Friction material block, particularly for mounting brake pads, and associated brake pads and methods
Incorporating hydrophobic wax into asbestos-free brake pad materials addresses the stiction issue by reducing the peel force, ensuring stable braking performance even in harsh conditions.
Patent Information
- Application Number
- JP2023517959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-17
- Filing Date
- 2021-09-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-09-17
AI Technical Summary
Brake pads tend to stick to brake discs under harsh conditions due to corrosion, leading to shocks, energy consumption issues, and potential vehicle failure, especially in wet weather.
Incorporating a hydrophobic wax with a melting point above 110°C into asbestos-free friction materials for brake pads, which reduces or eliminates the tendency for stiction by using inorganic and/or organic fibers, binders, lubricants, and abrasives, ensuring the material remains chemically stable under high temperatures and pressures.
The addition of hydrophobic wax significantly reduces the peel force required to separate brake pads from brake discs, minimizing stiction and maintaining effective braking performance even in wet conditions.
Smart Images

Figure 0007571288000007 
Figure 0007571288000008 
Figure 0007571288000009
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This patent application claims priority to Italian Patent Application No. 102020000021919, filed September 17, 2020, the entire disclosure of which is incorporated herein by reference. [Technical Field]
[0002] The present disclosure generally relates to friction blocks made of friction material, the blocks designed to mount brake pads, where the friction material can have a formulation that allows the friction block to reduce or eliminate the tendency of the friction block to stitch against the surface of the cooperating friction partner, a phenomenon known as "stiction." The present disclosure generally relates to friction blocks of brake pads and associated brake pads designed to cooperate with the surface of a vehicle disc brake to brake the vehicle. The present disclosure also generally relates to related methods. [Background technology]
[0003] It is known that, in particular, under harsh operating and / or environmental conditions, such as frequent off-road driving and / or driving on muddy roads or routes exposed to brackish air or acid rain, this can result in the "sticking" of one or more of the vehicle's brake pads to the associated brake disc, made of cast iron or steel, during use. This is generally due to corrosion phenomena that affect the brake disc and result in corrosion products that combine with the friction material of the brake pad during braking to cause the brake pad to accidentally adhere to the brake disc, this adhesion being maintained temporarily even when the vehicle brakes are deactivated. This phenomenon of adhesion is known by the English technical term "stiction," which is derived from the contraction and fusion of the terms "static" and "friction," i.e., the term "static friction."
[0004] Obviously, the occurrence of stiction in a vehicle during use is associated with various drawbacks, such as shock / distortion during braking and subsequent brake release, increased energy consumption, and in extreme cases, breakdown of the brake pad friction material leading to vehicle failure and / or premature brake pad replacement. As such, stiction is well known in the field of brake pads and also affects vehicles that are constantly driven on paved roads when exposed to wet weather conditions. Summary of the Invention
[0005] It is an object of the present disclosure to provide embodiments of friction blocks or layers made of friction material, wherein the friction material has a formulation that allows for reducing or eliminating the tendency of the friction block to stitch against the surface of a friction partner with which it cooperates.
[0006] In particular, it is an object of the present disclosure to provide embodiments of such friction blocks as an integral part of or integrated into brake pads designed to cooperate in use with brake discs made of steel or cast iron.
[0007] The present disclosure, therefore, relates to embodiments of friction blocks or layers made of friction materials formulated to reduce or eliminate the tendency of the friction blocks to stitch against the surface of their friction counterparts, as defined in the appended claims.
[0008] Generally speaking, the friction blocks or layers are either an integral part of a brake pad for a vehicle, which may be designed to cooperate in use with a brake disc made of steel or cast iron, or may be an integral part of a clutch disc for a vehicle or any other application.
[0009] The present disclosure further relates to embodiments of brake pads equipped with, or having as an integral component thereof, such friction blocks or layers.
[0010] The present disclosure also relates to embodiments of methods for manufacturing brake pads for vehicles that have a reduced or zero tendency to stitch against the friction surface of an associated brake disc, i.e., a reduced or zero tendency to stiction, particularly in wet weather.
[0011] EP 3507587, the entire contents of which are incorporated herein by reference, discloses a method for studying and determining the physicochemical conditions of adhesion between a first mechanical element and a second mechanical element, comprising a vehicle braking element and a braked element, respectively, the method comprising: - coupling a first mechanical element to a first support and a second mechanical element to a second support, wherein the first and second supports are positioned opposite each other and relatively axially movable, the second support facing the first support such that the second mechanical element is fully embedded within the second support, except for a first face of the second mechanical element that is not covered by the second support and is positioned flush with a front end of the second support facing the first support and the first mechanical element coupled thereto; - electrically connecting the second mechanical element to an insulated wire protruding in a liquid-tight manner from the second support; - adhering a first surface of a second mechanical element to a first mechanical element and then applying a first predetermined force to press the second support towards the first support, so as to obtain a stiction cell comprising first and second mechanical elements and first and second supports; - immersing the first and second mechanical elements together with the first and second supports in an electrolyte together with at least one counter electrode and a reference electrode so as to form an electrochemical cell in which the second mechanical element constitutes the working electrode; - electrically connecting the insulated wire, the counter electrode, and the reference electrode to a potential and / or current generator; - carrying out an electrochemical test by means of a potential and / or current generator, in which a gradually variable potential is applied between the working electrode and the reference electrode and / or a gradually variable current path is established between the counter electrode and the working electrode, by the action of which a corrosion phenomenon is induced between the second mechanical element and the first mechanical element; - detecting, using the potential / current generator or another device, the current passing through the electrolyte between the second mechanical element and the counter electrode as a function of the applied potential, or conversely, detecting the potential established between the second mechanical element and the reference electrode as a function of a predetermined current set on the potential / current generator. Equipped with.
[0012] In this way, "stiction" between the vehicle braking element under investigation (brake pad) and the element being braked (brake disc) is quickly obtained "artificially" under controlled conditions. The force required to separate the braking element from the brake disc is then measured, which gives an accurate estimate of the nature of the stiction phenomenon that has occurred.
[0013] Preferred but non-limiting embodiments will now be described in more detail with reference to some practical examples of its implementation, which are intended only to disclose in a non-exhaustive and non-limiting manner the features that are part of the subject matter of this disclosure, and with reference to the figures of the accompanying drawings. [Brief explanation of the drawings]
[0014] [Figure 1] 1 is a graph showing the results of a series of experiments conducted according to the procedures discussed in EP 3507587 for different friction materials. [Figure 2] 1 is a graph showing the results of experiments conducted according to the procedures discussed in EP 3507587 on the same friction material with and without additional component (additive) targets of the present disclosure. [Figure 3]1 is a graph showing the results of braking experiments conducted on vehicles under different braking conditions using brake pads made with the same friction material either with or without the additional component (additive) subject of the present disclosure. [Figure 4A] FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 4B] FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 4C] FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 5A] FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 5B] FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 5C]FIG. 1 shows comparative results of AK Master standard tests performed on brake pads of the same type and size, having the same composition, but provided with friction material blocks that do not and incorporate, respectively, additional component materials or “additives” according to the present disclosure. [Figure 6] 1 shows an illustrative, non-limiting embodiment of a brake pad made in accordance with the present disclosure, highlighting respective test areas for checking the hydrophobicity of the friction material thereof; [Figure 7] 1 illustrates a practical example of the implementation of a test method for determining the hydrophobicity of brake pads manufactured in accordance with the present disclosure. [Figure 8] 1 illustrates a practical example of the implementation of a test method for determining the hydrophobicity of brake pads manufactured in accordance with the present disclosure. [Figure 9] 1 is a flowchart illustrating a method of making a friction material according to embodiments described herein. DETAILED DESCRIPTION OF THE INVENTION
[0015] In some embodiments, friction blocks or layers made of asbestos-free friction material, particularly designed to be provided as an integral part of a vehicle brake pad, comprise as their constituent materials inorganic and / or organic and / or metallic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive.
[0016] Materials within the above general categories are well known in the braking art and are selected according to well-known criteria to obtain particular properties such as wear resistance, stable coefficient of friction during braking, fade, and limited use of braking fluid.
[0017] Exemplary embodiments of the fibrous component can be, but are not limited to, inorganic fibers such as glass fiber, rock wool, wollastonite, sepiolite, attapulgite, and / or metal fibers such as stainless steel and zinc, and organic fibers such as carbon fiber, aramid fiber, polyimide fiber, polyamide fiber, phenolic fiber, cellulose and acrylic fiber, or PAN (polyacrylonitrile). The fibrous substrate can be utilized in the form of short fibers or powder.
[0018] Numerous materials known in the art can be used as organic or inorganic fillers. Exemplary embodiments include, but are not limited to, calcium carbonate precipitate, barium sulfate, magnesium oxide, calcium hydroxide, calcium fluoride, hydrated lime, talc, molybdenum trioxide, zirconium silicate, iron oxide, mica, iron sulfide, silicon dioxide, vermiculite, rubber crumb (rubber powder and granules), nitrile rubber crumb (vulcanized products), metal crumb (excluding copper and its alloys), and acrylic rubber crumb (vulcanized products). These materials can be used alone or in combination of two or more. The loading of such fillers is preferably between 2% and 40% by volume, based on the total composition of the friction material.
[0019] Illustrative examples of suitable binders include, but are not limited to, phenolic resins, melamine resins, and epoxy resins; various modified phenolic resins, such as epoxy-modified phenolic resins, oil-modified phenolic resins, alkylbenzene-modified phenolic resins, and acrylonitrile-butadiene rubber (NBR). Any one of these compounds or a combination of two or more thereof may be used. The binder is preferably included in an amount of 2% to 30% by volume based on the total composition of the friction material.
[0020] Exemplary embodiments of the friction modifier may include, but are not limited to, 0% to 10% by volume (or about 0% to about 10% by volume) of solid lubricants, such as tin sulfides such as SnS and SnS, cashew nut flour, rubber crumb (ground tread rubber crumb), various unvulcanized rubber particles, various vulcanized rubber particles, inorganic fillers, such as barium sulfate, calcium carbonate, calcium hydroxide, vermiculite, and / or mica, abrasives, such as silicon carbide, alumina, zirconium silicate, lubricants, such as molybdenum disulfide, tin sulfides as identified above, zinc sulfide, iron and non-ferrous sulfides, metal particles other than copper and copper alloys, and / or combinations of all of the above.
[0021] In some embodiments, it may be advantageous to include graphite and / or coke in the composition. The graphite (and / or coke) can be added in an appropriately selected amount, which can preferably comprise 2% to 15% by volume of the total composition of the friction material. Friction material embodiments to which the present disclosure applies include those known as non-asbestos organic (NAO) friction materials.
[0022] The graphite (and / or coke) can be added in an appropriately selected amount, which can comprise 2% to 15% by volume (or about 2% to about 15% by volume) of the total composition of the friction material.
[0023] The fibers can be available in the form of short fibers or powder. In some embodiments, the fibers can have a total fiber length of 0.5 to 1.5 (or about 0.5 to about 1.5) mm and a fiber diameter of 40 to 150 microns, although the specific dimensions are not limited.
[0024] The amount of filler can be comprised between 2% and 40% by volume, based on the total composition of the friction material.
[0025] The binder may be included in an amount of 2% to 30% by volume, based on the total composition of the friction material.
[0026] Illustrative embodiments of suitable abrasives may be subdivided into weak abrasives, medium abrasives, and strong abrasives, and may consist of any one or more of flowing materials, although the following list is not intended to be exhaustive or limiting in any way: Weak abrasives (Mohs 1-3): talc, calcium hydroxide, potassium titanate, mica, kaolin, Medium abrasives (Mohs 4-6): barium sulfate, magnesium oxide, calcium fluoride, calcium carbonate, wollastonite, calcium silicate, iron oxide, silica, chromite, zinc oxide, Strong abrasives (Mohs 7-9): silicon carbide, zirconium sand (zirconium oxide), zirconium silicate, zirconia, corundum, alumina, mullite.
[0027] The ratio of abrasive to lubricant is between 3 and 10. In some embodiments, this ratio can be equal to 6 (or about 6).
[0028] The friction material composition according to the present disclosure may comprise aramid fibers, and the ratio between the binder and the aramid fibers is 0.5% to 8% by volume (or about 0.5% to about 8% by volume). In some embodiments, this ratio may be equal to 5 (or about 5).
[0029] According to an embodiment of the present disclosure, the asbestos-free friction material also contains, as an additional component or additive, a hydrophobic wax, the relative amount of the hydrophobic wax to the other material components mentioned above being selected depending on the chemical nature and amount of the other components of the asbestos-free friction material such that the friction block or layer of the asbestos-free friction material, after formation, has a hydrophobicity defined as the absorption time within the friction material of a droplet formed by 20 + / - 5 μL of distilled water by the method described herein below, of greater than 60 minutes.
[0030] According to an embodiment of the present disclosure, the asbestos-free friction material contains, as an additional constituent or additive, a hydrophobic wax, which is preferably in the form of a solid powder, has a melting point greater than 110°C, and is chemically stable at high temperatures and pressures.
[0031] Chemically stable means that the wax molecules do not undergo decomposition. "High temperature and pressure" refers to degrees Celsius and kg / cm, respectively. 2 This means that the temperature and pressure are on the order of 100 times higher than the
[0032] According to an embodiment of the present disclosure, the asbestos-free friction material contains, as an additional constituent or additive, a hydrophobic wax selected from the non-limiting group consisting of polyethylene (PE) wax, high density PE (HDPE) wax, polypropylene wax, micronized PE wax, oxidized PE wax, polytetrafluoroethylene (PTFE) modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and specialty waxes (bonded wax, modified PE wax, PTFE texture powder).
[0033] The hydrophobic wax can be present in the asbestos-free friction material in an amount comprised between 0.5% and 5% by volume (or between about 0.5% and about 5% by volume), calculated on the total amount of the asbestos-free friction material. In some embodiments, the wax can be present in an amount comprised between 1.0% and 2.0% by volume (or between about 1.0% and about 2.0% by volume).
[0034] A friction block or layer of asbestos-free friction material according to any of the above possible embodiments may have no or little tendency to stitch during use against the surface of its friction counterpart, typically a vehicle brake disc, when the friction block or layer of asbestos-free friction material is an integral part of / included in a brake pad. In particular, according to a test embodiment detailed in this disclosure, the friction block or layer is electrochemically stitched to a metal surface of steel, iron, or cast iron by pressing the friction block or layer of asbestos-free friction material against the metal surface and then inducing an electrochemical corrosion phenomenon thereon. According to this test, any of the embodiments of the friction block or layer of asbestos-free friction material according to the present disclosure can exhibit a peel force from the metal surface of less than 15 (or about 15) Newtons, indicating low or no tendency for stiction.
[0035] The friction blocks or layers of asbestos-free friction material can be incorporated into vehicle brake pads designed to cooperate in use with vehicle brake discs made of iron, steel, or cast iron, and the vehicle brake pads are operatively associated in use with the vehicle brake discs, although the particular material is not limited thereto.
[0036] When a friction block or layer of an asbestos-free friction material contains, as its component material, 0.5% to 5% by volume of a hydrophobic wax having a melting point higher than 110°C, the resulting friction partners consisting of a vehicle brake pad and a vehicle brake disc do not experience stiction in use or experience a very limited stiction phenomenon that allows the two friction partners to be easily separated with a low force, such as less than 15 Newtons.
[0037] The hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE modified polyethylene wax, micronized amide wax, micronized polypropylene wax, specialty wax (bonded wax, modified PE wax, PTFE texture powder) in an amount such that the vehicle brake pad has a reduced or no tendency for stiction, especially in wet weather.
[0038] The present disclosure also relates to the use of a hydrophobic wax in an asbestos-free friction material containing inorganic and / or organic and / or metallic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or an abrasive as further component materials thereof, wherein the hydrophobic wax is contained in the asbestos-free friction material in an amount of 0.5% to 5% by volume (or about 0.5% to about 5% by volume) calculated on the total volume of the asbestos-free friction material, so that the asbestos-free friction material exhibits a reduced or no tendency for stiction, especially in wet weather.
[0039] The present disclosure also relates to a method for manufacturing brake pads for vehicles that have a reduced or no tendency to stitch against the friction surface of an associated brake disc, i.e., have a reduced or no tendency to stiction, particularly in wet weather conditions, the method comprising: i) - preparing a test quantity of asbestos-free friction material, in particular of the NAO class, by mixing together the respective component materials comprising inorganic and / or organic and / or metallic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding a predetermined amount of hydrophobic wax as a further component material in step i) so as to be mixed with the component material of step i); iii) - forming a solid block or layer of asbestos-free friction material containing hydrophobic wax by pressing and heating the component materials mixed together in a mold to form a pad; iv) - subjecting the pad to a hydrophobicity test consisting of measuring the absorption time thereon of a drop formed by 20 + / - 5 μL of distilled water; v) - Repeating steps i) to iv) using different predetermined amounts of hydrophobic wax; vi) - Industrially producing brake pads using asbestos-free friction materials containing hydrophobic waxes that have the same chemical composition as those test friction materials produced by the previous steps i) to v) and that have shown a water droplet absorption time of more than 60 minutes in step iv); Equipped with.
[0040] The present disclosure further relates to a method for manufacturing brake pads for vehicles having a reduced or no tendency to stitch on the friction surface of an associated brake disc, i.e., having a reduced or no tendency to stiction, particularly in wet weather, the method comprising: i) - preparing an asbestos-free friction material, in particular of the NAO type, by mixing together the respective component materials comprising inorganic and / or organic and / or metallic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding an amount of a hydrophobic wax as a further component material in step i) to be mixed with the component material of step i), wherein the hydrophobic wax is selected from the group consisting of polyethylene (PE) wax, high density PE (HDPE) wax, polypropylene wax, micronized PE wax, oxidized PE wax, polytetrafluoroethylene (PTFE) modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and special waxes (bonded wax, modified PE wax, PTFE texture powder), and the hydrophobic wax is added to the asbestos-free friction material in an amount of 0.5% to 5% by volume (or about 0.5% to about 5% by volume), preferably 1.0% to 2.0% by volume (or about 1.0% to about 2.0% by volume), calculated based on the total amount of the asbestos-free friction material; iii) - forming a solid block or layer of asbestos-free friction material containing hydrophobic wax by pressing and heating the component materials mixed together in a mold to form a pad; A method comprising:
[0041] A possible non-limiting embodiment of a brake pad made in accordance with the present disclosure is shown schematically in FIG.
[0042] 6 shows a top plan view of a brake pad 1 comprising a metal support or "backplate" 2 and at least one pad or block or layer of hardened friction material 3. The backplate is made of a ferrous material, typically iron or steel, but can also be made of a light alloy such as an age-hardened Al alloy.
[0043] In the non-limiting example shown, brake pad 1 has two blocks or pads 3 of friction material arranged side by side and integral with backplate 2, e.g., co-molded onto backplate 2 or attached to backplate 2 after curing. Of course, in some embodiments it may be possible to have one single block or pad (or layer) of friction material integral with the backplate and large enough to cover substantially the entire surface 4 of backplate 2 that, in use, faces the element to be braked, such as a brake disc, as is known and is not shown for simplicity.
[0044] In Figure 6, brake pad 1 is shown with respective test points highlighted by small circles and numbered 10 through 15. At least two test points, i.e., points 10 and 11, are located near or in the central portion of brake pad 1, while the remaining test points are evenly distributed on both of the two blocks or pads 3 of friction material, preferably near or in opposing regions 16 of each of the blocks or pads 3, highlighted as dotted ovals in Figure 6.
[0045] Points 10-15 are used in a hydrophobicity test developed by the Applicant's engineers, as explained in more detail herein below, to test the absorption time of a droplet of distilled water in a block or pad 3 of friction material, as this measurement can be seen to relate to the tendency of the brake pad 1 to undergo stiction, i.e., the tendency of the brake pad to stitch in use against its friction mating surface, i.e., the friction surface of the brake disc.
[0046] FIG. 7 shows a photograph of an actual brake pad produced as described and substantially corresponding to brake pad 1 shown only diagrammatically in FIG. 6, with the test points used shown as small circles and numbered 1 through 6.
[0047] FIG. 8 is a photograph of the brake pad of FIG. 7 during a hydrophobicity test, as seen in more detail in the Examples.
[0048] 9 is a flow chart illustrating a method of making a friction material according to embodiments described herein. The various steps of the method briefly disclosed above are shown as sequentially arranged blocks, with an explanation of what happens at each step inserted within each block.
[0049] The present disclosure will now be completed by the content of the following non-limiting working examples. Example 1
[0050] Different compositions of friction materials were prepared, all of which were NAO Cu-free types, and all of which were asbestos-free friction materials.
[0051] The general generic composition of the prepared friction material is given in Table 1, although the components shown can be mixed together in different combinations. Table 1
[0052] [Table 1]
[0053] In Table 1, for weak abrasives, medium abrasives, and strong abrasives, one or more materials were selected as follows: Weak abrasives (Mohs 1-3): talc, calcium hydroxide, potassium titanate, mica, kaolin, Medium abrasives (Mohs 4-6): barium sulfate, magnesium oxide, calcium fluoride, calcium carbonate, wollastonite, calcium silicate, iron oxide, silica, chromite, zinc oxide, Strong abrasives (Mohs 7-9): silicon carbide, zirconium sand (zirconium oxide), zirconium silicate, zirconia, corundum, alumina, mullite.
[0054] Starting with the general effective compositions listed in Table 1, friction material compositions are prepared in test amounts, molded into pads, and subjected to stiction testing as described in EP 3507587, the contents of which are incorporated herein by reference in their entirety.
[0055] The test results are shown in the graph of FIG. 1 in terms of the force required to peel the friction material pad under test from a piece of commercial brake disc.
[0056] Friction material composition #4 contains a hydrophobic additive to combat creep groan as described in WO 2019 / 171325. Friction material #2 corresponds to a known composition known to be substantially free of stiction. Composition #1 contains a hydrophobic wax. Finally, composition #3 corresponds to a known composition known to be substantially susceptible to stiction.
[0057] The hydrophobic waxes that were tested are included in the following non-limiting and non-exhaustive list: Polyethylene wax HDPE wax Polypropylene wax PE wax micronization PE wax oxidation PTFE modified polyethylene wax Micronized Amide Wax Micronized Polypropylene Wax Special waxes (bonded wax, modified PE wax, PTFE texture powder)
[0058] As can be seen, all compositions containing hydrophobic wax (results for different hydrophobic waxes were completely superimposable) exhibited a peel force of less than 15 Newtons, which corresponds to a low risk of stiction, and generally even less than 10, which means that the risk of stiction is almost zero. As will be explained later, further tests performed on actual brake pads mounted on automobiles and subjected to braking have proven that peel force values between 15 and 30 correspond to a real risk of stiction, in the sense that stiction can occur under specific and / or severe environmental conditions (i.e., humidity, temperature, pollutants, salt, etc.) and braking dynamics conditions (hot clamping, etc.). Values above 30 correspond to severe stiction that will certainly occur under less severe or specific environmental and / or braking dynamics conditions. Example 2
[0059] Additional friction material compositions were prepared as shown in Table 2 below.
[0060] Material #1 in Table 2 is the same as Material #1 in Table 1 and contains 2.0% by volume of polyethylene wax, hereinafter also referred to as "Composition W," while Material #5 in Table 2 corresponds to a composition identical to that of Material #1 but without the wax, with the medium abrasive content increased by 2% by volume to compensate. Table 2
[0061] [Table 2]
[0062] Materials #1 and #5 from Table 2 were molded onto the same metal substrate / backing and conventionally cured to form identical brake pads, the only difference being that composition #5 contained no hydrophobic wax and was used as a reference, while the corresponding composition W under test contained 2.0% by volume of a commercially available polyethylene wax instead of the corresponding amount of medium abrasive.
[0063] Brake pad pressure is 150-1800kg / cm at a temperature of 60-200°C. 2 for a duration of 3 to 10 minutes at a pressure of 150 to 500 kg / cm at a temperature of 130 to 180 °C or otherwise preforming the mixture in a die. 2 The pressure was (14.7-49 MPa) for a duration of 3-10 minutes.
[0064] The resulting pressed article is typically post-cured by heat treatment at 150-400°C for 10 minutes to 10 hours, then spray or powder coated, kiln dried, and possibly machined as needed to produce the final product.
[0065] Each single pad has an effective braking area of 26.8cm 2 is. Example 3
[0066] The brake pads obtained using friction material compositions #5 and W were subjected to the following tests: Hydrophobicity test (water absorption test) The following operations were performed on each brake pad constituting the test sample: - Blowing and cleaning the raised surfaces of the brake pads (the surfaces intended to come into contact with the brake disc), Dry the sample at 105°C for 2 hours. Cool the sample to a temperature of 10-30°C. Apply 20 + / - 5 μL of distilled water to the same spot on the brake pad. -Measure the time period required for complete absorption.
[0067] In order to obtain reliable measurements regardless of possible anisotropy of the molded friction material, the tests are performed on multiple points of the brake pad, for example points 10-15 as shown schematically in Figure 6. Moreover, with reference to Figure 7, the overall value of hydrophobicity, expressed in minutes, is not calculated as a simple arithmetic mean value between measurements corresponding to different test points, but is calculated as follows, also diagrammed in Figure 7: Data 1: The average number between points 1 and 2. Data 2: The average number between points 3 and 4. Data 3: The average number between Data 1 and Data 2. Average absorption time: given as the average between the measurements at points 5, 6 and the value of data 3.
[0068] The results are reported in Table 3: Table 3
[0069] [Table 3]
[0070] FIG. 8 shows a test moment, in which a droplet of distilled water is poured onto a brake pad friction material block. As can be seen, the droplet forms an angle with the surface of the friction material block or pad, the measurement of which is typically taken as a unit of measurement for hydrophobicity. However, in this case, the hydrophobicity of the entire friction material block or pad, rather than the hydrophobicity of the surface, is being measured, making "traditional" measurement units inappropriate. Therefore, the test detailed above was developed and has proven to be easy to perform and reliable. Example 4
[0071] Some brake pads obtained using friction material compositions #5 and W were subjected to a stiction test according to EP 3507587. The results obtained are shown in Figure 2 and in Table 4 below: Table 4
[0072] [Table 4]
[0073] As can be seen, the test results are in full agreement with those reported in Figure 1. The simple addition of 2% hydrophobic wax to a particular composition reduces the release force from 21 to 13, marking a transition from a state of stiction risk to a state of very low risk.
[0074] Further experiments, not reported in detail for simplicity, showed that adding higher or lower amounts of wax or changing the type of wax made it possible to reduce the peel force values below 10, as shown in Figure 1. Example 5
[0075] Several brake pads obtained using friction material compositions #5 and W were subjected to vehicle testing conducted according to the following protocol: -Install new discs and pads on the vehicle; - Bedding with 10 brake stop applications from 50km / h to 0km / h Spray 2 liters of water onto each wheel, rotating the wheels while spraying. After parking overnight for six times, measure the torque with a torque wrench. -Perform 50 braking applications (50km / h to 0km / h) in city traffic without changing brake pads and rotors; Repeat points 4 and 5, then perform recovery bedding in urban traffic to verify that there is no corrosion on the disc surface.
[0076] The results of the torque verification using a torque wrench are reported in Figure 3 and are expressed in Nm (Newtons per meter).
[0077] As can be seen, even taking into account random variations in different experiments, the torque values measured on brake pads provided with friction material blocks or pads containing hydrophobic wax in their composition are dramatically lower than the values for brake pads having friction material blocks of the same composition but without wax. Example 6
[0078] Several brake pads obtained using friction material compositions #5 and W were subjected to various standard AK-Master tests according to the SAE J2522 standard.
[0079] A summary of the tests performed and key charts are shown in Figures 4A, B, and C for brake pads made with a friction material containing no wax, and in Figures 5A, B, and C for brake pads made with a friction material of the same composition but containing 2% hydrophobic wax.
[0080] As can be readily appreciated, both brake pads with and without hydrophobic wax exhibit similar braking behavior, confirming that the addition of hydrophobic wax to a standard friction material does not impair its braking performance.
[0081] The wear of the brake pads and brake discs was also evaluated and expressed as the difference in weight of each component before and after the AK-Master test. The results obtained are reported in Tables 5 and 6 below. Table 5 - No wax
[0082] [Table 5] Table 6 - Waxes
[0083] [Table 6]
[0084] As can be seen, the wear of the brake pads made with the friction material containing the hydrophobic wax is significantly reduced, while the wear of the disc, although greater, is not as great due to the disc's significantly greater mass. conclusion
[0085] From the above examples and disclosure, it is clear that in any possible friction material composition, the mere addition of even a reduced amount of one of the hydrophobic waxes as disclosed herein will consistently reduce or eliminate the tendency for stiction when compared to the same friction material composition but without the hydrophobic wax.
[0086] Friction materials containing hydrophobic additives other than wax, such as those according to WO2019 / 171325, the entire contents of which are incorporated herein by reference, generally have a lower tendency for stiction, but are not sufficient to significantly lower the risk of stiction, especially when the additive is used with a friction material that exhibits severe stiction in use (without any additive).
[0087] Because the siloxane coated silica powder is not chemically incompatible with either hydrophobic wax, the two additives (for creep growth and stiction) can be used together in the same friction material composition.
[0088] Thus, all objectives of the present disclosure are met. Certain technical terms
[0089] While certain braking devices, systems, and methods have been disclosed in the context of certain illustrative embodiments, it will be understood by those skilled in the art that the scope of the disclosure extends beyond the specifically disclosed embodiments to the use of other alternative embodiments and / or embodiments, as well as certain modifications and equivalents thereof. Use with any structure is clearly within the scope of the present invention. Various features and aspects of the disclosed embodiments can be combined with or substituted for one another to form various modes of assembly. The scope of the disclosure should not be limited by the specific disclosed embodiments described herein.
[0090] Certain features described in this disclosure in the context of separate implementations can also be implemented in combination in a single implementation. Conversely, various features described in the context of a single implementation can also be implemented in multiple implementations separately or in any suitable subcombination. Moreover, although features may be described above as acting in a particular combination, one or more features from a claimed combination can, in some cases, be deleted from that combination, and the combination can be claimed as any subcombination or variation of any subcombination.
[0091] Conditional language such as "can," "could," "might," or "may," unless otherwise expressly stated or understood otherwise within the context as used, is generally intended to convey that a particular embodiment includes or does not include certain features, elements, and / or steps. As such, such conditional language is generally not intended to imply that features, elements, and / or steps are in some way required for one or more embodiments.
[0092] Connecting language such as the phrase "at least one of X, Y, and Z," unless expressly stated otherwise, is understood differently with the context in which it is generally used to convey that an item, term, etc. can be either X, Y, or Z. Because of this, such connective language is generally not intended to imply that a particular embodiment requires the presence of at least one of X, at least one of Y, and at least one of Z.
[0093] Unless otherwise stated, the terms "approximately," "about," and "substantially," as used herein, refer to an amount close to the stated amount that still performs a desired function or achieves a desired result. For example, in some embodiments, as the context may dictate, the terms "approximately," "about," and "substantially" may refer to an amount within 10% or less of the stated amount. The term "generally," as used herein, refers to a value, amount, or characteristic that primarily includes or tends toward a particular value, amount, or characteristic. As an example, in certain embodiments, as the context may dictate, the term "generally parallel" may refer to a deviation from exact parallelism by 20 degrees or less.
[0094] Several embodiments have been described in connection with the accompanying drawings. While the figures are to scale, such scale should not be considered limiting, as dimensions and proportions other than those shown are contemplated and within the scope of the disclosed invention. Distances, angles, and the like are merely illustrative and do not necessarily bear an exact relationship to the actual dimensions and layout of the illustrated devices. Components may be added, removed, and / or rearranged. Furthermore, any particular features, aspects, methods, attributes, properties, qualities, attributes, elements, etc. disclosed herein relating to various embodiments may be used in all other embodiments described herein. Additionally, it will be recognized that any method described herein may be implemented using any device suitable for performing the recited steps. summary
[0095] Various exemplary embodiments of braking devices, systems, and methods have been disclosed. While the machines, systems, and methods are disclosed in the context of those embodiments, the disclosure extends beyond the specifically disclosed embodiments to other alternative embodiments and / or other uses of the embodiments, as well as certain modifications and equivalents thereof. The disclosure expressly contemplates that various features and aspects of the disclosed embodiments can be combined with or substituted for one another. Therefore, the scope of the disclosure should not be limited by the particular disclosed embodiments described above, but should instead be determined solely by a fair reading of the following claims and their full scope of equivalents. The inventions described in the original claims of this application are set forth below. [1] A friction block or layer (3) made of asbestos-free friction material, particularly designed to be provided as an integral part of a vehicle brake pad (1), the asbestos-free friction material comprising, as its constituent materials, inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive, wherein the asbestos-free friction material also contains, as an additional constituent or additive, a hydrophobic wax, the relative amount of which is selected depending on the chemical nature and amount of the other constituent materials of the asbestos-free friction material, such that the friction block or layer of the asbestos-free friction material has a hydrophobicity, defined as the absorption time of a droplet formed by 20 + / - 5 μL of distilled water within the friction material, of more than 60 minutes. [2] The hydrophobic wax is in the form of a solid powder and has a melting point greater than 110°C, and is soluble in Celsius and kg / cm, respectively. 2 Friction block or layer of asbestos-free friction material according to [1], characterized in that it is chemically stable at high temperatures and pressures of the order of 100 times higher than that of the asbestos-free friction material. [3] The friction block or layer of the asbestos-free friction material according to [1] or [2], characterized in that the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE-modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and special waxes (bonded wax, modified PE wax, PTFE texture powder). [4] The friction block or layer of the asbestos-free friction material according to any one of [1] to [3], wherein the hydrophobic wax is present in the asbestos-free friction material in an amount of 0.5% to 5% by volume, preferably 1.0% to 2.0% by volume, calculated based on the total amount of the asbestos-free friction material. [5] The friction block or layer of the asbestos-free friction material according to any one of [1] to [4], characterized in that the friction block or layer has no or almost no tendency to stitch against the surface of its friction counterpart, and the friction block or layer exhibits a peel force from the metal surface of less than 15 Newtons after being electrochemically stitched to the metal surface by pressing the friction block or layer of the asbestos-free friction material against the metal surface of steel, iron, or cast iron and causing a corrosion phenomenon thereon. [6] A vehicle brake pad (1) designed to cooperate in use with a vehicle brake disc made of iron, steel, or cast iron, said vehicle brake pad including a friction block or layer (3) of asbestos-free friction material operatively associated in use with said vehicle brake disc, said friction block or layer of asbestos-free friction material being characterized in that the friction block or layer contains, as one of its component materials, 0.5% to 5% by volume of a hydrophobic wax having a melting point greater than 110°C. [7] The vehicle brake pad according to [6], wherein the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE-modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and special waxes (bonded wax, modified PE wax, PTFE texture powder), so that the vehicle brake pad has a reduced or no tendency for stiction, particularly in wet weather. [8] Use of a hydrophobic wax in an asbestos-free friction material containing inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or an abrasive as further component materials thereof, wherein the hydrophobic wax is contained in the asbestos-free friction material in an amount of 0.5% to 5% by volume calculated on the total volume of the asbestos-free friction material, so that the asbestos-free friction material exhibits a reduced or no tendency for stiction, especially in wet weather. [9] A method for manufacturing a brake pad (1) for a vehicle having a reduced or no tendency to stitch against the friction surface of an associated brake disc, i.e. having a reduced or no tendency to stiction, particularly in wet weather, said method comprising: i) - preparing a test quantity of asbestos-free friction material, in particular of the NAO class, by mixing together the respective component materials comprising at least inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding a quantity of a hydrophobic wax as a further component material in step i) so as to be mixed with said component material of step i); iii) - forming a solid block or layer of said asbestos-free friction material containing said hydrophobic wax by pressing and heating said component materials mixed together in a mold to form a pad; iv) - subjecting said pad to a hydrophobicity test consisting of measuring the absorption time thereon of a drop formed by 20 + / - 5 μL of distilled water; v) - Repeating steps i) to iv) using different predetermined amounts of said hydrophobic wax; vi) - industrially producing brake pads (1) using asbestos-free friction materials containing said hydrophobic wax, which have the same chemical composition as those test friction materials produced by the previous steps i) to v) and which have shown a water droplet absorption time of more than 60 minutes in step iv); A method comprising:
[10] A method for manufacturing a brake pad (1) for a vehicle having a reduced or no tendency to stitch against the friction surface of an associated brake disc, i.e. having a reduced or no tendency to stiction, particularly in wet weather, said method comprising: i) - preparing an asbestos-free friction material, in particular of the NAO type, by mixing together the respective component materials comprising at least inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding an amount of a hydrophobic wax as a further component material in step i) to be mixed with the component material of step i), wherein the hydrophobic wax is selected from the group consisting of polyethylene (PE) wax, high density PE (HDPE) wax, polypropylene wax, micronized PE wax, oxidized PE wax, polytetrafluoroethylene (PTFE) modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and special waxes (bonded wax, modified PE wax, PTFE texture powder), and the hydrophobic wax is added to the asbestos-free friction material in an amount of 0.5% to 5% by volume (or about 0.5% to about 5% by volume), preferably 1.0% to 2.0% by volume (or about 1.0% to about 2.0% by volume), calculated based on the total amount of the asbestos-free friction material; iii) - forming a solid block or layer of the asbestos-free friction material containing the hydrophobic wax by pressing and heating the component materials mixed together in a mold to form a pad; A method comprising:
[11] The method according to [9] or
[10] , wherein the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE-modified polyethylene wax, micronized amide wax, micronized polypropylene wax, and special waxes (bonded wax, modified PE wax, and PTFE texture powder), and the hydrophobic wax is contained in the asbestos-free friction material in an amount of 0.5% to 5% by volume calculated based on the total volume of the asbestos-free friction material.
Claims
1. 1. A friction block or layer (3) made of an asbestos-free friction material, the asbestos-free friction material comprising as its constituent materials inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive, the asbestos-free friction material also containing as an additional constituent material or additive a hydrophobic wax, the relative amount of the hydrophobic wax being selected according to the chemical nature and amount of the other constituent materials of the asbestos-free friction material such that the friction block or layer of the asbestos-free friction material has a hydrophobicity defined as the absorption time in the friction material of a droplet formed by 20 + / - 5 μL of distilled water of more than 60 minutes.
2. The hydrophobic wax is in the form of a solid powder and has a melting point greater than 110° C., and is 0.1 to 1.0 MPa in degrees Celsius and kg / cm, respectively. 2 2. The friction block or layer of asbestos-free friction material according to claim 1, characterized in that the wax molecules do not undergo decomposition at high temperatures and pressures of the order of 100 of magnitude.
3. 3. The friction block or layer of the asbestos-free friction material according to claim 1 or 2, characterized in that the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE modified polyethylene wax, micronized amide wax, micronized polypropylene wax, specialty wax, bonded wax, modified PE wax or PTFE texture powder.
4. 4. The friction block or layer of asbestos-free friction material according to any one of claims 1 to 3, characterized in that the hydrophobic wax is present in the asbestos-free friction material in an amount comprised between 0.5% and 5% by volume, calculated on the total amount of the asbestos-free friction material.
5. The friction block or layer of an asbestos-free friction material as described in claim 4, wherein the hydrophobic wax is present in the asbestos-free friction material in an amount comprised between 1.0 volume % and 2.0 volume %.
6. A friction block or layer of asbestos-free friction material described in any one of claims 1 to 5, characterized in that the friction block or layer of asbestos-free friction material is designed to be provided as an integral part of a vehicle brake pad (1).
7. 7. A friction block or layer of asbestos-free friction material according to any one of claims 1 to 6, characterized in that the friction block or layer has no or almost no tendency to stitch against the surface of its friction counterpart, said friction block or layer exhibiting a peel force from a metal surface of steel, iron or cast iron of less than 15 Newtons after being electrochemically stitched against said metal surface by pressing said friction block or layer of asbestos-free friction material against said metal surface and inducing a corrosion phenomenon thereon.
8. 1. A vehicle brake pad (1) designed to cooperate in use with a vehicle brake disc made of iron, steel or cast iron, said vehicle brake pad comprising a friction block or layer (3) of asbestos-free friction material in operative association in use with said vehicle brake disc, said friction block or layer of asbestos-free friction material being characterized in that it contains, as one of its component materials, 0.5% to 5% by volume of a hydrophobic wax having a melting point above 110°C.
9. 9. The vehicle brake pad of claim 8, wherein the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE modified polyethylene wax, micronized amide wax, micronized polypropylene wax, specialty wax, bonded wax, modified PE wax or PTFE texture powder, so that the vehicle brake pad has a reduced or zero tendency to stiction.
10. 1. Use of a hydrophobic wax in an asbestos-free friction material containing inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or an abrasive as further component materials thereof, said hydrophobic wax having a melting point higher than 110° C. and contained as one of the component materials in said asbestos-free friction material in an amount comprised between 0.5% and 5% by volume calculated on the total volume of said asbestos-free friction material, so that said asbestos-free friction material shows a reduced or zero tendency to stiction.
11. A method for manufacturing a brake pad (1) for a vehicle having a reduced or zero tendency to stitch against the friction surface of an associated brake disc, i.e. having a reduced or zero tendency of stiction, said method comprising the steps of: i) - preparing a test quantity of asbestos-free friction material by mixing together respective component materials including at least inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding in step i) a quantity of a hydrophobic wax as a further component material so as to be mixed together with said component material of step i); iii)--forming a solid block or layer of said asbestos-free friction material containing said hydrophobic wax by pressing and heating said component materials mixed together in a mold to form a pad; iv) - subjecting said pad to a hydrophobicity test consisting of measuring the absorption time thereon of a drop formed by 20 + / - 5 μL of distilled water; v) - Repeating steps i) to iv) using different predetermined amounts of said hydrophobic wax; vi) - Industrially producing brake pads (1) using said hydrophobic wax-containing asbestos-free friction material having the same chemical composition as those test friction materials produced by the previous steps i) to v) and exhibiting a water drop absorption time of more than 60 minutes in step iv). A method comprising:
12. A method for manufacturing a brake pad (1) for a vehicle having a reduced or zero tendency to stitch against the friction surface of an associated brake disc, i.e. having a reduced or zero tendency of stiction, said method comprising the steps of: i) - preparing an asbestos-free friction material by mixing together respective component materials including at least inorganic and / or organic fibers, at least a binder, at least a friction modifier or lubricant, and at least a filler or abrasive; ii) - adding an amount of a hydrophobic wax in step i) as a further component material to be mixed with said component material of step i), wherein said hydrophobic wax is selected from the group consisting of polyethylene (PE) wax, high density PE (HDPE) wax, polypropylene wax, micronized PE wax, oxidized PE wax, polytetrafluoroethylene (PTFE) modified polyethylene wax, micronized amide wax, micronized polypropylene wax, specialty wax, bonded wax, modified PE wax or PTFE texture powder, said hydrophobic wax being added into said asbestos-free friction material in an amount comprised between 0.5% and 5% by volume calculated on the total amount of said asbestos-free friction material; iii) - forming a solid block or layer of said asbestos-free friction material containing said hydrophobic wax by pressing and heating said component materials mixed together in a mold to form a pad; A method comprising:
13. The method of claim 12, wherein the hydrophobic wax is added to the asbestos-free friction material in an amount comprised between 1.0 volume percent and 2.0 volume percent.
14. 12. The method of claim 11, wherein the hydrophobic wax is selected from the group consisting of polyethylene wax, HDPE wax, polypropylene wax, micronized PE wax, oxidized PE wax, PTFE modified polyethylene wax, micronized amide wax, micronized polypropylene wax, specialty wax, bonded wax, modified PE wax or PTFE texture powder, and the hydrophobic wax is contained in the asbestos-free friction material in an amount comprised between 0.5% and 5% by volume calculated on the total volume of the asbestos-free friction material.
Citation Information
Patent Citations
Composition for friction material
JP1994184524A
Friction material
JP2006125618A
Friction material and manufacturing method of friction material
JP2016065163A
Friction material composition, friction material, and friction member
WO2018163256A1