Epoxy resin composition and electronic component device
The epoxy resin composition with alumina particles and a non-reactive silane compound addresses the challenge of maintaining thermal conductivity and curability in miniaturized electronic devices, ensuring efficient heat dissipation and fluidity.
Patent Information
- Application Number
- JP2023048622
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-03-16
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2039-03-11
AI Technical Summary
The increasing heat generation in miniaturized and denser electronic component devices necessitates a resin composition that maintains thermal conductivity while suppressing viscosity increase and ensuring good curability, as conventional methods using inorganic fillers often lead to poor filling and wire flow due to increased viscosity.
An epoxy resin composition containing alumina particles and a specific silane compound with a functional group that does not react with the epoxy group, such as 3-methacryloxypropyltrimethoxysilane, is used to enhance thermal conductivity and maintain low viscosity, with the silane compound acting as a lubricant to improve compatibility and reduce frictional resistance.
The composition achieves excellent thermal conductivity, low viscosity, and maintains good curability, enabling effective heat dissipation and seamless filling in electronic components.
Smart Images

Figure 0007571814000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an epoxy resin composition and an electronic component device. [Background technology]
[0002] 2. Description of the Related Art Conventionally, packages (electronic component devices) in which elements such as transistors and ICs are sealed with resin such as epoxy resin have been widely used in electronic devices.
[0003] In recent years, the amount of heat generated by electronic devices has increased with the miniaturization and densification of the devices, and how to dissipate the heat has become an important issue. To address this issue, inorganic fillers with high thermal conductivity have been mixed into the sealing material to increase the thermal conductivity.
[0004] When an inorganic filler is mixed into a sealing material, as the amount of the inorganic filler increases, the viscosity of the sealing material increases and the fluidity decreases, which may cause problems such as poor filling, wire sweep, etc. Therefore, a method has been proposed in which a specific phosphorus compound is used as a curing accelerator to increase the fluidity of the sealing material (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-157497 Summary of the Invention [Problem to be solved by the invention]
[0006] However, with the progress of miniaturization and high density of electronic device, it is desired to provide a resin composition that can be used as a sealant, which can suppress the increase in viscosity while maintaining a higher level of thermal conductivity. It is also required that the curability during molding is not impaired while suppressing the increase in viscosity of the resin composition. In view of the above circumstances, an object of the present disclosure is to provide an epoxy resin composition that has excellent thermal conductivity, low viscosity, and maintains good curability, and an electronic component device including an element encapsulated using the epoxy resin composition. [Means for solving the problem]
[0007] The means for solving the above problems include the following aspects. <1> The epoxy resin composition comprises an epoxy resin, a curing agent, alumina particles, and a silane compound having a structure in which the functional group that does not react with an epoxy group but has a functional group that does not react with an epoxy group is bonded to a silicon atom or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms. <2> The content of the silane compound is 0.01% by mass to 20% by mass based on the total amount of the epoxy resin. <1> The epoxy resin composition according to claim 1. <3> The functional group that does not react with an epoxy group is at least one selected from the group consisting of a (meth)acryloyl group, a (meth)acryloyloxy group, and a vinyl group. <1> or <2> The epoxy resin composition according to claim 1. <4> The silane compound includes 3-methacryloxypropyltrimethoxysilane. <1> ~ <3> 13. The epoxy resin composition according to claim 12. <5> The content of the alumina particles is 50% by volume or more. <1> ~ <4> 13. The epoxy resin composition according to claim 12. <6> Further containing silica particles, <1> ~ <5> 13. The epoxy resin composition according to claim 12. <7> <1> ~ <6> 1. An electronic component device comprising an element encapsulated with the epoxy resin composition according to claim 1. Effect of the Invention
[0008] According to the present disclosure, there are provided an epoxy resin composition having excellent thermal conductivity, low viscosity, and maintaining good curability, and an electronic component device including an element encapsulated with the epoxy resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiment for carrying out the present invention will be described in detail. However, the present invention is not limited to the following embodiment. In the following embodiment, the components (including element steps, etc.) are not essential unless specifically stated. The same applies to the numerical values and their ranges, and they do not limit the present invention. In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of the corresponding substance. When multiple substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, multiple types of particles corresponding to each component may be included. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, a (meth)acryloyl group means at least one of an acryloyl group and a methacryloyl group, and a (meth)acryloyloxy group (also referred to as a (meth)acryloxy group) means at least one of an acryloyloxy group and a methacryloyloxy group.
[0010] <Epoxy resin composition> The epoxy resin composition of the present disclosure contains an epoxy resin, a curing agent, alumina particles, and a silane compound having a structure in which the functional group that does not react with an epoxy group, but has a functional group that does not react with an epoxy group, and the functional group that does not react with an epoxy group is bonded to a silicon atom or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms. In the present disclosure, "a silane compound having a structure in which the functional group that does not react with an epoxy group, but has a functional group that does not react with an epoxy group, and the functional group that does not react with an epoxy group is bonded to a silicon atom or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms" is also referred to as "specific silane compound". The epoxy resin composition may contain other components as necessary.
[0011] According to the above-mentioned constitution, it is possible to obtain an epoxy resin composition which has excellent thermal conductivity, suppresses an increase in viscosity, and maintains good curability. Although the detailed reason why the epoxy resin composition of the present disclosure exhibits the above-mentioned effects is not necessarily clear, it is presumed as follows. Generally, when a silane compound is used as a coupling agent in an epoxy resin composition, a silane compound having a functional group reactive with an epoxy resin is often used. The main purpose of this is to increase the dispersibility of the inorganic filler in the epoxy resin and to increase the fluidity of the composition by chemical bonding between the silanol group of the silane compound and the inorganic filler, and between the functional group of the silane compound and the epoxy resin. On the other hand, the specific silane compound in the epoxy resin composition of the present disclosure has a functional group that does not react with epoxy groups, and does not have a functional group that reacts with epoxy groups, so it is considered to be present on the surface of the alumina particles without bonding with the epoxy resin. Due to the nature of the surface state of alumina particles, it is generally easy to reduce the fluidity of a resin composition. However, when the specific silane compound is present on the surface of the alumina particles, the specific silane compound functions as a lubricant, which is considered to improve the compatibility of the alumina particles with the resin. It is presumed that this reduces the friction resistance between the alumina particles and reduces the melt viscosity. Furthermore, since the increase in the viscosity of the epoxy resin composition is suppressed, it is possible to increase the amount of alumina particles to be blended, which is considered to enable further improvement in thermal conductivity. On the other hand, generally, when the amount of components that do not contribute to curing increases, the curability may decrease, but when the specific silane compound is used, the curability of the epoxy resin composition does not decrease significantly. The reason for this is not clear, but it is speculated that this is because the specific silane compound has a structure in which a functional group that does not react with an epoxy group is bonded to a silicon atom, or is bonded to a silicon atom via a hydrocarbon group with a chain length of 5 carbon atoms or less, so that the distance between silicon and the functional group is relatively short and the curing reaction of the epoxy resin composition is not easily hindered.
[0012] (Epoxy resin) The epoxy resin composition contains an epoxy resin. The type of the epoxy resin is not particularly limited as long as it has an epoxy group in the molecule. Specific examples of epoxy resins include novolac-type epoxy resins (phenol novolac-type epoxy resins, orthocresol novolac-type epoxy resins, etc.) obtained by epoxidizing novolac resins obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcin, catechol, bisphenol A, bisphenol F, etc., and naphthol compounds such as α-naphthol, β-naphthol, dihydroxynaphthalene, etc., with an aliphatic aldehyde compound such as formaldehyde, acetaldehyde, propionaldehyde, etc., under an acidic catalyst; triphenylmethane-type epoxy resins obtained by epoxidizing triphenylmethane-type phenolic resins obtained by condensing or co-condensing the above-mentioned phenolic compound with an aromatic aldehyde compound such as benzaldehyde, salicylaldehyde, etc., under an acidic catalyst; and novolac resins obtained by co-condensing the above-mentioned phenolic compound and naphthol compound with an aldehyde compound under an acidic catalyst. diphenylmethane type epoxy resins which are diglycidyl ethers of bisphenol A, bisphenol F, etc.; biphenyl type epoxy resins which are diglycidyl ethers of alkyl-substituted or unsubstituted biphenols; stilbene type epoxy resins which are diglycidyl ethers of stilbene-based phenolic compounds; sulfur-containing epoxy resins which are diglycidyl ethers of bisphenol S, etc.; epoxy resins which are glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ester type epoxy resins which are glycidyl esters of polyvalent carboxylic acid compounds such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidylamine type epoxy resins in which active hydrogen bonded to nitrogen atoms of aniline, diaminodiphenylmethane, isocyanuric acid, etc. is substituted with a glycidyl group; dicyclopentadiene type epoxy resins which are epoxidized co-condensation resins of dicyclopentadiene and phenolic compounds;Alicyclic epoxy resins such as vinylcyclohexene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane, which are epoxy-modified epoxy resins in which the olefin bonds in the molecule have been epoxidized; paraxylylene-modified epoxy resins, which are glycidyl ethers of paraxylylene-modified phenolic resins; metaxylylene-modified epoxy resins, which are glycidyl ethers of metaxylylene-modified phenolic resins; terpene-modified epoxy resins, which are glycidyl ethers of terpene-modified phenolic resins; and dicyclopentadiene-modified phenolic resins, which are glycidyl ethers of dicyclopentadiene-modified phenolic resins. Examples of the epoxy resin include pentadiene-modified epoxy resins; cyclopentadiene-modified epoxy resins which are glycidyl ethers of cyclopentadiene-modified phenolic resins; polycyclic aromatic ring-modified epoxy resins which are glycidyl ethers of polycyclic aromatic ring-modified phenolic resins; naphthalene-type epoxy resins which are glycidyl ethers of naphthalene ring-containing phenolic resins; halogenated phenol novolac-type epoxy resins; hydroquinone-type epoxy resins; trimethylolpropane-type epoxy resins; linear aliphatic epoxy resins obtained by oxidizing olefin bonds with peracids such as peracetic acid; aralkyl-type epoxy resins obtained by epoxidizing aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins; and the like. Furthermore, examples of the epoxy resin include epoxidized silicone resins and epoxidized acrylic resins. These epoxy resins may be used alone or in combination of two or more.;
[0013] The epoxy equivalent (molecular weight / number of epoxy groups) of the epoxy resin is not particularly limited, but from the viewpoint of the balance of various properties such as moldability, reflow resistance, and electrical reliability, it is preferably 100 g / eq to 1000 g / eq, and more preferably 150 g / eq to 500 g / eq.
[0014] The epoxy equivalent of the epoxy resin is a value measured by a method conforming to JIS K 7236:2009.
[0015] When the epoxy resin is a solid, the softening point or melting point of the epoxy resin is not particularly limited, but is preferably 40°C to 180°C from the viewpoints of moldability and reflow resistance, and more preferably 50°C to 130°C from the viewpoint of handleability during preparation of the epoxy resin composition.
[0016] The melting point of the epoxy resin is a value measured by differential scanning calorimetry (DSC), and the softening point of the epoxy resin is a value measured by a method conforming to JIS K 7234:1986 (ring and ball method).
[0017] From the viewpoints of strength, fluidity, heat resistance, moldability, etc., the content of the epoxy resin in the epoxy resin composition is preferably 0.5% by mass to 50% by mass, more preferably 2% by mass to 30% by mass, and even more preferably 2% by mass to 20% by mass.
[0018] (hardening agent) The epoxy resin composition contains a curing agent. The type of the curing agent is not particularly limited and can be selected depending on the type of resin, the desired properties of the epoxy resin composition, and the like. Examples of the curing agent include a phenol curing agent, an amine curing agent, an acid anhydride curing agent, a polymercaptan curing agent, a polyaminoamide curing agent, an isocyanate curing agent, a blocked isocyanate curing agent, etc. From the viewpoint of improving heat resistance, the curing agent is preferably one having a phenolic hydroxyl group in the molecule (phenol curing agent).
[0019] Specific examples of the phenolic hardener include polyhydric phenolic compounds such as resorcin, catechol, bisphenol A, bisphenol F, and substituted or unsubstituted biphenol; novolak-type phenolic resins obtained by condensing or co-condensing at least one phenolic compound selected from the group consisting of phenolic compounds such as phenol, cresol, xylenol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and naphthol compounds such as α-naphthol, β-naphthol, and dihydroxynaphthalene, with an aldehyde compound such as formaldehyde, acetaldehyde, propionaldehyde, benzaldehyde, and salicylaldehyde, under an acid catalyst; and polyphenolic compounds such as dimethoxyparaxylene, bis(methoxymethyl)biphenol, and the like. Examples of the phenol curing agent include aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins synthesized from phenyl and the like; paraxylylene and / or metaxylylene modified phenolic resins; melamine modified phenolic resins; terpene modified phenolic resins; dicyclopentadiene-type phenolic resins and dicyclopentadiene-type naphthol resins synthesized by copolymerization of the above phenolic compounds and dicyclopentadiene; cyclopentadiene modified phenolic resins; polycyclic aromatic ring modified phenolic resins; biphenyl type phenolic resins; triphenylmethane type phenolic resins obtained by condensing or co-condensing the above phenolic compounds with aromatic aldehyde compounds such as benzaldehyde and salicylaldehyde under an acid catalyst; and phenolic resins obtained by copolymerizing two or more of these. These phenolic curing agents may be used alone or in combination of two or more.
[0020] Among them, biphenyl-type phenolic resins are preferred from the viewpoint of flame retardancy, aralkyl-type phenolic resins are preferred from the viewpoint of reflow resistance and curability, dicyclopentadiene-type phenolic resins are preferred from the viewpoint of low moisture absorption, triphenylmethane-type phenolic resins are preferred from the viewpoint of heat resistance, low expansion coefficient and low warpage, and novolac-type phenolic resins are preferred from the viewpoint of curability. The epoxy resin composition preferably contains at least one of these phenolic resins.
[0021] The functional group equivalent of the curing agent (hydroxyl group equivalent in the case of a phenolic curing agent) is not particularly limited. From the viewpoint of the balance of various properties such as moldability, reflow resistance, and electrical reliability, it is preferably 70 g / eq to 1000 g / eq, and more preferably 80 g / eq to 500 g / eq.
[0022] The functional group equivalent of the curing agent (hydroxyl group equivalent in the case of a phenolic curing agent) is a value measured by a method in accordance with JIS K 0070:1992.
[0023] When the curing agent is a solid, the softening point or melting point of the curing agent is not particularly limited, but is preferably 40° C. to 180° C. from the viewpoints of moldability and reflow resistance, and more preferably 50° C. to 130° C. from the viewpoint of handleability during production of the epoxy resin composition.
[0024] The melting point or softening point of the curing agent is a value measured in the same manner as the melting point or softening point of the epoxy resin.
[0025] The equivalent ratio of the epoxy resin to the curing agent, that is, the ratio of the number of functional groups in the curing agent to the number of epoxy groups in the epoxy resin (number of functional groups in the curing agent / number of epoxy groups in the epoxy resin), is not particularly limited. From the viewpoint of keeping the amount of unreacted components low, the equivalent ratio of the epoxy resin to the curing agent is preferably set in the range of 0.5 to 2.0, more preferably in the range of 0.6 to 1.3. From the viewpoint of moldability and reflow resistance, it is more preferable that the equivalent ratio of the epoxy resin to the curing agent is set in the range of 0.8 to 1.2.
[0026] (Alumina particles) The epoxy resin composition contains alumina particles as an inorganic filler. The epoxy resin composition may contain an inorganic filler other than alumina particles.
[0027] The content of the alumina particles in the epoxy resin composition is not particularly limited. From the viewpoint of thermal conductivity of the cured product, the content of the alumina particles is preferably 30% by volume or more, more preferably 35% by volume or more, even more preferably 40% by volume or more, particularly preferably 45% by volume or more, and extremely preferably 50% by volume or more, based on the total amount of the epoxy resin composition. The upper limit of the content of the alumina particles is not particularly limited, and from the viewpoint of improving fluidity, decreasing viscosity, etc., it is preferably less than 100% by volume, more preferably 99% by volume or less, and even more preferably 98% by volume or less. The content of the alumina particles in the epoxy resin composition is preferably 30% by volume or more and less than 100% by volume, more preferably 35% by volume to 99% by volume, even more preferably 40% by volume to 98% by volume, particularly preferably 45% by volume to 98% by volume, and extremely preferably 50% by volume to 98% by volume. The content of the alumina particles in the epoxy resin composition can be measured, for example, by a method for measuring the content of an inorganic filler described later.
[0028] The volume average particle diameter of the alumina particles is not particularly limited. The volume average particle diameter of the alumina particles is preferably 0.1 μm or more, more preferably 0.3 μm or more. The volume average particle diameter of the alumina particles is preferably 80 μm or less, more preferably 50 μm or less. When the volume average particle diameter of the alumina particles is 0.1 μm or more, the increase in viscosity of the epoxy resin composition is easily suppressed. When the volume average particle diameter of the alumina particles is 80 μm or less, the mixing property of the alumina particles in the epoxy resin composition is improved, the uneven distribution of the alumina particles is suppressed, and the variation in thermal conductivity in the cured product tends to be suppressed. In addition, even when used to seal a narrow area, the filling property of the alumina particles tends to be excellent. The volume average particle diameter of the alumina particles can be measured, for example, by a laser scattering diffraction method particle size distribution measuring device. In the present disclosure, the volume average particle size can be measured as the particle size (D50) at which the cumulative amount from the small diameter side reaches 50% in a volume-based particle size distribution measured by a laser scattering diffraction particle size distribution measuring device.
[0029] The shape of the alumina particles is not limited, and examples of such shapes include spherical and angular. From the viewpoint of flowability, the particle shape of the alumina particles is preferably spherical, and the particle size distribution of the alumina particles is preferably distributed over a wide range. For example, when the alumina particles are blended in an epoxy resin composition at 75% by volume or more, it is preferable that 70% by mass or more of the total amount of the alumina particles are spherical particles, and the particle diameter of the spherical particles is preferably distributed over a wide range of 0.1 μm to 80 μm. Since such alumina particles tend to have a close-packed structure, even if the blending amount is increased, the viscosity of the material does not increase much, and an epoxy resin composition with excellent flowability tends to be obtained.
[0030] The epoxy resin composition may contain an inorganic filler other than alumina particles. The inorganic filler other than alumina particles is not particularly limited, and examples of inorganic materials include particles of fused silica, crystalline silica, glass, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, magnesium oxide, silicon carbide, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, and mica. An inorganic filler having a flame retardant effect may be used. Examples of inorganic fillers having a flame retardant effect include aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as composite hydroxides of magnesium and zinc, and zinc borate. The inorganic fillers may be used alone or in combination of two or more. In particular, from the viewpoint of the balance of various properties such as the thermal conductivity and thermal expansion coefficient of the cured product, it is preferable to use alumina particles and silica particles in combination. In addition, from the viewpoint of thermal conductivity, it is also preferable to use magnesium oxide in combination.
[0031] The inorganic fillers other than alumina particles may be used alone or in combination of two or more. The term "use of two or more inorganic fillers" refers to, for example, use of two or more inorganic fillers having the same components but different volume average particle sizes, use of two or more inorganic fillers having the same volume average particle size but different components, and use of two or more inorganic fillers having different volume average particle sizes and types.
[0032] The content of the inorganic filler in the total mass of the epoxy resin composition is not particularly limited. From the viewpoint of thermal conductivity of the cured product, the content of the inorganic filler is preferably 30% by volume or more, more preferably 35% by volume or more, even more preferably 40% by volume or more, particularly preferably 45% by volume or more, and extremely preferably 50% by volume or more, based on the total amount of the epoxy resin composition. The upper limit of the content of the inorganic filler is not particularly limited, and from the viewpoint of improving fluidity, decreasing viscosity, etc., it is preferably less than 100% by volume, more preferably 99% by volume or less, and even more preferably 98% by volume or less. The content of the inorganic filler in the epoxy resin composition is preferably 30% by volume or more and less than 100% by volume, more preferably 35% by volume to 99% by volume, even more preferably 40% by volume to 98% by volume, particularly preferably 45% by volume to 98% by volume, and extremely preferably 50% by volume to 98% by volume.
[0033] The content of the inorganic filler in the total mass of the epoxy resin composition is measured as follows. First, the total mass of the cured product of the epoxy resin composition (also called an epoxy resin molded product) is measured, and the epoxy resin molded product is baked at 400°C for 2 hours and then at 700°C for 3 hours to evaporate the resin components, and the mass of the remaining inorganic filler is measured. The volume is calculated from the obtained mass and specific gravity, and the ratio of the volume of the inorganic filler to the total volume of the cured product of the epoxy resin composition (epoxy resin molded product) is obtained, which is the content of the inorganic filler.
[0034] The inorganic filler may have a controlled maximum particle size (also called cut point) from the viewpoint of improving the filling property in narrow gaps when the epoxy resin composition is used for mold underfill, etc. The maximum particle size of the inorganic filler may be appropriately adjusted, and from the viewpoint of filling property, it is preferably 105 μm or less, more preferably 75 μm or less, may be 60 μm or less, or may be 40 μm or less. The maximum particle size can be measured by a laser diffraction particle size distribution meter (manufactured by Horiba, Ltd., product name: LA920).
[0035] When the epoxy resin composition contains alumina particles and inorganic fillers other than alumina particles as inorganic fillers, the content of the alumina particles relative to the total amount of the inorganic fillers is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more. The upper limit of the content of the alumina particles relative to the total amount of the inorganic fillers is not particularly limited, and may be 100% by mass or less, 90% by mass or less, or 85% by mass or less.
[0036] (Specific silane compounds) The epoxy resin composition contains a specific silane compound. The specific silane compound does not have a functional group that reacts with an epoxy group, but has a functional group that does not react with an epoxy group, and has a structure in which the functional group that does not react with an epoxy group is bonded to a silicon atom or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms. Hereinafter, the functional group in the specific silane compound that does not react with an epoxy group is also referred to as a "specific functional group".
[0037] The term "functional group that does not react with epoxy groups" refers to a functional group that does not undergo a chemical reaction with epoxy groups or reacts so slowly that the change in the properties of the epoxy resin composition due to the reaction can be practically ignored. The term "functional group that reacts with epoxy groups" refers to a functional group other than the functional group that does not react with epoxy groups. The term "functional group" of a silane compound refers to an atom or atomic group that exists in the molecule of the silane compound and causes the reactivity of the silane compound. The fact that the functional group of a silane compound does not react with epoxy groups can be confirmed, for example, by a differential scanning calorimeter (DSC). In the above-mentioned "structure in which a functional group that does not react with an epoxy group is bonded to a silicon atom, or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms", the structure in which "a functional group that does not react with an epoxy group is bonded to a silicon atom" refers to a structure in which a specific functional group is directly bonded to a silicon atom.
[0038] Examples of the specific functional group include a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyl group, and a styryl group. On the other hand, examples of the "functional group reactive with an epoxy group" include an amino group, a group having an amine structure such as a phenylamino group, an epoxy group, a thiol group, an isocyanate group, an isocyanurate group, and a ureido group. The specific functional group is preferably at least one selected from the group consisting of a (meth)acryloyl group, a (meth)acryloyloxy group, and a vinyl group, and is more preferably a (meth)acryloyloxy group.
[0039] The specific silane compound may have one or more specific functional groups per molecule. The number of specific functional groups per molecule of the specific silane compound is preferably 1 to 4, more preferably 1 to 3, further preferably 1 or 2, and particularly preferably 1.
[0040] In the specific silane compound, the specific functional group is bonded to a silicon atom or bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms. When the specific functional group is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms, from the viewpoints of viscosity reduction and moldability, the number of carbon atoms in the chain hydrocarbon group is preferably 2 to 4, and more preferably 3. In the present disclosure, the number of carbon atoms in the chain hydrocarbon group means the number of carbon atoms not including carbons in branches or substituents. When the specific functional group is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms, the specific functional group may be present at the end of the chain hydrocarbon group or may be present on a side chain of the chain hydrocarbon group. From the viewpoint of suppressing viscosity, the specific functional group is preferably present at the end of the chain hydrocarbon group.
[0041] The chain-like hydrocarbon group may have a branched chain. When the chain-like hydrocarbon group has a branched chain, the number of carbon atoms in the branched chain is preferably 1 or 2. It is preferable that the chain-like hydrocarbon group does not have a branched chain. The chain hydrocarbon group may have a substituent other than the specific functional group. When the chain hydrocarbon group has a substituent, the substituent is not particularly limited and may be an alkoxy group, an aryl group, an aryloxy group, etc. It is preferable that the chain hydrocarbon group does not have a substituent other than the specific functional group. The chain hydrocarbon group may or may not contain an unsaturated bond, and preferably does not contain an unsaturated bond.
[0042] Hereinafter, the specific functional group directly bonded to a silicon atom, or a group bonded to a silicon atom and having both the chain hydrocarbon group having 1 to 5 carbon atoms and a specific functional group, is referred to as a "group containing a specific functional group." The number of groups containing a specific functional group in the specific silane compound may be 1 to 4, preferably 1 to 3, more preferably 1 or 2, and even more preferably 1. When the number of groups containing a specific functional group is 1 to 3, the other groups bonded to the silicon atom are not particularly limited and may be each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an aryl group, an aryloxy group, etc., preferably an alkyl group having 1 to 5 carbon atoms or an alkoxy group having 1 to 5 carbon atoms, and more preferably a methyl group, an ethyl group, a methoxy group, or an ethoxy group. Among them, it is preferable that one group containing a specific functional group is bonded to the silicon atom, and an alkyl group having 1 to 5 carbon atoms or an alkoxy group having 1 to 5 carbon atoms is bonded to the other three bonds, respectively, independently. It is more preferable that one group containing a specific functional group is bonded to the silicon atom, and a methyl group, an ethyl group, a methoxy group, or an ethoxy group is bonded to the other three bonds, respectively, independently.
[0043] Examples of the specific silane compound include 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and p-styryltrimethoxysilane. Among them, from the viewpoint of suppressing the increase in viscosity of the epoxy resin composition and curing properties, 3-(meth)acryloxypropyltrimethoxysilane is preferred. The specific silane compound may be used alone or in combination of two or more.
[0044] The specific silane compound may be synthesized or may be commercially available. Examples of commercially available specific silane compounds include KBM-502 (3-methacryloxypropylmethyldimethoxysilane), KBM-503 (3-methacryloxypropyltrimethoxysilane), KBE-502 (3-methacryloxypropylmethyldiethoxysilane), KBE-503 (3-methacryloxypropyltriethoxysilane), and KBM-5103 (3-acryloxypropyltrimethoxysilane), all of which are manufactured by Shin-Etsu Chemical Co., Ltd.
[0045] The content of the specific silane compound in the epoxy resin composition is not particularly limited. The content of the specific silane compound is preferably 0.01% by mass to 20% by mass with respect to the total amount of epoxy resin. For example, from the viewpoint of the balance between the viscosity and curability of the composition, the content of the specific silane compound may be 0.01% by mass to 10% by mass with respect to the total amount of epoxy resin. In addition, from the viewpoint of further suppressing the increase in viscosity, the content of the specific silane compound may be 10% by mass to 20% by mass, or may be 15% by mass to 20% by mass with respect to the total amount of epoxy resin.
[0046] The epoxy resin composition may further contain other silane compounds in addition to the specific silane compounds. The other silane compounds are not particularly limited as long as they are generally used in epoxy resin compositions, and may be silane compounds that react with epoxy groups or silane compounds that do not react with epoxy groups. Examples of the other silane compounds include epoxy silane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, (meth)acrylsilane (excluding the specific silane compounds), vinylsilane (excluding the specific silane compounds), etc. The other silane compounds may be used alone or in combination of two or more.
[0047] In order to satisfactorily exert the effect of the specific silane compound, the content of the other silane compounds relative to the total amount of the specific silane compound and the other silane compounds is preferably 30 mass% or less, more preferably 20 mass% or less, and even more preferably 10 mass% or less.
[0048] The epoxy resin composition may contain a coupling agent other than the silane compound. Examples of the coupling agent other than the silane compound include known coupling agents such as titanium compounds, aluminum chelate compounds, and aluminum / zirconium compounds. The other coupling agents may be used alone or in combination of two or more.
[0049] (Cure accelerator) The epoxy resin composition may contain a curing accelerator. The type of the curing accelerator is not particularly limited and can be selected depending on the type of epoxy resin, the desired properties of the epoxy resin composition, and the like. Examples of the curing accelerator include diazabicycloalkenes such as 1,5-diazabicyclo[4.3.0]nonene-5 (DBN) and 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), cyclic amidine compounds such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 2-heptadecylimidazole; derivatives of the cyclic amidine compounds; phenol novolac salts of the cyclic amidine compounds or their derivatives; and combinations of these compounds with maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, and the like. quinone compounds such as quinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone; compounds with intramolecular polarization formed by adding compounds with π bonds such as diazophenylmethane; cyclic amidines such as tetraphenylborate salt of DBU, tetraphenylborate salt of DBN, tetraphenylborate salt of 2-ethyl-4-methylimidazole, and tetraphenylborate salt of N-methylmorpholine; ammonium compounds; tertiary amine compounds such as pyridine, triethylamine, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; derivatives of the above tertiary amine compounds; ammonium salt compounds such as tetra-n-butylammonium acetate, tetra-n-butylammonium phosphate, tetraethylammonium acetate, tetra-n-hexylammonium benzoate, and tetrapropylammonium hydroxide; tertiary phosphines such as triphenylphosphine, diphenyl(p-tolyl)phosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, tris(alkylalkoxyphenyl)phosphine, tris(dialkylphenyl)phosphine, tris(trialkylphenyl)phosphine, tris(tetraalkylphenyl)phosphine, tris(dialkoxyphenyl)phosphine, tris(trialkoxyphenyl)phosphine, tris(tetraalkoxyphenyl)phosphine, trialkylphosphine, dialkylarylphosphine, and alkyldiarylphosphine;Phosphine compounds such as complexes of the tertiary phosphines and organic borons; compounds having intramolecular polarization obtained by adding the tertiary phosphines or the phosphine compounds to maleic anhydride, quinone compounds such as 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone, and compounds having a π bond such as diazophenylmethane; compounds having intramolecular polarization obtained by adding the tertiary phosphines or the phosphine compounds to 4-bromophenol, 3-bromophenol, 2-bromophenol, 4-chlorophenol, 3-chlorophenol, 2-chlorophenol, 4-iodophenol, and 3-iodophenol; Compounds having intramolecular polarization obtained by reacting halogenated phenol compounds such as phenol, 2-iodophenol, 4-bromo-2-methylphenol, 4-bromo-3-methylphenol, 4-bromo-2,6-dimethylphenol, 4-bromo-3,5-dimethylphenol, 4-bromo-2,6-di-t-butylphenol, 4-chloro-1-naphthol, 1-bromo-2-naphthol, 6-bromo-2-naphthol, and 4-bromo-4'-hydroxybiphenyl, followed by a dehydrohalogenation process; tetra-substituted phosphonium such as tetraphenylphosphonium, tetra-substituted phosphonium and tetra-substituted borates having no phenyl group bonded to a boron atom such as tetra-p-tolylborate; salts of tetraphenylphosphonium and phenol compounds. The curing accelerator may be used alone or in combination of two or more.;
[0050] When the epoxy resin composition contains a curing accelerator, the content is preferably 0.1 to 30 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the resin component (i.e., the total of the resin and the curing agent). When the amount of the curing accelerator is 0.1 parts by mass or more per 100 parts by mass of the resin component, the composition tends to cure well in a short time. When the amount of the curing accelerator is 30 parts by mass or less per 100 parts by mass of the resin component, the curing speed is not too fast and a good molded product tends to be obtained.
[0051] [Various additives] In addition to the above components, the epoxy resin composition may contain various additives such as ion exchangers, mold release agents, flame retardants, colorants, stress relievers, etc. exemplified below. The epoxy resin composition may contain various additives well-known in the art as needed in addition to the additives exemplified below.
[0052] (Ion exchanger) The epoxy resin composition may contain an ion exchanger. In particular, when the epoxy resin composition is used as a sealing molding material, it is preferable to contain an ion exchanger from the viewpoint of improving the moisture resistance and high-temperature storage characteristics of an electronic component device including an element to be sealed. The ion exchanger is not particularly limited, and conventionally known ones can be used. Specifically, hydrotalcite compounds, and hydrated oxides of at least one element selected from the group consisting of magnesium, aluminum, titanium, zirconium, and bismuth can be mentioned. The ion exchanger may be used alone or in combination of two or more. Among them, hydrotalcite represented by the following general formula (A) is preferable.
[0053] Mg (1-X) Al X (OH)2(CO3) X / 2 ·mH2O ……(A) (0 < X ≦ 0.5, m is a positive number)
[0054] When the epoxy resin composition contains an ion exchanger, its content is not particularly limited as long as it is sufficient to capture ions such as halogen ions. For example, it is preferably 0.1 part by mass to 30 parts by mass, more preferably 1 part by mass to 10 parts by mass, based on 100 parts by mass of the resin component.
[0055] (Mold release agent) The epoxy resin composition may contain a mold release agent from the viewpoint of obtaining good releasability from the mold during molding. The mold release agent is not particularly limited, and a conventionally known one may be used. Specific examples include carnauba wax, higher fatty acids such as montanic acid and stearic acid, higher fatty acid metal salts, ester waxes such as montanic acid esters, polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene, etc. The mold release agent may be used alone or in combination of two or more kinds.
[0056] When the epoxy resin composition contains a release agent, the content is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the resin component. When the amount of the release agent is 0.01 parts by mass or more based on 100 parts by mass of the resin component, sufficient releasability tends to be obtained. When the amount is 10 parts by mass or less, better adhesion and curability tend to be obtained.
[0057] (Flame retardant) The epoxy resin composition may contain a flame retardant. The flame retardant is not particularly limited, and a conventionally known one may be used. Specific examples include organic or inorganic compounds containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms, metal hydroxides, etc. The flame retardant may be used alone or in combination of two or more.
[0058] When the epoxy resin composition contains a flame retardant, the content is not particularly limited as long as it is an amount sufficient to obtain the desired flame retardant effect. For example, the content is preferably 1 to 30 parts by mass, more preferably 2 to 20 parts by mass, per 100 parts by mass of the resin component.
[0059] (Coloring agent) The epoxy resin composition may further contain a colorant. Examples of the colorant include known colorants such as carbon black, organic dyes, organic pigments, titanium oxide, red lead, and red iron oxide. The content of the colorant can be appropriately selected depending on the purpose. The colorant may be used alone or in combination of two or more.
[0060] (Stress reliever) The epoxy resin composition may contain a stress relaxation agent such as silicone oil or silicone rubber particles. By using the stress relaxation agent, the warpage deformation of the package and the occurrence of package cracks can be further reduced. Examples of the stress relaxation agent include known stress relaxation agents (also called flexible agents) that are generally used. Specific examples include thermoplastic elastomers such as silicone, styrene, olefin, urethane, polyester, polyether, polyamide, and polybutadiene, rubber particles such as NR (natural rubber), NBR (acrylonitrile-butadiene rubber), acrylic rubber, urethane rubber, and silicone powder, and rubber particles having a core-shell structure such as methyl methacrylate-styrene-butadiene copolymer (MBS), methyl methacrylate-silicone copolymer, and methyl methacrylate-butyl acrylate copolymer. The stress relaxation agent may be used alone or in combination of two or more types.
[0061] [Physical properties of epoxy resin composition] (Viscosity of epoxy resin composition) The viscosity of the epoxy resin composition is not particularly limited, and is preferably adjusted to a desired viscosity depending on the molding method, the composition of the epoxy resin composition, and the like. For example, when the epoxy resin composition is molded by compression molding, from the viewpoint of reducing wire sweep, the viscosity of the epoxy resin composition is preferably 200 Pa s or less, more preferably 150 Pa s or less, and even more preferably 100 Pa s or less at 175° C. The lower limit of the viscosity is not particularly limited, and may be, for example, 10 Pa s or more. Furthermore, for example, when the epoxy resin composition is molded by transfer molding, from the viewpoint of reducing wire sweep, the viscosity of the epoxy resin composition is preferably 200 Pa s or less, more preferably 150 Pa s or less, and even more preferably 100 Pa s or less at 175° C. The lower limit of the viscosity is not particularly limited, and may be, for example, 10 Pa s or more. The viscosity of the epoxy resin composition can be measured by a Koka type flow tester (for example, manufactured by Shimadzu Corporation).
[0062] The viscosity of the epoxy resin composition may be confirmed by spiral flow. For example, the viscosity is measured by subjecting the epoxy resin composition to a spiral flow measurement mold conforming to the standard (EMMI-1-66) at an oil pressure of 70 kgf / cm, which is calculated as the plunger bottom pressure. 2 (about 6.86 MPa) and molded at 175°C for 120 seconds. The flow distance measured under the above conditions is preferably 67 inches (170 cm) or more, more preferably 70 inches (178 cm) or more, even more preferably 75 inches (191 cm) or more, particularly preferably 80 inches (203 cm) or more, and extremely preferably 85 inches (216 cm) or more. The values in parentheses (cm) are converted values.
[0063] (Thermal conductivity when cured) The thermal conductivity of the epoxy resin composition when cured is not particularly limited. From the viewpoint of obtaining the desired heat dissipation, the thermal conductivity may be 3.0 W / (m·K) or more, 4.0 W / (m·K) or more, 5.0 W / (m·K) or more, 6.0 W / (m·K) or more, 7.0 W / (m·K) or more, or 8.0 W / (m·K) or more at room temperature (25°C). The upper limit of the thermal conductivity is not particularly limited, and may be 9.0 W / (m·K). The thermal conductivity of the cured product can be measured by a xenon flash (Xe-flash) method (for example, a Hyper Flash device manufactured by NETZSCH, trade name: LFA467 type).
[0064] (Hot hardness when cured) The hot hardness of the epoxy resin composition when cured is not particularly limited. For example, the hot hardness of the epoxy resin composition when molded under conditions of 175°C, 120 sec, and a pressure of 7 MPa, as measured using a Shore D hardness tester, is preferably 60 or more, more preferably 65 or more, and even more preferably 70 or more.
[0065] [Method for preparing epoxy resin composition] The method for preparing the epoxy resin composition is not particularly limited. A typical method is to mix each component thoroughly with a mixer or the like, then melt-knead with a mixing roll, an extruder, or the like, cool, and pulverize. More specifically, for example, the above-mentioned components are mixed and stirred, kneaded with a kneader, roll, extruder, or the like that has been heated to 70°C to 140°C in advance, cooled, and pulverized.
[0066] The epoxy resin composition may be solid or liquid at room temperature and normal pressure (for example, 25°C and atmospheric pressure), and is preferably solid. When the epoxy resin composition is solid, the shape is not particularly limited, and examples thereof include powder, granules, and tablets. When the epoxy resin composition is in tablet form, the dimensions and mass are preferably set to be suitable for the molding conditions of the package from the viewpoint of handling.
[0067] <Electronic component equipment> An electronic component device according to one embodiment of the present disclosure includes an element encapsulated with the above-described epoxy resin composition. Examples of electronic component devices include devices obtained by mounting elements (active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, and coils) on a support member such as a lead frame, a pre-wired tape carrier, a wiring board, glass, a silicon wafer, or an organic substrate, and then sealing the resulting element portion with an epoxy resin composition. More specifically, typical resin-sealed ICs, such as DIP (Dual Inline Package), PLCC (Plastic Leaded Chip Carrier), QFP (Quad Flat Package), SOP (Small Outline Package), SOJ (Small Outline J-lead package), TSOP (Thin Small Outline Package), and TQFP (Thin Quad Flat Package), have a structure in which an element is fixed on a lead frame, and terminal portions of the element, such as bonding pads, and leads are connected by wire bonding, bumps, or the like, and then sealed by transfer molding or the like using an epoxy resin composition; TCP (Tape Carrier Package), which has a structure in which an element connected to a tape carrier by bumps is sealed with an epoxy resin composition; and COB (Chip On Board) which has a structure in which an element is connected to wiring formed on a support member by wire bonding, flip chip bonding, solder, or the like, and then sealed with an epoxy resin composition. Examples of such devices include BGA (Ball Grid Array), CSP (Chip Size Package), MCP (Multi Chip Package), etc., which have a structure in which elements are mounted on the surface of a support member having terminals for connecting a wiring board formed on the back surface thereof, the elements are connected to wiring formed on the support member by bump or wire bonding, and then the elements are sealed with an epoxy resin composition. The epoxy resin composition can also be suitably used in printed wiring boards.
[0068] Methods for encapsulating electronic device components using an epoxy resin composition include low pressure transfer molding, injection molding, compression molding, and the like. EXAMPLES
[0069] The above embodiment will be specifically described below using examples, but the scope of the above embodiment is not limited to these examples.
[0070] <Preparation of Epoxy Resin Composition> First, the following components were prepared.
[0071] [Epoxy resin] Epoxy resin A: Bisphenol F type epoxy resin with an epoxy equivalent of 187g / eq to 197g / eq and a melting point of 61℃ to 71℃ (manufactured by Nippon Steel Chemical & Material Co., Ltd., product name: YSLV-80XY) Epoxy resin B: Epoxy resin with an epoxy equivalent of 192 g / eq and a melting point of 106°C (manufactured by Mitsubishi Chemical Corporation, product name: YX-4000)
[0072] [Hardening agent] Triphenylmethane type phenolic resin with a hydroxyl equivalent of 102g / eq and a softening point of 70°C (Air Water Inc., product name: HE910)
[0073] [Curing Accelerator] Phosphorus-based hardening accelerator
[0074] [Silane Compound] Silane compound A: 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-503) Silane compound B: N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-573) Silane compound C: 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-803)
[0075] [Inorganic filler] Silica particles: Volume average particle size 0.2μm Alumina particle A: Volume average particle size 10 μm, cut point 55 μm Alumina particle B: Volume average particle size 1 μm, cut point 25 μm Magnesium oxide: Volume average particle size: approx. 2 μm
[0076] [Additives] Release agent: Hoechst wax (Clariant, product name: HW-E) Pigment: Carbon black (manufactured by Mitsubishi Chemical Corporation, product name: MA-600MJ-S) Ion exchanger: Hydrotalcite (manufactured by Sakai Chemical Industry Co., Ltd., product name: STABIACE HT-P)
[0077] The epoxy resin compositions were prepared by mixing the components shown in Table 1 in the amounts shown in the table, kneading, cooling, and pulverizing. In the table, unless otherwise specified, the unit of the amount of each component is parts by mass. In the table, "-" indicates that the component was not mixed.
[0078] <Viscosity evaluation (spiral flow evaluation)> Using a spiral flow measurement mold conforming to the standard (EMMI-1-66), the epoxy resin composition was subjected to a plunger bottom pressure of 70 kgf / cm 2 (approximately 6.86 MPa), and molded under conditions of 175°C and 120 seconds. The length of the molded product was evaluated as the flow distance.
[0079] <Evaluation of thermal conductivity> The epoxy resin composition was molded in a high-temperature vacuum molding machine under conditions of 175°C, 120 sec, and a pressure of 7 MPa, and processed into a test piece having a thickness of 1 mm and a square of 10 mm. The test piece was measured at room temperature (25°C) using a Hyper Flash device (trade name: LFA467 model, manufactured by NETZSCH), and the value calculated by the xenon flash method was taken as the thermal conductivity.
[0080] <Evaluation of hot hardness> The above epoxy resin composition was molded in a high-temperature vacuum molding machine under conditions of 175° C., 120 seconds, and a pressure of 7 MPa, and the value measured using a Shore D hardness tester was taken as the hardness.
[0081] [Table 1]
[0082] As a result of the evaluation, in Examples 1 and 2 in which silane compound A was blended, the viscosity was reduced and the thermal conductivity of the cured product was good. In addition, the hot hardness did not decrease significantly compared to the comparative example, and good curability was maintained.
[0083] The disclosure of Japanese Patent Application No. 2018-049153 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. Epoxy resin, A curing agent containing a triphenylmethane type phenolic resin; Alumina particles, and A silane compound having a structure in which, while it does not have a functional group that reacts with an epoxy group, it has a functional group that does not react with an epoxy group, and the functional group that does not react with an epoxy group is bonded to a silicon atom or is bonded to a silicon atom via a chain hydrocarbon group having 1 to 5 carbon atoms. Contains The content of the alumina particles is 50% by volume or more based on the total amount of the epoxy resin composition, the functional group that does not react with an epoxy group includes a (meth)acryloyloxy group, Using a spiral flow measurement mold conforming to EMMI-1-66, the epoxy resin composition is injected at a hydraulic pressure of 70 kgf / cm 2 (calculated as the plunger bottom pressure) and molded under conditions of 175°C and 120 sec., and the flow distance measured as the length of the molded product is 191 cm or more; An epoxy resin composition for encapsulating elements of electronic device components by low pressure transfer molding, injection molding, or compression molding, the composition being solid at 25° C. and atmospheric pressure.
2. 2. The epoxy resin composition according to claim 1, wherein the content of the silane compound is 0.01% by mass to 20% by mass based on the total amount of the epoxy resin.
3. The epoxy resin composition according to claim 1 or claim 2, wherein the silane compound comprises 3-methacryloxypropyltrimethoxysilane.
4. The epoxy resin composition according to any one of claims 1 to 3, further comprising silica particles.
5. An epoxy resin composition described in any one of claims 1 to 4, further containing a curing accelerator.
6. The epoxy resin composition according to any one of claims 1 to 5, wherein the epoxy resin composition is molded under conditions of 175°C, 120 sec, and a pressure of 7 MPa, and a test piece is machined into a thickness of 1 mm and a square of 10 mm, and the measured thermal conductivity calculated by a xenon flash method at 25°C is 4.0 W / (m / k) or more.
7. An electronic component device comprising an element encapsulated with the epoxy resin composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Epoxy resin composition for sealing semiconductor and semiconductor device sealed with the same
JP1997157497A
Epoxy resin molding material for sealing and electronic device
JP2003165892A
Epoxy resin composition for sealing semiconductor and resin-sealed semiconductor device
JP2005200533A
Epoxy resin composition and semiconductor device
JP2008297530A
Epoxy resin composition for sealing semiconductor and semiconductor device using the same