 15 parts by mass, per 100 parts by mass of the composition for sintered compacts, from the viewpoint of maintaining good moldability in injection molding and further suppressing cracks and swelling during the degreasing process.
[0017] (Polyacetal resin) The polyacetal resin may be a polyacetal homopolymer, a polyacetal copolymer, or a mixture thereof. Among these, the polyacetal resin is preferably a polyacetal copolymer from the viewpoint of thermal stability. The polyacetal resins may be used alone or in combination of two or more.
[0018] The polyacetal homopolymer may be a polymer having an oxymethylene unit in the main chain, and both ends of the polymer may be blocked with an ester group or an ether group. The polyacetal homopolymer may be obtained from formaldehyde and a known molecular weight regulator as raw materials, and may be obtained from these raw materials by a known slurry method using a known onium salt polymerization catalyst and a hydrocarbon as a solvent, for example, the polymerization method described in JP-B-47-6420 and JP-B-47-10059. The polyacetal homopolymer is preferably one in which 99.8 mol % or more of the main chain excluding both ends is composed of oxymethylene units, and more preferably the main chain excluding both ends is composed only of oxymethylene units.
[0019] The polyacetal copolymer includes a polymer having an oxymethylene unit and an oxyethylene unit in the main chain, and can be obtained, for example, by copolymerizing trioxane with a cyclic ether and / or a cyclic formal in the presence of a polymerization catalyst. Trioxane is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous formalin solution in the presence of an acid catalyst.
[0020] The trioxane may contain impurities such as water, methanol, formic acid, and methyl formate that can cause chain transfer, and it is therefore preferable to remove these impurities by, for example, distillation or other methods for purification. In this case, the total amount of impurities that can cause chain transfer is preferably 1×10 per mol of trioxane. -3 mol or less, and more preferably 0.5×10 -3 By reducing the amount of impurities to the above values, the polymerization reaction rate can be increased sufficiently for practical use, and the resulting polymer can have excellent thermal stability.
[0021] The cyclic ether and / or cyclic formal are components that can be copolymerized with the above-mentioned trioxane, and examples thereof include ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epibromohydrin, styrene oxide, oxatane, 1,3-dioxolane, ethylene glycol formal, propylene glycol formal, diethylene glycol formal, triethylene glycol formal, 1,4-butanediol formal, 1,5-pentanediol formal, and 1,6-hexanediol formal. In particular, ethylene oxide and 1,3-dioxolane are preferred. These may be used alone or in combination of two or more.
[0022] The amount of the cyclic ether and cyclic formal added is preferably 1.0 mol% or more, more preferably 3.0 mol% or more, and even more preferably 3.5 mol% or more, based on 1 mol of the trioxane. Also, the amount is preferably 8.0 mol% or less, more preferably 7.0 mol% or less, and even more preferably 5.0 mol% or less, based on 1 mol of the trioxane.
[0023] The polymerization catalyst includes boric acid, tin, titanium, phosphorus, arsenic and antimonides, which are typified by Lewis acids. In particular, boron trifluoride, boron trifluoride hydrates, and boron trifluoride coordination complexes containing organic compounds containing oxygen or sulfur atoms. For example, boron trifluoride, boron trifluoride diethyl etherate, and boron trifluoride-di-n-butyl etherate are preferred. These may be used alone or in combination of two or more.
[0024] The amount of polymerization catalyst added was 0.1×10 -5 ~0.1×10 -3 mol range is preferred, and 0.3×10 -5 ~0.5×10 -4 mol, more preferably 0.5×10 -5 ~0.4×10 -4When the amount of the polymerization catalyst added is within the above range, the polymerization reaction can be stably carried out for a long period of time.
[0025] In the production of polyacetal copolymers, deactivation of a polymerization catalyst is carried out by putting a polyacetal resin obtained by a polymerization reaction into an aqueous solution or organic solvent liquid containing at least one catalyst neutralizing deactivator such as amines such as ammonia, triethylamine, tri-n-butylamine, or hydroxides of alkali metals or alkaline earth metals, inorganic acid salts, organic acid salts, etc., and stirring the mixture in a slurry state for generally several minutes to several hours. The slurry after catalyst neutralization and deactivation is filtered and washed to remove unreacted monomers, catalyst neutralizing deactivators, and catalyst neutralization salts, and then dried.
[0026] In addition, the polymerization catalyst can be deactivated by contacting the polyacetal copolymer with vapor of ammonia, triethylamine, or the like, or by contacting the polyacetal resin with at least one of hindered amines, triphenylphosphine, calcium hydroxide, or the like in a mixer.
[0027] Alternatively, without deactivating the polymerization catalyst, the polyacetal copolymer may be heated in an inert gas atmosphere at a temperature equal to or lower than the melting point of the polyacetal copolymer to reduce the volatilization of the polymerization catalyst, and then the terminal stabilization treatment described below may be carried out using the polyacetal copolymer. The above-mentioned deactivation operation of the polymerization catalyst and the operation of reducing the volatilization of the polymerization catalyst may be carried out after pulverizing the polyacetal resin obtained by the polymerization reaction, if necessary.
[0028] The terminal stabilization treatment of the obtained polyacetal resin involves decomposing and removing the unstable terminal moiety by the following method: For example, the unstable terminal moiety can be decomposed and removed by melting the polyacetal resin using a vented single screw extruder or a vented twin screw extruder in the presence of a known basic substance capable of decomposing unstable terminal moieties, such as ammonia, fatty acid amines such as triethylamine and tributylamine, hydroxides of alkali metals or alkaline earth metals such as calcium hydroxide, inorganic weak acid salts, or organic weak acid salts, as a notching agent.
[0029] The mass proportion of the polyacetal resin in the organic binder is preferably 5 to 95 mass %, more preferably 5 to 70 mass %, and particularly preferably 5 to 60 mass %, relative to 100 mass % of the organic binder. When the organic binder is removed from the green molded body by heating, the mass ratio of the polyacetal resin is preferably 5 to 50 mass%, more preferably 5 to 45 mass%, and particularly preferably 10 to 40 mass%, relative to 100 mass% of the organic binder. By setting the ratio of the polyacetal resin in the organic binder within the above range, the shape of the green molded body tends to be well maintained.
[0030] The melt flow index of the polyacetal resin is preferably 70 g / 10 min or more and 200 g / 10 min or less, more preferably 90 g / 10 min or more and less than 200 g / 10 min, and even more preferably 90 g / 10 min or more and less than 140 g / 10 min, as measured in accordance with ASTM-D-1238-57T at 190° C. and 2.16 kg. By making the melt flow index 70 g / 10 min or more, the fluidity of the composition for sintered compacts is improved, and by making the melt flow index 200 g / 10 min or less, the strength of the green compact can be improved. The melt flow index of the polyacetal resin can be manipulated to be larger by increasing the amount of a molecular weight regulator (e.g., methylal, methanol, formic acid, methyl formate, etc.) added during polymerization.
[0031] The melting point of the polyacetal resin is preferably 100 to 200° C., and more preferably 140 to 180° C. The melting point is a peak melting temperature measured according to JIS K7121, and when multiple melting temperatures exist, it is the higher melting point.
[0032] (Polyolefin resin) The polyolefin resin is a homopolymer or copolymer having a structural unit derived from an alkene having 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms.
[0033] From the viewpoint of kneadability of the polyacetal resin with the sinterable inorganic powder and injection moldability, the melt flow index of the polyolefin resin measured under the conditions of 190°C and 2.16 kg is preferably 40 g / 10 min or more. More preferably, it is 50 g / 10 min or more, even more preferably 70 g / 10 min or more, and particularly preferably 80 g / 10 min or more. If the melt flow index of the polyolefin resin is greater than the lower limit value described above, the thin-wall moldability tends to be excellent and the degreasing property of the heat degreasing tends to be more excellent. From the viewpoint of improving the strength of the molded body, the melt flow index of the polyolefin resin is preferably 200 g / 10 min or less, more preferably 150 g / 10 min or less.
[0034] Specific examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, polybutadiene, etc. Polyethylene, polypropylene, and mixtures thereof are preferred, and polyethylene or polypropylene is more preferred from the viewpoint of shape retention in the degreasing step and suppression of cracking and swelling in the degreasing step. Suitable examples of commercially available polyethylene include Santech HD series (manufactured by Asahi Kasei), Santech LD series (manufactured by Asahi Kasei), Santech EVA series (manufactured by Asahi Kasei), Neozex, Ultzex, and Evolue (all manufactured by Prime Polymer), and examples of polypropylene include Sumitomo Noblen (manufactured by Sumitomo Chemical), Novatec PP (manufactured by Japan Polypropylene), Sanallomer PM series (manufactured by Sanallomer), and Prime Polypro (manufactured by Prime Polymer).
[0035] From the viewpoint of shape retention of a molded product after acid degreasing, the polyolefin resin is preferably not easily decomposed by acid. From the viewpoint of shape retention of a molded product after acid degreasing, the weight of the polyolefin resin after immersion in a 30% aqueous nitric acid solution at 23°C (room temperature) and 70°C for 24 hours according to the method described in JIS K 7114 is preferably 10% or less, more preferably 5% or less, and particularly preferably 1% or less, of the weight before immersion.
[0036] From the viewpoint of maintaining the shape of the green molded body and maintaining the shape of the molded body after acid degreasing well, the mass proportion of the polyolefin resin in the organic binder is preferably 5 to 95 mass%, more preferably 5 to 70 mass%, and particularly preferably 5 to 60 mass%, relative to 100 mass% of the organic binder. The mass ratio of the polyolefin resin to 100 parts by mass of the polyacetal resin is preferably from 1 to 200 parts by mass, more preferably from 5 to 150 parts by mass, and further preferably from 10 to 120 parts by mass.
[0037] The total mass ratio of the polyacetal resin and the polyolefin resin in 100% by mass of the organic binder is preferably 45% by mass or more. The total mass ratio of the polyacetal resin, the polyolefin resin, and a fluidity imparting agent described below in 100% by mass of the organic binder is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.
[0038] From the viewpoint of further reducing cracks and blistering during the degreasing step, the difference between the thermal decomposition onset point (°C) of the polyacetal resin and the thermal decomposition onset point (°C) of the polyolefin resin is preferably 30°C or more, more preferably 30 to 100°C. The thermal decomposition onset point is a temperature measured using a thermogravimetric differential thermal analyzer.
[0039] (Fluidity imparting agent) The composition for sintered compact of the present embodiment preferably further contains a fluidity imparting agent. By containing the fluidity imparting agent, the fluidity of the composition for sintered compact is further improved. The fluidity imparting agent is a compound other than the polyacetal resin and polyolefin resin, and examples thereof include waxes. Examples of the waxes include paraffin wax, polyethylene wax, polypropylene wax, carnauba wax, polyethylene glycol, polytetramethylene glycol, polytetraethylene glycol, polyisobutylene, microcrystalline wax, montan wax, beeswax, Japan wax, synthetic wax, poly-1,3-dioxolane, poly-1,3-dioxepane, etc. Among them, paraffin wax, polyethylene glycol, and polytetramethylene glycol are preferred from the viewpoint of providing a more excellent fluidity of the composition for sintered molded body in injection molding.
[0040] From the viewpoint of achieving even better fluidity of the composition for sintered molded bodies during injection molding, the mass proportion of the fluidity imparting agent is preferably 5 to 60 mass %, more preferably 5 to 50 mass %, and particularly preferably 10 to 50 mass %, relative to 100 mass % of the organic binder.
[0041] (Nitrogen-containing compounds, fatty acid metal salts) The polyacetal resin preferably further contains a nitrogen-containing compound and / or a fatty acid metal salt, and more preferably contains a nitrogen-containing compound and a fatty acid metal salt. By including the nitrogen-containing compound and the fatty acid metal salt, the extrudability, thermal stability, and foreign matter suppression during the production of polyacetal resin can be improved. In addition, the flowability of the composition for sintered compact kneaded with metal powder and the strength of the green compact tend to be improved at the same time. By including the nitrogen-containing compound and the fatty acid metal salt, the composition for sintered compact has improved thermal stability.
[0042] The nitrogen-containing compound is not particularly limited, but examples thereof include polyamide resins, amide compounds, urea derivatives, triazine derivatives, etc., and among them, polyamide resins are preferred from the viewpoint of providing a composition for sintered compacts with better thermal stability and a green compact with better strength. These compounds may be used alone or in combination of two or more.
[0043] Examples of the polyamide resin include, but are not limited to, nylon 6, nylon 11, nylon 12, nylon 66, nylon 6·10, nylon 6 / 6·10, nylon 6 / 6·6, nylon 6·6 / 6·10, nylon 6 / 6·6 / 6·10, poly-β-alanine, and the like, which are obtained by condensation of diamines and dicarboxylic acids, condensation of amino acids, ring-opening polymerization of lactams, etc.
[0044] Examples of the amide compound include, but are not limited to, stearyl stearamide, stearyl oleamide, stearyl erucamide, ethylenediamine-distearate amide, ethylenediamine-dibehenate amide, hexamethylenediamine-distearate amide, ethylenediamine-dierucate amide, xylylenediamine-dierucate amide, di(xylylenediamine-stearate amide), and sebacate amide, which are produced from an aliphatic monocarboxylic acid, an aliphatic dicarboxylic acid, an aromatic monocarboxylic acid, or an aromatic dicarboxylic acid and an aliphatic monoamine, an aliphatic diamine, an aromatic monoamine, or an aromatic diamine.
[0045] The urea derivative is not particularly limited, but examples thereof include N-phenylurea, N,N'-diphenylurea, N-phenylthiourea, and N,N'-diphenylthiourea.
[0046] The triazine derivative is not particularly limited, but examples thereof include melamine, benzoguanamine, N-phenylmelamine, melem, N,N'-diphenylmelamine, N-methylolmelamine, N,N'-trimethylolmelamine, 2,4-diamino-6-cyclohexyltriazine, and melam.
[0047] The mass ratio of the nitrogen-containing compound is preferably 0.005 to 0.2 parts by mass, and particularly preferably 0.005 to 0.1 parts by mass, relative to 100 parts by mass of the polyacetal resin. The mass ratio of the nitrogen-containing compound within the above range is preferable from the viewpoint of improving the thermal stability of the polyacetal resin when kneading the sinterable inorganic powder and the organic binder.
[0048] The fatty acid metal salt is not particularly limited, but examples thereof include fatty acid metal salts obtained from a saturated or unsaturated fatty acid having 10 to 35 carbon atoms or a fatty acid substituted with a hydroxyl group and an alkali metal or alkaline earth metal hydroxide, oxide, or chloride.
[0049] Examples of the fatty acid of the fatty acid metal salt include capric acid, undecylic acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, nonadecanoic acid, arachic acid, behenic acid, liglyceric acid, cerotic acid, heptacosanoic acid, montanic acid, undecylenic acid, oleic acid, elaidic acid, cetoleic acid, erucic acid, brassidic acid, sorbic acid, linoleic acid, linolenic acid, arachidonic acid, propiolic acid, stearic acid, 12-hydroxydodecanoic acid, 3-hydroxydecanoic acid, 16-hydroxyhexadecanoic acid, 10-hydroxyhexadecanoic acid, 12-hydroxyoctadecanoic acid, and 10-hydroxy-8-octadecanoic acid. The metal compound is a hydroxide or chloride of an alkali metal such as lithium, sodium, or potassium, an alkaline earth metal such as magnesium, calcium, strontium, or barium, or zinc or aluminum. Of these, the fatty acid is preferably myristic acid, palmitic acid, or stearic acid, and the metal compound is preferably a hydroxide, oxide, or chloride of calcium, and more preferably calcium myristate, calcium palmitate, or calcium stearate.
[0050] When the nitrogen-containing compound and the fatty acid metal salt are added to the composition for sintered molded bodies, the ratio of the mass of the fatty acid metal salt to the mass of the nitrogen-containing compound (mass of fatty acid metal salt / mass of nitrogen-containing compound) is preferably within a specific range, specifically, the ratio is 1 to 15, preferably 1 to 10. By setting the ratio to 1 to 15, the thermal stability of the polyacetal resin in the organic binder can be improved, which is preferable.
[0051] <Sinterable inorganic powder> In this embodiment, the "sinterable inorganic powder" can be selected from any of the known suitable sinterable inorganic powders. Preferably, it is selected from metal powders, alloy powders, metal carbonyl powders, and mixtures thereof. Among them, metal powders and ceramic powders are particularly preferred in order to impart functionality. The above sinterable inorganic powders may be used alone or in combination of two or more kinds.
[0052] Specific examples of the metal powders include powders of aluminum, magnesium, barium, calcium, cobalt, zinc, copper, nickel, iron, silicon, titanium, tungsten, and metal compounds and metal alloys based on these metals, whereby not only already completed alloys but also mixtures of the individual alloy components can be used.
[0053] Examples of ceramic powders include oxides such as zinc oxide, aluminum oxide, and zirconia; hydroxides such as hydroxyapatite; carbides such as silicon carbide; nitrides such as silicon nitride and boron nitride; halides such as fluorite; silicates such as stearite; titanates such as barium titanate and lead zirconate titanate; carbonates; phosphates; ferrite; high-temperature superconducting materials; and the like.
[0054] The inorganic powders described above may be used alone, or may be used in combination with several inorganic substances such as various metals, metal alloys, ceramics, etc. Particularly preferred metals and alloys include titanium alloys and stainless steels such as SUS316L, and preferred ceramics include Al2O3 and ZrO2.
[0055] The average particle size of the inorganic powder is preferably 30 μm or less, and more preferably 20 μm or less. The average particle size can be measured, for example, by a particle size distribution measuring device employing a laser diffraction method.
[0056] The mass ratio of the sinterable inorganic powder is preferably 70 to 95 parts by mass, more preferably 75 to 95 parts by mass, and particularly preferably 80 to 95 parts by mass, relative to 100 parts by mass of the composition for sintered compacts. By having the sinterable inorganic powder within the above range, a composition for sintered compacts having a melt viscosity suitable for injection molding can be obtained, and a green compact with high strength can be obtained.
[0057] <Other additives> Additives other than the above-mentioned components that can be added to the composition for sintered compacts are not limited as long as they do not impair the effects of the present invention. Preferred additives include antioxidants.
[0058] Examples of the antioxidant include n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, n-octadecyl-3-(3'-methyl-5'-t-butyl-4'-hydroxyphenyl)propionate, n-tetradecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, 1,6-hexanediol-bis-(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 1,4-butanediol-bis-(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, triethylene glycol-bis-(3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate), tetradecyl-3-(3',5'-di-t-butyl-4-hydroxyphenyl)propionate, ... Examples of the hydroxyphenyl ether include trachys(methylene 3-(3'-t-butyl-4-hydroxyphenyl)propionate)methane, N,N'-bis-(3-(3,5-di-t-butyl-4-hydroxyphenol)propionyl)hydrazine, N,N'-tetramethylene-bis-3-(3'-methyl-5'-t-butyl-4-hydroxyphenol)propionyldiamine, N,N'-bis-3-(3',5'-di-t-butyl-4-hydroxyphenol)propionylhexamethylenediamine, 3-(N-salicyloyl)amino-1,2,4-triazole, N,N'-bis-(2-(3-(3,5-dibutyl-4-hydroxyphenyl)propionyloxy)ethyl)oxyamide, and N,N'-hexamethylene-bis-(3-3,5-t-butyl-4-hydroxyphenyl)propanamide). These antioxidants may be used alone or in combination of two or more.
[0059] The content of the antioxidant is 0.01 to 1.0 part by mass, and preferably 0.05 to 0.5 part by mass, relative to 100 parts by mass of the polyacetal resin. When the content is within the above range, the thermal stability is improved.
[0060] The melt flow index of the composition for sintered compacts of this embodiment is preferably 80 g / 10 min or more and less than 200 g / 10 min, more preferably 90 g / 10 min or more and less than 180 g / 10 min, and even more preferably 90 g / 10 min or more and less than 140 g / 10 min, as measured in accordance with ASTM-D-1238-57T at 190 ° C. and 2.16 kg. By making the melt flow index 80 g / 10 min or more, the fluidity of the composition for sintered compacts is improved, and by making the melt flow index less than 200 g / 10 min, the strength of the green compact can be improved. The melt flow index of the composition for sintered molded bodies can be controlled within the above range, for example, by the type and mass proportion of the polyacetal resin used, and the melt flow index of the composition for sintered molded bodies tends to increase as the melt flow index of the polyacetal resin increases.
[0061] [Method of producing a composition for sintered compact] The method for producing the composition for sintered compact is not particularly limited and can be produced by a known method. Specifically, the composition for sintered compact can be produced by mixing the above-mentioned sinterable inorganic powder and organic binder with, for example, a Henschel mixer, a tumbler, a V-shaped blender, etc., and then melt-kneading the mixture in a semi-molten state with a kneader such as a single-screw extruder, a twin-screw extruder, a heating roll, a kneader, or a Banbury mixer, and can be obtained as a product in various forms such as a strand shape or a pellet shape.
[0062] [Green compact] The composition for sintered compacts in this embodiment can be used as a raw material for molding when a green compact, which is a preform for a sintered compact, is molded by injection molding. The composition for sintered compacts can be used to obtain a green compact using a screw-type or piston-type injection molding machine. The green body of this embodiment preferably has at least a portion having a thickness of 1 mm, and has a surface area of 1 mm. 2 In the above-mentioned molding method, it is more preferable that the part having a thickness of 1 mm has a surface area of 1 mm or more. 2 A green body having the above properties can be obtained.
[0063] (Strength of green compact) The green molded body obtained by the above molding method is subjected to a three-point bending test, and the product of the maximum bending strength (MPa) and the elastic modulus (MPa) at 0.05 to 0.1% strain is preferably 50,000 or more, more preferably 100,000 or more. The maximum bending strength and elastic modulus can be measured by the method described in the Examples below. If the product of the maximum bending strength and the elastic modulus at 0.05 to 0.1% strain is less than 50,000, the green molded body obtained by injection molding is likely to be distorted or damaged when transported.
[0064] (Debinding and sintering of green compacts) The green compact is placed in a closed debinding / sintering furnace and debinding / sintered under desired conditions to obtain a sintered compact. In the case of a method of degreasing by heating, degreasing is performed by increasing the temperature from room temperature to 500° C. to 600° C. in a nitrogen atmosphere. A fluidity imparting agent may be dissolved in a solvent before heating. Then, the temperature is raised to the sintering temperature of the sinterable inorganic powder, whereby a sintered compact can be obtained. In the case of degreasing using an acid, degreasing is carried out by circulating nitric acid gas in a nitrogen atmosphere and raising the temperature from room temperature to 110 to 120°C. Next, the temperature is raised to the sintering temperature of the sinterable inorganic powder, whereby a sintered compact can be obtained. EXAMPLES
[0065] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples. The terms and measurement methods for properties in the examples and comparative examples are as follows.
[0066] [Raw materials] (A Polyacetal resin) (A-1) A jacketed two-shaft paddle-type continuous polymerization reactor (Kurimoto Iron Works, Ltd., diameter 2B, L / D=14.8) capable of passing a heat transfer medium was adjusted to a temperature of 80° C. Polymerization was carried out by continuously supplying to the polymerization reactor 69 g / hr of a catalyst preparation prepared by diluting boron trifluoride-di-n-butyl etherate to 0.26 mass % with cyclohexane as a polymerization catalyst, 3500 g / hr of trioxane, 121 g / hr of 1,3-dioxolane, and 7.1 g / hr of methylal as a molecular weight regulator. The material discharged from the polymerization reactor was put into a 0.5% by mass aqueous solution of triethylamine to deactivate the polymerization catalyst, and then filtered, washed, and dried. Next, the mixture was fed to a vented twin-screw extruder (L / D=40) set at 200°C, and a 0.8% by mass aqueous solution of triethylamine was added to the terminal stabilization zone to give a nitrogen content of 20 ppm, and the mixture was stabilized while being degassed under reduced pressure at 90 kPa, and pelletized with a pelletizer. The mixture was then dried at 100°C for 2 hours to obtain polyacetal resin (A-1). The resulting polyacetal resin (A-1) had a melting point of 164° C. and a melt flow index of 70 g / 10 min.
[0067] (A-2) A polyacetal resin (A-2) was produced in the same manner as in the production method of polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was 7.9 g / hr. The resulting polyacetal resin (A-2) had a melting point of 164°C and a melt flow index of 90 g / 10 min.
[0068] (A-3) A polyacetal resin (A-3) was produced in the same manner as in the production method of polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was 9.4 g / hr. The resulting polyacetal resin (A-3) had a melting point of 164°C and a melt flow index of 121 g / 10 min.
[0069] (A-4) A polyacetal resin (A-4) was produced in the same manner as in the production method of polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was 10.6 g / hr. The resulting polyacetal resin (A-4) had a melting point of 164°C and a melt flow index of 180 g / 10 min.
[0070] (A-5) A polyacetal resin (A-5) was produced in the same manner as in the production method of polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was 11.6 g / hr. The resulting polyacetal resin (A-5) had a melting point of 164°C and a melt flow index of 213 g / 10 min.
[0071] (A-6) A polyacetal resin (A-6) was produced in the same manner as in the production method of polyacetal resin (A-1), except that the flow rate of methylal as a molecular weight regulator was set to 6.9 g / hr. The resulting polyacetal resin (A-6) had a melting point of 164°C and a melt flow index of 60 g / 10 min.
[0072] (A-7) A polyacetal resin (A-7) was produced in the same manner as in the production method of polyacetal resin (A-1), except that 1,4-butanediol formal was used at 121 g / hr instead of 1,3-dioxolane, and the flow rate of methylal as a molecular weight regulator was 7.1 g / hr. The resulting polyacetal resin (A-7) had a melting point of 164°C and a melt flow index of 64 g / 10 min.
[0073] (B Polyolefin resin) B-1: Polypropylene (Sumitomo Chemical Co., Ltd., Sumitomo Noblen UH501E1 MFR100g / 10min) B-2: Polyethylene (Suntec TM LDPE M6555 MFR55g / 10min manufactured by Asahi Kasei Corporation) B-3: Polypropylene (Novatec PP BC08C MFR60g / 10min, manufactured by Japan Polypropylene Corporation) B-4: Polyethylene (prototype MFR100g / 10min) The polyethylene of B-4 was polymerized by the following procedure. 1) Solid catalyst A After removing oxygen and moisture from inside the autoclave with dry nitrogen, 1.6 liters of a hexane solution of 0.5 mol / l trichlorosilane and 1.2 liters of hexane were charged and the temperature was raised to 70°C. 0.15 Mg(n-Bu) 1.75 (O-nBu) 0.7 45 L of (an octane solution with a metal concentration of 0.8 mol / L) and 0.35 L of hexane were introduced at 70°C over 1 hour. 0.6 L of hexane containing 0.7 g of TiO4 was further introduced and the reaction was carried out at 70°C for 1 hour. The reaction mixture was filtered and washed with hexane. This was used as solid catalyst A. 2) Solid catalyst B 3.0 mol of the reaction product of (C2H5)(n-C4H9)Mg and hydromethylpolysiloxane having a viscosity of 15 centistokes (Si / Mg=1.0 / 1.0) and 3.0 mol of titanium tetrachloride were placed in an autoclave together with 6 liters of hexane and reacted at -10°C for 3 hours. The reaction mixture was post-treated in the same manner as in the case of solid catalyst A, to obtain solid catalyst B. 3) Polymerization of polyethylene with MFR of 100g / 10min Two 100L reactors were connected in series. The first reactor was continuously fed with 0.20g / hr of solid catalyst A, 2.5mmol / hr of triisobutylaluminum (Al(i-C4H9)3), 100L / hr of cyclohexane solvent, 8kg / hr of ethylene, 5kg / hr of 1-butene, and 1.0L / hr of hydrogen. The polymerization solution was continuously taken out from the first reactor and fed to the second reactor. At the same time, the second reactor was continuously fed with 0.10g / hr of solid catalyst B, 1.5mmot / h of triisobutylaluminum (Al(i-C4H9)3), 50L / h of cyclohexane, 4kg / hr of ethylene, and 0.03L / hr of hydrogen. The polymerization was carried out at a temperature of 140℃ in the first reactor and 180℃ in the second reactor. The MFR of the obtained ethylene-1-butene copolymer was 100g / 10min.
[0074] (C nitrogen-containing compounds) Nylon 66 (molecular weight 10,000)
[0075] (D fatty acid metal salt) Calcium stearate
[0076] (E Fluidity imparting agent) E-1: Paraffin wax (Paraffin wax-145, manufactured by Nippon Seiro Co., Ltd.) E-2: Polyethylene glycol (Sigma-Aldrich) E-3: Polytetramethylene glycol (Mitsubishi Chemical)
[0077] [Production of Composition for Sintered Compacts] 0.05 parts by mass of (C) nylon 66 and 0.3 parts by mass of (D) calcium stearate were uniformly added and mixed to 100 parts by mass of the polyacetal resins (A-1) to (A-7), and the mixture was fed to a vented twin-screw extruder (L / D=40) set at 200°C, and pelletized while degassing under reduced pressure at 90 kPa. The mixture was then dried at 100°C for 2 hours.
[0078] SUS316L (average particle size 10 μm) was used as the sinterable inorganic powder, and the polyacetal resin composition, (B) polyolefin resin, and (E) flowability imparting agent were mixed in the proportions shown in Tables 1 and 2 to prepare a composition for sintered compacts.
[0079] [evaluation] (Melt Flow Index (MI)) The MI (Melt Flow Index: g / 10 min) was measured under conditions of 190°C and 2160 g using a MELT INDEXER manufactured by Toyo Seiki Co., Ltd. in accordance with ASTM-D-1238.
[0080] (Molding of green body) The compositions for sintered compacts according to Examples 1 to 18 and Comparative Examples 1 to 11 were kneaded in a pressure kneader at 170°C for 1 hour, and then the kneaded products were cooled and crushed to obtain injection molding materials. The injection molding machine (ROBOSHOT α-50iA manufactured by Fanuc) was used to mold the materials at a molding temperature of 175 to 200°C to obtain dumbbell-shaped green compact test pieces conforming to ISO 10724-1. The thickness of the test pieces can be changed to 1mm or 2mm.
[0081] (Moldability) The ease of molding the green body was evaluated according to the following criteria. 〇(Good): Can be collected without problems △ (partially defective): Rarely, chips are found on the edges of the molded body. × (defective): It is impossible to obtain a molded product without any chips or other defects.
[0082] (Strength of green compact) The strength of the green compact was measured by a three-point bending test. That is, the dumbbell test piece was measured by an autograph (Instron Dual column flore model 5581) with a support jig interval of 50 mm and the maximum strength and elastic modulus when the load cell was lowered at a speed of 2 mm / min. The product of the maximum bending strength (MPa) and the elastic modulus (MPa) was calculated, and the product was evaluated according to the following criteria. ◎(Excellent): 100,000 or more 〇 (Good): Less than 100,000 50,000 or more × (defective): Less than 50,000 A composition for sintered compacts having a high product of maximum bending strength and elastic modulus is resistant to plastic deformation and is less likely to retain permanent set, making it a suitable material for green compacts.
[0083] (degreasing) (Acid degreasing) In Examples 1 to 6 and Comparative Examples 1 to 4, degreasing was performed with acid. The green compact was supported at two points with an interval of 50 mm and set in a degreasing furnace. The furnace was first heated to 110°C and substituted with 500 l / hr of nitrogen for 30 minutes. Then, 30 ml / hr of 98% nitric acid was supplied while maintaining nitrogen purging. The acid supply was maintained for 2.5 hours, followed by substitution with 500 l / hr of nitrogen for 45 minutes and cooling to room temperature for degreasing. The appearance of the degreasing green compact was visually observed and evaluated according to the following criteria. 〇(Good): No cracks, swelling or other abnormal appearances are observed. × (Fail): Cracks, swelling, and other abnormal appearances are observed. - (Not implemented): Items that could not be injection molded
[0084] (heat degreasing) In Examples 7 to 18 and Comparative Examples 5 to 11, thermal debinding was performed. The green compact was supported at two points with an interval of 50 mm and set in a debinding furnace. The inside of the debinding furnace was then purged with nitrogen gas, and the temperature was raised to 500°C at a first heating rate of 30°C / hr and a second heating rate of 45°C / hr, and the debinding was performed by holding the temperature at 500°C for 2 hours. The appearance of the debinding green compact was visually observed and evaluated according to the following criteria. 〇 (Excellent): No cracks, blistering or other abnormal appearance was observed under either the first or second condition. △ (Good): No abnormal appearance such as cracks or blisters was observed under the first condition, but cracks or blisters were observed under the second condition. × (Poor): Cracks and swelling were observed under both the first and second conditions. - (Not implemented): Items that could not be injection molded
[0085] [Table 1]
[0086] [Table 2]
Claims
1. A sinterable inorganic powder and an organic binder are included, the organic binder contains at least a polyacetal resin and a polyolefin resin, The polyacetal resin has a melt flow index (190° C., 2.16 kg) of 90 to 200 g / 10 min.
2. 2. The composition for sintered molded bodies according to claim 1, wherein the polyolefin resin has a melt flow index (190° C., 2.16 kg) of 40 g / 10 min or more.
3. The composition for sintered compacts according to claim 1 or 2, wherein the organic binder contains 5 to 95 mass% of the polyacetal resin and 5 to 95 mass% of the polyolefin resin, based on the mass of the organic binder.
4. The composition for sintered compacts according to any one of claims 1 to 3, wherein the sinterable inorganic powder is contained in an amount of 70 to 95 parts by mass per 100 parts by mass of the composition for sintered compacts.
5. The composition for sintered compacts according to any one of claims 1 to 4, wherein the organic binder contains 5 to 60 mass% of a fluidity imparting agent based on the mass of the organic binder.
6. The composition for sintered compacts according to any one of claims 1 to 5, wherein the polyacetal resin contains an oxymethylene unit and an oxyethylene unit.
7. The composition for sintered compacts according to any one of claims 1 to 6, comprising 5 to 50 mass% of the polyacetal resin based on the mass of the organic binder.
8. The composition for sintered compacts according to any one of claims 1 to 7, wherein the organic binder comprises a nitrogen-containing compound and a fatty acid metal salt.
9. A green compact obtained by molding the composition for sintered compacts according to any one of claims 1 to 8.
10. The part with a thickness of 1 mm or less is 100 mm 2 The green compact according to claim 9 , wherein
11. A method for producing a sintered composite material comprising: a sinterable inorganic powder and an organic binder; the organic binder contains at least a polyacetal resin and a polyolefin resin, The polyacetal resin has a melt flow index (190° C., 2.16 kg) of 70 to 200 g / 10 min; The organic binder contains a nitrogen-containing compound and a fatty acid metal salt. A composition for sintered compacts comprising:
Citation Information
Patent Citations
Metal powder injection-molding composition
JP1993125403A
Injection-molding composition
JP1994158107A
Composition for injection molding of metal powder, injection molding and sintering method using the composition
JP1999343503A
Resin material for blow injection molding and blow molded article
JP2003212942A
Lubricant for powder metallurgy and metal powder compositions containing the lubricant
JP2019056178A