Oxygen absorber, oxygen absorber package, and food package
The granular oxygen absorber with inorganic fine particles and a specific composition enhances oxygen absorption capacity, addressing the slow rate of organic scavengers and ensuring effective mold prevention in food packaging.
Patent Information
- Application Number
- JP2020090560
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-25
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-05-25
AI Technical Summary
Existing organic oxygen scavengers have a slower oxygen absorption rate than iron-based scavengers, making it difficult to maintain an oxygen concentration below 0.1% within 24 hours to prevent mold growth, and existing enhancements like reaction catalysts and pH adjustment are insufficient.
A granular oxygen absorber with inorganic fine particles attached to a porous carrier containing an oxygen-absorbing composition, including an alkaline compound and transition metal compound, with specific hydrophobicity and pH levels, is used to enhance oxygen absorption capacity.
The granular oxygen absorber achieves a higher and sustained oxygen absorption rate, meeting the requirement of less than 0.1% oxygen concentration within 24 hours, suitable for food preservation and metal detector compatibility.
Smart Images

Figure 0007571393000002 
Figure 0007571393000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to an oxygen absorber and an oxygen absorber package, and also to a food package having the oxygen absorber package. [Background technology]
[0002] One method for long-term food preservation is to enclose an oxygen absorber in the food packaging. In this method, the food and the oxygen absorber are enclosed in a gas-barrier sealed bag or container, and the oxygen in the sealed container is absorbed by the oxygen absorber, maintaining a substantially oxygen-free atmosphere inside the sealed container, thereby suppressing quality deterioration due to oxidation and the growth of bacteria and microorganisms.
[0003] There are two main types of oxygen absorbers currently in common use: inorganic oxygen absorbers that use iron as the main ingredient, and organic oxygen absorbers that use ascorbic acid-based oxygen absorbing substances as the main ingredient. These are used depending on the purpose and the food they are intended for, but in recent years, there has been an increasing need to pass products through metal detectors, so there is a growing demand for organic oxygen absorbers that can be passed through metal detectors.
[0004] Organic oxygen absorbers have the disadvantage of absorbing oxygen more slowly than iron-based oxygen absorbers. When using oxygen absorbers to improve the shelf life of food, it is desirable to reduce the oxygen concentration to less than 0.1% within 24 hours in order to prevent the growth of mold, which grows in as little as 24 to 48 hours. However, it is not easy to meet this requirement with organic oxygen absorbers. Therefore, in order to increase the oxygen absorption rate in organic oxygen absorbers, it has been proposed to add a reaction catalyst or a reaction promoter that promotes the oxidation reaction of the oxygen absorbing substance, or to add an alkaline compound to achieve an optimal pH (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3541859 Summary of the Invention [Problem to be solved by the invention]
[0006] Based on the above prior art, the inventors have succeeded in increasing the oxygen absorption capacity by a different approach.
[0007] An object of the present invention is to further improve the oxygen absorption capacity of a granular oxygen absorber. [Means for solving the problem]
[0008] A first aspect of the present invention is an oxygen scavenger in which inorganic fine particles are attached to the surface of a granulated product containing a porous support and an oxygen absorbing composition supported on the support. The oxygen absorbing composition includes a liquid agent containing an oxygen absorbing material, an alkaline compound, and a transition metal compound. The inorganic fine particles have a hydrophobicity of 15% or less. The pH of inorganic particles is 8.0 or higher It is 9.0 or less.
[0009] A second aspect of the present invention is an oxygen absorber package in which the oxygen absorber according to the first aspect is housed in a breathable packaging material. A third aspect of the present invention is a food package comprising the oxygen absorber package according to the second aspect and a packaging container in which the oxygen absorber package and food are sealed. [Effects of the Invention]
[0010] According to the present invention, the oxygen absorbing capacity of the granular oxygen absorber can be further improved. [Brief explanation of the drawings]
[0011] [Figure 1] 1 is a diagram showing an oxygen absorber package according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0012] Hereinafter, one embodiment of the present invention will be described with reference to FIG. 1 is a diagram showing an oxygen absorber package 1 according to this embodiment. The oxygen absorber package 1 includes a breathable packaging material 10 and an oxygen absorber 20 housed in the packaging material 10.
[0013] The oxygen absorber 20 contains a porous support and a powder or granule containing an oxygen absorbing composition supported on the support, or a granulation thereof, and a plurality of composite particles mainly composed of inorganic fine particles attached to the surface of the granule. Note that the powder or granule here means an aggregate composed of a large number of fine particles that maintains fluidity as a whole, and does not include a single solid tablet formed by the fine particles adhering to each other as a whole. The number of composite particles contained in the oxygen absorber 20 may be, for example, 10 to 10,000 per 1 g of the oxygen absorber 20.
[0014] The mass of each composite particle constituting the granulated product of the oxygen absorber 20 may be 0.3 mg or more, or 0.5 mg or more, and may be 10.0 mg or less, or 7.0 mg or less per composite particle. When the composite particles are this small, a higher oxygen absorption capacity tends to be obtained.
[0015] The support may be any porous particle capable of supporting the oxygen absorbing composition. Usually, the oxygen absorbing composition is impregnated into the support, thereby supporting the oxygen absorbing material on the support. As the support, for example, one or more types selected from activated carbon, zeolite particles, bentonite particles, activated alumina particles, activated clay, calcium silicate particles, and diatomaceous earth can be used.
[0016] The oxygen absorbing composition contains a liquid agent containing an oxygen absorbing substance, an alkaline compound, and a transition metal compound. By preparing such an oxygen absorbing composition, a sufficient oxygen absorption rate can be obtained.
[0017] The liquid agent containing an oxygen absorbing substance may be an oxygen absorbing substance that is liquid at room temperature (5 to 35°C), or may be a solution containing a liquid or solid oxygen absorbing substance. The oxygen absorbing substance is the main component of the oxygen absorbing composition and is a substance that absorbs oxygen. Organic oxygen absorbing substances are generally compounds that consume and absorb oxygen by oxidizing themselves.
[0018] In this embodiment, an oxygen-absorbing substance that is liquid at room temperature or dissolved in a solvent can be used. Examples of such oxygen-absorbing substances include one or more compounds selected from the group consisting of ascorbic acid, erythorbic acid, glycerin, 1,2-glycols, and sugar alcohols. Specific examples of 1,2-glycols include ethylene glycol and propylene glycol, and specific examples of sugar alcohols include erythritol, arabitol, xylitol, adonitol, mannitol, and sorbitol. When the liquid preparation is a solution of an oxygen absorbing substance, examples of the solvent in which the oxygen absorbing substance dissolves include water; lower aliphatic alcohols such as methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, secondary butanol, tertiary butanol, and tertiary amyl alcohol; and glycols such as ethylene glycol, propylene glycol, and trimethylene glycol. The oxygen absorbing substance can be any of the above-mentioned compounds used alone or in combination. By incorporating an oxygen absorbing substance into the liquid preparation, dispersibility with the carrier and alkaline compound is improved, making it easier to achieve oxygen absorption performance.
[0019] When the oxygen-absorbing substance itself is liquid at room temperature, water can be added to the liquid formulation as needed. The amount of water added as needed is usually 0 to 80 parts by mass, or may be 20 to 60 parts by mass, relative to 100 parts by mass of the oxygen-absorbing substance. The amount of water is usually 0 to 90 parts by mass, or may be 20 to 70 parts by mass, relative to 100 parts by mass of the support.
[0020] The amount of the oxygen absorbing substance is usually 80 to 200 parts by mass, or may be 100 to 180 parts by mass, per 100 parts by mass of the support. When the amount of the oxygen absorbing substance is within this range, it tends to be easier to obtain an oxygen scavenger with appropriate oxygen absorption capacity.
[0021] An alkaline compound is a compound that forms an alkaline aqueous solution when dissolved in water. When the oxygen absorbing substance has a hydroxyl group, the alkaline compound ionizes the hydroxyl group, activating the oxygen absorption reaction. In the state of the oxygen absorbing composition, a portion of the alkaline compound is often dissolved in the liquid containing the oxygen absorbing substance. The alkaline compound can be a hydroxide, carbonate, bicarbonate, triphosphate, diphosphate, etc. of an alkali metal or alkaline earth metal. Specific examples of the alkaline compound include one or more compounds selected from the group consisting of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, beryllium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, radium hydroxide, lithium carbonate, sodium carbonate, calcium carbonate, magnesium carbonate, potassium carbonate, potassium bicarbonate, sodium bicarbonate, lithium bicarbonate, trisodium phosphate, trisodium potassium phosphate, dibasic sodium phosphate, and dibasic potassium phosphate. Among these, calcium hydroxide is particularly preferred. This is because calcium hydroxide forms a soluble complex with glycerin, which facilitates the promotion of the oxidation reaction.
[0022] The amount of the alkaline compound is usually 90 to 300 parts by mass, or may be 150 to 250 parts by mass, per 100 parts by mass of the support. When the amount of the alkaline compound is within this range, it tends to be easier to obtain an oxygen scavenger with appropriate oxygen absorption capacity.
[0023] The transition metal compound is a compound containing a transition metal element and is added to promote the oxygen absorption reaction of the oxygen absorbing substance. In the state of the oxygen absorbing composition, the transition metal compound is often dissolved in a liquid containing the oxygen absorbing substance. Specific examples of the transition metal element include iron, cobalt, nickel, copper, zinc, and manganese. The transition metal compound may be, for example, a transition metal halide, sulfate, nitrate, phosphate, carbonate, organic acid salt, oxide, hydroxide, or chelate compound. The transition metal compound may also be a double salt containing a transition metal element. The transition metal compound may be one or more compounds selected from the group consisting of copper(I) chloride, copper(II) chloride, copper(II) sulfate, copper(II) hydroxide, copper(I) oxide, copper(II) oxide, manganese chloride, manganese nitrate, manganese carbonate, and nickel chloride.
[0024] The amount of the transition metal compound is usually 10 to 70 parts by mass, or may be 30 to 50 parts by mass, per 100 parts by mass of the support. When the amount of the transition metal compound is within this range, it tends to be easier to obtain an oxygen scavenger with appropriate oxygen absorption capacity.
[0025] The oxygen-absorbing composition may further contain a binder to facilitate the formation of granules. Specific examples of binders include gum arabic, polyvinyl alcohol, sodium alginate, gelatin, and cellulose. The amount of the binder is usually 0 to 30 parts by mass, and may be 10 to 20 parts by mass, relative to 100 parts by mass of the support.
[0026] The particle size (maximum width) of the granulated material before the inorganic fine particles are attached is not particularly limited, and may be, for example, 0.3 mm or more, 8.0 mm or less, 4.5 mm or less, 1.8 mm or less, or 1.5 mm or less. The shape of the granulated material is not particularly limited, and may be, for example, cylindrical. In the case of cylindrical granulated material, the diameter may be 0.3 mm or more, and 4.5 mm or less. The height of the cylindrical granulated material may be 0.3 mm or more, 1.8 mm or less, or 1.5 mm or less. A smaller particle size or diameter of the granulated material tends to result in a higher oxygen absorption capacity.
[0027] A granulated product comprising a support and an oxygen-absorbing composition can be obtained by granulating a mixture containing the support and the components constituting the oxygen-absorbing composition. The components constituting the oxygen-absorbing composition may be mixed together or separately. The mixer used for mixing is not particularly limited, and may be, for example, a rotating container mixer such as a cylindrical type or V-type, or a fixed container mixer such as a ribbon type, horizontal screw type, paddle type, or planetary motion type.
[0028] The granules can be obtained by granulation, for example, by extrusion granulation, stirring granulation, fluidized bed granulation, rolling granulation, or compression granulation. Extrusion granulation can be carried out, for example, using a screen with predetermined openings. Granules obtained by extrusion granulation are often cylindrical.
[0029] The inorganic fine particles generally contain 50% by mass or more of inorganic substances based on the total mass of the particles, and examples of the inorganic substances include silicon dioxide, calcium silicate hydrate, magnesium oxide, and magnesium silicate.
[0030] There are no particular limitations on the average particle size of the inorganic fine particles, and they may be 0.1 to 100 μm, which is the general definition of fine particles. The surface of the granulated product usually has minute irregularities, and inorganic fine particles with small particle sizes tend to penetrate into the recesses on the surface of the granulated product. This results in a significant increase in the surface area of the granulated product, which is thought to contribute to improving the oxygen absorption capacity.
[0031] The inorganic fine particles exemplified above can be produced by a conventional method, or can be obtained by appropriately selecting from commercially available products.
[0032] The amount of inorganic fine particles adhering to the surface of the granulated product (adhesion amount) is preferably 1 part by mass or more per 100 parts by mass of the granulated product. When the amount of inorganic fine particles is within this range, the oxygen absorbing ability of the oxygen scavenger is likely to be appropriate. There is no particular upper limit to the amount of inorganic fine particles adhering to the surface of the granulated product, but from the viewpoints of adhesion to the surface and cost, it is preferably 15 parts by mass or less. Note that, although independent inorganic fine particles not adhering to the granulated product may be mixed with the particles of the oxygen scavenger, the amount of independent inorganic fine particles is not included in the above-mentioned adhesion amount.
[0033] The method for adhering inorganic fine particles to the surface of the granulated material is not particularly limited, but an example thereof is a method of mixing a granulated material powder containing a plurality of granulated materials each containing a support and an oxygen absorbing composition with a plurality of inorganic fine particles. For example, the granulated material and the inorganic fine particles are mixed, and the resulting mixture is shaken, thereby allowing the inorganic fine particles to adhere to the granulated material.
[0034] The inorganic fine particles adhered to the granulated material by the above-described powder-mixing method form a relatively thin layer on the surface of the granulated material. In this respect, the form of the oxygen absorber 20 of this embodiment differs from, for example, a tablet having an outer shell obtained by tableting. Specifically, the inorganic fine particles adhered to the surface of the granulated material can form a layer with a thickness of 1 mm or less. The thin layer of inorganic fine particles can also be confirmed by detecting elements contained in the materials constituting the granulated material (oxygen absorbing substances, alkaline compounds, or transition metal compounds) when the surface of the composite particles is subjected to elemental analysis by energy dispersive X-ray analysis (EDX analysis). Generally, in the case of the oxygen absorber 20 of this embodiment, at least one element contained in the materials constituting the granulated material is often detected at a concentration of 0.05 atomic percent (at%) or more, or 0.1 at% or more, in surface EDX analysis. On the other hand, when an outer shell of a certain thickness enclosing the granulated material is formed by tableting, elements of the materials constituting the granulated material are rarely detected in surface EDX analysis. It is not necessary that the surface of the granules is completely covered with inorganic fine particles, and the inorganic fine particles may be distributed over the entire surface of the granules with spaces between them.
[0035] In the oxygen absorber 20 of this embodiment, when the oxygen absorbing composition that has migrated to the inorganic fine particles reacts with the atmosphere, the oxygen absorbing composition contained inside the granules gradually migrates to the surface layer of the granules (sustained release effect), so that the oxygen absorbing performance is equivalent to that when used as a powder. As a result, high oxygen absorbing performance is maintained for a long period of time. The inventors have conducted extensive research into the conditions under which the above-mentioned effects of inorganic fine particles are optimally exhibited. As a result, they have found that the hydrophobicity of the inorganic fine particles is closely related to the above-mentioned effects. Specifically, they have found that a hydrophobicity of 15% or less makes it easier to obtain high oxygen absorption performance. For example, when the inorganic fine particles are silicon dioxide, the hydrophobicity can be changed by controlling the density of silanol groups, which are hydrophilic groups. A specific example of such a method is to bring silicon dioxide powder into contact with a gaseous silylating agent such as alkylhalogenosilane, alkylalkoxysilane, or alkyldisilazane to impart hydrophobicity.
[0036] The mechanism by which the hydrophobicity of the inorganic fine particles modifies the oxygen absorption performance of the oxygen absorber 20 has not been fully elucidated, but is presumed to be as follows. When the hydrophobicity of inorganic fine particles is 15% or less, the inorganic fine particles have a high affinity with the liquid agent contained in the oxygen absorbing composition, so that the inorganic fine particles adhere firmly to the surface of the granules. This allows the oxygen collecting substance to smoothly migrate to the inorganic fine particles. Since the inorganic fine particles have a higher specific surface area than the granules themselves, the contact area between the oxygen absorbing substance and air (oxygen) increases, which is thought to contribute to improving the oxygen absorption capacity of the oxygen absorber.
[0037] The hydrophobicity of inorganic particles can be expressed as an index called the methanol hydrophobicity (M value). The M value is a concept that indicates the degree of hydrophobicity of particles, with a higher M value indicating higher hydrophobicity. The M value refers to the minimum methanol ratio in a mixed solution of water and methanol at which the measurement sample can be uniformly dispersed, and can be determined using the following method. (Measurement of M value) 0.2g of the target particles to be measured is added to 50mL of water in a 150mL beaker, and methanol is slowly added dropwise from a burette. The solution in the beaker is gently stirred with a magnetic stirrer, and the addition is stopped when all of the particles have settled to the bottom of the beaker. The volume percentage of methanol in the water-methanol mixture in the beaker at the end of the addition is taken as the M value.
[0038] Furthermore, the inventors' investigations have revealed that the pH of the inorganic fine particles also contributes to the above-mentioned effect. As will be shown in more detail in the Examples, it has been found that the above-mentioned effect is more reliably exhibited when the pH of the inorganic fine particles is between 4.0 and 9.0. Although the mechanism behind this has not been fully elucidated, it is speculated as follows. Because alkaline compounds are involved in the oxygen absorption reaction, inorganic fine particles with a pH of 5.5 or higher tend to exhibit oxygen absorption performance, with a range of 5.5 to 8.0 being particularly preferable. Within this range, the alkaline compounds act to cause a charge imbalance in the carbon portion of the oxygen absorbing material, making it unstable, making the oxygen absorbing material more susceptible to oxidation, i.e., more likely to bond with oxygen. If the pH of the inorganic fine particles is too high, the alkaline compounds are less likely to act on the oxygen absorbing material, potentially resulting in reduced performance. In view of the above, it is assumed that the oxygen absorption performance of inorganic microparticles will decrease as the pH of the inorganic microparticles becomes more acidic. However, the inventors' investigations have confirmed that generally stable oxygen absorption performance can be obtained within the pH range of approximately 4.0 to 9.0.
[0039] As described above, the oxygen absorber 20 of this embodiment has the following advantages. (1) By making the degree of methanol hydrophobicity of the inorganic fine particles 15% or less, a granular oxygen absorber can be obtained which has an improved oxygen absorption rate and maintains its oxygen absorption capacity for a long period of time. (2) In the oxygen absorber 20, if the pH of the inorganic fine particles is 4.0 or more and 9.0 or less, the above effect can be more reliably obtained. (3) In the oxygen absorber 20, if the amount of inorganic fine particles is 1 to 15 parts by mass per 100 parts by mass of the granulated material, the oxygen absorption rate can be more effectively increased while suppressing the production cost. (4) In the oxygen absorber 20, if the mass of the composite particles is in the range of 0.3 to 10.0 mg per composite particle, the oxygen absorption rate can be increased more effectively.
[0040] The oxygen absorber package 1 of this embodiment is completed when the oxygen absorber 20 is housed in the breathable packaging material 10 and sealed.
[0041] The food package according to this embodiment is obtained by enclosing the oxygen absorber package 1 in a packaging container containing food and sealing it. Because the oxygen absorber 20 is organic, the oxygen absorber package 1 can also be used suitably for foods that undergo quality inspection using a metal detector. In the food package according to this embodiment, the type of packaging container is not particularly limited as long as it can be sealed, and can be appropriately selected from those commonly used in the field of food packaging. Examples of packaging containers include bags, deep-draw packages, tray packages, stretch packages, etc.
[0042] The oxygen scavenger according to this embodiment will be further explained using examples, although the technical scope of the present invention is not limited to the specific contents of these examples.
[0043] (Preparation of oxygen absorber) The following oxygen scavenger materials were mixed uniformly in a sealed state, and the resulting mixture was granulated in an extrusion granulator equipped with a screen with a screen hole diameter of 1.0 mmφ and an opening rate of 22.6% to obtain a granulated product. (oxygen absorber material) ·Activated carbon 100 parts 150 parts glycerin Calcium hydroxide 216.7 parts ·Copper(II) sulfate 45.2 parts ·Wednesday 60.3 parts Cellulose 16.7 parts
[0044] The following inorganic fine particles were prepared, each with a different degree of methanol hydrophobicity (M value) and pH. The material, M value, and pH of each inorganic fine particle are as follows. The M value was measured by the method described above, and the pH was measured according to JIS K 5101-17-2. <Silicon dioxide (SiO2)> Inorganic fine particle AM value 0 pH 7.8 Inorganic fine particle BM value 0 pH 3.6 Inorganic fine particle CM value 15 pH 7.0 Inorganic fine particles DM value 10 pH 7.2 Inorganic fine particles EM value 2 pH 6.2 Inorganic fine particle FM value 0 pH 5.5 Inorganic fine particle GM value 0 pH 6.5 Inorganic fine particles HM value 35 pH 6.5 Inorganic fine particles IM value 60 pH 5.0 <Amorphous calcium silicate hydrate (CaO·mSiO2·nH2O)> Inorganic fine particles JM value 0 pH 9.1 Magnesium silicate (Mg8Si 12 O 30 (OH)4(OH2)4·8H2O> Inorganic fine particle KM value 0 pH 8.7
[0045] 0.9 g of any of the inorganic fine particles described above was placed in an oxygen-barrier bag, after which 30 g of the granules was placed and the bag was heat-sealed. The bag was shaken to thoroughly mix the contents, yielding an oxygen absorber in which the granules were coated with inorganic fine particles. As a result, oxygen absorbers according to Examples 1 to 9 and Comparative Examples 2 and 3 were obtained. The inorganic fine particles used in each example are shown in Table 1. When the surface of this oxygen absorber was analyzed by EDX under conditions of an acceleration voltage of 20 kV and an analysis time of 100 seconds (live time), Cu elements derived from copper sulfate constituting the granulated product were detected at a concentration of 1.06 at %, confirming that the inorganic fine particles were very thinly adhered to the surface of the granulated product. For confirmation, a tablet was prepared having a core made of the same oxygen absorbing composition and an outer shell made of a mixture of calcium silicate and silicon dioxide, and its surface was analyzed by EDX, but no Cu element was detected. The oxygen absorbers of each example prepared were stored in a vacuum state until the time of preparing oxygen absorber packages (described later).
[0046] Example 10 An oxygen scavenger according to Example 10 was obtained in the same manner as in Example 1, except that the amount of inorganic fine particles was changed to 0.3 g. Example 11 An oxygen scavenger according to Example 10 was obtained in the same manner as in Example 1, except that the amount of inorganic fine particles was changed to 3.0 g. Example 12 An oxygen scavenger according to Example 11 was obtained in the same manner as in Example 1, except that the amount of inorganic fine particles was changed to 4.5 g.
[0047] (Comparative Example 1) The granules were used as an oxygen absorber according to Comparative Example 1 without adding inorganic fine particles.
[0048] (Production of oxygen absorber packaging) 2.5 g of the oxygen absorber according to each example was placed in a bag (60 mm long, 60 mm wide) made of breathable packaging material to prepare an oxygen absorber package according to each example. The breathable packaging material used was a laminated material with a layer structure of polyethylene terephthalate / polyethylene / paper / polyethylene.
[0049] (Production of food packaging) Absorbent cotton soaked in 10 mL of 44% sucrose aqueous solution was placed in a bag-shaped packaging container with oxygen barrier properties. The oxygen absorber package according to each example was then placed in the packaging container and sealed under a roughly vacuum. 500 mL of air was then injected into the packaging container using a syringe, and the container was resealed to obtain the food package according to each example. This resulted in a water activity of 0.95 within the packaging container. Water activity refers to the proportion of free water in the water content of a system, and a water activity of 0.95 simulates the condition of high-moisture foods such as cheese, ham, and sausages being stored inside.
[0050] (Oxygen concentration measurement) The food packages of each example were left to stand in an atmosphere at 25° C. After 15 hours and 24 hours, the oxygen concentration inside the packages was measured using a needle-type oxygen concentration meter. The results are shown in Table 1.
[0051] [Table 1]
[0052] As shown in Table 1, each example in which inorganic fine particles with a hydrophobicity of 15% or less were attached to the granulated material exhibited higher oxygen absorption performance than comparison examples 2 and 3 in which inorganic fine particles with a hydrophobicity of 15% or more were attached, and met the condition of "oxygen concentration of less than 0.1% 24 hours after production," which is a guideline for effectively preventing the growth of mold, bacteria, etc. in food packaging. No oxygen absorption performance was obtained in Comparative Example 1, in which no inorganic fine particles were attached. In Comparative Examples 2 and 3, in which the inorganic fine particles had a high degree of hydrophobicity, the oxygen absorption performance was low despite the fact that the same amount of inorganic fine particles was attached as in Examples 1 to 9, and the oxygen absorption performance of Comparative Example 3 was similar to that of Comparative Example 1, in which no inorganic fine particles were attached.
[0053] In Example 4, where the pH of the inorganic fine particles was 3.6, the oxygen absorption performance was slightly lower than in the other Examples. This indicates that stable oxygen absorption performance can be obtained if the pH of the inorganic fine particles is within the range of 4.0 to 9.0. Among these, a pH of approximately 5.5 to 8.0 was the best.
[0054] The results of Examples 10 to 12, in which the amount of inorganic fine particles attached was changed, confirmed that the oxygen absorption performance did not decrease significantly even when the amount of attached inorganic fine particles was increased to about 15 parts by mass. Since no particular benefit was observed from increasing the amount of attached inorganic fine particles, it was considered that the amount of attached inorganic fine particles should be 1 part by mass or more and 15 parts by mass or less.
[0055] Although one embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and configuration changes and combinations within the scope that do not deviate from the gist of the present invention are also included. [Industrial Applicability]
[0056] INDUSTRIAL APPLICABILITY The present invention can be used in oxygen absorber packages and food packages that improve the shelf life of foods and the like. [Explanation of symbols]
[0057] 1. Oxygen absorber packaging 10 Packaging material 20. Oxygen absorber
Claims
1. An oxygen scavenger comprising a porous carrier and an oxygen absorbing composition supported on the carrier, the inorganic fine particles being attached to a surface of the granulated material, The oxygen absorbing composition includes a liquid agent containing an oxygen absorbing substance, an alkaline compound, and a transition metal compound, The degree of methanol hydrophobicity of the inorganic fine particles is 15% or less, The pH of the inorganic fine particles is 8.0 or more and 9.0 or less. Oxygen absorber.
2. The amount of the inorganic fine particles is 1 to 15 parts by mass per 100 parts by mass of the granules. The oxygen scavenger according to claim 1.
3. The mass of the oxygen scavenger is 0.3 to 10.0 mg per piece. The oxygen scavenger according to claim 1.
4. The inorganic fine particles form a layer having a thickness of 1 mm or less that covers the surface of the granules. The oxygen scavenger according to claim 1.
5. The oxygen absorber according to any one of claims 1 to 4 is contained in a breathable packaging material. Oxygen absorber packaging.
6. The oxygen absorber package according to claim 5, A packaging container in which the oxygen absorber package and food are enclosed; Equipped with Food packaging.
Citation Information
Patent Citations
Deoxidant and method for producing the same
JP2017104845A
Deoxidizer and production method of the same
JP2017104846A
Oxygen scavenger and manufacturing method thereof
JP2017225952A
Oxygen absorber and its package
JP3541859B2