Roughening sheet, formwork panel using same, and method for manufacturing concrete body using said formwork panel
A woven or knitted fabric with a thermoplastic resin layer transfers an uneven pattern to the concrete surface, addressing the inefficiencies of existing methods by providing controlled roughening and reducing damage, while ensuring effective mortar adhesion and tile stability.
Patent Information
- Application Number
- JP2020168711
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-05
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-10-05
AI Technical Summary
Existing methods for roughening concrete surfaces to enhance mortar adhesion are time-consuming, labor-intensive, and result in scattering particles, damage to the site, and economic and environmental issues with reusable sheets.
A roughening sheet composed of a woven or knitted fabric with multifilaments and a laminated thermoplastic resin layer, which transfers an uneven pattern to the concrete surface, is used in conjunction with a formwork panel to create irregularities.
The method allows for controlled roughening with high accuracy, reduces damage during demolding, and facilitates reuse of the sheet, enhancing mortar adhesion and tile stability.
Smart Images

Figure 0007571967000004 
Figure 0007571967000005 
Figure 0007571967000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a roughening sheet for roughening the surface of a concrete body, a formwork panel using the same, and a method for manufacturing a concrete body using the formwork panel. [Background technology]
[0002] Concrete structures are used in buildings such as apartment buildings. Some concrete structures have a concrete framework (hereafter referred to as the concrete framework) on the surface of which mortar is applied as a base (hereafter referred to as the mortar base), and tiles are then attached on top of the mortar.
[0003] If the surface of the concrete structure after hardening is smooth, the mortar base will not adhere well, and the tile and mortar base will peel off, which will cause the tiles to easily fall off the building over time, creating a great danger. Therefore, in order to increase the adhesion between the concrete surface and the mortar, a roughening method has been used in which high-pressure water is sprayed onto the hardened concrete using a high-pressure washer or the like to roughen the concrete surface (Patent Document 1).
[0004] In recent years, a simpler method has been proposed in which a sheet with projections and recesses is attached to the inside of a formwork used when pouring concrete, thereby embossing the projections and recesses onto the concrete surface (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2004-092216 [Patent Document 2] Patent Publication No. 2006-336229 Summary of the Invention [Problem to be solved by the invention]
[0006] The method described in Patent Document 1 is good in terms of the adhesion of mortar, but has problems such as being time-consuming and putting a strain on the workers, the fine scraping of the concrete surface causes chips to fly around the site, which requires care in the area around the site, the need for curing as a countermeasure, and variation in the accuracy of the roughening.
[0007] According to the method described in Patent Document 2, special equipment and on-site curing are no longer necessary. However, there is still a problem in that the work of attaching the sheet to the formwork at the construction site is time-consuming. In addition, there are cases where a part of the sheet is damaged during removal from the formwork and remains attached to the surface of the concrete structure. If the sheet remains, there is a problem that the adhesive strength between the mortar base and the concrete structure is reduced when the mortar base is applied to the surface of the concrete structure in the later process. In addition, since the sheet is damaged, it is difficult to reuse it and it must be discarded, which is problematic in terms of economic rationality and environmental consideration.
[0008] The present invention aims to provide a roughening sheet that can roughen the surface of a concrete body in a simple manner, that allows control of the roughening accuracy, and that is not easily damaged when removed from the form, a formwork panel equipped with said roughening sheet, and a method for manufacturing a concrete body using said formwork panel. [Means for solving the problem]
[0009] The above problem can be solved by a roughening sheet which comprises a woven or knitted fabric using multifilaments and a sheet-like thermoplastic resin layer laminated on at least one side of the woven or knitted fabric, the woven or knitted fabric having an uneven pattern caused by the rise and fall of the multifilaments, and which imparts unevenness to the surface of a concrete structure by transferring the uneven pattern of the woven or knitted fabric via the thermoplastic resin layer.
[0010] The above problems can also be solved by a formwork panel in which the roughening sheet is attached to plywood.
[0011] In addition, the above-mentioned problems can be solved by a method for manufacturing a concrete body in which concrete is poured into a formwork assembled using the formwork panels, and after the concrete has hardened, the formwork with the roughening sheet attached is removed, thereby transferring the uneven pattern of the roughening sheet to the surface of the hardened concrete body, forming unevenness.
[0012] In the above-mentioned method for producing the roughening sheet, the formwork panel, or the concrete body, it is preferable that both the multifilament and the thermoplastic resin layer are made of polyolefin resin. It is also preferable that the thickness of the thermoplastic resin layer is 30 to 150 μm. It is also preferable that the thermoplastic resin layer is laminated on the woven or knitted fabric by extrusion lamination. It is also preferable that the above-mentioned formwork panel is made by bonding the roughening sheet and the plywood with an adhesive. Effect of the Invention
[0013] According to the present invention, it is possible to provide a roughening sheet that can roughen the surface of a concrete body in a simple manner, that can control the accuracy of the roughening, and that is less likely to be damaged when removed from the form, a formwork panel equipped with said roughening sheet, and a method for manufacturing a concrete body using said formwork panel. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic diagram showing one embodiment of a roughening sheet. [Diagram 2] A schematic diagram showing a cross section of concrete during construction using the roughening sheet of Figure 1. [Diagram 3] FIG. 1 is a diagram showing the configuration of a specimen used in a strain tracking test. [Figure 4] This is an example of a graph used to determine the elongation percentage T until the tile completely peels off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Below, we will explain one embodiment of the roughening sheet of the present invention (hereinafter sometimes simply referred to as the sheet) and a method of manufacturing a concrete body using the roughening sheet. However, the technical scope of the present invention is not limited to this embodiment, and the configuration can be appropriately changed depending on the construction content, etc.
[0016] 1 and 2 show an embodiment of the roughening sheet. As shown in FIG. 1, the roughening sheet 1 of this embodiment is formed by laminating a thermoplastic resin layer 3 on a woven or knitted fabric 2 using multifilaments. As will be described in detail later, in the roughening sheet 1 of this embodiment, a thermoplastic resin layer 3 is arranged on one side, and a protective layer 7 is arranged on the other side. In the example of FIG. 2, the roughening sheet 1 made of a woven or knitted fabric 2 of multifilaments 4 in which a thermoplastic resin layer 3 and a protective layer 7 are laminated is fixed to a plywood 8 by an adhesive 6 so that the protective layer 7 faces the plywood 8, forming a formwork panel. When concrete is poured as a formwork, concrete 5 is filled so as to contact the surface of the thermoplastic resin layer 3.
[0017] As the multifilament, a drawn yarn formed by a known manufacturing method can be used. The multifilament is a yarn made by combining a large number of low-fineness single yarns (for example, 30 to 200 yarns). Woven or knitted fabrics using the multifilament have strength and flexibility, and are easy to handle. In addition, since the multifilament is twisted in a bundled state so that the individual single yarns do not come apart, the cross section is approximately circular, and the woven or knitted fabric using the multifilament is more likely to have an uneven surface than a woven or knitted fabric using a flat yarn, making it ideal as a roughening sheet.
[0018] The main raw material constituting the multifilament is not particularly limited and may be appropriately selected from thermoplastic resins such as polyester, polyamide, polyolefin, polyvinyl alcohol, etc., but it is particularly desirable to use a polyolefin-based resin. Polyolefin-based resins have a small specific gravity, and can finish the woven or knitted fabric into a light and strong sheet. In addition, for the reasons described below, the thermoplastic resin layer is preferably a polyolefin-based resin, and if it is intended to firmly bond the woven or knitted fabric and the thermoplastic resin layer by extrusion lamination, it is preferable that both the multifilament and the thermoplastic resin are polyolefin-based resins. As the polyolefin-based resin, for example, polyethylene-based resins such as linear low-density polyethylene, branched low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid alkyl ester copolymer, or ethylene-α-olefin copolymer produced by a metallocene catalyst; or polypropylene-based resins such as polypropylene, propylene-ethylene block copolymer, or propylene-ethylene random copolymer, etc. are used. These may be used alone or in a mixture of two or more kinds. Among these, polypropylene is preferable because it can obtain high strength by the stretching effect.
[0019] The fineness of the multifilament is not particularly limited, but is preferably in the range of 300 to 3,000 decitex (hereinafter referred to as dt), and more preferably in the range of 500 to 2,000 dt. If the fineness is less than 300 dt, the mechanical properties of the woven or knitted fabric may be insufficient, and the surface unevenness may be insufficient when the fabric is made into a woven or knitted fabric, which is not preferable. In addition, if the fineness exceeds 3,000 dt, the flexibility may be insufficient, which is not preferable. The twist applied to the multifilament is appropriately selected, but is preferably in the range of 15 to 200 times / m, and if it is less than 15 times / m, the single yarns are likely to come apart, and the surface unevenness may be insufficient when the fabric is made into a woven or knitted fabric, which is not preferable. In addition, if the number of twists exceeds 200 times / m, the flexibility is impaired, and in extrusion lamination, the thermoplastic resin layer is unlikely to be entangled with the multifilament, making it difficult to obtain sufficient adhesion.
[0020] The multifilaments are woven to form a woven or knitted fabric. In the sheet of this embodiment, the multifilaments constituting the woven or knitted fabric rise and fall regularly, so that the multifilaments cross and overlap with each other. The uneven pattern caused by the rise and fall of the multifilaments is utilized to impart unevenness to the surface of the concrete structure. Examples of weaving structures when the multifilaments are used to make a woven fabric include plain weave, twill weave, leno weave, and imitation weave. Examples of knitting structures when the multifilaments are used to make a knitted fabric include weft knitting and warp knitting, and specific examples include tricot knitting, Milanese knitting, and Russell knitting.
[0021] In the case of woven or knitted fabrics, it is desirable that the surface has a concave-convex pattern with sufficient height differences, that the arrangement of the concave-convex pattern is as uniform as possible, and that the woven or knitted fabric has little stretch or shrinkage so that the thermoplastic resin layer can be easily laminated. For these reasons, woven fabrics are more preferable than knitted fabrics.
[0022] If the weave or stitch of the woven or knitted fabric is made into a coarse mesh with large openings, the thermoplastic resin layer may be easily torn at the weave or stitch part. In addition, it may be difficult to ensure the adhesive strength between the woven or knitted fabric and the thermoplastic resin layer. If a coarse mesh is used as a roughening sheet, concrete may be excessively embedded in the weave or stitch part, making it difficult to remove the woven or knitted fabric from the concrete after hardening. Therefore, it is particularly preferable that the woven or knitted fabric has a plain weave or twill weave structure, and at least one of the warp threads or weft threads is woven so as to fill the gaps. For example, the interval between the convex parts transferred to the concrete is preferably in the range of 0.5 mm to 5 mm, and the laying density in the case of making the woven fabric is preferably in the range of 10 to 30 threads / 2.54 cm, more preferably in the range of 14 to 22 threads / 2.54 cm. It is considered that the laying density affects the interval between the convex parts transferred to the concrete, and also affects the peeling resistance of the tile when the tile is attached to the poured concrete. From this viewpoint, it is preferable that the laying density is in the above range.
[0023] In the roughening sheet of this embodiment, a sheet-shaped thermoplastic resin layer is laminated on the woven or knitted fabric made of the multifilament. The thermoplastic resin layer is a layer provided on one side of the woven or knitted fabric, and is a layer that is brought into contact with the concrete to be roughened. If the woven or knitted fabric is brought into direct contact with the concrete in transferring the uneven pattern of the woven or knitted fabric, the fibers of the multifilament will bite into the concrete, making it difficult to peel it off from the concrete. Even if it can be peeled off from the concrete, the fibers will remain on the concrete side, causing a decrease in the quality of the concrete structure and causing defects when attaching tiles in a later process. In addition, the fibers will be damaged in the process of peeling off from the concrete, and pieces of concrete will remain in the fibers, making it difficult to reuse the roughening sheet. Furthermore, by applying the multifilament, which is an aggregate of thin fibers, to the surface of the concrete before it hardens, it may absorb moisture from the concrete and inhibit the hardening of the concrete.
[0024] Regarding the resin used in the thermoplastic resin layer, there is no particular restriction on the main raw material used, and it may be appropriately selected from the same thermoplastic resin as the material constituting the multifilament. In particular, the resin used in the thermoplastic resin layer is preferably a resin having a high affinity with the resin used in the multifilament constituting the woven or knitted fabric. The roughening sheet of this embodiment needs to be peeled off from the surface of the concrete building block after the concrete has hardened. If the peel strength between the woven or knitted fabric and the thermoplastic resin layer is weak at that time, the sheet may peel off between the woven or knitted fabric and the thermoplastic resin layer depending on the conditions. In order to obtain a high affinity, it is preferable that the resins are the same, and it is preferable that both the multifilament and the thermoplastic resin layer are resins of the same system. In addition, when the roughening sheet is peeled off from the surface of the concrete building block, it is desirable that the concrete does not adhere firmly to the thermoplastic resin layer. From this point of view, it is preferable that the thermoplastic resin layer is hydrophobic. In addition, in order to transfer the uneven pattern of the woven or knitted fabric to the surface of the concrete building block, it is preferable that the thermoplastic resin layer has flexibility so as to follow the uneven pattern of the woven or knitted fabric. Furthermore, since concrete is highly alkaline, it is preferable that the thermoplastic resin layer in contact with the concrete surface has alkali resistance. From these viewpoints, the resin used for the thermoplastic resin layer is preferably a polyolefin-based resin. When peeling the sheet from the surface of the concrete structure, the thermoplastic resin layer is more difficult to break and less likely to leave fragments if it is stretchable, so it is more preferable that the thermoplastic resin layer contains a polyolefin-based thermoplastic elastomer.
[0025] The resin constituting the roughening sheet may contain commonly used additives such as antioxidants, UV absorbers, light stabilizers, dispersants, lubricants, antistatic agents, pigments, inorganic fillers, crosslinking agents, foaming agents, and nucleating agents, as long as the addition does not deviate from the spirit of the present invention.
[0026] The thermoplastic resin layer may be laminated by a known method such as extrusion lamination, calendaring, coating, or dipping. The uneven pattern of the woven or knitted fabric must be reflected on the surface of the thermoplastic resin layer, and the thermoplastic resin layer must be laminated so as to conform to the uneven pattern of the woven or knitted fabric. Therefore, the thermoplastic resin layer is preferably laminated by extrusion lamination.
[0027] The extrusion lamination method is a method in which a thermoplastic resin is extruded in a molten state onto a substrate in the form of a film, and cooled and pressed to form a laminate. According to the extrusion lamination method, not only is the molten resin penetrated into the substrate, but the layers can be bonded and laminated by utilizing the affinity between the molten resin and the substrate. If the thermoplastic resin layer is laminated by penetrating the substrate with high pressure, the uneven pattern of the woven or knitted fabric will be damaged, so it is preferable to laminate using the affinity between the molten resin and the substrate in combination. According to lamination by the extrusion lamination method, the molten resin penetrates the woven or knitted fabric appropriately, so that the multifilament is not completely fixed, and the roughening sheet is formed in a state in which the multifilament has a degree of freedom. The roughening sheet is used to give the concrete surface an uneven shape, but if the uneven pattern of the roughening sheet penetrates into the concrete more than necessary, it becomes difficult to remove the roughening sheet after hardening, and the sheet is pulled by the concrete surface, and depending on the conditions, the sheet may be damaged. If the multifilaments retain some degree of freedom, even if the uneven pattern cuts into the concrete, the multifilaments may be able to deform, preventing the sheet from being damaged.
[0028] The thickness of the thermoplastic resin layer is not particularly limited. However, if the thickness of the thermoplastic resin layer is too thick, depending on the conditions, it may be difficult to reflect the uneven pattern of the woven or knitted fabric on the surface of the roughened sheet. Also, if the thickness is too thin, depending on the conditions, it may be difficult to obtain sufficient adhesion between the thermoplastic resin layer and the woven or knitted fabric, and the thermoplastic resin layer may be easily damaged. Therefore, the thickness of the thermoplastic resin layer is preferably about 30 to 150 μm.
[0029] The tensile strength or tear strength of the roughening sheet is not particularly limited, and does not need to be extremely high. However, the roughening sheet needs to be peeled off from the surface of the concrete body after the concrete hardens. In order to reliably prevent damage to the sheet, it is preferable that the tensile strength and tear strength are somewhat high. If these are low, it is assumed that the roughening sheet may break and remain on the concrete body when peeled off from the surface of the concrete body under certain conditions. As will be described later, when the roughening sheet is used by attaching it to plywood, wrinkles may occur in the roughening sheet. When the sheet is peeled off, stress is concentrated in the wrinkled parts, making the sheet more likely to break. The roughening sheet of this embodiment uses a multifilament woven or knitted fabric, and can have a high tensile strength. This can solve the above-mentioned problem of breakage. In addition, if the tensile strength of the roughening sheet is high, the effect of suppressing warping of the formwork can be obtained by bonding the roughening sheet to the entire surface. Furthermore, by laminating the thermoplastic resin layer by the extrusion lamination method as described above, high tear strength can be maintained. For example, the tensile strength according to JIS L 1096 can be 1,000 to 5,000 N / 5 cm, and the tear strength according to JIS L 1096 A-1 method (single tongue method) can be 50 to 1,000 N.
[0030] The roughening sheet obtained as described above may be attached to a formwork assembled according to the shape of the concrete to be produced. The material of the formwork is not particularly limited and may be any of wood, resin, or metal, but plywood is often used for the formwork used when pouring concrete that requires roughening, and it is preferable to attach the roughening sheet to a formwork made of plywood. The roughening sheet and the formwork can also be attached at the construction site using nails, tackers, adhesives, adhesive tapes, etc. In this case, it is necessary to cut the sheet to the dimensions of the formwork at the construction site and attach the sheet. Furthermore, it is often difficult to sufficiently adhere the entire surface of the sheet to the formwork, and the sheet and the formwork are not partially adhered, so the sheet is likely to wrinkle. If the sheet wrinkles, the wrinkle pattern may be transferred to the manufactured concrete. Furthermore, if the adhesion between the sheet and the formwork is only partial, when the sheet is removed after the concrete has hardened, stress will be concentrated near the adhesive part, making the sheet more likely to be damaged, and it is not necessarily possible to reliably reuse the sheet.
[0031] Since the occurrence of wrinkles causes the above-mentioned problems, when bonding the roughening sheet to the formwork, it is preferable to ensure that the bonding surface is bonded uniformly over the entire surface. In order to bond the bonding surface uniformly over the entire surface, it is preferable to use a roll coater or the like to place adhesive over the entire surface and bond the sheets. Therefore, it is preferable to bond the sheets to the formwork material (mainly plywood) in advance to form a formwork panel, and then bring the formwork panel to the construction site to assemble the formwork. If the sheet and plywood are bonded in advance, there is no need to perform bonding work on site, and construction can be carried out efficiently.
[0032] The adhesive may be any known adhesive. The adhesive may be any of water-soluble adhesives or aqueous emulsion adhesives, or solvent-type adhesives, and may be appropriately selected in consideration of the adhesiveness between the sheet and the plywood. The amount of application may also be appropriately selected in consideration of the type and adhesiveness of the adhesive.
[0033] When a roughened sheet and plywood are attached with an adhesive to form a formwork panel, it is preferable to provide a protective layer made of a thermoplastic resin on the surface of the roughened sheet opposite to the surface on which the thermoplastic resin layer of the woven or knitted fabric is arranged. Depending on the type or conditions of the adhesive used, much of the adhesive may soak into the woven or knitted fabric when it comes into contact with the woven or knitted fabric, resulting in insufficient adhesion. By providing a protective layer, the adhesive can be prevented from soaking into the woven or knitted fabric and can be arranged more uniformly. It is preferable that the protective layer has the same structure as the thermoplastic resin layer. If the front and back have different structures, curling may occur depending on the conditions. Curling can also cause poor adhesion. By providing the protective layer with the same structure as the thermoplastic resin layer, curling can be prevented.
[0034] When a protective layer is provided, the sheet is fixed to the plywood via an adhesive applied to the protective layer. The surface of the protective layer is preferably corona discharge treated in order to further increase the adhesion between the protective layer and the adhesive. This makes it possible to increase the adhesive strength between the sheet and the plywood compared to the adhesive strength between the thermoplastic resin layer and the concrete structure. With this configuration, for example, after the concrete has hardened, it becomes possible to remove the formwork and the sheet as a unit from the concrete structure with the sheet attached to the formwork.
[0035] When constructing concrete using a roughening sheet, it can be constructed in the same way as normal concrete construction, except that a formwork with a roughening sheet attached is used. After the concrete has hardened, the formwork with the roughening sheet attached is removed, and the uneven surface of the hardened concrete is formed by transferring the uneven pattern of the roughening sheet.
[0036] The roughening sheet of this embodiment has a structure in which a thermoplastic resin layer is disposed on one side of a woven or knitted fabric, and a protective layer is disposed on the other side of the woven or knitted fabric. As long as the roughening sheet has a woven or knitted fabric and a thermoplastic resin layer, the protective layer may be omitted, or other layers may be included. EXAMPLES
[0037] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0038] [Example 1] <Making roughening sheets> Polypropylene multifilament (fineness 760dt, number of ply yarns 120, 100m / twist) was used as warp and weft yarns, and woven in a plain weave with a weaving density of 18x20 / 2.54cm to obtain a woven fabric. Next, a mixture of 80% by weight of polyolefin thermoplastic elastomer (reactor type TPO) and 20% by weight of linear low density polyethylene was prepared and laminated to a thickness of 70μm on both sides of the woven fabric by extrusion lamination. Then, one side was subjected to corona discharge treatment to obtain sheet a having the configuration shown in Figures 1 and 2. Sheet a had the following physical properties. The tensile strength according to JIS L 1096 was 2,160N / 5cm in the warp direction and 2,332N / 5cm in the weft direction. The tear strength according to JIS L 1096 A-1 method (single tongue method) was 180N in the warp direction and 150N in the weft direction.
[0039] [Comparative Example 1] Commercially available polypropylene / polyethylene thermal bonded nonwoven fabric (weight: 200 g / m 2 ) was prepared and designated as sheet b.
[0040] [Comparative Example 2] Polypropylene was molded by the inflation method using a round die with grooves on the die lip to produce a polypropylene film (basis weight 60 g / m2) with projections and recesses formed along the length on one side. 2 ) was prepared and designated as sheet c.
[0041] <Test 1: Roughness test> A wooden formwork (300 mm x 360 mm x 100 mm) was prepared, and the sheets shown in Example 1, Comparative Example 1, and Comparative Example 2 were laid on the bottom surface. Concrete was then poured from the top surface. The formwork was removed on the fifth day, and each sheet was peeled off on the 12th day. The roughening state and workability were evaluated on a three-point scale, and the results are shown in Table 1. [Table 1]
[0042] Example 1: When sheet 1 was peeled off, the woven uneven pattern of sheet a was transferred to the surface of the concrete, creating a uniformly uneven and rough surface. The sheet was easy to attach and remove, and even after removal, sheet a had almost no concrete attached to it. Comparative Example 1: Many fiber fragments were found attached to the surface of the concrete after sheet b was peeled off. Because sheet b absorbed the moisture from the concrete before it hardened, the surface of the concrete did not harden sufficiently, and it was brittle and prone to crumbling. Comparative Example 2: When sheet c was peeled off, the striped uneven pattern from sheet c was transferred to the surface of the concrete. It was difficult to lay and fix sheet c in a wrinkle-free state to the formwork, and the concrete was poured with some wrinkles in sheet c, so the wrinkle pattern was also transferred to the concrete. There was almost no adhesion of concrete to sheet c after it was removed.
[0043] <Test 2: Plywood bonding test> A water-based emulsion adhesive (Bond CVC360H / hardener NV manufactured by Konishi Co., Ltd.) was applied to softwood plywood using a roll coater, and the sheets of Example 1 and Comparative Example 2 were placed on the plywood and pressed down, and the sheets were cured at ambient temperature for one week before being attached to obtain a formwork panel in which the plywood and the sheets were integrated. The sheet of Example 1 was attached so that the corona discharge treated surface of sheet a faced the plywood. The obtained formwork panel was subjected to a class 1 immersion peel test according to the Japanese Agricultural Standards for plywood (Ministry of Agriculture, Forestry and Fisheries Notification No. 303 of 2014) and a 180-degree peel adhesion strength test (test piece width: 25 mm, tensile speed: 200 mm / min) using Shimadzu Corporation's Autograph AG5000A. The results are shown in Table 2. [Table 2]
[0044] Example 1: In the formwork panel to which the sheet A of Example 1 was attached, no abnormalities in appearance were observed in the first-class immersion peel test. The 180-degree peel strength test also showed sufficient peel strength, with the numerical value being the value at which the softwood plywood material was destroyed. Comparative Example 2: The formwork panel to which the sheet c of Comparative Example 2 was attached showed no abnormal appearance in the first-class immersion peel test. In the 180-degree peel adhesion strength test, the sheet c was torn off immediately, and similarly was not in a condition to be measured.
[0045] <Test 3: Preparation of concrete structure> A form was assembled using the form panel to which the sheet a of Example 1 was attached, concrete was poured, and cured until the age of the material reached 7 days. The form was removed from the hardened concrete, and a concrete skeleton was prepared.
[0046] The uneven pattern of sheet a was transferred to the surface of the concrete structure, forming obvious irregularities and a rough texture. The irregularities were uniform. Removal of the form was not particularly difficult, and when sheet a was examined after removal of the form, there was almost no concrete adhering to it, and the formwork was in a condition that could be reused. There was also no damage to sheet a itself, and sheet 1 was in a condition that could be used repeatedly. A base mortar was applied to a 58-day-old concrete structure produced using sheet a, and tiles were attached with the mortar, but there were no problems with the attachment work or the adhesion of the tiles.
[0047] <Test 4: Strain follow-up test> A steel formwork (100 mm × 400 mm × 100 mm) and a formwork in which the formwork members constituting the two sides in the longitudinal direction of the formwork were replaced with formwork panels to which the sheet a of Example 1 was attached were prepared. Concrete (water-cement ratio 47%, nominal strength 33 N / mm 2) was poured. The next day, the respective forms were removed from the hardened concrete to obtain a rectangular columnar specimen without a pattern and a rectangular columnar specimen a onto which the uneven pattern of sheet a had been transferred. The rectangular columnar specimen without a pattern at 57 days of age was roughened by ultra-high pressure washing to obtain a roughened rectangular columnar specimen b. Ultra-high pressure washing was performed on two opposing side surfaces extending in the longitudinal direction of the rectangular columnar specimen without a pattern.
[0048] As shown in Figure 3, mortar was applied to the uneven pattern surface of specimen a and the rough surface of specimen b, and multiple tiles were attached to each specimen. The tiles were attached at the following positions. A vertical line was assumed to be at the center of the short side of the mortar-coated surface, and multiple tiles were attached along the vertical line. As shown in Figure 3, a total of five tiles were attached to one side of the specimen, and a total of five tiles were attached to the other side of the specimen. The tiles were attached so that the edge of the lower tile was 72.5 mm from the lower end of the specimen, the edge of the upper tile was 72.5 mm from the upper end of the specimen, and there was a 5 mm gap between each tile. The shape of the tiles was a square of 45 mm x 45 mm. After the tiles were attached, the specimen was left to cure for 83 days, obtaining rectangular column-shaped specimen a' with tiles attached to two sides of specimen a, and rectangular column-shaped specimen b' with tiles attached to two sides of specimen b.
[0049] As shown in Figure 3, strain gauges were attached to the center of the specimen in the longitudinal and transverse directions, and strain follow-up tests were performed on the above specimens a' and b' based on JIS A 1108 (Concrete Compressive Strength Test Method). Concrete strain was measured using strain gauge PL-60-11 manufactured by Tokyo Measurement Laboratory Co., Ltd. Tile strain was measured using PFL-10-11 manufactured by the same company and recorded using strain recorder DC204R manufactured by the same company. The results are shown in Table 3. The "strain transmission rate α" indicates the ratio of tile strain to concrete strain. The "elongation T until complete tile peeling" indicates the area between the tile strain-concrete strain curve and the concrete strain axis from the point where the tile strain starts to decrease to the point where the tile is completely peeled off (shaded area in Figure 4). [Table 3]
[0050] Specimen a' obtained using sheet a of Example 1 had a degree of elongation T until the tile completely peeled off that was about five times higher than that of specimen b' roughened by ultra-high pressure washing, and more energy was required for the tile to peel off. In other words, roughening with sheet a of Example 1 makes it easier to obtain resistance to tile peeling compared to roughening with ultra-high pressure washing. The reason why the degree of elongation T until the tile completely peeled off was 150,000 or more, and especially 200,000 or more, is presumably because the unevenness of the concrete formed by sheet a of Example 1 was of appropriate depth, spacing, and uniformity. [Explanation of symbols]
[0051] 1 Roughening sheet 2 Woven knitted fabric 3 Thermoplastic resin layer 4 Multifilament 5. Concrete 6. Adhesive 7 layers of protection 8. Plywood
Claims
1. A roughening sheet that creates an uneven pattern on the surface of a concrete structure to allow a mortar base to adhere to it. The present invention has a woven or knitted fabric using multifilaments, and a sheet-like thermoplastic resin layer laminated on at least one side of the woven or knitted fabric, The woven or knitted fabric has an uneven pattern due to the ups and downs of the multifilaments, The concave-convex pattern of the woven or knitted fabric is transferred through the thermoplastic resin layer, A roughening sheet that creates an uneven texture on the surface of a concrete structure.
2. 2. The roughening sheet according to claim 1, wherein both the multifilaments and the thermoplastic resin layer are made of a polyolefin resin.
3. 3. The roughening sheet according to claim 1, wherein the thermoplastic resin layer has a thickness of 30 to 150 μm.
4. 4. The roughening sheet according to claim 1, wherein the thermoplastic resin layer is laminated on the woven or knitted fabric by extrusion lamination.
5. A formwork panel comprising a plywood and a roughening sheet according to any one of claims 1 to 4 attached thereto.
6. 6. The form panel according to claim 5, wherein the roughening sheet and the plywood are attached with an adhesive.
7. A method for manufacturing a concrete structure, comprising pouring concrete into a formwork assembled using the formwork panels according to claim 5 or 6, and removing the formwork with the roughening sheet attached after the concrete has hardened, thereby transferring the uneven pattern of the roughening sheet to the surface of the hardened concrete structure, thereby forming unevenness.
Citation Information
Patent Citations
A composite material for attachment to a concrete panel
EP0429730A1
Concrete placing form
JP1989203564A
Lining sheet for concrete formwork
JP1995006392U
Template for formative wall
JP1995269103A
Form with sheet
JP1998002107A