Low thermal expansion castings and their manufacturing method

A low thermal expansion casting with controlled Ni and Co content and heat treatments addresses the low strength issue of Invar alloys, providing high yield strength and low thermal expansion for CFRP molds.

JP7572028B2Active Publication Date: 2024-10-23SHINHOKOKU STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020122920
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-17
Publication Date
2024-10-23
Estimated Expiration
2040-07-17

AI Technical Summary

Technical Problem

Conventional Invar and super Invar alloys used in CFRP molds suffer from low strength at high temperatures, leading to mold damage.

Method used

A low thermal expansion casting with controlled Ni and Co content in Fe-Ni-Co alloys, combined with specific heat treatments like cryo treatment and recrystallization, enhances yield strength at high temperatures.

Benefits of technology

The casting achieves high yield strength and low thermal expansion coefficients, suitable for ultra-precision equipment like CFRP molds, preventing damage at operating temperatures up to 400°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572028000001
    Figure 0007572028000001
Patent Text Reader

Abstract

To provide a low thermal expansion casting having sufficient strength even at a high temperature and having a low thermal expansion coefficient.SOLUTION: A low thermal expansion casting of the present invention is obtained by applying an appropriate thermal treatment to a casting that contains, in mass%, C: 0 to 0.100%, Si: 0 to 1.00%, Mn: 0 to 1.00%, Nb: 0.50 to 3.50%, Co: 13.00 to 17.50% and Ni satisfying -3.5×%Ni+115≤%Co≤-3.5×%Ni+121 (%Ni and %Co are Ni and CO content respectively (mass%)), and the balance of Fe and inevitable impurities, to result in 0.2% proof stress of tensile test at 400°C of 140 MPa or larger, an average thermal expansion coefficient at 25 to 350°C of 6.0 ppm / °C or lower, and a Curie temperature of 300°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a low thermal expansion casting, and more particularly to a low thermal expansion casting having excellent high temperature strength. [Background technology]

[0002] With the recent development of communication technology, parabolic antennas and other devices used in transmission and reception equipment have become extremely large, and require not only low thermal expansion but also high processing precision, i.e., castability, machinability, vibration absorption capacity, mechanical strength, etc. For example, carbon fiber reinforced plastics (CFRP), which has high rigidity and corrosion resistance, is commonly used as an antenna reflector.

[0003] The thermal expansion coefficient of CFRP is smaller than that of steel, and in order to ensure high dimensional accuracy even after molding, the molding die must be made of a material with a similar thermal expansion coefficient. For this reason, Invar alloys and Super Invar alloys are chosen as the molding die material.

[0004] Patent Document 1 discloses a forming die for a cast iron having a graphite structure in an austenitic matrix iron, the composition of which, expressed by weight, is 0.09% or more and 0.43% or less of solid solution carbon, less than 1.0% of silicon, 29% or more and 34% or less of nickel, 4% or more and 8% or less of cobalt, the balance being iron, and the thermal expansion coefficient in the temperature range of 0 to 200°C is 4 × 10 -6 It discloses the use of low thermal expansion cast iron, which has a thermal expansion coefficient of 1 / °C or less.

[0005] Patent Document 2 discloses a CFRP mold for use as a member of an ultra-precision device, which comprises 0.1 wt.% or less of C, 0.1 to 0.4 wt.% of Si, 0.15 to 0.4 wt.% of Mn, more than 2 to 4 wt.% of Ti, 1 wt.% or less of Al, 30.7 to 43.0 wt.% of Ni, and 14 wt.% or less of Co, and the contents of Ni and Co satisfy the following formula (1), with the remainder being Fe and unavoidable impurities, and the thermal expansion coefficient in the temperature range of -40°C to 100°C is 4×10 -6 / ℃ or less, and Young's modulus is 16100kgf / mm 2 As described above, the use of alloy steel having excellent thermal shape stability and rigidity is disclosed.

[0006] 37.7≦Ni+0.8×Co≦43 (1) [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 6-172919 [Patent Document 2] Japanese Patent Application Publication No. 11-293413 Summary of the Invention [Problem to be solved by the invention]

[0008] The Invar alloy and Super Invar alloy used in conventional CFRP molding dies have low strength at high temperatures, which is the operating temperature range of the dies. This means that the dies are easily damaged, which is an issue that needs to be resolved.

[0009] In view of the above circumstances, an object of the present invention is to provide a low thermal expansion casting that has sufficient strength even at 400°C, which is the operating temperature range of a CFRP mold, and has a low thermal expansion coefficient in the range of 25 to 350°C. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into methods for increasing the high-temperature yield strength of low-thermal expansion castings, and have found that it is possible to increase the high-temperature yield strength of an Fe-Ni-Co alloy without using expensive alloy elements such as Ti and Al by controlling the Ni and Co contents within appropriate ranges and by carrying out an appropriate heat treatment after casting.

[0011] The present invention has been made based on the above findings, and the gist of the present invention is as follows.

[0012] (1) A low thermal expansion casting having a composition, in mass%, of C: 0-0.100%, Si: 0-1.00%, Mn: 0-1.00%, Nb: 0.50-3.50%, Co: 13.00-17.50%, and Ni that satisfies -3.5 x %Ni + 115 ≦ %Co ≦ -3.5 x %Ni + 121 (%Ni and %Co are the Ni and Co contents (mass%), respectively), with the balance being Fe and unavoidable impurities, and having a 0.2% proof stress in a tensile test at 400°C of 140 MPa or more, an average thermal expansion coefficient at 25 to 350°C of 6.0 ppm / °C or less, and a Curie temperature of 300°C or more.

[0013] (2) a cryo-treatment step of cooling a casting having the composition of (1) from room temperature to below the Ms point, holding the temperature below the Ms point for 0.5 to 3 hours, and then heating the casting to room temperature; and A method for producing low thermal expansion castings, comprising the steps of heating the casting to 800 to 1200°C, holding it there for 0.5 to 5 hours, and then quenching it through a recrystallization process.

[0014] (3) a first cryo-treatment step of cooling a casting having the composition of (1) from room temperature to a temperature below the Ms point, holding the temperature below the Ms point for 0.5 to 3 hours, and then heating the casting to room temperature; A method for manufacturing low thermal expansion castings, comprising, in order: a recrystallization process in which the casting is heated to 800-1200°C, held there for 0.5-5 hours, and then rapidly cooled; a second cryo-treatment process in which the casting is cooled from room temperature to below the Ms point, held at a temperature below the Ms point for 0.5-3 hours, and then heated to room temperature; and a reverse transformation process in which the casting is heated to 600-750°C, held there for 0.5-5 hours, and then rapidly cooled.

[0015] (4) A method for producing a low thermal expansion casting, comprising the steps of: cooling a casting having the chemical composition of (1) from room temperature to below the Ms point, holding the temperature below the Ms point for 0.5 to 3 hours, and then raising the temperature to room temperature; and heating the casting to 600 to 750°C, holding the temperature for 0.5 to 5 hours, and then quenching the casting. Effect of the Invention

[0016] According to the present invention, it is possible to obtain a low thermal expansion casting having high yield strength in high temperature ranges and a low thermal expansion coefficient, and therefore the casting can be applied to components of ultra-precision equipment such as CFRP dies used at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below. In the following, "%" regarding the composition of a component represents "mass %" unless otherwise specified. First, the composition of the casting of the present invention will be described.

[0018] In the present invention, Ni and Co are essential elements that contribute to lowering the thermal expansion coefficient by adding them in combination. In particular, in the present invention, a certain amount of Co is contained in order to make the Curie temperature 300° C. or higher, and an appropriate amount of Ni is contained according to the amount of Co in order to make the thermal expansion coefficient sufficiently small over a wide temperature range. If the amounts of Ni and Co are too large, the Ms point becomes too low, making it difficult to cause martensitic transformation by cooling, which will be described later, so the ranges of the amounts of Ni and Co are determined taking this into consideration.

[0019] In order to set the Curie temperature to 300°C or higher and to make the thermal expansion coefficient sufficiently small over a wide temperature range, the Co content is 13.00 to 17.50%, and the Ni content is in a range that satisfies -3.5×%Ni+115≦%Co≦-3.5×%Ni+121, where the Co content is %Co (mass%) and the Ni content is %Ni (mass%).

[0020] The Curie temperature is set to 300°C or higher in order to obtain a low coefficient of thermal expansion even at high temperatures. There is a close relationship between the Curie temperature and the coefficient of thermal expansion, and with an Invar alloy, the coefficient of thermal expansion is close to 0 below the Curie temperature, but the coefficient of thermal expansion increases rapidly above the Curie temperature. The low thermal expansion casting of the present invention is intended for use at around 400°C, which is the operating temperature range of CFRP dies, and the Curie temperature is set to 300°C or higher in order to obtain a low coefficient of thermal expansion in this temperature range.

[0021] C dissolves in austenite and contributes to increasing strength, so it may be included as necessary. This effect can be obtained even with a small amount, but it is effective and preferable to set the C content to 0.010% or more. If the C content is high, the thermal expansion coefficient increases, and further, ductility decreases, making casting cracks more likely to occur, so the content is set to 0.100% or less, preferably 0.050% or less, and more preferably 0.020% or less. In the low thermal expansion casting of the present invention, C is not an essential element, and the content may be 0.

[0022] Silicon may be added as a deoxidizer. It can also improve the fluidity of the molten metal. This effect can be obtained even with a small amount, but it is effective and preferable to set the silicon content to 0.05% or more. If the silicon content exceeds 1.00%, the thermal expansion coefficient increases, so the silicon content is set to 1.00% or less, preferably 0.50% or less, and more preferably 0.20% or less. In the low thermal expansion casting of the present invention, silicon is not an essential element, and the content may be 0.

[0023] Mn may be added as a deoxidizer. It also contributes to improving strength through solid solution strengthening. This effect can be obtained even with a small amount, but it is effective and preferable to set the Mn content to 0.10% or more. If the Mn content exceeds 1.00%, the effect saturates and the cost increases, so the Mn content is set to 1.00% or less, preferably 0.50% or less. In the low thermal expansion casting of the present invention, Mn is not an essential element, and the content may be 0.

[0024] Nb is an element that dissolves in austenite and improves the yield strength at high temperatures through its solution strengthening effect. It also acts as an inoculant in the molten metal, making it easier to generate solidification nuclei. To obtain these effects, the Nb content must be 0.50% or more. As the Nb content increases, the toughness deteriorates significantly, so the content must be 3.50% or less.

[0025] The balance of the composition is Fe and inevitable impurities. The inevitable impurities refer to those that are inevitably mixed in from raw materials, the manufacturing environment, etc., when the steel having the composition specified in the present invention is industrially manufactured. Specifically, the inevitable impurities include 0.02% or less of P, S, O, N, etc.

[0026] Next, the method for producing a low thermal expansion casting of the present invention will be described.

[0027] First, a casting having a desired composition is produced by casting. The mold used for casting, and the device and method for pouring molten steel into the mold are not particularly limited, and known devices and methods may be used.

[0028] The resulting casting is subjected to one of the following heat treatments.

[0029] [1] First cryo-treatment process → Recrystallization process [2] First cryo-treatment process → recrystallization process → second cryo-treatment process → reverse transformation process [3] First cryo-treatment process → reverse transformation process

[0030] Each step will be described below.

[0031] (First cryo treatment process) The casting is cooled to below the Ms point, held at a temperature below the Ms point for 0.5 to 3 hours, and then heated to room temperature. There are no particular limitations on the cooling method. The Ms point referred to here is the Ms point at a stage before the effects of the present invention are realized. The cooling temperature may be set to a temperature sufficiently lower than the Ms point, so there is no need to know the exact Ms point at this stage. In general, the Ms point can be estimated using the components of the steel according to the following formula.

[0032] Ms=521-353C-22Si-24.3Mn-7.7Cu-17.3Ni -17.7Cr-25.8Mo Here, C, Si, Mn, Cu, Ni, Cr, and Mo are the contents (mass%) of each element. Elements that are not contained are regarded as 0.

[0033] In the case of the component composition of the low thermal expansion casting of the present invention, the Ms point calculated by the above formula is from room temperature to about -100°C or less, depending on the Ni content in particular, so dry ice and methyl alcohol or ethyl alcohol can be used as a cooling medium up to -80°C. For an even lower temperature of -196°C, a method of immersion in liquid nitrogen or a method of spraying liquid nitrogen can be used. This forms a structure containing martensite. The temperature can be raised by raising the material to the air at room temperature.

[0034] (Recrystallization process) The casting is reheated to 800-1200°C, held at 800-1200°C for 0.5-5 hours, and then quenched to room temperature. As a result, the structure in which martensite has been formed returns to an austenite structure. The crystal grain size of the structure formed by normal solidification is about 1-10 mm, but by going through the above cryo-treatment process and the subsequent recrystallization process, the austenite grain size is refined and the structure becomes a structure centered on equiaxed crystals with random crystal orientation, and the structure after quenching becomes a structure of fine equiaxed crystals with an average grain size of about 30-800 μm. This makes it possible to increase the Young's modulus and obtain a high 0.2% proof stress at 400°C. The method of quenching is not particularly limited, but water cooling is preferable.

[0035] (Second cryo-treatment process) Following the recrystallization treatment, the casting is cooled again to below the Ms point, held at that temperature for 0.5 to 3 hours, and then heated to room temperature. The cooling and heating in the second cryo-treatment step may be performed in the same manner as in the first cryo-treatment step. This treatment causes the structure of the casting to once again contain martensite.

[0036] (Reverse transformation process) Following cryo-treatment, the casting is heated to 600-750°C, held there for 0.5-5 hours, and then rapidly cooled to room temperature to convert the structure to austenite. When the structure transforms into martensite during the cryo-treatment process, plastic deformation occurs. The strain (dislocations) that occurs during this process remains in the structure that has become austenite through reverse transformation treatment. This allows for a higher 0.2% yield strength than that at 400°C.

[0037] The martensite structure reverts to austenite when heated to 600°C or higher, but if the heating temperature exceeds 750°C, dislocations act as the driving force for austenite recrystallization, so the heating temperature must be 750°C or lower. Note that the size of the austenite grains does not change as a result of the cryo-treatment process and the subsequent reverse transformation process.

[0038] As described above, a high Young's modulus and a high 0.2% yield strength at 400°C can be obtained by the cryo-treatment process followed by the recrystallization process, and an even higher 0.2% yield strength at 400°C can be obtained by the cryo-treatment process followed by the reverse transformation process. Therefore, the above steps [1] to [3] can be selected depending on the required characteristics.

[0039] After the first cryo-treatment step and the second cryo-treatment step, a tempering treatment step may be provided in which the casting is heated to 300 to 500°C and held at that temperature for 2 to 6 hours. The tempering treatment step may be provided after either the first cryo-treatment step or the second cryo-treatment step, or after both steps. The tempering may lower the temperature of the subsequent recrystallization and reverse transformation, which may improve the efficiency of the treatment.

[0040] Prior to the first cryo-treatment step, a solution treatment step may be performed in which the casting is heated to 800 to 1200°C, held for 0.5 to 5 hours, and then rapidly cooled to room temperature. The solution treatment causes the precipitates that precipitated during casting to dissolve, improving ductility and toughness. The method of rapid cooling is not particularly limited, but water cooling is preferred.

[0041] When producing a casting, the molten metal may contain Ti, B, Mg, Ce, or La as an inoculant to facilitate the formation of solidification nuclei. In addition, the molten metal may be coated with an inoculant such as Co(AlO2), CoSiO3, or Co-borate, together with a mold wash that is usually applied to the mold, to facilitate the formation of solidification nuclei. Furthermore, the molten metal in the mold may be stirred and flowed by a method using an electromagnetic stirring device, a method of mechanically vibrating the mold, or a method of ultrasonically vibrating the molten metal. By applying these methods, the structure of the casting is more likely to become equiaxed crystals, so that the low thermal expansion casting of the present invention can be produced more efficiently.

[0042] The excellent high-temperature strength of the low thermal expansion casting of the present invention can be evaluated by the results of a tensile test at 400° C. Specifically, the low thermal expansion casting of the present invention has a 0.2% yield strength of 140 MPa or more measured in a tensile test at 400° C.

[0043] The low thermal expansion casting of the present invention can further obtain a low thermal expansion coefficient over a wide temperature range, with an average thermal expansion coefficient of 6.0 ppm / °C or less at 25 to 350°C. By adjusting the components so that the average thermal expansion coefficient is 4.0 to 6.0 ppm, it matches the thermal expansion coefficient of CFRP, making it suitable as a member of a die for molding CFRP.

[0044] The low thermal expansion casting of the present invention has a high Curie temperature, so that the thermal expansion coefficient does not increase significantly even at high temperatures, and has high high-temperature resistance, so that even when used for components of ultra-precision equipment used at high temperatures, such as CFRP molds, damage can be suppressed. EXAMPLES

[0045] Using a high-frequency melting furnace, molten metal adjusted to have the composition shown in Table 1 was poured into a mold to manufacture a Y-block. Then, the following heat treatment was performed.

[0046] Process No.1: First cryo-treatment process → Recrystallization process Process No. 2: First cryo-treatment process → Recrystallization process → Second cryo-treatment process → Reverse transformation process Process No.3: First cryo-treatment process → reverse transformation process Process No.0: No heat treatment

[0047] In the first cryo-treatment step, the Y-block was immersed in liquid nitrogen and cooled to below the Ms point, and then held there for 1.5 hours. Thereafter, it was removed from the liquid nitrogen and allowed to stand at room temperature until it was warmed up to room temperature.

[0048] In the recrystallization process, the Y-block was heated to the temperature shown in Table 1, held at that temperature for 3 hours, and then cooled in water.

[0049] In the second cryo-treatment step, the same treatment as in the first cryo-treatment step was carried out.

[0050] In the reverse transformation treatment process, the Y-block was heated to the temperature shown in Table 1, held at that temperature for 3 hours, and then cooled in water.

[0051] Two samples were taken from the resulting casting and subjected to a tensile test (based on JIS G 0567) at 400°C to measure the 0.2% yield strength using the offset method, and the average of the two values ​​was taken as the measured value. Similarly, a test piece was taken for measuring the thermal expansion coefficient, and the average thermal expansion coefficient from 25 to 350°C and the Curie temperature were measured. The Curie temperature was determined from the bending point obtained from the elongation-temperature chart during the measurement.

[0052] The results are shown in Table 1.

[0053] The low thermal expansion casting of the present invention has a low thermal expansion coefficient, and furthermore, in a tensile test at 400°C, it exhibited a high 0.2% yield strength.

[0054] In contrast, in the comparative example, the target characteristics of at least one of the 0.2% proof stress at 400° C. and the thermal expansion coefficient were not obtained.

[0055] [Table 1]

Claims

1. The composition is, in mass%, C: 0-0.100%, Si: 0 to 1.00%, Mn: 0 to 1.00%, Nb: 0.50-3.50% Co: 13.00 to 17.50%, and Ni satisfying -3.5 x %Ni + 115 ≦ %Co ≦ -3.5 x %Ni + 121 (%Ni and %Co are the Ni and Co contents (mass%), respectively) The balance being Fe and unavoidable impurities; 0.2% yield strength of tensile test at 400°C is 140 MPa or more, Average thermal expansion coefficient at 25 to 350°C is 6.0 ppm / °C or less; Curie temperature is 300℃ or higher A low thermal expansion casting characterized by:

2. A method for producing the low thermal expansion casting according to claim 1, comprising: A cryo-treatment step of cooling a casting having the composition according to claim 1 from room temperature to a temperature below the Ms point, holding the temperature below the Ms point for 0.5 to 3 hours, and then raising the temperature to room temperature; A recrystallization process in which the casting is heated to 800-1200°C, held for 0.5-5 hours, and then rapidly cooled. A method for producing a low thermal expansion casting, comprising the steps of:

3. A method for producing the low thermal expansion casting according to claim 1, comprising: A first cryo-treatment step of cooling a casting having the composition according to claim 1 from room temperature to a temperature not higher than the Ms point, holding the temperature not higher than the Ms point for 0.5 to 3 hours, and then heating the casting to room temperature; A recrystallization process in which the casting is heated to 800 to 1200°C, held for 0.5 to 5 hours, and then rapidly cooled. A second cryo-treatment step of cooling the casting from room temperature to below the Ms point, holding the casting at the temperature below the Ms point for 0.5 to 3 hours, and then raising the temperature to room temperature; and A reverse transformation process in which the casting is heated to 600-750°C, held for 0.5-5 hours, and then rapidly cooled. A method for producing a low thermal expansion casting, comprising the steps of:

4. A method for producing the low thermal expansion casting according to claim 1, comprising: A cryo-treatment step of cooling a casting having the composition according to claim 1 from room temperature to a temperature below the Ms point, holding the temperature below the Ms point for 0.5 to 3 hours, and then heating the casting to room temperature; A method for manufacturing a low thermal expansion casting, comprising the steps of heating the casting to 600 to 750°C, holding it for 0.5 to 5 hours, and then quenching it in a reverse transformation process.

Citation Information

Patent Citations

  • Machine tool, precision measuring instrument and molding die using low thermal expansion cast iron

    JP1994172919A

  • Member of ultraprecision equipment using alloy steel excellent in thermal shape stability and rigidity

    JP1999293413A

  • High-rigidity low-thermal expansion casting and method for producing the same

    JP2016027187A

  • Low-thermal expansion cast steel product and method for producing the same

    JP2016027188A

  • High young modulus low thermal expansion cast alloy for plastic working or casting and method of producing the same

    JP2016117924A