Anode composition, anode for lithium secondary battery including the same, lithium secondary battery including the anode, and method for producing the anode composition

The use of a silicon-based negative electrode composition with controlled functional group content in conductive materials addresses the volume expansion issue, enhancing the performance and stability of lithium secondary batteries.

JP7571308B2Active Publication Date: 2024-10-22LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023549665
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-01
Filing Date
2022-09-30
Publication Date
2024-10-22
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Silicon-based negative electrodes experience significant volume expansion during charging and discharging, leading to conductive path disruption and performance deterioration, limiting their application in high-capacity lithium secondary batteries.

Method used

A negative electrode composition comprising a silicon-based active material, a point-like conductive material with a functional group content of 0.01% to 0.05%, and a plate-like conductive material, which enhances dispersibility and maintains conductive paths despite volume expansion.

Benefits of technology

The composition improves the C rate and output characteristics of lithium secondary batteries by maintaining a stable conductive network and reducing the impact of volume expansion, thereby extending the battery's life and capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571308000003
    Figure 0007571308000003
  • Figure 0007571308000004
    Figure 0007571308000004
  • Figure 0007571308000001
    Figure 0007571308000001
Patent Text Reader

Abstract

The present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, a lithium secondary battery including the negative electrode, and a method for producing the negative electrode composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2021-0130945, filed with the Korean Intellectual Property Office on October 1, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, a lithium secondary battery including the negative electrode, and a method for producing the negative electrode composition. [Background technology]

[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is the field of power generation and storage using electrochemical reactions.

[0004] At present, a representative example of an electrochemical element that uses such electrochemical energy is a secondary battery, and the range of its use is tending to expand more and more.

[0005] As technological development and demand for mobile devices increases, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used. In addition, research into methods for manufacturing high-density electrodes with higher energy density per unit volume as electrodes for such high-capacity lithium secondary batteries is being actively conducted.

[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode contains a negative electrode active material that inserts and removes lithium ions released from the positive electrode. Silicon-based particles having a large discharge capacity can be used as the negative electrode active material.

[0007] In particular, with the recent demand for high-density energy batteries, Si / C and SiO, which have capacities 10 times larger than those of graphite-based materials, are being used as negative electrode active materials. x However, silicon-based compounds, which are high-capacity materials, have a larger capacity than conventionally used graphite, but they have a problem in that their volume expands rapidly during charging, cutting off the conductive path and reducing the battery characteristics.

[0008] In order to solve the problems associated with using silicon-based compounds as negative electrode active materials, various methods have been discussed, such as a method of adjusting the driving potential, a method of additionally coating a thin film on the active material layer, a method of controlling the particle size of the silicon-based compound, and other methods of suppressing the volume expansion itself or preventing the conductive path from being broken. However, the above methods have limitations in their application because they may actually degrade the performance of the battery, and there are still limitations in the commercialization of negative electrode batteries with a high content of silicon-based compounds.

[0009] Furthermore, in the case of a negative electrode containing a silicon-based active material, the volume of the electrode expands more than in the case of a negative electrode containing a carbon-based active material, which makes it difficult to ensure a conductive path during charging and discharging.

[0010] Therefore, even when silicon-based compounds are used as active materials to improve capacity performance, research is needed into conductive materials that can prevent the conductive paths from being damaged due to the volume expansion of the silicon-based compounds. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2009-080971 A Summary of the Invention [Problem to be solved by the invention]

[0012] Silicon-based negative electrodes have a high proportion of aqueous binder, making it easier to disperse conductive materials than carbon-based negative electrodes. Therefore, it has been found that by adjusting the content of functional groups in dot-shaped conductive materials, which were previously used by increasing the content of functional groups for dispersion, and using them together with sheet-shaped conductive materials, dispersibility is improved and problems such as gas generation and securing conductive paths can be solved.

[0013] Thus, the present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, a lithium secondary battery including the negative electrode, and a method for producing the negative electrode composition. [Means for solving the problem]

[0014] One embodiment of the present specification provides a negative electrode composition including a silicon-based active material; a negative electrode conductive material; and a negative electrode binder, in which the negative electrode conductive material includes a dot-like conductive material and a plate-like conductive material, the dot-like conductive material has a functional group content (volatile matter) of 0.01% or more and less than 0.05%, and the silicon-based active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0015] In another embodiment, there is provided a method for producing a negative electrode composition, the method including: mixing a dot-shaped conductive material and a binder to form a mixture; adding water to the mixture to perform a first mixing; and adding a silicon-based active material to the mixed mixture to perform a second mixing; wherein the method for producing a negative electrode composition further includes a step of including a plate-shaped conductive material in the step of forming the mixture or the step of second mixing, and the dot-shaped conductive material has a functional group content (volatile content) of 0.01% or more and less than 0.05%.

[0016] In yet another embodiment, there is provided a negative electrode for a lithium secondary battery, comprising: a negative electrode current collector layer; and a negative electrode active material layer comprising a negative electrode composition according to the present application formed on one or both sides of the negative electrode current collector layer.

[0017] Finally, there is provided a lithium secondary battery, comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator disposed between the positive electrode and the negative electrode; and an electrolyte. Effect of the Invention

[0018] In the case of a negative electrode composition according to one embodiment of the present invention, when a silicon-based active material, which is a high-capacity material, is used to produce a high-capacity battery, the negative electrode conductive material includes a dot-like conductive material and a plate-like conductive material, and the dot-like conductive material satisfies the requirement that the content of functional groups (volatile content) be 0.01% or more and less than 0.05%, thereby not significantly affecting the life characteristics of conventional lithium secondary batteries, increasing the number of points at which charging and discharging are possible, and providing the characteristic of excellent output characteristics at a high C rate.

[0019] Conventional dot-shaped conductive materials used as carbon-based negative electrodes are generally hydrophobic, making them difficult to disperse in water. When used in negative electrodes made from aqueous dispersion slurry, materials with a high content (volatile content) of functional groups are used for dispersion, which increases the affinity with water and improves dispersibility, but the large number of functional groups causes problems with gas generation due to side reactions. However, the negative electrode composition according to one embodiment of the present invention is applied to silicon-based negative electrodes, and has a high binder ratio, making it easier to disperse than conventional carbon-based negative electrodes. By using a dot-shaped conductive material with a functional group content (volatile content) of 0.01% or more but less than 0.05%, the functional group content is low, the hydrophobicity is strong, and the composite strength with the surrounding conductive material and binder is high.

[0020] That is, in the case of a negative electrode composition according to one embodiment of the present invention, when a silicon-based active material, which is a high-capacity material, is used to produce a high-capacity battery, the proportion of aqueous binder is higher than when used as a conventional carbon-based negative electrode, and therefore a hydrophobic conductive material having a functional group content (volatile content) of 0.01% or more and less than 0.05% can be used as the dot-shaped conductive material. This improves the bonding strength with the conductive material / binder located in the vicinity, and the main feature is that even if expansion occurs during charging / discharging of the Si-based negative electrode, the bonds in the negative electrode composition are strengthened, and performance such as ensuring a conductive path is improved.

[0021] In addition, when a conventional silicon-based active material is used, the volume expansion during charging and discharging can be minimized by using the negative electrode composition of the present invention. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a diagram showing a laminated structure of a negative electrode for a lithium secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 1 is a diagram showing a stacked structure of a lithium secondary battery according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Before describing the present invention, some terms will first be defined.

[0024] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, not excluding other components, unless specifically stated to the contrary.

[0025] In this specification, "p to q" means a range of "not less than p and not more than q."

[0026] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mino II manufactured by BEL Japan Ltd. That is, in this application, the BET specific surface area may mean the specific surface area measured by the above-mentioned measurement method.

[0027] In this specification, "Dn" means the average particle size, which means the particle size at the n% point of the cumulative particle number distribution according to the particle size. That is, D50 is the particle size at the 50% point of the cumulative particle number distribution according to the particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution according to the particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution according to the particle size. Meanwhile, the average particle size can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in the diffraction pattern according to the particle size is measured when the particles pass through a laser beam to calculate the particle size distribution.

[0028] In this specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer participates in a polymerization reaction and is contained as a repeating unit in the polymer. When a polymer contains a monomer, this is interpreted as the same as when a polymer contains a monomer as a monomer unit.

[0029] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless otherwise specified as a "homopolymer."

[0030] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using commercially available monodisperse polystyrene polymers (standard samples) with various degrees of polymerization as standard substances for molecular weight measurement. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0031] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily implement the present invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0032] One embodiment of the present specification provides a negative electrode composition including a silicon-based active material; a negative electrode conductive material; and a negative electrode binder, in which the negative electrode conductive material includes a dot-like conductive material and a plate-like conductive material, the dot-like conductive material has a functional group content (volatile content) of 0.01% or more and less than 0.05%, and the silicon-based active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0033] In the case of the negative electrode composition according to one embodiment of the present invention, when a silicon-based active material, which is a high-capacity material, is used to produce a high-capacity battery, the proportion of aqueous binder is higher than that in the case of a conventional carbon-based negative electrode. Therefore, a hydrophobic conductive material having a functional group content (volatile content) of 0.01% or more and less than 0.05% can be used as the dot-shaped conductive material. This improves the bonding strength with the conductive material / binder located in the vicinity, and the main feature is that even if expansion occurs during charging / discharging of the Si-based negative electrode, the bonds in the negative electrode composition are strengthened, and performance such as securing a conductive path is improved.

[0034] In one embodiment of the present application, the content of the functional group (volatile content) is a numerical representation of the content of the functional group contained in the conductive material, which can be calculated by the weight loss rate as follows: Weight loss rate = [(weight of the substance before heat treatment - weight of the substance after heat treatment) / weight of the substance before heat treatment] × 100

[0035] The amount lost by heat treatment may be a functional group present on the surface of the substance before the heat treatment. The functional group may be at least any one selected from the group consisting of a hydroxy group, a carboxy group, an aldehyde group, a phenol group, a ketone group, an anhydride group, a lactone group, a peroxide group, an ether group, a hemiacetal group, a quinone group, and an amino group.

[0036] The content (volatile content) of the functional group according to the present application is measured using an analytical method capable of confirming the mass while raising the temperature using thermal analysis. The method used in the present application is the TPD mass method. Specifically, it can be measured by a method of raising the temperature of the measurement sample to 950 °C and confirming the amount of the volatilized compound. The analyzed amount can be represented by the content of the functional group present on the surface of the dot conductive material.

[0037] In one embodiment of the present application, the silicon-based active material is SiO x (x = 0), SiO x (0 < x < 2), SiC, and one or more selected from the group consisting of Si alloys, to provide a negative electrode composition.

[0038] In one embodiment of the present application, the silicon-based active material is SiO x (x = 0), SiO x (0 < x < 2), and one or more selected from the group consisting of metal impurities. Based on 100 parts by weight of the silicon-based active material, the SiO x (x = 0) contains 70 parts by weight or more to provide a negative electrode composition.

[0039] In another embodiment, based on 100 parts by weight of the silicon-based active material, the SiO x (x = 0) may contain 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more, and may contain 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.

[0040] In one embodiment of the present application, the silicon-based active material may be, in particular, pure silicon (Si) as the silicon-based active material. The use of pure silicon (Si) as the silicon-based active material means that, based on a total of 100 parts by weight of the silicon-based active material as described above, pure Si particles (SiO x (x=0)) may be included in the above range.

[0041] Silicon-based active materials have a significantly higher capacity than the conventionally used graphite-based active materials, and so attempts to use them are increasing. However, because of their high volume expansion rate during the charge and discharge process, they have only been used in small amounts mixed with graphite-based active materials.

[0042] Therefore, in the case of the present invention, in order to improve capacity performance and achieve high energy density, only a silicon-based active material is used as the negative electrode active material, but in order to solve the above-mentioned problems, a negative electrode conductive material containing a dot-shaped conductive material and a plate-shaped conductive material and having a functional group content (volatile content) of 0.01% or more and less than 0.05% is used, thereby solving the conventional problems.

[0043] Meanwhile, the average particle size (D50) of the silicon-based active material of the present invention may be 5 μm to 10 μm, specifically 5.5 μm to 8 μm, and more specifically 6 μm to 7 μm. When the average particle size is less than 5 μm, the specific surface area of ​​the particles increases excessively, and the viscosity of the negative electrode slurry increases excessively. As a result, the particles constituting the negative electrode slurry are not dispersed smoothly. When the size of the silicon-based active material is too small, the contact area between the silicon particles and the conductive material is reduced by the composite of the conductive material and the binder in the negative electrode slurry, so that the conductive network is likely to be disconnected, and the capacity retention rate is reduced. When the average particle size exceeds 10 μm, the silicon particles are too large, and the surface of the negative electrode is not smooth, which causes non-uniformity in the current density during charging and discharging. When the silicon particles are too large, the phase stability of the negative electrode slurry becomes unstable, and the processability is reduced. As a result, the capacity retention rate of the battery is reduced.

[0044] In one embodiment of the present application, the silicon-based active material generally has a characteristic BET specific surface area. The BET specific surface area of ​​the silicon-based active material is preferably less than 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m 2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET specific surface area is determined in accordance with DIN 66131 (with nitrogen).

[0045] In one embodiment of the present application, silicon-based active material may be, for example, in crystalline or amorphous form, and is preferably non-porous.Silicon particles are preferably spherical or shard particles.Alternatively, but less advantageously, silicon particles may have a fibrous structure or be in the form of silicon-containing film or coating.

[0046] In one embodiment of the present application, there is provided a negative electrode composition, in which the silicon-based active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0047] In another embodiment, the silicon-based active material may be included in an amount of 60 parts by weight or more, preferably 65 parts by weight or more, more preferably 70 parts by weight or more, based on 100 parts by weight of the negative electrode composition, and may be included in an amount of 95 parts by weight or less, preferably 90 parts by weight or less, more preferably 80 parts by weight or less.

[0048] The negative electrode composition according to the present application uses a specific negative electrode conductive material and a negative electrode binder that can suppress the volume expansion rate during charge and discharge, so that even when the silicon-based active material having an extremely high capacity is used within the above range, the negative electrode composition does not deteriorate the performance of the negative electrode and has the characteristic of excellent output characteristics during charge and discharge.

[0049] In one embodiment of the present application, the silicon-based active material may have a non-spherical shape, and the circularity thereof is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.

[0050] In this application, the circularity is determined by the following formula 1, where A is the area and P is the perimeter. [Formula 1] 4πA / P 2

[0051] In the past, it was common to use only graphite-based compounds as negative electrode active materials, but in recent years, as the demand for high-capacity batteries has increased, attempts to mix silicon-based compounds to increase capacity have been increasing. However, silicon-based compounds have a limitation in that their volume expands rapidly during the charge / discharge process, damaging the conductive path formed in the negative electrode active material layer and reducing the performance of the battery.

[0052] Therefore, in one embodiment of the present application, the negative electrode conductive material includes a dot-shaped conductive material and a plate-shaped conductive material, and the dot-shaped conductive material may have a functional group content (volatile content) of 0.01% or more and less than 0.05%. By using the conductive material, even when the silicon-based active material expands, the conductive material can be positioned consistently on the surface of the particles, between the particles, and between the particle aggregates, so that the conductive path formed by the conductive material is not affected by the volume expansion, and the battery performance can be maintained well.

[0053] In one embodiment of the present application, the dot-like conductive material refers to a dot-like or spherical conductive material that can be used to improve the conductivity of the negative electrode, does not induce chemical changes, and has conductivity. Specifically, the dot-like conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably includes carbon black in terms of realizing high conductivity and excellent dispersibility.

[0054] In one embodiment of the present application, the point-like conductive material has a BET specific surface area of ​​40 m 2 / g or more 70m 2 / g or less, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.

[0055] In one embodiment of the present application, the dotted conductive material may have a functional group content (volatile content) of 0.01% or more and less than 0.05%, preferably 0.01% or more and 0.04% or less, and more preferably 0.01% or more and 0.03% or less.

[0056] In particular, when the content of the functional group of the dot-shaped conductive material satisfies the above range, the functional group is present on the surface of the dot-shaped conductive material, and when water is used as a solvent, the dot-shaped conductive material can be smoothly dispersed in the solvent. In particular, the present invention uses a silicon-based active material and a specific binder (mainly a water-based binder) to reduce the content of the functional group of the dot-shaped conductive material, thereby having an outstanding effect in improving dispersibility.

[0057] In one embodiment of the present application, the silicon-based active material is characterized by including a dot-shaped conductive material having a functional group content within the above range, and the content of the functional group can be adjusted according to the degree of heat treatment of the dot-shaped conductive material.

[0058] In other words, in the preparation of point-like conductive material, a high content of functional groups means that there is a lot of foreign matter, and a low content of functional groups means that more heat treatment processing has been performed. The point-like conductive material according to the present application is characterized in that a certain portion of the heat treatment is performed on the point-like conductive material so that the functional group content satisfies the above range, thereby satisfying the above-mentioned functional group content range.

[0059] Specifically, since the dispersibility of the dot-like conductive material is improved, even if the content of the dot-like conductive material is increased in a negative electrode slurry having the same solid content, the viscosity of the negative electrode slurry can be maintained at an appropriate level, thereby maintaining stable processability and improving the uniformity of the formed negative electrode.

[0060] In one embodiment of the present application, the particle size of the dotted conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.

[0061] In one embodiment of the present application, the negative electrode conductive material may include a plate-shaped conductive material.

[0062] The plate-shaped conductive material can improve conductivity by increasing surface contact between silicon particles in the negative electrode and can also serve to suppress disconnection of the conductive path due to volume expansion. The plate-shaped conductive material can be referred to as a sheet-shaped conductive material or a bulk-shaped conductive material.

[0063] In one embodiment of the present application, the plate-shaped conductive material may include at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and may be preferably plate-shaped graphite.

[0064] In one embodiment of the present application, the sheet-shaped conductive material may be provided in a form that is bonded to the surface of the silicon-based particle. Specifically, the sheet-shaped conductive material may be provided in a form that is bonded to the hydrophilic groups of the sheet-shaped conductive material and the -OH groups or -O groups on the surface of the silicon-based particle.

[0065] In one embodiment of the present application, the average particle diameter (D50) of the plate-shaped conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. When the above range is satisfied, the sufficient particle size does not cause an excessive increase in viscosity of the negative electrode slurry, and dispersion is easy. Therefore, the dispersion effect is excellent when dispersing using the same device and time.

[0066] In one embodiment of the present application, there is provided a negative electrode composition, wherein the plate-shaped conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.

[0067] In one embodiment of the present application, the plate-shaped conductive material may be a plate-shaped conductive material having a high BET specific surface area; or a plate-shaped conductive material having a low specific surface area.

[0068] In one embodiment of the present application, the plate-shaped conductive material may be a plate-shaped conductive material with a high specific surface area or a plate-shaped conductive material with a low specific surface area, without any limitations. However, since the dispersion of the plate-shaped conductive material according to the present application may have some effect on the electrode performance, it is particularly preferable to use a plate-shaped conductive material with a low specific surface area in which dispersion does not cause problems.

[0069] In one embodiment of the present application, the plate-shaped conductive material has a BET specific surface area of ​​1 m 2 / g or more.

[0070] In another embodiment, the plate-shaped conductive material has a BET specific surface area of ​​1 m 2 / g or more 500m 2 / g or less, preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 300m 2 / g or less.

[0071] In still another embodiment, the plate-shaped conductive material is a plate-shaped conductive material having a high specific surface area, and the BET specific surface area is 50 m 2 / g or more 500m 2 / g or less, preferably 80m 2 / g or more 300m 2 / g or less, more preferably 100m 2 / g or more 300m 2 / g or less.

[0072] In still another embodiment, the plate-shaped conductive material is a plate-shaped conductive material having a low specific surface area and a BET specific surface area of ​​1 m 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 / g or less.

[0073] Other examples of the negative electrode conductive material include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may include a plurality of carbon nanotube units. Specifically, unless otherwise specified, the term "bundle type" refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged side by side or entangled with the longitudinal axes of the carbon nanotube units in substantially the same orientation. The carbon nanotube unit has a graphite sheet having a cylindrical shape with a nano-sized diameter and an sp2 bond structure. In this case, the graphite sheet may exhibit conductive or semiconductive properties depending on the angle and structure at which it is rolled. The bundled carbon nanotubes can be dispersed more uniformly during the manufacture of the negative electrode than entangled type carbon nanotubes, and can smoothly form a conductive network in the negative electrode, thereby improving the conductivity of the negative electrode.

[0074] However, the present invention is characterized in that it does not use linear conductive material as described above, but instead includes dot-like and plate-like conductive material as the conductive material, and in particular adjusts the content of functional groups in the dot-like conductive material, thereby improving the output characteristics of the secondary battery of the present invention.

[0075] In one embodiment of the present application, there is provided a negative electrode composition, in which the negative electrode conductive material is 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode composition.

[0076] In another embodiment, the negative electrode conductive material may be included in an amount of 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, and more preferably 15 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode composition.

[0077] In one embodiment of the present application, there is provided a negative electrode composition comprising, based on 100 parts by weight of the negative electrode conductive material, 45 to 60 parts by weight of the dot-like conductive material; and 40 to 55 parts by weight of the plate-like conductive material.

[0078] In another embodiment, the negative electrode may contain 45 to 60 parts by weight, preferably 47 to 58 parts by weight, and more preferably 50 to 55 parts by weight of the dot-shaped conductive material, based on 100 parts by weight of the negative electrode conductive material.

[0079] In another embodiment, the negative electrode may contain 40 to 55 parts by weight, preferably 42 to 53 parts by weight, and more preferably 45 to 50 parts by weight of the plate-shaped conductive material based on 100 parts by weight of the negative electrode conductive material.

[0080] In one embodiment of the present application, the negative electrode conductive material may include dot-shaped conductive materials and plate-shaped conductive materials, and a ratio of the dot-shaped conductive materials:plate-shaped conductive materials may satisfy 1:0.8 to 1:1.2.

[0081] In one embodiment of the present application, the ratio of the dot-shaped conductive materials to the plate-shaped conductive materials may satisfy 1:1.

[0082] In one embodiment of the present application, the negative electrode conductive material includes a dot-like conductive material and a plate-like conductive material, and the above-mentioned compositions and ratios are respectively satisfied, so that the battery has the characteristics of excellent output characteristics at a high C rate, without significantly affecting the life characteristics of conventional lithium secondary batteries, and has more points at which charging and discharging are possible.

[0083] The biggest cause of performance degradation is the continuous cracking of the active material due to the volumetric expansion / contraction of silicon, and the breakage of particles leading to conductive short circuits. Therefore, when constructing an electrode containing a silicon-based active material, the most important factor is how long the original state of the silicon-based electrode can be maintained, rather than how to improve its performance.

[0084] To solve the above problems, various negative electrode conductive materials are used, but carbon black / plate-like / CNT systems are generally used. Usually, a network is formed using negative electrode conductive materials that connect various intervals according to the particle size and aspect ratio.

[0085] The negative electrode conductive material according to the present application includes two types of conductive materials, namely, dot-shaped conductive material and plate-shaped conductive material, which have the above characteristics. If the plate-shaped conductive material is not included, the silicon particles expand / contract irregularly, and the conductive network cannot be maintained at intervals, causing short-circuiting of the active material, which causes performance deterioration. In the case of plate-shaped conductive materials, since graphite material is mostly used, it has the advantage of having fewer side reactions compared to dot-shaped conductive materials, and unlike dot-shaped conductive materials, it is partially capable of charging / discharging, so it is more efficient in terms of Li ions moving to the periphery than using a dot-shaped conductive material alone. In other words, if the plate-shaped conductive material is not used, it will show the characteristic of deterioration, so the main feature of the present invention is that it solves the problem of silicon-based active materials by including two types of specific dot-shaped conductive material and plate-shaped conductive material.

[0086] The negative electrode conductive material according to the present application has a completely different structure from the conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present application serves to form a contact between silicon-based active materials whose volume expands significantly due to charging and discharging, while the positive electrode conductive material serves as a buffer during rolling and also serves to impart some electrical conductivity, and has a completely different structure and role from the negative electrode conductive material of the present invention.

[0087] In addition, the negative electrode conductive material according to the present application is applied to a silicon-based active material and has a completely different structure from a conductive material applied to a graphite-based active material. That is, a conductive material used in an electrode having a graphite-based active material has particles that are simply smaller than the active material, and therefore has the properties of improving output characteristics and imparting some electrical conductivity, and has a completely different structure and role from a negative electrode conductive material applied together with a silicon-based active material as in the present invention.

[0088] In one embodiment of the present application, the plate-shaped conductive material used as the negative electrode conductive material has a structure and function different from that of a carbon-based active material generally used as a negative electrode active material. Specifically, the carbon-based active material used as a negative electrode active material may be artificial graphite or natural graphite, and refers to a material that is processed into a spherical or dot-like shape to facilitate the storage and release of lithium ions.

[0089] On the other hand, the plate-like conductive material used as the negative electrode conductive material is a material having a sheet or plate shape and can be expressed as plate-like graphite. That is, it is a material contained in the negative electrode active material layer to maintain a conductive path, and does not play a role in storing and releasing lithium, but means a material for securing a conductive path in a sheet shape inside the negative electrode active material layer.

[0090] That is, in the present application, the use of plate-like graphite as a conductive material means that it is processed into a sheet or plate shape and used as a material to ensure a conductive path, not to store or release lithium. In this case, the negative electrode active material contained therein has high capacity characteristics for storing and releasing lithium, and plays a role in storing and releasing all the lithium ions transferred from the positive electrode.

[0091] In contrast, in the present application, the term "carbon-based active material is used as an active material" means that the carbon-based active material is processed into a dot-like or spherical shape and is used as a material that serves to store or release lithium.

[0092] In one embodiment of the present application, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.

[0093] The negative electrode binder according to one embodiment of the present application plays a role of holding the silicon-based active material and the negative electrode conductive material together to prevent distortion and structural deformation of the negative electrode structure when the volume of the silicon-based active material expands and relaxes. As long as the above role is satisfied, all common negative electrode binders can be applied, and specifically, a water-based binder may be used, and more specifically, a PAM-based binder may be used.

[0094] In one embodiment of the present application, the negative electrode binder may be contained in an amount of 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, based on 100 parts by weight of the negative electrode composition, or may be contained in an amount of 5 parts by weight or more, or 10 parts by weight or more.

[0095] Compared to conventional carbon-based negative electrodes, when a Si-based negative electrode is used, a water-based binder is applied in the above weight parts, so that a dot-shaped conductive material having a low content of functional groups can be used. Due to the above characteristics, the dot-shaped conductive material has hydrophobicity, and therefore has the characteristic of excellent bonding strength between the conductive material and the binder.

[0096] In one embodiment of the present application, there is provided a method for producing a negative electrode composition, the method including: mixing a dot-like conductive material and a negative electrode binder to form a mixture; adding water to the mixture to perform a first mixing; and adding a silicon-based active material to the mixed mixture to perform a second mixing, the method including further including a plate-like conductive material in the step of forming the mixture or the step of second mixing, wherein the dot-like conductive material has a functional group content (volatile content) of 0.01% or more and less than 0.05%.

[0097] In the method for producing the negative electrode composition, each component contained in the negative electrode composition is the same as that described above.

[0098] In one embodiment of the present application, there is provided a method for producing a negative electrode composition, wherein the first mixing and second mixing steps are steps of mixing at 2,000 rpm to 3,000 rpm for 10 minutes to 60 minutes.

[0099] In one embodiment of the present application, the negative electrode may be formed by coating one or both sides of a current collector with a negative electrode slurry containing the negative electrode composition to form a negative electrode for a lithium secondary battery.

[0100] In one embodiment of the present application, the negative electrode slurry may include: a negative electrode composition; and a slurry solvent.

[0101] In one embodiment of the present application, the solid content of the negative electrode slurry may be 5% or more and 40% or less.

[0102] In another embodiment, the solid content of the negative electrode slurry may be in the range of 5% to 40%, preferably 7% to 35%, more preferably 10% to 30%.

[0103] The solid content of the negative electrode slurry refers to the content of the negative electrode composition contained in the negative electrode slurry, and may refer to the content of the negative electrode composition based on 100 parts by weight of the negative electrode slurry.

[0104] When the solid content of the negative electrode slurry satisfies the above range, the viscosity during the formation of the negative electrode active material layer is suitable, and the particle aggregation phenomenon of the negative electrode composition is minimized, so that the negative electrode active material layer can be efficiently formed.

[0105] In one embodiment of the present application, the slurry solvent can be any solvent capable of dispersing the above-mentioned negative electrode composition, and specifically, water or NMP may be used.

[0106] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, comprising: a negative electrode current collector layer; and a negative electrode active material layer formed on one or both sides of the negative electrode current collector layer, the negative electrode active material layer comprising the negative electrode composition according to the present application.

[0107] Fig. 1 is a diagram showing a laminated structure of a negative electrode for a lithium secondary battery according to an embodiment of the present application. Specifically, a negative electrode for a lithium secondary battery 100 including a negative electrode active material layer 20 on one side of a negative electrode current collector layer 10 can be seen. Although Fig. 1 shows a negative electrode active material layer formed on one side, it may be formed on both sides of the negative electrode current collector layer.

[0108] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative electrode current collector layer is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0109] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode current collector layer has a thickness of 1 μm or more and 100 μm or less, and the negative electrode active material layer has a thickness of 20 μm or more and 500 μm or less.

[0110] However, the thickness may vary depending on the type and application of the negative electrode used, and is not limited thereto.

[0111] In one embodiment of the present application, the porosity of the negative electrode active material layer may be in the range of 10% or more and 60% or less.

[0112] In another embodiment, the porosity of the negative electrode active material layer may be in the range of 10% or more and 60% or less, preferably 20% or more and 50% or less, and more preferably 30% or more and 45% or less.

[0113] The porosity varies depending on the composition and content of the silicon-based active material, conductive material, and binder contained in the negative electrode active material layer, and in particular, the above range is satisfied by containing the silicon-based active material and conductive material according to the present application at a specific composition and content, thereby allowing the electrical conductivity and resistance of the electrode to have suitable ranges.

[0114] In one embodiment of the present application, there is provided a lithium secondary battery comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.

[0115] 2 is a diagram showing a laminated structure of a lithium secondary battery according to an embodiment of the present application. Specifically, a negative electrode 100 for a lithium secondary battery including a negative electrode active material layer 20 on one side of a negative electrode current collector layer 10 can be seen, and a positive electrode 200 for a lithium secondary battery including a positive electrode active material layer 40 on one side of a positive electrode current collector layer 50 can be seen, and the negative electrode 100 for a lithium secondary battery and the positive electrode 200 for a lithium secondary battery are stacked with a separator 30 interposed therebetween.

[0116] A secondary battery according to an embodiment of the present specification may include the negative electrode for a lithium secondary battery described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the negative electrode is the same as the negative electrode described above. The negative electrode has been described above, so a detailed description thereof will be omitted.

[0117] The positive electrode may include a positive electrode current collector, and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material.

[0118] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may generally have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0119] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 Ni-site type lithium nickel oxide represented by the chemical formula LiMn 2-c3 Mc3 Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese oxide represented by Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.6) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li metal.

[0120] In one embodiment of the present application, the positive electrode active material includes a lithium transition metal composite compound including nickel (Ni), cobalt (Co), and manganese (Mn), and the lithium transition metal composite compound includes single particles or secondary particles, and the average particle size (D50) of the single particles may be 1 μm or more.

[0121] For example, the average particle size (D50) of the single particles may be 1 μm or more and 12 μm or less, 1 μm or more and 8 μm or less, 1 μm or more and 6 μm or less, more than 1 μm and 12 μm or less, more than 1 μm and 8 μm or less, or more than 1 μm and 6 μm or less.

[0122] The single particle can have excellent particle strength even if it is formed to have a small particle size (D50) of 1 μm or more and 12 μm or less. For example, the single particle has a strength of 650 kgf / cm 2 The particle strength may be 100 to 300 MPa when the particle is rolled with a force of 650 kgf / cm. 2 Even if the electrode is rolled with a strong force, the phenomenon of an increase in fine particles in the electrode due to particle cracking is mitigated, thereby improving the life characteristics of the battery.

[0123] The single particles can be produced by mixing a transition metal precursor and a lithium source material and sintering the mixture. The secondary particles can be produced by a method different from that of the single particles, and the composition of the secondary particles can be the same as or different from that of the single particles.

[0124] The method for forming the single particles is not particularly limited, but may generally be formed by over-firing at an elevated firing temperature, using additives such as grain growth promoters that aid in over-firing, or by changing the starting material.

[0125] For example, the firing is performed at a temperature at which single particles can be formed. In order to form the single particles, the firing must be performed at a temperature higher than that at which the secondary particles are produced. For example, when the precursor composition is the same, the firing must be performed at a temperature about 30°C to 100°C higher than that at which the secondary particles are produced. The firing temperature for forming the single particles may vary depending on the metal composition in the precursor. For example, when a high-content nickel (High-Ni) NCM-based lithium transition metal composite oxide having a nickel (Ni) content of 80 mol% or more is to be formed into single particles, the firing temperature may be about 700°C to 1000°C, preferably about 800°C to 950°C. When the firing temperature satisfies the above range, a positive electrode active material including single particles having excellent electrochemical properties can be produced. When the firing temperature is less than 790°C, a positive electrode active material including a lithium transition metal composite compound in the form of secondary particles is produced, and when the firing temperature exceeds 950°C, the firing is performed excessively, and the layered crystal structure is not properly formed, and the electrochemical properties may be deteriorated.

[0126] In this specification, the term "single particle" is used to distinguish it from conventional secondary particles formed by agglomeration of tens to hundreds of primary particles, and is a concept that includes a single particle consisting of one primary particle and a similar-single particle that is an agglomeration of 30 or less primary particles.

[0127] Specifically, in the present invention, the single particle may be a single particle consisting of one primary particle or a quasi-single particle which is an aggregate of 30 or less primary particles, and the secondary particle may be in the form of an aggregate of several hundred primary particles.

[0128] In one embodiment of the present application, the lithium transition metal composite compound that is the positive electrode active material further includes secondary particles, and the average particle size (D50) of the single particles is smaller than the average particle size (D50) of the secondary particles.

[0129] In the present invention, the single particle may be a single particle consisting of one primary particle or a quasi-single particle which is an aggregate of 30 or less primary particles, and the secondary particle may be in the form of an aggregate of several hundred primary particles.

[0130] The lithium transition metal composite compound may further include secondary particles. The secondary particles refer to a form formed by agglomeration of primary particles, and can be distinguished from the concept of single particles including one primary particle, one single particle, or a similar-single particle form that is an agglomeration of 30 or less primary particles.

[0131] The particle diameter (D50) of the secondary particles may be 1 μm to 20 μm, 2 μm to 17 μm, and preferably 3 μm to 15 μm. The specific surface area (BET) of the secondary particles is 0.05 m 2 / g~10m 2 / g, preferably 0.1m 2 / g~1m 2 / g, more preferably 0.3m 2 / g~0.8m 2 / g.

[0132] In a further embodiment of the present application, the secondary particles are aggregates of primary particles, and the primary particles have an average particle size (D50) of 0.5 μm to 3 μm. Specifically, the secondary particles may be in the form of aggregates of several hundreds of primary particles, and the primary particles may have an average particle size (D50) of 0.6 μm to 2.8 μm, 0.8 μm to 2.5 μm, or 0.8 μm to 1.5 μm.

[0133] When the average particle size (D50) of the primary particles satisfies the above range, a single particle positive electrode active material having excellent electrochemical properties can be formed. If the average particle size (D50) of the primary particles is too small, the number of agglomerates of the primary particles forming the lithium nickel oxide particles increases, and the effect of suppressing particle cracking during rolling decreases. If the average particle size (D50) of the primary particles is too large, the lithium diffusion path inside the primary particles becomes long, increasing resistance and causing a decrease in output characteristics.

[0134] According to a further embodiment of the present application, the average particle size (D50) of the single particles is smaller than the average particle size (D50) of the secondary particles, so that the single particles can have excellent particle strength even when formed to have a small particle size, and thus the phenomenon of an increase in fine particles in the electrode due to particle cracking can be mitigated, thereby improving the life characteristics of the battery.

[0135] In one embodiment of the present application, the average particle size (D50) of the single particles is smaller than the average particle size (D50) of the secondary particles by 1 μm to 18 μm.

[0136] For example, the average particle size (D50) of the single particles may be 1 μm to 16 μm smaller, 1.5 μm to 15 μm smaller, or 2 μm to 14 μm smaller than the average particle size (D50) of the secondary particles.

[0137] When the average particle size (D50) of the single particles is smaller than the average particle size (D50) of the secondary particles, for example, when the above range is satisfied, the single particles can have excellent particle strength even if they are formed to have a small particle size, and thus the phenomenon of an increase in fine particles in the electrode due to particle cracking is mitigated, resulting in an improvement in the life characteristics and energy density of the battery.

[0138] According to a further embodiment of the present application, the single particles are contained in an amount of 15 parts by weight to 100 parts by weight relative to 100 parts by weight of the positive electrode active material. The single particles may be contained in an amount of 20 parts by weight to 100 parts by weight, or 30 parts by weight to 100 parts by weight relative to 100 parts by weight of the positive electrode active material.

[0139] For example, the single particles may be included in an amount of 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 35 parts by weight or more, 40 parts by weight or more, or 45 parts by weight or more, based on 100 parts by weight of the positive electrode active material. The single particles may be included in an amount of 100 parts by weight or less, based on 100 parts by weight of the positive electrode active material.

[0140] When the single particles are contained in the above range, excellent battery characteristics can be exhibited in combination with the above-mentioned negative electrode material. In particular, when the single particles are 15 parts by weight or more, the phenomenon of an increase in fine particles in the electrode due to particle cracking during rolling after electrode preparation can be mitigated, thereby improving the life characteristics of the battery.

[0141] In one embodiment of the present application, the lithium composite transition metal compound may further include secondary particles, and the secondary particles may be 85 parts by weight or less relative to 100 parts by weight of the positive electrode active material. The secondary particles may be 80 parts by weight or less, 75 parts by weight or less, or 70 parts by weight or less relative to 100 parts by weight of the positive electrode active material. The secondary particles may be 0 parts by weight or more relative to 100 parts by weight of the positive electrode active material.

[0142] When the above range is satisfied, the above-mentioned effect due to the presence of the single particle positive electrode active material can be maximized. When the secondary particle positive electrode active material is included, the component may be the same as or different from the components exemplified as the single particle positive electrode active material described above, and may refer to a form in which the single particles are aggregated.

[0143] In one embodiment of the present application, the positive electrode active material in 100 parts by weight of the positive electrode active material layer may be contained in an amount of 80 parts by weight or more and 99.9 parts by weight or less, preferably 90 parts by weight or more and 99.9 parts by weight or less, more preferably 95 parts by weight or more and 99.9 parts by weight or less, and even more preferably 98 parts by weight or more and 99.9 parts by weight or less.

[0144] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material.

[0145] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.

[0146] In addition, the positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.

[0147] The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a secondary battery can be used without any particular limitation. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte moisture absorption ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or a multilayer structure.

[0148] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.

[0149] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0150] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0151] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, can be preferably used as high-viscosity organic solvents, because they have a high dielectric constant and dissociate lithium salts well. When such cyclic carbonates are mixed in an appropriate ratio with linear carbonates having low viscosity and low dielectric constant, such as dimethyl carbonate and diethyl carbonate, an electrolyte having high electrical conductivity can be prepared, and therefore such a mixture can be used even more preferably.

[0152] As the metal salt, a lithium salt may be used. The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.

[0153] In addition to the constituents of the electrolyte, the electrolyte may further include one or more additives such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0154] According to an embodiment of the present invention, there is provided a battery module including the secondary battery as a unit cell, and a battery pack including the battery module. The battery module and the battery pack include the secondary battery having high capacity, high rate characteristics, and high cycle characteristics, and therefore can be used as a power source for a medium- to large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system.

[0155] Below, preferred examples are presented to aid in understanding the present invention. However, these examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present description. Naturally, such changes and modifications fall within the scope of the appended claims.

[0156] <Example> <Production of negative electrodes> (Example 1: Production of negative electrode) A silicon-based active material, Si (average particle size (D50): 3.5 μm), a first conductive material, a second conductive material, and polyacrylamide as a binder were added in a weight ratio of 70:10:10:10 to distilled water as a solvent for forming a negative electrode slurry to produce a negative electrode slurry (solid content concentration 25 wt%).

[0157] The first conductive material is carbon black C (specific surface area: 58 m 2 / g, diameter: 37 nm, volatile content: 0.01%), and the second conductive material is plate-shaped graphite (specific surface area: 17 m 2 / g, average particle size (D50): 3.5 μm.

[0158] The mixing method was as follows: the first conductive material, the second conductive material, the binder, and water were dispersed using a homomixer at 2500 rpm for 30 minutes, and then the active material was added and dispersed at 2500 rpm for 30 minutes to prepare a slurry.

[0159] The negative electrode current collector was a copper current collector (thickness: 8 μm) on both sides of which the negative electrode slurry was applied at 85 mg / 25 cm. 2 The negative electrode active material layer (thickness: 33 μm) was formed by coating with a loading amount of 10.0 μm, rolling, and drying in a vacuum oven at 130° C. for 10 hours, and the negative electrode active material layer (thickness: 33 μm) was used as the negative electrode (negative electrode thickness: 41 μm, negative electrode porosity: 40.0%).

[0160] (Example 2: Production of negative electrode) The negative electrode of Example 2 was manufactured in the same manner as in Example 1, except that the mixing method was changed to dispersing the first conductive material, binder, and water using a homomixer at 2500 rpm for 30 minutes, adding the silicon-based active material and plate-shaped graphite, and dispersing at 2500 rpm for 30 minutes to prepare a slurry.

[0161] (Example 3: Production of negative electrode) A negative electrode was prepared in the same manner as in Example 1, except that carbon black C having a functional group content of 0.03% was used as the first conductive material.

[0162] (Example 4: Production of negative electrode) A negative electrode was manufactured in the same manner as in Example 1, except that the silicon-based active material was Si (average particle size (D50): 3.5 μm), the first conductive material, the second conductive material, and polyacrylamide as a binder were used in a ratio of 80:5:5:10.

[0163] (Comparative Example 1: Production of Negative Electrode) Carbon black C (specific surface area: 63 m) was used as the first conductive material. 2 A negative electrode of Comparative Example 1 was prepared in the same manner as in Example 1, except that the composition ratio was changed to 1.0 / g, diameter: 35 nm, and volatile content: 0.15%).

[0164] (Comparative Example 2: Production of Negative Electrode) In the above-mentioned Example 1, carbon black C (specific surface area: 45 m 2 The negative electrode of Comparative Example 2 was prepared in the same manner as in Example 1, except that the composition ratio was changed to 0.1 / g, diameter: 30-50 nm, and volatile content: 0.40%).

[0165] (Comparative Example 3: Production of negative electrode) In the above-mentioned Example 1, carbon black C (specific surface area: 45 m 2 The negative electrode of Comparative Example 3 was prepared in the same manner as in Example 1, except that the composition ratio was changed to 0.05% by weight, diameter: 30-50 nm, and volatile content: 0.05%).

[0166] (Comparative Example 4: Production of Negative Electrode) In the first embodiment, instead of the second conductive material, a third conductive material having a BET specific surface area of ​​about 1000 to 1500 m was used. 2 The negative electrode of Comparative Example 4 was manufactured in the same manner as in Example 1, except that a linear conductive material (SWCNT) satisfying the densities of 100 / g and having an aspect ratio of 10,000 or more was used, and Si (average particle size (D50): 3.5 μm) was used as the silicon-based active material, the first conductive material, the third conductive material, and polyacrylamide were used as the binder in a weight ratio of 80:10:0.5:9.5.

[0167] (Comparative Example 5: Production of Negative Electrode) The negative electrode of Comparative Example 5 was manufactured in the same manner as in Example 1, except that the second conductive material was not used, and Si (average particle size (D50): 3.5 μm) was used as the silicon-based active material, the first conductive material, and polyacrylamide was used as the binder in a weight ratio of 70:15:15.

[0168] (Comparative Example 6: Production of Negative Electrode) The negative electrode of Comparative Example 6 was prepared in the same manner as in Example 1, except that the silicon-based active material was Si (average particle size (D50): 3.5 μm), the first conductive material, the second conductive material, and polyacrylamide as the binder were used in a weight ratio of 55:15:10:20.

[0169] (Comparative Example 7: Production of negative electrode) A negative electrode slurry was prepared by mixing 68 parts by weight of secondary particle artificial graphite having a D50 of 16.7 μm and a tap density of 0.91 g / cc, 7 parts by weight of natural graphite, 10 parts by weight of a first conductive material, 10 parts by weight of a second conductive material, 4.0 parts by weight of styrene butadiene rubber (SBR) as a binder polymer, and 1.0 part by weight of carboxymethyl cellulose (CMC), and adding water as a dispersion medium. At this time, the solid content of the negative electrode slurry was 49 wt%.

[0170] The first conductive material and the second conductive material are similar to the first conductive material and the second conductive material in the first embodiment described above.

[0171] The negative electrode slurry was applied to both sides of a copper current collector (thickness: 8 μm) at 145 mg / 25 cm. 2 The negative electrode of Comparative Example 7 was manufactured to have the same capacity as that of Example 1, and as a result, the negative electrode active material layer was formed thick in order to achieve the same capacity.

[0172] <Secondary battery manufacturing> LiNi as the positive electrode active material 0.6 Co 0.2 Mn 0.2 O2 (average particle size (D50): 15 μm), carbon black (product name: Super C65, manufacturer: Timcal) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were added in a weight ratio of 97:1.5:1.5 to N-methyl-2-pyrrolidone (NMP) as a solvent for forming a positive electrode slurry to produce a positive electrode slurry (solid concentration 78 wt%).

[0173] The positive electrode current collector was an aluminum current collector (thickness: 12 μm) and the positive electrode slurry was applied to both sides at 537 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a positive electrode active material layer (thickness: 65 μm) to prepare a positive electrode (thickness of positive electrode: 77 μm, porosity: 26%).

[0174] A polyethylene separator was interposed between the positive electrode and the negative electrode of Example 1, and an electrolyte was injected into the separator, thereby producing the secondary battery of Example 1.

[0175] The electrolyte was an organic solvent in which fluoroethylene carbonate (FEC) and diethyl carbonate (DEC) were mixed in a volume ratio of 30:70, to which vinylene carbonate was added at 3 wt % based on the total weight of the electrolyte, and LiPF6 was added as a lithium salt at a concentration of 1 M.

[0176] Secondary batteries were manufactured in the same manner as above, except that the negative electrodes of the Examples and Comparative Examples were used.

[0177] (Experimental Example 1: Evaluation of Capacity Retention Rate of Coin Half Cell) The capacity retention rate of the secondary batteries manufactured in the examples and comparative examples was evaluated using an electrochemical charger / discharger.

[0178] The number of cycles required to charge a coin half-cell battery (0.5C CC / CV charge, 0.005V, 0.005C cutoff) and discharge (0.5C CC discharge, 1.0V cutoff) was confirmed until the 1st capacity reached 80%.

[0179] The capacity retention rate after the Nth charge was evaluated using the following formula, and the results are shown in Table 1 below. Capacity retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} x 100

[0180] [Table 1]

[0181] As can be seen from Table 1, Examples 1 to 4, which use carbon black C with a low content (volatile content) of functional groups, have a higher number of cycles until the capacity reaches 80% compared to the comparative example, and therefore it was confirmed that they are effective in maintaining capacity in the life evaluation of a coin half cell with a Li metal counter electrode.

[0182] For reference, the negative electrodes in Comparative Examples 1 to 3 are those in which the content of functional groups in the dot-like conductive material exceeds the limit, the negative electrode in Comparative Example 4 satisfies the dot-like conductive material of the present invention but is applied with a linear conductive material instead of a sheet-like conductive material, the negative electrode in Comparative Example 5 is one in which the dot-like conductive material of the present invention is applied alone (without applying a sheet-like conductive material), and the negative electrode in Comparative Example 6 is one in which the silicon content is below the range of the present application. In addition, the negative electrode in Comparative Example 7 is one in which a conventional carbon-based negative electrode is applied, rather than a silicon-based negative electrode.

[0183] In particular, in the case of Comparative Example 7, graphite with low capacity was prepared to match the capacity of the silicon-based electrode of Example 1. As a result, the thickness of the electrode became very thick, and it was confirmed that the performance was inferior to Examples 1 to 4 due to the detachment phenomenon from the negative electrode current collector layer and the increase in electrode resistance.

[0184] (Experimental Example 2: Evaluation of secondary battery life) The secondary batteries manufactured in the above examples and comparative examples were subjected to a life evaluation using an electrochemical charger / discharger, and the capacity retention rate was evaluated. The secondary batteries were 1) charged (0.33C CC / CV charge, 4.2V, 0.05C cut) and discharged (0.33C CC discharge, 3.0V cut) as the first cycle, and 2) charged (1.0C CC / CV charge, 4.2V, 0.05C cut) and discharged (0.5C CC discharge, 3.0V cut) under the conditions of charging and discharging, and the cycles from the second cycle until the capacity retention rate reached 80% were confirmed.

[0185] The capacity retention rate after the Nth charge was evaluated using the following formula, and the results are shown in Table 2 below. Capacity retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} x 100

[0186] [Table 2]

[0187] As can be seen from Table 2, the embodiment in which carbon black C having a low content (volatile content) of functional groups was used had a higher number of cycles until the capacity reached 80% compared to the comparative example, and therefore it was confirmed that the embodiment is effective in maintaining the capacity even in a secondary battery using a positive electrode active material as the counter electrode.

[0188] That is, as can be seen from the above experiment, in the case of the negative electrode composition according to the present invention, when a silicon-based active material, which is a high-capacity material, is used to prepare a high-capacity battery, the proportion of aqueous binder is higher than that in the case of a conventional carbon-based negative electrode. Therefore, the dot-shaped conductive material can be a hydrophobic conductive material having a functional group content (volatile content) of 0.01% or more and less than 0.05%, and thus the bonding strength with the conductive material / binder located in the vicinity is improved, and it has been confirmed that even if expansion occurs during charging / discharging of the Si-based negative electrode, the bonding in the negative electrode composition is strengthened and performance is improved.

[0189] In Tables 1 and 2, in the case of Comparative Examples 1 to 3, a dot-shaped conductive material with a high content of functional groups was applied, and it was confirmed that the capacity retention rate and lifespan were reduced due to the problem of side reactions such as gas generation caused by the functional groups on the surface of the dot-shaped conductive material. In the case of Comparative Examples 4 and 5, the dot-shaped conductive material of the present invention was used, but a sheet-shaped conductive material was not used (Comparative Example 5) or was used in combination with a linear conductive material (Comparative Example 4). It was confirmed that the absence of a sheet-shaped conductive material that can compensate for the shortcomings of the dot-shaped conductive material resulted in a decrease in performance despite the advantages unique to the linear conductive material. In the case of Comparative Example 6, the content of the silicon-based active material was low, and the lifespan or capacity retention rate was higher than in the other comparative examples, but the content of the silicon-based active material was low, so there was a drawback in that high capacity and high energy density could not be formed.

[0190] Finally, in the case of Comparative Example 7, graphite with a low capacity was prepared to match the capacity of the silicon-based electrode of Example 1. As a result, the thickness of the electrode became very thick, and it was confirmed that the performance according to Tables 1 and 2 was deteriorated compared to Examples 1 to 4 due to the detachment phenomenon from the negative electrode current collector layer and the increase in electrode resistance. [Explanation of symbols]

[0191] 10...Negative electrode current collector layer 20...Negative electrode active material layer 30. Separator 40...Cathode active material layer 50 Positive electrode current collector layer 100 Negative electrode for lithium secondary batteries 200 ···Positive electrodes for lithium secondary batteries

Claims

1. A negative electrode composition comprising: a silicon-based active material; a negative electrode conductive material; and a negative electrode binder, The negative electrode conductive material includes a dot-shaped conductive material and a plate-shaped conductive material, The dot-shaped conductive material has a functional group content (volatile content) of 0.01% or more and less than 0.05%, The silicon-based active material is present in an amount of 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

2. 2. The negative electrode composition according to claim 1, comprising: 45 to 60 parts by weight of the dot-like conductive material; and 40 to 55 parts by weight of the plate-like conductive material, based on 100 parts by weight of the negative electrode conductive material.

3. The negative electrode composition according to claim 1 , wherein the negative electrode conductive material is present in an amount of 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode composition.

4. The negative electrode composition according to claim 1 , wherein the plate-shaped conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.

5. The silicon-based active material is SiO x (x=0), SiO x 2. The negative electrode composition of claim 1, comprising one or more selected from the group consisting of (0<x<2), SiC, and a Si alloy.

6. The silicon-based active material is SiO x (x=0), SiO x (0<x<2), and metal impurities, and based on 100 parts by weight of the silicon-based active material, the SiO x The negative electrode composition of claim 1 , comprising 70 parts by weight or more of (x=0).

7. mixing the dot-shaped conductive material; and the negative electrode binder to form a mixture; adding water to the mixture and performing a first mixing; and adding a silicon-based active material to the mixed mixture and performing a second mixing step; forming the mixture; or further including a plate-shaped conductive material in the second mixing step; The method for producing a negative electrode composition, wherein the dotted conductive material has a functional group content (volatile content) of 0.01% or more and less than 0.05%.

8. 8. The method for producing a negative electrode composition according to claim 7, wherein the first mixing and the second mixing are performed at 2,000 rpm to 3,000 rpm for 10 minutes to 60 minutes.

9. A negative electrode current collector layer; and A negative electrode active material layer comprising the negative electrode composition according to any one of claims 1 to 6, which is formed on one or both sides of the negative electrode current collector layer; A negative electrode for a lithium secondary battery comprising:

10. The thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, 10. The negative electrode for a lithium secondary battery according to claim 9, wherein the negative electrode active material layer has a thickness of 20 μm or more and 500 μm or less.

11. Positive electrode; The negative electrode for a lithium secondary battery according to claim 9 ; A separator disposed between the positive electrode and the negative electrode; and Electrolyte; A lithium secondary battery comprising:

Citation Information

Patent Citations

  • Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery using it

    JP2007165079A

  • Anode for lithium ion battery

    JP2009080971A

  • Negative electrode for lithium-ion secondary battery and lithium-ion secondary battery

    JP2015018663A

  • Negative electrode for power storage device, and power storage device

    JP2017069039A

  • Anode and manufacturing method of anode

    JP2020123465A