CATALYST, ELECTRODE, WATER ELECTROLYSIS METHOD, AND METHOD FOR PRODUCING CATALYST

A catalyst made of metal sulfides coated with β-C3N4 addresses the high overvoltage issue in oxygen generating anodes, enhancing catalytic activity and efficiency in water electrolysis.

JP7571351B2Active Publication Date: 2024-10-23NIIGATA UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021519323
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-13
Filing Date
2020-04-20
Publication Date
2024-10-23
Estimated Expiration
2040-04-20

AI Technical Summary

Technical Problem

Conventional oxygen generating anodes in water electrolysis devices suffer from high oxygen generating overvoltage, limiting the efficiency of hydrogen production.

Method used

A catalyst composed of metal sulfides, such as nickel sulfide, coated with a compound of carbon and nitrogen (β-C3N4) is used, which exhibits specific X-ray diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)°, enhancing catalytic activity and reducing overvoltage to 150 mV or less at a current density of 10 mA/cm².

Benefits of technology

The catalyst achieves high catalytic activity, enabling efficient oxygen generation with reduced overvoltage, thereby improving the efficiency of water electrolysis and hydrogen production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571351000001
    Figure 0007571351000001
  • Figure 0007571351000002
    Figure 0007571351000002
  • Figure 0007571351000003
    Figure 0007571351000003
Patent Text Reader

Abstract

A catalyst according to the present invention is characterized by being configured from a material that contains a metal sulfide and β-C3N4. It is preferable that nickel sulfide is contained as the metal sulfide. It is particularly preferable that NiS and Ni3S2 are contained as the nickel sulfide. It is also preferable that the overvoltage required for oxygen production at a current density of 10 mA / cm2 is 150 mV or less. The present invention is able to provide: a catalyst having high catalytic activity; an electrode which contains a catalyst having high catalytic activity; a water electrolysis method by which water is able to be efficiently electrolyzed; and a method for producing a catalyst, by which the above-described catalyst is able to be suitably produced.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst, an electrode, a water electrolysis method, and a method for producing a catalyst. [Background technology]

[0002] Water electrolysis devices are attracting a great deal of attention as a next-generation hydrogen production system. In a water electrolysis device, an oxygen generating anode and a hydrogen generating cathode are essential, and various oxygen generating anodes and hydrogen generating cathodes have been proposed (for example, Non-Patent Document 1).

[0003] However, conventional oxygen evolving anodes have a problem in that they have a high oxygen evolving overvoltage. [Prior art documents] [Patent documents]

[0004] [Non-Patent Document 1] P. Zhang, L. Li, D. Nordlund, H. Chen, L. Fan, B. Zhang, X. Sheng, Q. Daniel and L. Sun, Nat. Commun., 2018, 9, 381. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a catalyst having high catalytic activity, an electrode including a catalyst having high catalytic activity, a water electrolysis method capable of efficiently electrolyzing water, and a method for suitably producing the catalyst. [Means for solving the problem]

[0006] Such objectives are as follows: 19 This is achieved by the present invention described in (1) A catalyst for use in the electrolysis of water, comprising: The compound contains a metal sulfide and a compound of C and N which shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays, In the catalyst, the compound consisting of C and N coats the metal sulfide in a sheath shape. A catalyst comprising:

[0008] (2) A catalyst for use in the electrolysis of water, comprising: Contains a metal sulfide and β-C3N4, In the catalyst, the β-C3N4 is characterized in that it covers the metal sulfide in a sheath shape. A catalyst that is characteristic of

[0010] ( 3 The metal sulfide contained in the above (1) is nickel sulfide. Or (2) The catalyst according to claim 1.

[0011] ( 4 The nickel sulfide is the above-mentioned ( 3 ) The catalyst described in

[0012] (5) A catalyst for use in the electrolysis of water, comprising: The material is made of nickel sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays, A catalyst comprising NiS and Ni3S2 as the nickel sulfide. (6) The catalyst according to (5) above, wherein the compound consisting of C and N is contained in the catalyst in a form that is adhered to the surface of the nickel sulfide. (7) A catalyst for use in the electrolysis of water, comprising: It is composed of a material containing nickel sulfide and β-C3N4, A catalyst comprising NiS and Ni3S2 as the nickel sulfide. (8) The catalyst according to (7) above, wherein the β-C3N4 is contained in the catalyst in a form attached to the surface of the metal sulfide. (9) 10mA / cm 2 The catalyst according to any one of the above (1) to (8), wherein the overvoltage required for oxygen production at a current density of 150 mV or less.

[0013] (10) A catalyst comprising any one of the above (1) to (9). Water electrolysis electrode Electrode characterized by:

[0015] ( 11 ) The electrode is the above-mentioned catalytic electrode for oxygen generation. (10) The electrode according to claim 1.

[0016] ( 12 ) the above (10) or A water electrolysis method comprising electrolyzing water using the electrode according to (11).

[0017] ( 13 ) 1. A method for producing a catalyst for use in the electrolysis of water, comprising the steps of: The method includes a step of performing a heat treatment in a state where a metal material and thiourea are present together, A method for producing a catalyst, comprising obtaining a catalyst composed of a material containing a metal sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays.

[0018] ( 14 ) 1. A method for producing a catalyst for use in the electrolysis of water, comprising the steps of: The method includes a step of performing a heat treatment in a state where a metal material and thiourea are present together, A method for producing a catalyst, comprising obtaining a catalyst composed of a material containing a metal sulfide and β-C3N4. ( 15 The above-mentioned metal material is contacted with the thiourea and then heat-treated.13 )or( 14 ) A method for producing the catalyst described in

[0019] ( 16 The metal material is embedded in the thiourea powder and then heat-treated. 13 ) or ( 15 ) A method for producing the catalyst according to any one of the preceding claims. ( 17 ) The above-mentioned heat treatment is performed multiple times. 15 )or( 16 ) A method for producing the catalyst described in

[0020] ( 18 The metal material is nickel. 13 ) or ( 17 ) A method for producing the catalyst according to any one of the preceding claims.

[0021] ( 19 The above-mentioned ( 13 ) or ( 18 ) A method for producing the catalyst according to any one of the preceding claims. Effect of the Invention

[0022] Effects of the Invention The present invention can provide a catalyst having high catalytic activity, an electrode including a catalyst having high catalytic activity, a water electrolysis method capable of efficiently electrolyzing water, and a method for suitably producing the catalyst. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a diagram showing the correspondence between the X-ray diffraction (XRD) pattern for the catalyst obtained in Example 2 and the X-ray diffraction (XRD) patterns for the porous nickel raw material, NiS and Ni3S2 as metal sulfides, and β-C3N4. [Diagram 2] FIG. 2 is a SEM (scanning electron microscope) photograph of the catalyst obtained in Example 2. [Diagram 3]FIG. 3 is a SEM (scanning electron microscope) photograph of the porous nickel used in the production of the catalyst of Example 2 (corresponding to the sample of Comparative Example 1). [Figure 4] FIG. 4 is a diagram showing X-ray diffraction (XRD) patterns for the catalysts obtained in Comparative Examples 4 to 6. [Diagram 5] FIG. 5 is a graph showing the change over time in the overvoltage required for oxygen generation when water is electrolyzed at a current density of 10 mA / cm for the catalysts obtained in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3. [Figure 6] FIG. 6 shows the X-ray diffraction (XRD) patterns of the catalyst of Example 2 before and after water electrolysis. [Figure 7] FIG. 7 is a TEM (transmission electron microscope) photograph of fine parts formed on the surface of the catalyst obtained in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Preferred embodiments of the present invention will now be described in detail. [1] Catalyst First, the catalyst of the present invention will be described.

[0025] The catalyst of the present invention is composed of a material containing a metal sulfide and a compound consisting of C and N that satisfies certain conditions.

[0026] More specifically, the catalyst of the present invention is composed of a material containing a metal sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays.

[0027] Moreover, the catalyst of the present invention is composed of a material containing metal sulfide and β-C3N4 (hexagonal carbon nitride). With this configuration, it is possible to provide a catalyst having high catalytic activity.

[0028] Whether the catalyst contains metal sulfide and β-C3N4 can be confirmed by various analytical methods such as X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), and energy dispersive X-ray analysis (EDS).

[0029] More specifically, it can be determined that β-C3N4 (hexagonal carbon nitride) is contained by showing diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays. The diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° are characteristic of β-C3N4 (hexagonal carbon nitride). In addition to the above diffraction peaks, β-C3N4 (hexagonal carbon nitride) also shows diffraction peaks at 2θ=(32.2±0.5)° and 2θ=(40.9±0.5)°. In addition, in the X-ray diffraction pattern obtained by X-ray diffraction method, graphene-like carbon nitride shows diffraction peaks at 2θ=(13.0±0.5)° and 2θ=(27.0±0.5)°, but does not show diffraction peaks at 2θ=(16.0±0.5)°, 2θ=(27.8±0.5)°, 2θ=(32.2±0.5)°, and 2θ=(40.9±0.5)° as shown in the compound composed of C and N according to the present invention, β-CN4. The diffraction peak at 2θ=(27.0±0.5)° of graphene-like carbon nitride and the diffraction peak at 2θ=(27.8±0.5)° of the compound composed of C and N according to the present invention, β-C3N4, are in close regions and may be difficult to distinguish between them. However, the presence or absence of a diffraction peak at 2θ=(16.0±0.5)° makes it possible to determine whether or not the compound composed of C and N according to the present invention, β-C3N4, is contained.

[0030] In the following explanation, "an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays" may be simply referred to as "an X-ray diffraction pattern obtained by an X-ray diffraction method" or "an X-ray diffraction pattern."

[0031] In addition, for metal sulfides, the type of metal sulfide contained in the catalyst can be suitably identified by comparison with a database of X-ray diffraction patterns.

[0032] In the following explanation, "a compound consisting of C and N which shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by X-ray diffraction method" and "β-C3N4 (hexagonal carbon nitride)" are collectively referred to as "a compound consisting of C and N which satisfies specified conditions".

[0033] The metal element constituting the metal sulfide is not particularly limited, and examples thereof include Ni, Cu, Mn, Fe, Co, Cr, Ti, Ag, Au, etc., and the metal sulfide may contain one or more selected from these.

[0034] Depending on the type of metal element that constitutes the metal sulfide, for example, the function of the catalyst can be adjusted.

[0035] Applications of the catalyst of the present invention include water oxidation catalysts, water reduction catalysts, oxygen reduction catalysts, carbon dioxide reduction catalysts, hydrogen oxidation catalysts, etc. The water oxidation catalyst is a catalyst used in a reaction to electrochemically generate oxygen from water, and can be suitably used as an anode catalyst, etc. in the fields of energy conversion, hydrogen generation, etc. The water reduction catalyst is a catalyst used in a reaction to electrochemically generate hydrogen from water, and can be suitably used as a cathode catalyst, etc. in the fields of energy conversion, hydrogen generation, etc.

[0036] For example, by including one or more metal elements selected from Ni, Cu, Mn, Fe, Co, Cr, Ti, Ag, and Au as metal elements constituting the metal sulfide, the catalyst of the present invention can function as a water oxidation catalyst, etc.

[0037] Furthermore, by containing one or more metal elements selected from Ni, Cu, Mn, Fe, Co, Cr, Ti, Ag and Au as metal elements constituting the metal sulfide, the catalyst of the present invention functions as a water reduction catalyst, etc.

[0038] In particular, when the catalyst of the present invention contains nickel sulfide as the metal sulfide, it can have an especially excellent function as a water oxidation catalyst.

[0039] When the catalyst of the present invention contains nickel sulfide, it is preferable that the nickel sulfide contains NiS and Ni3S2. This makes it possible to further improve the function as a water oxidation catalyst.

[0040] The metal sulfide and the compound consisting of C and N that satisfies the specified conditions may be contained in any form in the catalyst of the present invention, but it is preferable that the compound consisting of C and N that satisfies the specified conditions is contained in the catalyst in a form attached to the surface of the metal sulfide.

[0041] This allows the above-mentioned catalytic function to be more stably exhibited. In particular, when the material is used as an electrode material for an electrode of a water electrolysis device, electrical conductivity can be stably ensured, and the material can more stably exhibit the function as an electrode.

[0042] In the catalyst, when a compound consisting of C and N that satisfies certain conditions is contained in a form that is adhered to the surface of a metal sulfide, the compound consisting of C and N that satisfies the certain conditions may, for example, be adhered only to a part of the surface of the metal sulfide, or may cover the entire surface of the metal sulfide.

[0043] Furthermore, in the case where a compound consisting of C and N that satisfies certain conditions is contained in the catalyst in a form attached to the surface of a metal sulfide, the compound consisting of C and N that satisfies the certain conditions may, for example, be attached in an island form only to a part of the surface of the metal sulfide, or may be a sheath-like coating on the metal sulfide that is in the form of a protrusion, fiber, plate, column, beam, or the like.

[0044] The catalyst of the present invention may contain other components in addition to the metal sulfide and the compound consisting of C and N that satisfies the predetermined conditions. For example, the catalyst of the present invention may contain a metal material.

[0045] This allows the catalyst as a whole to have excellent electrical conductivity, and the catalyst of the present invention can be suitably used as an electrode material (particularly, an electrode material for a water electrolysis device, etc.) In addition, the catalyst of the present invention can be suitably joined to other members.

[0046] Examples of the metallic material include elemental metals and alloys, and the metallic material may contain impurities (for example, impurities of 5 mass % or less).

[0047] When the catalyst of the present invention contains a metal material, the metal material may have any relationship with the metal sulfide, but it is preferable that the metal material contains a metal element common to the metal elements constituting the metal sulfide.

[0048] This makes it possible to provide excellent affinity between the metal material and the metal sulfide, and more effectively prevent the metal material and the metal sulfide from being unintentionally separated in the catalyst. As a result, the above-mentioned catalytic function can be more stably exerted. In particular, when used as an electrode material for electrodes of a water electrolysis device, it is possible to ensure stable electrical conductivity, and the electrode function can be more stably exerted.

[0049] Furthermore, when the catalyst of the present invention contains a metal material containing a metal element common to the metal element constituting the metal sulfide, for example, by sulfurizing only a portion of the metal material as a raw material and leaving an unreacted portion, the catalyst of the present invention in a state in which the metal material and the metal sulfide are in close contact with each other can be obtained. In this case, the production of the catalyst is facilitated and the adhesion between the metal material and the metal sulfide can be improved.

[0050] When the catalyst of the present invention is a water oxidation catalyst, the catalyst has a current of 10 mA / cm 2 The overvoltage required for oxygen production at this current density is preferably 150 mV or less, more preferably 100 mV or less, and even more preferably 50 mV or less.

[0051] This allows, for example, the oxygen generation reaction by oxidation of water (for example, the reaction at the oxygen generation anode of a water electrolysis device) to proceed more efficiently, thereby making it possible to improve the efficiency of oxygen generation.

[0052] The overvoltage required for oxygen generation can be measured by, for example, electrolysis of water under the following conditions: That is, a water electrolysis device is manufactured using the catalyst of the present invention as an oxygen generation anode and a platinum wire as a hydrogen generation cathode, and the water electrolysis device is used to electrolyze 1M potassium hydroxide aqueous solution at a current of 10 mA / cm. 2 By passing a current at a current density of 100 kcal / s for 5 hours, the overvoltage value one hour after the start of current passage during water electrolysis can be used.

[0053] The shape and size of the catalyst of the present invention are not particularly limited, and can be appropriately adjusted depending on the application of the catalyst.

[0054] For example, the shape of the catalyst of the present invention may be a powder, a film, a plate, a block (lump), or the like.

[0055] The catalyst of the present invention may be a dense body, but is preferably a porous body. This makes it possible to increase the surface area of ​​the catalyst and to improve the catalytic activity.

[0056] In particular, by supporting the compound consisting of C and N that satisfies the specified conditions in the pores of the porous body, it is possible to more suitably prevent the compound consisting of C and N that satisfies the specified conditions from falling off unintentionally even when the catalyst is used for a long period of time or in a harsh environment, and as a result, the durability of the catalyst can be improved.

[0057] [2] Catalyst manufacturing method Next, the method for producing the catalyst of the present invention will be described.

[0058] The method for producing a catalyst of the present invention is characterized by having a heat treatment step in which a metal material and thiourea are heat-treated in the coexistence of the metal material to obtain a catalyst composed of a material containing a metal sulfide and a compound composed of C and N that satisfies the above-mentioned specified conditions.

[0059] This allows the metal material to react with thiourea, and the catalyst of the present invention, which is composed of a material containing the above-mentioned metal sulfide and a compound consisting of C and N that satisfies the specified conditions, can be efficiently obtained. More specifically, thiourea functions as a sulfur source for sulfurizing the metal material, and also functions as a carbon source and a nitrogen source for generating a compound consisting of C and N that satisfies the specified conditions, and can efficiently generate the metal sulfide and the compound consisting of C and N that satisfies the specified conditions, and can efficiently produce the catalyst of the present invention. In addition, it is advantageous from the viewpoint of effectively preventing undesirable reactions from proceeding, preventing a decrease in the performance of the catalyst produced, and preventing waste of raw materials.

[0060] The heat treatment step may be carried out in a state where the metal material and thiourea coexist. For example, the heat treatment may be carried out by contacting the metal material with a block (lump) of thiourea. However, it is preferable to carry out the heat treatment in a state where the metal material is embedded in thiourea powder.

[0061] This allows the metal material to be suitably contacted with thiourea at each desired site. More specifically, the concentration of thiourea in contact with the surface of the metal material can be more suitably increased, and the desired reaction proceeds more efficiently. In particular, such effects can be obtained even when the metal material has a complex or fine shape. In addition, impurities derived from the solvent or the like can be more effectively prevented from being generated or contained in the catalyst to be produced, which is advantageous from the viewpoint of preventing a decrease in the performance of the catalyst to be produced and improving the productivity of the catalyst. In addition, by subjecting the metal material to heat treatment in a state where it is buried in thiourea powder, for example, a sudden temperature change of the metal material as the base material (workpiece) during this process and unintended temperature variations at each site of the metal material can be more effectively prevented, and the generation of internal stress and unintended deformation in the catalyst to be produced can be more effectively prevented. In addition, by using powdered thiourea, a commercially available product can be suitably used, which is particularly advantageous in terms of improving the productivity of the catalyst.

[0062] The average particle size of the particles constituting the thiourea powder is preferably 1.0 μm or more and 10 mm or less, more preferably 5.0 μm or more and 3.0 mm or less, and even more preferably 10 μm or more and 1.0 mm or less.

[0063] This makes the thiourea powder easy to handle and improves the fluidity of the thiourea powder, allowing it to come into better contact with metal materials of various shapes as base materials (workpieces), and allows the above-mentioned reaction to proceed more efficiently.

[0064] In this specification, the term "average particle size" refers to the average particle size based on number, unless otherwise specified.

[0065] The shape and size of the metal material subjected to the heat treatment step are not particularly limited, but are usually determined by the size and shape of the catalyst to be produced.

[0066] The metal material subjected to the heat treatment step may be either a dense body or a porous body, but is preferably a porous body.

[0067] This not only increases the specific surface area of ​​the metal material and enhances the reactivity with thiourea, but also improves the catalytic activity of the catalyst produced. In addition, the compound consisting of C and N that satisfies the specified conditions can be favorably supported in the pores, and even when the catalyst produced is used for a long period of time or in a harsh environment, the compound consisting of C and N that satisfies the specified conditions can be more favorably prevented from falling off. As a result, the durability of the catalyst can be improved.

[0068] The metal material may be any material containing the metal elements that constitute the metal sulfide of the catalyst to be produced, and may be, for example, various simple metals or various alloys (e.g., stainless steel, brass, bronze, etc.) The metal material may contain impurities (e.g., 5 mass% or less of impurities).

[0069] Among them, the metal material subjected to the heat treatment step is preferably nickel. This allows the reaction in the heat treatment step to proceed more efficiently, and also allows the production of a catalyst that contains nickel sulfide as a metal sulfide and has excellent functionality as a water oxidation catalyst.

[0070] The metal member used in this step may have portions with different compositions. For example, the metal material may have a base and a coating with a composition different from that of the base, may be a laminate having multiple layers, or may be composed of a gradient material in which the composition of the constituent materials changes in a gradient manner.

[0071] Furthermore, the base material (work) member subjected to the reaction with thiourea in this process may have, for example, a portion made of a material other than a metal material having reactivity with thiourea. For example, the base material (work) member subjected to the reaction with thiourea in this process may have a portion made of a metal material having reactivity with thiourea, and a portion made of a ceramic material having no reactivity with thiourea.

[0072] Furthermore, the base material (workpiece) to be reacted with thiourea in this step may be partially covered with a mask.

[0073] This makes it possible to suitably manufacture the final catalyst having a surface portion made of a metal material, for example, and as a result, for example, it is possible to more suitably ensure electrical conductivity to an electrode by connecting to an external wiring.

[0074] In the method for producing a catalyst of the present invention, the heat treatment may be carried out at least once, but it is preferable to carry out the heat treatment a plurality of times.

[0075] This makes it possible to more suitably proceed the sulfurization reaction of the metal material and the reaction of producing a compound made of C and N that satisfies predetermined conditions.

[0076] In particular, by replenishing thiourea after the previous heat treatment and then carrying out the subsequent heat treatment, it is possible to suitably replenish the thiourea that was lost in the previous heat treatment not only through the reaction with the metal material but also through decomposition, sublimation, and the like. As a whole, it is possible to more suitably proceed with the sulfurization reaction of the metal material and the reaction for producing a compound composed of C and N that satisfies predetermined conditions, thereby improving the productivity of the catalyst.

[0077] This step may be carried out in any atmosphere, for example, in the air or under reduced pressure such as in vacuum, but is preferably carried out in an inert gas atmosphere such as helium or argon.

[0078] This makes it possible to more effectively prevent thiourea from being excessively removed from the system due to sublimation, while more effectively preventing undesirable reactions from producing components other than metal sulfides and compounds composed of C and N that satisfy specified conditions.

[0079] The heating temperature in this step varies depending on the type of metal material, the state in which the metal material and thiourea coexist, etc., but is preferably from 250°C to 800°C, more preferably from 300°C to 750°C, and even more preferably from 350°C to 700°C.

[0080] This makes it possible to effectively prevent unintended deformation of the metal material serving as the base material (workpiece) and to more suitably proceed with the desired reaction.

[0081] Furthermore, the heating time in this step (particularly the total heating time at 350°C or higher) is preferably from 10 minutes to 1200 minutes, more preferably from 30 minutes to 900 minutes, and even more preferably from 60 minutes to 600 minutes.

[0082] This allows the target reaction to proceed more smoothly and the productivity of the catalyst to be improved. However, when performing heat treatments multiple times as described above, it is preferable that the total heating time of these heat treatments satisfies the above condition.

[0083] In this step, for example, the treatment may be performed at different temperatures. More specifically, after maintaining at a first heating temperature for a predetermined time, the temperature may be changed to a second temperature different from the first temperature and maintained for a further predetermined time.

[0084] In this step, it is preferable to use an excess amount of thiourea. Specifically, the amount of thiourea used relative to the metal material to be sulfurized is, in mass ratio, preferably 10 times or more, more preferably 20 times or more, and even more preferably 30 times or more. When the heat treatment is carried out multiple times, it is preferable that the total amount of thiourea used in these heat treatments satisfies the above condition.

[0085] In this step, the heat treatment may be carried out by any means, and for example, it can be suitably carried out using various electric furnaces. Among them, it is preferable to carry out the heat treatment using a tubular furnace.

[0086] This makes it easy to control the temperature in the heat treatment process, and makes it possible to achieve excellent temperature uniformity at each location in the furnace. In addition, it is easy to adjust the atmosphere in the heat treatment process. As a result, it is possible to more appropriately manage the production conditions for the catalyst, and to more stably produce a high-quality catalyst.

[0087] In addition, this step may be performed, for example, in a state in which a part of the surface of the metal material as the base material (workpiece) is prevented from contacting with thiourea. More specifically, for example, this step may be performed in a state in which a part of the surface of the metal material is covered with a mask.

[0088] This allows the above-mentioned reaction to proceed selectively in areas of the surface of the metal material as the base material (workpiece) where contact with thiourea is not inhibited (e.g., areas not covered with a mask), and allows the catalyst to be suitably manufactured with the metal material partially exposed on the surface. As a result, for example, the catalyst can be more suitably energized. Also, for example, the catalyst can be more suitably bonded to other conductive members (e.g., terminals, wiring, etc.).

[0089] The material constituting the mask is not particularly limited as long as it has the function of preventing contact between the metal material and thiourea in the areas covered by the mask, but it is preferable that the material be easily removable after the heat treatment step. Examples of such materials include various resin materials.

[0090] [3] Electrode Next, the electrode of the present invention will be described.

[0091] The electrode of the present invention is characterized by containing the above-mentioned catalyst of the present invention. That is, the electrode of the present invention includes a catalyst constituted of a material containing a metal sulfide and a compound consisting of C and N that satisfies the above-mentioned predetermined conditions. This makes it possible to provide an electrode containing a catalyst having high catalytic activity.

[0092] The electrode of the present invention may contain the above-mentioned catalyst of the present invention, and may contain other components. In other words, the above-mentioned catalyst of the present invention may be used alone as the electrode of the present invention, or may be used in combination with other materials as the electrode of the present invention.

[0093] The electrode of the present invention may have a portion mainly containing the catalyst of the present invention described above and a portion mainly containing components other than the catalyst of the present invention. More specifically, for example, the electrode of the present invention may have, in addition to the portion mainly containing the catalyst of the present invention described above, a portion mainly made of a metal material or a conductive carbon-based material such as graphite bonded to the catalyst of the present invention.

[0094] However, in the electrode of the present invention, it is preferable that at least a part of the catalyst of the present invention is exposed on the surface thereof. This allows the effects of the present invention to be more suitably exhibited as described above.

[0095] The electrode of the present invention may be used in any application as long as the function of the catalyst of the present invention is exhibited by passing an electric current through it. Examples of the application of the electrode of the present invention include an electrode for water electrolysis, an electrode for oxygen generation catalyst, an electrode for carbon dioxide decomposition, an electrode for carbon monoxide generation, and an electrode for ammonia generation.

[0096] When the electrode of the present invention is used as an electrode for water electrolysis, by using it as an anode, it can be suitably used in a reaction for electrochemically producing oxygen from water, for example, in the fields of energy conversion, hydrogen generation, etc. In this way, when the electrode of the present invention is used as an anode for water electrolysis, the electrode can also be said to be a catalytic electrode for oxygen generation.

[0097] Furthermore, when the electrode of the present invention is used as an electrode for water electrolysis, by using it as a cathode, it can be suitably used in a reaction for electrochemically producing hydrogen from water, for example, in the fields of energy conversion, hydrogen generation, etc. In this way, when the electrode of the present invention is used as a cathode for water electrolysis, the electrode can also be said to be a catalytic electrode for hydrogen generation.

[0098] The electrode of the present invention may be used as a catalytic electrode for oxygen generation in a form other than that of an electrode for water electrolysis.

[0099] The electrode of the present invention can be suitably produced by applying the above-mentioned method for producing the catalyst of the present invention. That is, the electrode of the present invention can be suitably produced by using a method having a heat treatment step in which a metal material and thiourea are heat-treated in the coexistence of each other.

[0100] The member obtained by the heat treatment process may be used as it is as the electrode of the present invention, or the member obtained by the heat treatment process may be subjected to post-treatment. For example, the method may include a step of exposing the unreacted metal material by removing a part of the region formed on the surface of the member obtained by the heat treatment process and composed of a material containing a metal sulfide and a compound consisting of C and N that satisfies the above-mentioned predetermined conditions. This allows the external wiring to be suitably connected to the metal material, and the electrical conductivity to the electrode of the present invention can be more suitably ensured.

[0101] Methods for removing a part of the region formed of a material containing metal sulfide and a compound consisting of C and N that satisfies the above-mentioned predetermined conditions on the surface of the member obtained by the heat treatment process include, for example, cutting, grinding, polishing, etc. Examples of polishing include mechanical polishing, chemical polishing, chemical mechanical polishing, etc.

[0102] Furthermore, prior to the heat treatment step, a part of the surface of the metallic material may be masked with a non-metallic material, and the mask may be removed after the heat treatment step, whereby the unreacted metallic material can be suitably exposed on a part of the surface of the member obtained by the heat treatment step, and external wiring can be suitably connected to the metallic material, thereby more suitably ensuring electrical conductivity to the electrode of the present invention.

[0103] [4] Water electrolysis method Next, the water electrolysis method of the present invention will be described.

[0104] The water electrolysis method of the present invention is characterized in that water is electrolyzed using the above-mentioned electrode of the present invention. This makes it possible to provide a water electrolysis method capable of efficiently electrolyzing water.

[0105] In the water electrolysis method of the present invention, the electrode of the present invention may be used as either a cathode or an anode.

[0106] By using the electrode of the present invention as a cathode, as described above, the electrode of the present invention functions as a catalytic electrode for hydrogen generation, and by using the electrode of the present invention as an anode, as described above, the electrode of the present invention functions as a catalytic electrode for oxygen generation.

[0107] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.

[0108] For example, the method for producing a catalyst of the present invention may include steps other than the steps described above (for example, a pretreatment step, an intermediate treatment step, a posttreatment step, etc.).

[0109] More specifically, for example, a washing step of washing the obtained product may be included after the heat treatment step.

[0110] Furthermore, after the heat treatment step, a grinding / disintegration step of grinding or disintegrating the obtained product may be included.

[0111] This makes it possible to more suitably obtain a powdered catalyst. Furthermore, by appropriately adjusting the pulverization and crushing conditions, the particle size and other properties of the obtained catalyst powder can be adjusted.

[0112] When both the washing step and the pulverization / disintegration step are performed, the order is not particularly limited, and the washing step may be performed after the pulverization / disintegration step, or the pulverization / disintegration step may be performed after the washing step. In addition, the washing step and the pulverization / disintegration step may be performed simultaneously, for example, by employing a wet pulverization method.

[0113] Furthermore, after the heat treatment step, the resulting product may be subjected to mechanical processing such as cutting and polishing.

[0114] Furthermore, for example, the catalyst of the present invention may be made of a material containing a metal sulfide and a compound consisting of C and N that satisfies certain conditions, and may be manufactured by a method other than the method described above.

[0115] Furthermore, the electrode of the present invention may be made of a material containing the catalyst of the present invention, and may be manufactured by a method other than the above-mentioned method. EXAMPLES

[0116] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Note that the treatments and measurements not specifically indicated as temperature conditions were carried out at 20°C.

[0117] [5] Catalyst production Example 1 First, we prepared NI-318161 (pure metal nickel porous body, 1.6 x 100 x 110 mm) manufactured by Nilaco Corporation, which is made of metallic Ni, and cut five sheet-like test pieces (metallic material as workpieces) measuring 1 cm x 2 cm from it.

[0118] Next, the test piece was buried in 4 g of powdered thiourea, and in this state, the temperature was raised from room temperature to 450°C over a period of 5 hours in a nitrogen gas atmosphere using a tubular electric furnace (manufactured by AS ONE Corporation, programmable tubular electric furnace TMF-700N), and the temperature was held at 450°C for 1 hour (heat treatment process), and then the test piece was naturally cooled.

[0119] Thereafter, the same amount of thiourea was replenished and the same heat treatment as above was repeated two more times. The total heating time at 350° C. or higher was 600 minutes. This gave a catalyst.

[0120] Example 2 A catalyst was produced in the same manner as in Example 1, except that the number of heat treatments in the heat treatment step was changed to two.

[0121] Example 3 A catalyst was produced in the same manner as in Example 1, except that the number of heat treatments in the heat treatment step was changed to four.

[0122] Example 4 A catalyst was produced in the same manner as in Example 1, except that the heating temperature (maximum temperature) in the heat treatment step was changed to 400°C.

[0123] Example 5 A catalyst was produced in the same manner as in Example 1, except that the heating temperature (maximum temperature) in the heat treatment step was changed to 700°C.

[0124] Moreover, each of the above-mentioned Examples had a portion constituted of Ni as a metal material in addition to metal sulfide and β-C3N4.

[0125] Comparative Example 1 A sheet-like test piece measuring 1 cm x 2 cm was cut out from NI-318161 (pure metal nickel porous body, 1.6 x 100 x 110 mm) manufactured by Nilaco Corporation used in Example 1 in the same manner as described above, and the test piece was used as it is as a catalyst without being subjected to heat treatment.

[0126] Comparative Example 2 First, a sheet-like test piece measuring 1 cm×2 cm was cut out from NI-318161 (pure metal nickel porous body, 1.6×100×110 mm) manufactured by Nilaco Corporation used in Example 1 in the same manner as described above.

[0127] On the other hand, hexachloroiridic acid (H2[IrCl6]) was added to a beaker containing 0.1M sodium hydroxide solution, and the mixture was stirred to hydrolyze H2[IrCl6]. Note that the amount of sodium hydroxide solution was 50 equivalents of NaOH to Ir.

[0128] Thereafter, a solution containing the reaction mixture obtained by the hydrolysis was applied to the test piece by dipping.

[0129] Next, the test piece was heated at 80°C to remove the solvent from the solution applied to the test piece, and then heat-treated in air at 350°C for 60 minutes, followed by natural cooling to obtain a catalyst in which an iridium oxide film was provided on the surface of a nickel substrate. The rate of temperature rise to the maximum temperature was 5°C / min.

[0130] Comparative Example 3 A catalyst was produced in the same manner as in Example 1, except that urea powder was used instead of thiourea powder, thereby obtaining a catalyst in which β-C3N4 was formed on the substrate.

[0131] Comparative Example 4 First, a sheet-like test piece measuring 1 cm×2 cm was cut out from NI-318161 (pure metal nickel porous body, 1.6×100×110 mm) manufactured by Nilaco Corporation used in Example 1 in the same manner as described above.

[0132] Next, a 1M aqueous solution of thiourea was applied to the test piece by dipping. The test piece was then heated at 80°C to remove the solvent from the solution applied to the test piece, and then heated from room temperature to 450°C over a period of 5 hours in a nitrogen gas atmosphere using a tubular electric furnace (TMF-700N, programmable tubular electric furnace, manufactured by AS ONE Corporation), and held at 450°C for 1 hour. Thereafter, the test piece was naturally cooled to obtain a catalyst.

[0133] Comparative Example 5 A catalyst was produced in the same manner as in Comparative Example 4, except that the test piece was dipped into the 1M aqueous solution of thiourea four times.

[0134] Comparative Example 6 A catalyst was produced in the same manner as in Comparative Example 5, except that a 3 M aqueous solution of thiourea was used instead of the 1 M aqueous solution of thiourea.

[0135] The catalysts obtained in the above-mentioned Examples and Comparative Examples were analyzed by X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS) and energy dispersive X-ray analysis (EDS).

[0136] As a result, it was confirmed that the catalysts of each of the above examples were composed of materials containing NiS and Ni3S2 as metal sulfides and β-C3N4, whereas in each of the comparative examples, the coexistence of metal sulfides and β-C3N4 was not confirmed.

[0137] The catalysts obtained in each of the examples and comparative examples were observed with a scanning electron microscope (SEM), and it was confirmed that the gaps (mesh) in the network structure of the catalysts in each of the examples were smaller than the porosity of the raw material nickel. This is believed to be due to the sulfurization reaction of the metallic material Ni, which produced metal sulfides and expanded the catalyst. In addition, the catalysts in each of the examples had fibrous and cotton-like substances attached to the surface. It was confirmed that this was β-C3N4 attached to the surface of the nickel sulfide.

[0138] FIG. 1 shows the X-ray diffraction (XRD) pattern of the catalyst obtained in Example 2 and the X-ray diffraction (XRD) patterns of the porous nickel as a raw material, NiS and Ni3S2 as metal sulfides, and β-C3N4. FIG. 2 shows an SEM (scanning electron microscope) photograph of the catalyst obtained in Example 2. FIG. 3 shows an SEM (scanning electron microscope) photograph of the porous nickel (corresponding to the sample of Comparative Example 1) used in the production of the catalyst of Example 2. FIG. 4 shows the X-ray diffraction (XRD) patterns of the catalysts obtained in Comparative Examples 4 to 6. FIG. 7 shows a TEM (transmission electron microscope) photograph of the fine part generated on the surface of the catalyst obtained in Example 2. From a comparison of FIG. 2 and FIG. 7 with FIG. 3, it was confirmed that in the catalyst obtained in Example 2, β-C3N4 was attached to the surface of the nickel sulfide, and in particular, the surface of the metal sulfide was covered with β-C3N4 in a sheath shape. In addition, although not shown, it was confirmed that the catalysts obtained in other Examples also had the same configuration. In FIG. 1, the nickel porosity is indicated by "NF."

[0139] [6] Evaluation [6-1] High catalytic activity (overvoltage required to generate oxygen) A water electrolysis device was manufactured using the catalyst obtained in each of the Examples and Comparative Examples as an oxygen generating anode and a platinum wire as a hydrogen generating cathode.

[0140] Using this water electrolysis device, a current of 10 mA / cm2 was applied to a 1M potassium hydroxide aqueous solution. 2 Water was electrolyzed by passing a current at a current density of 1000 kcal / s for 5 hours, and the change in the overvoltage required for oxygen generation at the oxygen generating anode with time was measured.

[0141] As a result, in the present invention, the overvoltage required for oxygen generation was 50 mV or less in all cases, whereas in the comparative examples, the overvoltage required for oxygen generation was 220 mV or more in all cases.

[0142] FIG. 5 shows the change over time in the overvoltage required for oxygen production when water is electrolyzed under the above-mentioned conditions for the catalysts obtained in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3.

[0143] [6-2] Catalyst durability The catalyst (oxygen generating anode) according to each of the above examples used in the manufacture of the water electrolysis device in [6-1] above was analyzed by X-ray diffraction (XRD) after 6 hours of electrolysis, and the X-ray diffraction (XRD) patterns before and after the electrolysis of water were compared. As a result, in each of the examples, the X-ray diffraction (XRD) patterns before and after the electrolysis of water were substantially not observed. This shows that the catalyst of the present invention is not easily deteriorated by the electrolysis of water.

[0144] The X-ray diffraction (XRD) patterns of the catalyst of Example 2 before and after water electrolysis are shown in FIG.

[0145] In addition, catalysts were produced in the same manner as in the above-mentioned Examples, except that instead of Ni, the metal material used as the workpiece was Cu, Ti, Ag, or stainless steel (SUS316L). As a result, catalysts composed of materials containing metal sulfide and β-C3N4 were obtained in the same manner as in the above-mentioned Examples. It was confirmed that these catalysts have sufficiently high catalytic function compared to materials composed of materials not containing at least one of metal sulfide and β-C3N4.

[0146] In addition, catalysts were produced in the same manner as in the above-mentioned Examples, except that a dense body was used instead of a porous body as the metal material used as the workpiece, and catalysts composed of a material containing metal sulfide and β-C3N4 were obtained in the same manner as described above. These catalysts were confirmed to have sufficiently high catalytic function compared to materials composed of materials not containing at least one of metal sulfide and β-C3N4, but their catalytic function was lower than that of those produced using a porous body.

[0147] In addition, a catalyst was produced in the same manner as in each of the above-mentioned Examples, except that a part of the metal material as the workpiece was covered with a resin mask and the heat treatment process was performed. As a result, a catalyst composed of a material containing metal sulfide and β-C3N4 was obtained as described above, but the part covered with the mask did not contain metal sulfide or β-C3N4. It was confirmed that these catalysts have sufficiently high catalytic function compared to materials composed of materials not containing at least one of metal sulfide and β-C3N4.

[0148] Furthermore, a catalyst was produced in the same manner as in each of the above Examples, except that the electrolysis time was changed from 6 hours to 7 hours, and the same results as above were obtained. [Industrial Applicability]

[0149] The catalyst of the present invention is composed of a material containing a metal sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays. The catalyst of the present invention is also composed of a material containing a metal sulfide and β-C3N4. This makes it possible to provide a catalyst having high catalytic activity.

[0150] The electrode of the present invention contains the catalyst of the present invention, thereby making it possible to provide an electrode containing a catalyst having high catalytic activity.

[0151] Furthermore, the water electrolysis method of the present invention uses the electrode of the present invention to electrolyze water, thereby making it possible to provide a water electrolysis method capable of efficiently electrolyzing water.

[0152] The method for producing a catalyst of the present invention includes a step of performing a heat treatment in a state where a metal material and thiourea are coexisting, and obtains a catalyst composed of a material containing a metal sulfide and a compound consisting of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-ray. The method for producing a catalyst of the present invention includes a step of performing a heat treatment in a state where a metal material and thiourea are coexisting, and obtains a catalyst composed of a material containing a metal sulfide and β-C3N4. This makes it possible to provide a method for producing a catalyst that can suitably produce a catalyst having high catalytic activity.

[0153] Therefore, the catalyst, electrode, water electrolysis method, and catalyst production method of the present invention have industrial applicability.

Claims

1. A catalyst for use in the electrolysis of water, comprising: The compound includes a metal sulfide and a compound of C and N that shows diffraction peaks at 2θ = (16.0 ± 0.5) ° and 2θ = (27.8 ± 0.5) ° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as a measuring X-ray, A catalyst characterized in that in the catalyst, the compound consisting of C and N coats the metal sulfide in a sheath-like form.

2. A catalyst for use in the electrolysis of water, comprising: Metal sulfide and β-C 3 N 4 and In the catalyst, the β-C 3 N 4 The catalyst is characterized in that the metal sulfide is coated in a sheath shape.

3. 3. The catalyst according to claim 1, wherein the metal sulfide comprises nickel sulfide.

4. The nickel sulfide includes NiS and Ni 3 S 2 The catalyst according to claim 3, comprising:

5. A catalyst for use in the electrolysis of water, comprising: The material is made of nickel sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as measuring X-rays, The nickel sulfide includes NiS and Ni 3 S 2 A catalyst comprising:

6. 6. The catalyst according to claim 5, wherein the compound consisting of C and N is contained in the catalyst in a form attached to the surface of the nickel sulfide.

7. A catalyst for use in the electrolysis of water, comprising: Nickel sulfide and β-C 3 N 4 and The nickel sulfide includes NiS and Ni 3 S 2 A catalyst comprising:

8. In the catalyst, the β-C 3 N 4 The catalyst according to claim 7, wherein said metal sulfide is contained in a form adhered to a surface of said metal sulfide.

9. 10mA / cm 2 9. The catalyst according to claim 1, wherein the overvoltage required for oxygen production at a current density of 150 mV or less.

10. 10. An electrode for water electrolysis comprising the catalyst according to claim 1.

11. The electrode according to claim 10, wherein the electrode is a catalytic electrode for oxygen evolution.

12. A method for electrolyzing water, comprising electrolyzing water using the electrode according to claim 10 or 11.

13. A method for producing a catalyst for use in the electrolysis of water, comprising the steps of: The method includes a step of performing a heat treatment in a state where a metal material and thiourea are present together, A method for producing a catalyst, comprising obtaining a catalyst composed of a material containing a metal sulfide and a compound of C and N that shows diffraction peaks at 2θ=(16.0±0.5)° and 2θ=(27.8±0.5)° in an X-ray diffraction pattern obtained by an X-ray diffraction method using Cu Kα rays as the measuring X-rays.

14. A method for producing a catalyst for use in the electrolysis of water, comprising the steps of: The method includes a step of performing a heat treatment in a state where a metal material and thiourea are present together, Metal sulfide and β-C 3 N 4 A method for producing a catalyst, comprising obtaining a catalyst composed of a material comprising:

15. The method for producing a catalyst according to claim 13 or 14, wherein a heat treatment is carried out in a state where the metal material and the thiourea are in contact with each other.

16. 16. The method for producing a catalyst according to claim 13, wherein the metal material is subjected to a heat treatment in a state where the metal material is embedded in the thiourea powder.

17. The method for producing a catalyst according to claim 15 or 16, wherein the heat treatment is carried out multiple times.

18. The method for producing a catalyst according to any one of claims 13 to 17, wherein the metal material is nickel.

19. The method for producing a catalyst according to any one of claims 13 to 18, wherein the heat treatment is carried out using a tubular furnace.

Citation Information

Patent Citations

  • NiS / C3N4 binary compound and preparation method and application method thereof

    CN107892284A

  • Composite, a method of making thereof, and a method for degrading a pollutant

    US20180305231A1

  • Gas generator and method for generating gas

    WO2011030546A1