Composition for forming resist underlayer film containing diol structure

The resist underlayer film composition with a low molecular weight compound and additives addresses the challenges of void-free fine pattern formation and sublimation, offering improved embeddability and chemical resistance for semiconductor manufacturing.

JP7571912B2Active Publication Date: 2024-10-23NISSAN CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024058760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-12
Filing Date
2024-04-01
Publication Date
2024-10-23
Estimated Expiration
2041-06-11

Smart Images

  • Figure 0007571912000047
    Figure 0007571912000047
  • Figure 0007571912000048
    Figure 0007571912000048
  • Figure 0007571912000001
    Figure 0007571912000001
Patent Text Reader

Abstract

To provide a resist underlay film forming composition capable of filling up fine pores on a semiconductor substrate of which micronization is advanced without voids and is less in a sublimation substance generated during firing at the time of forming a film, and a chemical liquid resistant protective film composition attaining semiconductor substrate processing as a function as the protective film to the wet etching chemical liquid.SOLUTION: There are provided a compound with a theoretical molecular weight of 999 or less, represented by the following formula (1), and a resist under layer film forming composition or a protective film forming composition containing an organic solvent. [In formula (1), Z1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p represents an integer of 2-4.] [In formula (2), * indicates a binding portion to Z1.]SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resist underlayer film forming composition that has excellent embedding properties in fine structure substrates and produces less sublimation during film formation in the lithography process of semiconductor manufacturing. The present invention also relates to a method for manufacturing a substrate with a resist pattern using the resist underlayer film, and a method for manufacturing a semiconductor device. The present invention also relates to a protective film for processing a substrate with a wet etching solution during semiconductor manufacturing. [Background technology]

[0002] In semiconductor manufacturing, a lithography process is widely known in which a resist underlayer film is provided between a substrate and a resist film formed thereon to form a resist pattern of a desired shape. Patent Document 1 discloses a resist underlayer film-forming composition that contains a reaction product between a compound containing a triazine skeleton having three epoxy groups and a dicarboxylic acid compound containing a disulfide bond. In addition, in the lithography process of semiconductor manufacturing, when forming a resist underlayer film using the resist underlayer film forming composition, a new problem has arisen in that sublimation components (sublimation products) derived from low molecular weight compounds such as the polymer resin, crosslinking agent, and crosslinking catalyst are generated during baking. Such sublimation products are concerned that they will adhere to and accumulate in a film forming apparatus in the semiconductor device manufacturing process, contaminating the inside of the apparatus, and that they will adhere to the wafer as foreign matter, causing defects, etc. Therefore, there is a demand for a proposal for a new underlayer film composition that suppresses the generation of sublimation products from such resist underlayer films as much as possible, and studies are also being conducted on resist underlayer films that exhibit such low sublimation properties, such as those in Patent Document 2. Furthermore, Patent Document 3 discloses a protective film-forming composition for a semiconductor wet etching solution, which contains a compound having at least one pair of adjacent hydroxyl groups in the molecule, or a polymer thereof, and a solvent. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 151471 [Patent Document 2] JP 2010-237491 A [Patent Document 3] International Publication No. 2019 / 124474 Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional resist underlayer film-forming compositions are required as resist underlayer films to solve problems (such as defective shape) that occur during resist pattern formation, and are required to fill, without voids, fine patterns (e.g., widths of 10 nm or less) on semiconductor substrates, which are becoming increasingly finer, while also appropriately controlling the optical constants of the film itself, and it has been difficult to achieve both of these performance requirements. Furthermore, sublimates generated during film baking in the formation of the resist underlayer film are also a cause of equipment contamination and voids, and so further reductions are being sought. Furthermore, in the semiconductor manufacturing process, the above-mentioned resist underlayer film may be required to function as a protective film for non-processed areas, since substrate processing may be performed using wet etching chemicals (e.g., SC-1 (ammonia-hydrogen peroxide solution)). An object of the present invention is to solve the above problems. [Means for solving the problem]

[0005] The present invention encompasses the following: [1] A resist underlayer film forming composition comprising a compound represented by the following formula (1) and having a theoretical molecular weight of 999 or less, and an organic solvent: [ka] [In formula (1), Z1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4.] [ka] [In formula (2), R1 represents an alkylene group having 1 to 4 carbon atoms, A1 to A3 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and X represents -COO-, -OCO-, -O-, -S-, or -NR a - represents either R a represents a hydrogen atom or a methyl group; Y represents an alkylene group having 1 to 4 carbon atoms which may be directly bonded or substituted; R2, R3, and R4 each represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted, or an aryl group having 6 to 40 carbon atoms; R5 represents a hydrogen atom or a hydroxyl group; n represents an integer of 0 or 1; m1 and m2 each independently represent an integer of 0 or 1; and * represents a bonding site to Z1. [2] The resist underlayer film forming composition according to [1], wherein Z1 is represented by the following formula (3): [ka] [In formula (3), Q3 represents the following formula (4), formula (5), or formula (6)] [ka] [In formula (4), formula (5) and formula (6), R 11 , R 12 , R 13 and R 14 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group is optionally substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 atoms, a nitro group, a cyano group and an alkylthio group having 1 to 6 carbon atoms. R 15represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by a hydrogen atom, an oxygen atom or a sulfur atom and which may be substituted by a hydroxy group, an alkenyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group may be substituted by at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, a nitro group, a cyano group, an alkylthio group having 1 to 6 carbon atoms, and the monovalent organic group represented by U in formula (1). * represents a bonding portion to U.] [3] R 15 is an alkyl group having 1 to 10 carbon atoms or a monovalent organic group represented by U in formula (1). [4] R 11 and R 12 is each independently an alkyl group having 1 to 10 carbon atoms. [5] The resist underlayer film forming composition according to any one of [1] to [4], wherein X is -S- and Y is a methylene group. [6] The resist underlayer film forming composition according to [1], further comprising an acid compound. [7] The resist underlayer film forming composition according to any one of [1] to [6], further comprising a surfactant. [8] A resist underlayer film, which is a fired product of a coating film comprising the resist underlayer film forming composition according to any one of [1] to [7]. [9] A protective film-forming composition for a wet etching solution for semiconductors, comprising: a compound represented by the following formula (1), having a theoretical molecular weight of 999 or less and containing two or more nitrogen atoms and six or more oxygen atoms in the molecule; and an organic solvent: [ka] [In formula (1), Z1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4.] [ka] [In formula (2), R1 represents an alkylene group having 1 to 4 carbon atoms, A1 to A3 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and X represents -COO-, -OCO-, -O-, -S-, or -NR a - represents either R a represents a hydrogen atom or a methyl group; Y represents an alkylene group having 1 to 4 carbon atoms which may be directly bonded or substituted; R2, R3, and R4 each represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted, or an aryl group having 6 to 40 carbon atoms; R5 represents a hydrogen atom or a hydroxyl group; n represents an integer of 0 or 1; m1 and m2 each independently represent an integer of 0 or 1; and * represents a bonding site to Z1.

[10] The composition according to [9], wherein Z1 is represented by the following formula (3): [ka] [In formula (3), Q3 represents the following formula (4), formula (5), or formula (6)] [ka] [In formula (4), formula (5) and formula (6), R 11 , R 12 , R 13 and R 14each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group is optionally substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 atoms, a nitro group, a cyano group and an alkylthio group having 1 to 6 carbon atoms. R 15 represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by a hydrogen atom, an oxygen atom or a sulfur atom and which may be substituted by a hydroxy group, an alkenyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group may be substituted by at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, a nitro group, a cyano group, an alkylthio group having 1 to 6 carbon atoms, and the monovalent organic group represented by U in formula (1). * represents a bonding portion to U.]

[11] The protective film-forming composition according to [9] or

[10] , further comprising an acid compound and / or a crosslinking agent.

[12] A protective film, which is a fired product of a coating film made of the protective film-forming composition according to any one of [9] to

[11] .

[13] A method for producing a substrate having a resist pattern, comprising the steps of applying the resist underlayer film-forming composition according to any one of [1] to [7] onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a resist film on the resist underlayer film, and then exposing and developing the resist film to form a resist pattern, the method being used in the production of a semiconductor.

[14] A method for manufacturing a semiconductor device, comprising the steps of forming a resist underlayer film on a semiconductor substrate, which may have an inorganic film formed on its surface, using the resist underlayer film forming composition according to any one of [1] to [7], forming a resist pattern on the resist underlayer film, dry etching the resist underlayer film using the resist pattern as a mask to expose a surface of the inorganic film or the semiconductor substrate, and etching the inorganic film or the semiconductor substrate using the resist underlayer film after dry etching as a mask.

[15] A method for manufacturing a semiconductor device, comprising the steps of forming a protective film on a semiconductor substrate, on whose surface an inorganic film may be formed, using a protective film-forming composition according to any one of [9] to

[11] , forming a resist pattern on the protective film, dry-etching the protective film using the resist pattern as a mask to expose a surface of the inorganic film or the semiconductor substrate, and wet-etching and cleaning the inorganic film or the semiconductor substrate using a semiconductor wet etching solution using the protective film after the dry etching as a mask. Effect of the Invention

[0006] The resist underlayer film forming composition of the present invention can fill fine patterns (e.g., widths of 10 nm or less) on semiconductor substrates, which are becoming increasingly finer, without creating voids (gaps), while resolving problems (such as defective shapes) that occur during resist pattern formation as a resist underlayer film. Furthermore, compared with conventional resist underlayer films, less sublimates are generated during film baking during resist underlayer film formation. Furthermore, it has resistance to wet etching chemicals used in substrate processing in the semiconductor manufacturing process, and because it has a higher dry etching rate than conventional wet etching protective films, it is possible to reduce damage to the substrate when removing the resist underlayer film and protective film.

[0007] As the molecular weight of a polymer increases, the molecular size and viscosity also increase, which makes it difficult to embed the polymer in a fine pattern. Therefore, the resist underlayer film forming composition of the present invention uses a compound with a theoretical molecular weight of 999 or less, which makes it possible to embed the polymer in a fine structure compared to a composition using a high molecular weight polymer. Furthermore, by having many hydroxyl groups in the compound, the boiling point of the compound increases and sublimation is suppressed, and the adhesion to some substrates is improved by interaction, and resistance to wet etching chemical treatment is obtained. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view of an embeddability evaluation substrate according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional SEM photograph for evaluating the embedding ability of the resist underlayer film forming composition of Example 2 into a stepped substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Resist underlayer film forming composition> The resist underlayer film forming composition according to the present invention contains a compound represented by the following formula (1) and having a theoretical molecular weight of 999 or less, and an organic solvent. The theoretical molecular weight refers to a molecular weight calculated based on the chemical structure of the compound represented by formula (1). From the viewpoint of increasing the dry etching rate, the compound preferably contains 2 or more, 3 or more, or 4 or more nitrogen atoms and 6 or more, 8 or more, 9 or more, 10 or more, or 15 or more oxygen atoms in the molecule, and further preferably contains 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more sulfur atoms in the molecule. <Compound represented by formula (1) and having a theoretical molecular weight of 999 or less> The compound having a theoretical molecular weight of 999 or less contained in the resist underlayer film forming composition of the present application is represented by the following formula (1):

[0010] [ka]

[0011] [In formula (1), Z1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4.]

[0012] [ka]

[0013] [In formula (2), R1 represents an alkylene group having 1 to 4 carbon atoms, A1 to A3 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and X represents -COO-, -OCO-, -O-, -S-, or -NR a - represents either R a represents a hydrogen atom or a methyl group, Y represents an alkylene group having 1 to 4 carbon atoms which may be directly bonded or substituted, R2, R3 and R4 each represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted or an aryl group having 6 to 40 carbon atoms, R5 represents a hydrogen atom or a hydroxyl group, n represents an integer of 0 or 1, m1 and m2 each independently represent an integer of 0 or 1, and * represents a bonding portion to Z1. It is preferable that m2 is 1, and more preferably, m1 is 1. It is most preferred that when m2 is 1, m1 is 0.

[0014] In formula (1), Z1 is preferably represented by the following formula (3).

[0015] [ka]

[0016] [In formula (3), Q3 represents the following formula (4), formula (5), or formula (6)]

[0017] [ka]

[0018] [In formula (4), formula (5) and formula (6), R 11 , R 12 , R 13 and R 14 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group is optionally substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 atoms, a nitro group, a cyano group and an alkylthio group having 1 to 6 carbon atoms.

[0019] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, a cyclopentyl group, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl -n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclopentyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-i-propyl-cyclopropyl, 2-i-propyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,Examples of the cyclopropyl group include a 3-trimethylcyclopropyl group, a 1-ethyl-2-methylcyclopropyl group, a 2-ethyl-1-methylcyclopropyl group, a 2-ethyl-2-methylcyclopropyl group, a 2-ethyl-3-methylcyclopropyl group, and a decyl group.

[0020] Examples of the alkenyl group include a 1-propenyl group, a 2-propenyl group, a 1-methyl-1-ethenyl group, a 1-butenyl group, a 2-butenyl group, a 3-butenyl group, a 2-methyl-1-propenyl group, a 2-methyl-2-propenyl group, a 1-ethylethenyl group, a 1-methyl-1-propenyl group, a 1-methyl-2-propenyl group, a 1-pentenyl group, a 2-pentenyl group, a 3-pentenyl group, a 4-pentenyl group, a 1-n-propylethenyl group, a 1-methyl-1-butenyl group, a 1-methyl-2-butenyl group, a 1-methyl-3-butenyl group, a 2-ethyl-2-propenyl group, a 2-methyl ethyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, 3-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group, 3-cyclopentenyl group, 1-hexenyl group, 2-hexenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, 1-methyl-1-pentenyl group, 1-methyl -2-pentenyl group, 1-methyl-3-pentenyl group, 1-methyl-4-pentenyl group, 1-n-butylethenyl group, 2-methyl-1-pentenyl group, 2-methyl-2-pentenyl group, 2-methyl-3-pentenyl group, 2-methyl-4-pentenyl group, 2-n-propyl-2-propenyl group, 3-methyl-1-pentenyl group, 3-methyl-2-pentenyl group, 3-methyl-3-pentenyl group, 3-methyl-4-pentenyl group, 3-ethyl-3-butenyl group, 4-methyl-1-pentenyl group, 4-methyl-2-pentenyl group, 4-methyl-3-pentenyl group, 4-methyl-4-pentenyl group, 1,1-dimethyl-2-butenyl group, 1,1-dimethyl-3-butenyl group, 1,2-dimethyl-1-butenyl group, 1,2-dimethyl-2-butenyl group, 1,2-dimethyl-3-butenyl group, 1-methyl-2-ethyl-2-propenyl group, 1-s-butylethenyl group, 1,3-dimethyl-1-butenyl group, 1,3-dimethyl-2-butenyl group, 1,3-dimethyl-3-butenyl group, 1-i-butylethenyl group, 2,2-dimethyl-3-butenyl group, 2,3-dimethyl-1-butenyl group, 2,3-dimethyl-2-butenyl group, 2,3-dimethyl-3-butenyl group, 2-i-propyl-2-propenyl group, 3,3-dimethyl-1-butenyl group, 1-ethyl-1-butenyl group, 1-ethyl-2-butenyl group, 1-ethyl-3-butenyl group, 1-n-propyl-1-propenyl group, 1-n-propyl-2-propenyl group, 2-ethyl-1-butenyl group, 2-ethyl-2-butenyl group, 2-ethyl-3-butenyl group, 1,1,2-trimethyl-2-propenyl group, 1-t-butylethenyl group, 1-methyl-1-ethyl-2-propenyl group, 1-ethyl-2-methyl-1-propenyl group, 1-ethyl-2-methyl-2-propenyl group, 1-i-propyl-1-propenyl group, 1-i-propyl-2-propenyl group Examples of the cyclopentyl group include a cyclopentyl group, a 1-methyl-2-cyclopentenyl group, a 1-methyl-3-cyclopentenyl group, a 2-methyl-1-cyclopentenyl group, a 2-methyl-2-cyclopentenyl group, a 2-methyl-3-cyclopentenyl group, a 2-methyl-4-cyclopentenyl group, a 2-methyl-5-cyclopentenyl group, a 2-methylene-cyclopentyl group, a 3-methyl-1-cyclopentenyl group, a 3-methyl-2-cyclopentenyl group, a 3-methyl-3-cyclopentenyl group, a 3-methyl-4-cyclopentenyl group, a 3-methyl-5-cyclopentenyl group, a 3-methylene-cyclopentyl group, a 1-cyclohexenyl group, a 2-cyclohexenyl group, and a 3-cyclohexenyl group.

[0021] Examples of the alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 2-butynyl group, and a 3-butynyl group.

[0022] The phenyl group may be substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms.

[0023] The alkyl group is as exemplified above.

[0024] Examples of halogen atoms include fluorine, chlorine, bromine and iodine atoms.

[0025] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentyloxy group, a 2-methyl-n-pentyloxy group, a 3-methyl-n-pentyloxy group, a 4-methyl-n n-pentyloxy group, 1,1-dimethyl-n-butoxy group, 1,2-dimethyl-n-butoxy group, 1,3-dimethyl-n-butoxy group, 2,2-dimethyl-n-butoxy group, 2,3-dimethyl-n-butoxy group, 3,3-dimethyl-n-butoxy group, 1-ethyl-n-butoxy group, 2-ethyl-n-butoxy group, 1,1,2-trimethyl-n-propoxy group, 1,2,2-trimethyl-n-propoxy group, 1-ethyl-1-methyl-n-propoxy group, 1-ethyl-2-methyl-n-propoxy group, n-heptyloxy group, n-octyloxy group and n-nonyloxy group.

[0026] Examples of the alkylthio group include a methylthio group, an ethylthio group, and a butylthio group.

[0027] In the above formula (3), when Q3 represents formula (4), R in formula (4) 11 and R 12 are each preferably an alkyl group having 1 to 10 carbon atoms.

[0028] In the above formula (3), when Q3 represents formula (5), R in formula (5) 13 and R 14 are each preferably an alkyl group having 1 to 10 carbon atoms.

[0029] In the above formula (3), when Q3 represents formula (6), R in formula (6) 15represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by a hydrogen atom, an oxygen atom, or a sulfur atom and which may be substituted by a hydroxy group, an alkenyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group, or a phenyl group, and the phenyl group may be substituted by at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, a nitro group, a cyano group, an alkylthio group having 1 to 6 carbon atoms, and a monovalent organic group represented by U in formula (1).

[0030] The alkyl group, alkenyl group, alkynyl group, halogen atom, alkoxy group and alkylthio group are as exemplified above.

[0031] Preferably, the R 15 represents an alkyl group having 1 to 10 carbon atoms or a monovalent organic group represented by U in formula (1), and p represents an integer of 2 to 4.

[0032] [ka]

[0033] In formula (2), R1 represents an alkylene group having 1 to 4 carbon atoms. Examples of the alkylene group include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, a cyclopropylene group, an n-butylene group, an isobutylene group, an s-butylene group, a t-butylene group, a cyclobutylene group, a 1-methyl-cyclopropylene group, and a 2-methyl-cyclopropylene group. A1 to A3 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and X represents any one of -COO-, -OCO-, -O-, -S-, and -NR1-. a - When expressing R a represents a hydrogen atom or a methyl group. Preferably, X is -S-.

[0034] In formula (2), Y represents an alkylene group having 1 to 4 carbon atoms which may be directly bonded or substituted. The alkylene group is as exemplified above, and Y is preferably a methylene group. R2, R3 and R4 each represent a hydrogen atom, or an optionally substituted alkyl group having 1 to 10 carbon atoms or an optionally substituted aryl group having 6 to 40 carbon atoms. The phrase "optionally substituted with a substituent" means that some or all of the hydrogen atoms present in the functional group to be substituted may be substituted with, for example, a hydroxy group, a halogen atom, a carboxyl group, a nitro group, a cyano group, a methylenedioxy group, an acetoxy group, a methylthio group, an amino group, or an alkoxy group having 1 to 9 carbon atoms. R5 is a hydrogen atom or a hydroxy group.

[0035] Examples of the aryl group include a phenyl group, an o-methylphenyl group, an m-methylphenyl group, a p-methylphenyl group, an o-chlorophenyl group, an m-chlorophenyl group, a p-chlorophenyl group, an o-fluorophenyl group, a p-fluorophenyl group, an o-methoxyphenyl group, a p-methoxyphenyl group, a p-nitrophenyl group, a p-cyanophenyl group, an α-naphthyl group, a β-naphthyl group, an o-biphenylyl group, an m-biphenylyl group, a p-biphenylyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group. m1 and m2 each independently represent an integer of 0 or 1, with m2 preferably being 1, and m1 preferably being 1. It is most preferred that when m2 is 1, m1 is 0.

[0036] The compound represented by formula (1) of the present application can be obtained, for example, by reacting an epoxy group or allyl group of the compound represented by the following formulae (a) to (ak) with 1-thioglycerol (3-mercapto-1,2-propanediol, CAS No. 96-27-5) by a known method, but is not limited thereto. Furthermore, the compound may contain a diol structure formed by hydrolysis of the epoxy group. The diol structure derived from the reaction of the epoxy group or allyl group with 1-thioglycerol is preferred, and the diol structure derived from the reaction of the epoxy group with 1-thioglycerol is more preferred. [ka] [ka]

[0037] Specific examples of the compound represented by formula (1) are as follows. The synthesis method is described in detail in the Examples section. (Theoretical molecular weight of the compound represented by formula (X-1): 799, Theoretical molecular weight of the compound represented by formula (X-2): 621, Theoretical molecular weight of the compound represented by formula (X-3): 471, Theoretical molecular weight of the compound represented by formula (X-4): 456, Theoretical molecular weight of the compound represented by formula (X-5): 573, Theoretical molecular weight of the compound represented by formula (X-6): 795) [ka] [ka] [ka] [ka] [ka] [ka]

[0038] The theoretical molecular weight of the compound represented by formula (1) is 400-999, and preferably 450-800.

[0039] <Organic solvent> The resist underlayer film forming composition of the present invention can be prepared by dissolving the above-mentioned components in an organic solvent, and is used in the state of a homogeneous solution.

[0040] As the organic solvent for the resist underlayer film-forming composition according to the present invention, any organic solvent can be used without particular limitation as long as it can dissolve the above-mentioned compounds and solid components such as the acid catalyst described below. In particular, since the protective film-forming composition according to the present invention is used in the state of a homogeneous solution, in consideration of its coating performance, it is recommended to use an organic solvent that is generally used in lithography processes in combination with the composition.

[0041] Examples of the organic solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone. Examples of the solvent include cyclopentane, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more.

[0042] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, cyclohexanone, etc. are preferred, with propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate being particularly preferred.

[0043] The resist underlayer film forming composition of the present application may further contain an acid catalyst (acid compound). As the acid catalyst, in addition to an acidic compound or a basic compound, a compound that generates an acid or a base by heat can be used. As the acidic compound, a sulfonic acid compound or a carboxylic acid compound can be used, and as a compound that generates an acid by heat, a thermal acid generator can be used.

[0044] Examples of the sulfonic acid compound or carboxylic acid compound include p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium trifluoromethanesulfonate (=pyridinium trifluoromethanesulfonic acid), pyridinium-p-toluenesulfonate, pyridinium-4-hydroxybenzenesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-phenolsulfonic acid, pyridinium-4-phenolsulfonate, benzenedisulfonic acid, 1-naphthalenesulfonic acid, 4-nitrobenzenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid.

[0045] Examples of thermal acid generators include K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, and TAG2689 (all manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (all manufactured by Sanshin Chemical Industry Co., Ltd.).

[0046] These acid catalysts can be used alone or in combination of two or more. As the basic compound, an amine compound or an ammonium hydroxide compound can be used, and as the compound that generates a base by heat, urea can be used.

[0047] Examples of the amine compound include tertiary amines such as triethanolamine, tributanolamine, trimethylamine, triethylamine, tri-normal propylamine, triisopropylamine, tri-normal butylamine, tri-tert-butylamine, tri-normal octylamine, triisopropanolamine, phenyldiethanolamine, stearyldiethanolamine, and diazabicyclooctane, and aromatic amines such as pyridine and 4-dimethylaminopyridine.Other examples of the amine compound include primary amines such as benzylamine and normal butylamine, and secondary amines such as diethylamine and di-normal butylamine.These amine compounds can be used alone or in combination of two or more.

[0048] Examples of ammonium hydroxide compounds include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, cetyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, and phenyltriethylammonium hydroxide.

[0049] As a compound that generates a base by heat, for example, a compound that has a thermolabile group such as an amide group, a urethane group, or an aziridine group and generates an amine by heating can be used. Other examples of the compound that generates a base by heat include urea, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylphenylammonium chloride, benzyldodecyldimethylammonium chloride, benzyltributylammonium chloride, and choline chloride.

[0050] When the resist underlayer film forming composition of the present application contains an acid catalyst, the content thereof is 0.0001 to 20 mass %, preferably 0.01 to 15 mass %, and more preferably 0.1 to 10 mass %, based on the total solid content of the resist underlayer film forming composition.

[0051] The solid content of the resist underlayer film forming composition according to the present invention is usually 0.1 to 70 mass%, preferably 0.1 to 60 mass%. The solid content is the content of all components excluding the solvent from the resist underlayer film forming composition. The proportion of the polymer in the solid content is preferably 1 to 100 mass%, 1 to 99.9 mass%, 50 to 99.9 mass%, 50 to 95 mass%, and 50 to 90 mass%, in that order.

[0052] <Crosslinking agent> The resist underlayer film forming composition of the present invention may contain a crosslinking agent. Examples of the crosslinking agent include melamine-based, substituted urea-based, and polymers thereof. A crosslinking agent having at least two crosslinking-forming substituents is preferred, and is a compound such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguwanamine, butoxymethylated benzoguwanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or methoxymethylated thiourea. Condensates of these compounds may also be used.

[0053] In addition, a crosslinking agent having high heat resistance can be used as the crosslinking agent. As the crosslinking agent having high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be used. Examples of such compounds include compounds having a partial structure of the following formula (5-1) and polymers or oligomers having a repeating unit of the following formula (5-2).

[0054] [ka]

[0055] Above R 11 , R 12 , R 13 , and R 14 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and specific examples of these alkyl groups are as described above. m1 is 1≦m1≦6-m2, m2 is 1≦m2≦5, m3 is 1≦m3≦4-m2, and m4 is 1≦m4≦3. Examples of the compounds, polymers and oligomers of the formula (5-1) and the formula (5-2) are shown below.

[0056] [ka]

[0057] [ka]

[0058] The above compounds are available as products from Asahi Yukizai Kogyo Co., Ltd. and Honshu Chemical Industry Co., Ltd. For example, among the above crosslinking agents, the compound of formula (6-22) is available from Honshu Chemical Industry Co., Ltd. under the trade name TMOM-BP.

[0059] The amount of the crosslinking agent added varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is usually 0.001 to 80 mass%, preferably 0.01 to 50 mass%, and more preferably 0.1 to 40 mass% based on the total solid content of the resist underlayer film-forming composition. These crosslinking agents may cause a crosslinking reaction by self-condensation, but when crosslinkable substituents are present in the above-mentioned polymer of the present invention, they can cause a crosslinking reaction with the crosslinkable substituents.

[0060] <Surfactant> The resist film-forming composition of the present invention may contain a surfactant to improve the coating property on a semiconductor substrate. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, and polyoxyethylene sorbitan monostearate. nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan trioleate and polyoxyethylene sorbitan tristearate; fluorosurfactants such as F-TOP (registered trademark) EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Megafac (registered trademark) F171, F173, R-30, R-30N, R-40, and R-40-LM (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by Sumitomo 3M Limited), Asahiguard (registered trademark) AG710, Surflon (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants can be used alone or in combination of two or more. When the protective film-forming composition contains a surfactant, the content thereof is 0.0001 to 10% by weight, preferably 0.01 to 5% by weight, based on the total solid content of the protective film-forming composition.

[0061] <Protective film forming composition> The protective film-forming composition of the present application is characterized by containing a compound represented by the following formula (1), having a theoretical average molecular weight of 999 or less and containing 2 or more, 3 or more, 4 or more nitrogen atoms and 6 or more, 8 or more, 9 or more, 10 or more, 15 or more oxygen atoms in the molecule, and an organic solvent. Furthermore, the compound preferably contains 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more sulfur atoms. The reason why the specific atoms are contained in a certain number or more is to improve the dry etching rate of the protective film.

[0062] [ka]

[0063] [In formula (1), Z1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4.]

[0064] [ka]

[0065] [In formula (2), R1 represents a single bond or an alkylene group having 1 to 4 carbon atoms, A1 to A3 each independently represent a hydrogen atom, a methyl group, or an ethyl group, and X represents -COO-, -OCO-, -O-, -S-, or -NR a - represents either R a represents a hydrogen atom or a methyl group; Y represents an alkylene group having 1 to 4 carbon atoms which may be directly bonded or substituted; R2, R3, and R4 each represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted, or an aryl group having 6 to 40 carbon atoms; R5 represents a hydrogen atom or a hydroxyl group; n represents an integer of 0 or 1; m1 and m2 each independently represent an integer of 0 or 1; and * represents a bonding site to Z1. It is preferable that m2 is 1, and more preferably, m1 is 1. It is most preferred that when m2 is 1, m1 is 0. Preferably, Z1 is represented by the following formula (3).

[0066] [ka] [In formula (3), Q3 represents the following formula (4), formula (5), or formula (6)]

[0067] [ka]

[0068] [In formula (4), formula (5) and formula (6), R 11 , R 12 , R 13 and R 14 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group is optionally substituted with at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 atoms, a nitro group, a cyano group and an alkylthio group having 1 to 6 carbon atoms. R 15 represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by a hydrogen atom, an oxygen atom or a sulfur atom and which may be substituted by a hydroxy group, an alkenyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 3 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group or a phenyl group, and the phenyl group may be substituted by at least one monovalent functional group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, a nitro group, a cyano group, an alkylthio group having 1 to 6 carbon atoms, and the monovalent organic group represented by U in formula (1). * represents a bonding portion to U.]

[0069] Preferably, the R 15 is an alkyl group having 1 to 10 carbon atoms or a monovalent organic group represented by U in formula (1). Preferably, the R 11 and R 12 are each independently an alkyl group having 1 to 10 carbon atoms. Preferably, X is -S-. Preferably, Y is a methylene group.

[0070] Preferably, the protective film-forming composition further contains an acid compound and / or a crosslinking agent. Preferably, the protective film-forming composition further contains a surfactant.

[0071] The acid catalyst, the content of the acid catalyst, and the organic solvent are the same as those in the above-mentioned resist underlayer film-forming composition.

[0072] The solid content of the protective film-forming composition according to the present invention is usually 0.1 to 70% by mass, preferably 0.1 to 60% by mass. The solid content is the content of all components excluding the solvent from the protective film-forming composition. The proportion of the polymer in the solid content is preferably 1 to 100% by mass, 1 to 99.9% by mass, 50 to 99.9% by mass, 50 to 95% by mass, and 50 to 90% by mass, in that order.

[0073] <Crosslinking agent> The protective film-forming composition of the present invention may contain a crosslinking agent, which may be the same as that used in the resist underlayer film-forming composition.

[0074] <Surfactant> The protective film-forming composition of the present invention may contain a surfactant in order to improve the coating property on the semiconductor substrate. The surfactant may be the same as that in the resist underlayer film-forming composition.

[0075] <Methods of manufacturing resist underlayer film, protective film, substrate with resist pattern, and semiconductor device> Hereinafter, a method for producing a substrate having a resist pattern and a method for producing a semiconductor device using the resist underlayer film-forming composition (protective film-forming composition) according to the present invention will be described.

[0076] The substrate having a resist pattern according to the present invention can be produced by applying the above-mentioned resist underlayer film-forming composition (protective film-forming composition) onto a semiconductor substrate and baking it.

[0077] Examples of semiconductor substrates to which the resist underlayer film forming composition (protective film forming composition) of the present invention is applied include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.

[0078] When a semiconductor substrate having an inorganic film formed on its surface is used, the inorganic film is formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin-coating (spin-on-glass: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, silicon oxynitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium oxynitride film, tungsten nitride film, gallium nitride film, and gallium arsenide film. The semiconductor substrate may be a stepped substrate having so-called vias (holes), trenches (grooves), and the like formed therein. For example, the via has an approximately circular shape when viewed from above, and the diameter of the approximately circular shape is, for example, 1 nm to 20 nm, and the depth is, for example, 50 nm to 500 nm, and the trench has, for example, a groove (recess in the substrate) with a width of 2 nm to 20 nm and a depth of 50 nm to 500 nm. The resist underlayer film-forming composition (protective film-forming composition) of the present application has a small theoretical average molecular weight and average particle size of the compound contained in the composition, and therefore the composition can be embedded in the above-mentioned uneven substrate without defects such as voids (gaps), etc. The absence of defects such as voids is an important property for the next steps in semiconductor manufacturing (wet etching / dry etching of the semiconductor substrate, resist pattern formation).

[0079] On such a semiconductor substrate, the resist underlayer film forming composition (protective film forming composition) of the present invention is applied by a suitable application method such as a spinner or coater. Then, the composition is baked using a heating means such as a hot plate to form a resist underlayer film (protective film). The baking conditions are appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 minutes to 60 minutes. Preferably, the baking temperature is 120°C to 350°C, the baking time is 0.5 minutes to 30 minutes, and more preferably, the baking temperature is 150°C to 300°C, and the baking time is 0.8 minutes to 10 minutes. The thickness of the protective film formed is, for example, 0.001 μm to 10 μm, preferably 0.002 μm to 1 μm, more preferably 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.05 μm (50 nm) to 0.3 μm (300 nm), or 0.05 μm (50 nm) to 0.2 μm (200 nm). If the baking temperature is lower than the above range, crosslinking may be insufficient, and the resist underlayer film (protective film) formed may be less resistant to resist solvents or basic hydrogen peroxide aqueous solutions. On the other hand, if the baking temperature is higher than the above range, the resist underlayer film (protective film) may be decomposed by heat.

[0080] Exposure is performed through a mask (reticle) for forming a predetermined pattern, and for example, i-rays, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet) or EB (electron beam) is used. An alkaline developer is used for development, and the development temperature is appropriately selected from 5°C to 50°C and the development time is appropriately selected from 10 seconds to 300 seconds. As the alkaline developer, for example, aqueous solutions of alkalis such as inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-butylamine, tertiary amines such as triethylamine and methyldiethylamine, alcohol amines such as dimethylethanolamine and triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, cyclic amines such as pyrrole and piperidine, etc. can be used. Furthermore, an appropriate amount of alcohols such as isopropyl alcohol and surfactants such as nonionic surfactants can be added to the aqueous solutions of the above alkalis. Among these, the preferred developer is a quaternary ammonium salt, more preferably tetramethylammonium hydroxide and choline. Furthermore, a surfactant or the like can be added to these developers. Instead of the alkaline developer, a method can be used in which development is performed with an organic solvent such as butyl acetate to develop the part of the photoresist where the alkaline dissolution rate is not improved.

[0081] Next, the resist underlayer film (protective film) is dry-etched using the formed resist pattern as a mask, whereby if the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and if the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed.

[0082] Furthermore, a desired pattern is formed by wet etching using a semiconductor wet etching solution, using the resist underlayer film (protective film) after dry etching (if a resist pattern remains on the resist underlayer film / protective film, the resist pattern as well) as a mask.

[0083] As the wet etching solution for semiconductors, a general chemical solution for etching semiconductor wafers can be used, and for example, either an acidic substance or a basic substance can be used.

[0084] Examples of substances that exhibit acidity include hydrogen peroxide, hydrofluoric acid, ammonium fluoride, acidic ammonium fluoride, ammonium hydrogen fluoride, buffered hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, and mixtures of these.

[0085] Examples of substances that exhibit basicity include basic hydrogen peroxide solution, which is obtained by mixing an organic amine such as ammonia, sodium hydroxide, potassium hydroxide, sodium cyanide, potassium cyanide, or triethanolamine with hydrogen peroxide solution to make the pH basic. A specific example is SC-1 (ammonia-hydrogen peroxide solution). Other substances that can make the pH basic, such as mixing urea with hydrogen peroxide solution and heating to cause thermal decomposition of the urea to generate ammonia, and finally making the pH basic, can also be used as a wet etching chemical.

[0086] Among these, acidic hydrogen peroxide solution or basic hydrogen peroxide solution is preferable.

[0087] These chemical solutions may contain additives such as a surfactant.

[0088] The temperature at which the semiconductor wet etching solution is used is preferably 25° C. to 90° C., and more preferably 40° C. to 80° C. The wet etching time is preferably 0.5 to 30 minutes, and more preferably 1 to 20 minutes. EXAMPLES

[0089] The present invention will now be described in detail with reference to Synthesis Examples and Examples, but the present invention is not limited to these. The weight average molecular weight of the polymer shown in the following synthesis examples of this specification is the result of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). For the measurement, a GPC device manufactured by Tosoh Corporation was used, and the measurement conditions are as follows. Column temperature: 40℃ Flow rate: 0.6mL / min Eluent: N,N-dimethylformamide (DMF) Standard sample: Polystyrene (Tosoh Corporation)

[0090] <Synthesis Example 1> A reaction flask containing 4.00 g of 1,3,4,6-(tetraglycidyl)glycouril (product name: TG-G, manufactured by Shikoku Chemical Industry Co., Ltd.), 6.26 g of 1-thioglycerol (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), 0.54 g of tetrabutylphosphonium bromide (manufactured by Hokko Chemical Co., Ltd.), and 43.26 g of propylene glycol monomethyl ether was heated and stirred at 105°C for 22 hours under a nitrogen atmosphere. The obtained reaction product corresponds to formula (X-1), has a theoretical molecular weight of 799, and has a weight average molecular weight Mw of 980 measured in terms of polystyrene by GPC.

[0091] [ka]

[0092] <Synthesis Example 2> A reaction flask containing 5.00 g of triglycidyl isocyanuric acid (product name TEPIC, manufactured by Nissan Chemical Industries, Ltd.), 5.45 g of 1-thioglycerol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 0.21 g of tetrabutylphosphonium bromide (manufactured by Hokko Chemical Industries, Ltd.), and 42.68 g of propylene glycol monomethyl ether was heated and stirred at 105°C for 23 hours under a nitrogen atmosphere. The obtained reaction product corresponds to formula (X-2), has a theoretical molecular weight of 621, and has a weight average molecular weight Mw of 870 measured in terms of polystyrene by GPC.

[0093] [ka]

[0094] <Synthesis Example 3> A reaction flask containing 16.00 g of diglycidyl methylisocyanurate (product name: MeDGIC, manufactured by Shikoku Chemical Industry Co., Ltd., 28.8 wt% propylene glycol monomethyl ether solution), 3.88 g of 1-thioglycerol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 0.45 g of tetrabutylphosphonium bromide (manufactured by Hokko Chemical Co., Ltd.), and 24.52 g of propylene glycol monomethyl ether was heated and stirred at 105°C for 18 hours under a nitrogen atmosphere. The obtained reaction product corresponds to formula (X-3), has a theoretical molecular weight of 471, and has a weight average molecular weight Mw of 600 measured in terms of polystyrene by GPC.

[0095] [ka]

[0096] <Synthesis Example 4> A solution of 3.00 g of glycerin monomethacrylate (product name: Blenmer GLM, manufactured by NOF Corporation), 0.90 g of 2,2'-azobis(methyl isobutyrate) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and 16.44 g of propylene glycol monomethyl ether was added to a dropping funnel, and the solution was dropped into a reaction flask containing 4.11 g of propylene glycol monomethyl ether at 100°C under a nitrogen atmosphere, and heated and stirred for 15 hours. The resulting reaction product corresponded to formula (X-7), and the weight average molecular weight Mw measured in terms of polystyrene by GPC was 4160.

[0097] [ka]

[0098] <Synthesis Example 5> A reaction flask containing 11.00 g of diglycidyl methylisocyanurate (product name: MeDGIC, manufactured by Shikoku Chemical Industry Co., Ltd., 28.8 wt% propylene glycol monomethyl ether solution), 1.16 g of succinic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.53 g of 1-thioglycerol (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.), 0.29 g of ethyltriphenylphosphonium bromide (manufactured by Tokyo Chemical Industry Co., Ltd.), and 12.85 g of propylene glycol monomethyl ether was heated and stirred at 100°C for 18 hours under a nitrogen atmosphere. The obtained reaction product corresponds to the formula (X-8), and the weight average molecular weight Mw measured in terms of polystyrene by GPC was 2800.

[0099] [ka]

[0100] <Example 1> 0.06 g of pyridinium trifluoromethanesulfonate (Tokyo Chemical Industry Co., Ltd.), 0.01 g of a surfactant (product name: Megafac R-40, DIC Corporation), 18.84 g of propylene glycol monomethyl ether, and 2.87 g of propylene glycol monomethyl ether acetate were added to 8.22 g of a solution (solid content: 15.5 wt%) of the reaction product corresponding to the formula (X-1) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0101] <Example 2> 0.06 g of pyridinium trifluoromethanesulfonate (Tokyo Chemical Industry Co., Ltd.), 0.01 g of a surfactant (product name: Megafac R-40, DIC Corporation), 19.90 g of propylene glycol monomethyl ether, and 2.87 g of propylene glycol monomethyl ether acetate were added to 7.12 g of a solution (solid content: 17.8 wt%) of the reaction product corresponding to the formula (X-2) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0102] <Example 3> 0.06 g of pyridinium trifluoromethanesulfonate (Tokyo Chemical Industry Co., Ltd.), 0.01 g of a surfactant (product name: Megafac R-40, DIC Corporation), 19.94 g of propylene glycol monomethyl ether, and 2.87 g of propylene glycol monomethyl ether acetate were added to 7.12 g of a solution (solid content: 17.9 wt%) of the reaction product corresponding to the formula (X-3) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0103] <Example 4> 0.17g of 3,3',5,5'-tetrakis(methoxymethyl)-4,4'-dihydroxybiphenyl (product name: TMOM-BP, manufactured by Honshu Chemical Industry Co., Ltd.), 0.06g of pyridinium trifluoromethanesulfonate (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.01g of a surfactant (product name: Megafac R-40, manufactured by DIC Corporation), 19.47g of propylene glycol monomethyl ether, and 2.87g of propylene glycol monomethyl ether acetate were added to 6.32g of a solution (solid content: 17.8% by weight) of the reaction product corresponding to the formula (X-2) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0104] <Comparative Example 1> 0.03 g of pyridinium trifluoromethanesulfonate (Tokyo Chemical Industry Co., Ltd.), 0.01 g of a surfactant (product name: Megafac R-40, DIC Corporation), 9.21 g of propylene glycol monomethyl ether, and 1.44 g of propylene glycol monomethyl ether acetate were added to 4.32 g of a solution (solid content: 13.1 wt%) of the reaction product corresponding to the formula (X-7) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0105] <Comparative Example 2> 0.21 g of 3,3',5,5'-tetrakis(methoxymethyl)-4,4'-dihydroxybiphenyl (product name: TMOM-BP, manufactured by Honshu Chemical Industry Co., Ltd.), 0.01 g of pyridinium-4-hydroxybenzenesulfonate, 0.01 g of surfactant (product name: Megafac R-40, manufactured by DIC Corporation), 20.82 g of propylene glycol monomethyl ether, and 2.87 g of propylene glycol monomethyl ether acetate were added to 6.09 g of the solution of the reaction product corresponding to the formula (X-8) (solid content: 17.5 wt%) to obtain a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a resist underlayer film (protective film) forming composition.

[0106] [Resist Solvent Resistance Test] Each of the resist underlayer film (protective film) forming compositions prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was applied (spin-coated) onto a silicon wafer using a spin coater. The silicon wafer after application was heated on a hot plate at 220°C for 1 minute to form a coating (protective film) with a thickness of 100 nm. Next, in order to confirm the resist solvent resistance of the protective film, the silicon wafer after the protective film formation was immersed in a solvent in which propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate were mixed at a weight ratio of 7:3 for 1 minute, spin-dried, and then baked at 100°C for 30 seconds. The thickness of the protective film before and after immersion in the mixed solvent was measured using an optical interference film thickness meter (product name: Nanospec 6100, manufactured by Nanometrics Japan Co., Ltd.).

[0107] Resist solvent resistance was evaluated by calculating the percent reduction in thickness of the protective film removed by solvent immersion using the formula: ((film thickness before solvent immersion) - (film thickness after solvent immersion)) ÷ (film thickness before solvent immersion) x 100. The results are shown in Table 1. It should be noted that a film thickness reduction rate of approximately 1% or less can be said to have sufficient resist solvent resistance.

[0108] [Table 1]

[0109] From the above results, the resist underlayer films (protective films) of Examples 1 to 4 and Comparative Examples 1 and 2 showed very little change in film thickness even after immersion in a resist solvent. Therefore, the protective film-forming compositions of Examples 1 to 4 have sufficient resist solvent resistance to function as resist underlayer films.

[0110] [Test for resistance to basic hydrogen peroxide] To evaluate resistance to basic hydrogen peroxide solution, each of the resist underlayer film-forming compositions (protective film-forming compositions) prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was applied to a titanium nitride (TiN) vapor-deposited substrate having a thickness of 50 nm, and heated at 220°C for 1 minute to form a protective film having a thickness of 100 nm. Next, 28% ammonia water, 33% hydrogen peroxide, and water were mixed in a weight ratio of 1:4:20, respectively, to prepare basic hydrogen peroxide solution. The TiN vapor-deposited substrate coated with the resist underlayer film-forming composition (protective film-forming composition) was immersed in this basic hydrogen peroxide solution heated to 50°C, and the time (peeling time) from immediately after immersion until the protective film was completely peeled off from the substrate was measured. The results of the resistance test to basic hydrogen peroxide solution are shown in Table 2. It can be said that the longer the peeling time, the higher the resistance to the wet etching solution using basic hydrogen peroxide solution.

[0111] [Table 2]

[0112] The results in the above table show that the coating films prepared using the resist underlayer film-forming compositions (protective film-forming compositions) prepared in Examples 1 to 4 have sufficient resistance to a basic hydrogen peroxide aqueous solution. That is, it was found that these coating films can serve as protective films against a basic hydrogen peroxide aqueous solution. Moreover, it can be said that Examples 1 to 4 show better resistance to a wet etching solution using a basic hydrogen peroxide aqueous solution than Comparative Examples 1 and 2. Therefore, Examples 1 to 4 show better chemical solution resistance to a basic hydrogen peroxide aqueous solution than Comparative Examples 1 and 2, and are therefore more useful as protective films against a wet etching solution for semiconductors.

[0113] [Evaluation of etching selectivity] For the evaluation of the etching selectivity, each of the resist underlayer film forming compositions (protective film forming compositions) prepared in the above-mentioned Examples 1 to 4 and Comparative Example 1 was applied onto a silicon wafer and heated at 220° C. for 1 minute to form a protective film with a thickness of 100 nm. Next, the formed protective film was dry-etched using a dry etching apparatus (product name: RIE-10NR, manufactured by Samco Inc.) with chlorine gas and a mixed gas of nitrogen gas and hydrogen gas to measure the dry etching rate ratio (selective ratio of dry etching rate) of the protective film. The measurement results of the etching selectivity are shown in Table 3. It can be said that the higher the etching selectivity, the faster the dry etching rate.

[0114] [Table 3]

[0115] From the above results, it can be said that Examples 1 to 4 have a higher dry etching selectivity and therefore a faster dry etching rate than Comparative Example 1. That is, Examples 1 to 4 are useful because they can reduce the dry etching time required to remove the protective film and therefore reduce damage to the underlying substrate.

[0116] That is, Examples 1 to 4 have better resistance to a wet etching solution for semiconductors using a basic hydrogen peroxide solution than Comparative Examples 1 and 2, and have a faster etching rate than Comparative Example 1. Therefore, according to the present invention, it is possible to provide a protective film-forming composition that has both high wet etching solution resistance and a high etching rate.

[0117] [Evaluation of optical parameters] The resist underlayer film-forming compositions (protective film-forming compositions) prepared in Examples 1 to 3 and Comparative Examples 1 to 2 described herein were each applied (spin-coated) onto a silicon wafer using a spin coater. The applied silicon wafer was heated on a hot plate at 220° C. for 1 minute to form a protective film-forming composition (film thickness 100 nm). Then, the n value (refractive index) and k value (attenuation coefficient or absorption coefficient) of these protective film-forming compositions at a wavelength of 193 nm were measured using a spectroscopic ellipsometer (product name: VUV-VASE VU-302, manufactured by JA Woollam Co., Ltd.). The measurement results of the optical parameters are shown in Table 4.

[0118] [Table 4]

[0119] [Measurement of the amount of sublimation] The amount of sublimation was measured using a sublimation amount measuring device described in International Publication No. 2007 / 111147. First, the resist underlayer film forming compositions prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were applied to a silicon wafer substrate having a diameter of 4 inches using a spin coater so as to give a film thickness of 100 nm. The wafer coated with the resist underlayer film was set in the sublimation amount measuring device integrated with a hot plate and baked for 120 seconds, and the sublimation was collected in a QCM (Quartz Crystal Microbalance) sensor, that is, a quartz oscillator with an electrode formed thereon. The QCM sensor can measure minute changes in mass by utilizing the property that when a sublimation adheres to the surface (electrode) of a quartz oscillator, the frequency of the quartz oscillator changes (decreases) depending on the mass of the sublimation.

[0120] The detailed measurement procedure is as follows. The hot plate of the sublimation amount measurement device is heated to the measurement temperature shown in Table 5, and the pump flow rate is set to 2.4 m 3 / s, and the device was left for the first 60 seconds to stabilize. Immediately after that, the wafer coated with the resist underlayer film was quickly placed on the hot plate from the slide port, and the sublimate was collected from the 60 second point to the 180 second point (120 seconds). The flow attachment (detection part) that connects the QCM sensor and the collection funnel part of the sublimate amount measurement device was used without a nozzle, so that the air flow flows in without being throttled from the flow path (diameter: 32 mm) of the chamber unit with a distance of 30 mm from the sensor (quartz crystal oscillator). In addition, the QCM sensor used had a material (AlSi) mainly composed of silicon and aluminum as an electrode, a diameter of the quartz crystal oscillator (sensor diameter) of 14 mm, an electrode diameter on the surface of the quartz crystal oscillator of 5 mm, and a resonance frequency of 9 MHz. The obtained frequency change was converted into grams from the characteristic value of the quartz crystal resonator used in the measurement, and the relationship between the amount of sublimation of one wafer coated with the resist underlayer film and the passage of time was clarified. The first 60 seconds was a time period during which the device was left to stabilize (no wafer was set), and the measured values ​​from 60 seconds after the wafer was placed on the hot plate to 180 seconds were the measured values ​​related to the amount of sublimation of the wafer. The amount of sublimation of the resist underlayer film quantified from the device is shown in Table 5 as a sublimation amount ratio. The amount of sublimation is shown by converting the value of Comparative Example 1 to 1.

[0121] [Table 5]

[0122] [Evaluation of embeddability into substrate] A resist underlayer film-forming composition was applied onto a silicon processed substrate (after silicon oxide film deposition: 10 nm trench (L (line) / S (space))) on which a silicon oxide film was formed on the surface of the trench, which was prepared by depositing a silicon oxide film of about 20 nm by a CVD method on a silicon substrate on which a 50 nm trench (L (line) / S (space)) was formed. The substrate was then heated on a hot plate at 220°C for 1 minute to form a resist underlayer film with a film thickness of about 100 nm. A scanning electron microscope (SEM) was used to observe the cross-sectional shape (Figure 1) of the substrate having a trench on which the resist underlayer film-forming composition obtained in Example 2 was applied, thereby evaluating the embeddability. It was found that the resist underlayer film-forming composition of the example was embedded into the 10 nm trench (L (line) / S (space)) substrate, which is the gap of the silicon oxide film, without generating voids (air gaps, etc.) (Figure 2). [Industrial Applicability]

[0123] The resist underlayer film forming composition or protective film forming composition of the present invention is useful as a resist underlayer film in a semiconductor lithography process, and further as a protective film when a semiconductor substrate is subjected to wet etching.

Claims

1. A resist underlayer film-forming composition comprising a compound represented by the following formula (1) and having a theoretical molecular weight of 999 or less, and an organic solvent: 【Chemical Formula 34】 [In formula (1), Z 1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4. 【Chemistry 35】 [In formula (2), * represents Z 1 The bond to the The resist underlayer film forming composition, wherein Z 1 is represented by the following formula (3): 【Chemical 36】 [In formula (3), Q 3 represents the following formula (6)] 【Chemical 37】 [In formula (6), R 15 represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom and which may be substituted by a hydroxy group.

2. The resist underlayer film forming composition described in claim 1, further comprising an acid compound and / or a crosslinking agent.

3. A resist underlayer film forming composition according to claim 1 or 2, further comprising a surfactant.

4. A resist underlayer film, which is a fired product of a coating film comprising the resist underlayer film forming composition according to any one of claims 1 to 3.

5. A protective film forming composition for a semiconductor wet etching solution which is a basic aqueous hydrogen peroxide solution, comprising a compound represented by the following formula (1), having a theoretical molecular weight of 999 or less and containing two or more nitrogen atoms and six or more oxygen atoms in the molecule, and an organic solvent. 【Chemical Formula 38】 [In formula (1), Z 1 contains a nitrogen-containing heterocycle, U is a monovalent organic group represented by the following formula (2), and p is an integer of 2 to 4.] 【Chemical 39】 [In formula (2), * indicates the bond to Z 1 ] The protective film-forming composition, wherein Z 1 is represented by the following formula (3): 【Chemistry 40】 [In formula (3), Q 3 represents the following formula (6)] 【Chemistry 41】 [In formula (6), R 15 represents an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom and which may be substituted by a hydroxy group.]

6. A protective film forming composition as described in claim 5, further comprising an acid compound and / or a crosslinking agent.

7. A protective film characterized by being a fired product of a coating film made of the protective film-forming composition described in claim 5 or 6.

8. A method for producing a substrate with a resist pattern, comprising the steps of applying the resist underlayer film forming composition described in any one of claims 1 to 3 onto a semiconductor substrate and baking the composition to form a resist underlayer film, forming a resist film on the resist underlayer film, and then exposing and developing the resist film to form a resist pattern, the method being used in the production of semiconductors.

9. A method for manufacturing a semiconductor device, comprising the steps of forming a resist underlayer film on a semiconductor substrate, which may have an inorganic film formed on its surface, using the resist underlayer film forming composition described in any one of claims 1 to 3, forming a resist pattern on the resist underlayer film, dry etching the resist underlayer film using the resist pattern as a mask to expose a surface of the inorganic film or the semiconductor substrate, and etching the inorganic film or the semiconductor substrate using the resist underlayer film after dry etching as a mask.

10. A method for manufacturing a semiconductor device, comprising the steps of forming a protective film on a semiconductor substrate, which may have an inorganic film formed on its surface, using the protective film forming composition described in claim 5 or 6, forming a resist pattern on the protective film, dry etching the protective film using the resist pattern as a mask to expose the surface of the inorganic film or the semiconductor substrate, and wet etching and cleaning the inorganic film or the semiconductor substrate using a semiconductor wet etching solution which is a basic aqueous hydrogen peroxide solution, using the protective film after dry etching as a mask.

Citation Information

Patent Citations

  • Composition for forming resist underlayer film and method of forming resist pattern using the same

    JP2010237491A

  • Protective film-forming composition having diol structure

    WO2019124474A1

  • Resist underlayer film formation composition having disulfide structure

    WO2019151471A1