Film forming method
By forming a silicon nitride film through trisilylamine decomposition at 450°C and alternating gas supply, the method addresses the challenge of low etching resistance, achieving a high-quality silicon nitride film with reduced hydrogen and improved etching properties.
Patent Information
- Application Number
- JP2021017307
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-05
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-02-05
AI Technical Summary
Existing film forming methods struggle to produce silicon nitride films with high etching resistance.
A method involving the formation of a trisilylamine film on a substrate surface without a nitriding agent, breaking the Si-H bond at a temperature of 450°C or higher, and intermittently supplying trisilylamine and inert gas to desorb hydrogen, forming a silicon nitride film with low hydrogen concentration.
The method results in a silicon nitride film with enhanced etching resistance and reduced hydrogen content, demonstrating improved wet etching resistance and higher refractive index.
Smart Images

Figure 0007572124000001 
Figure 0007572124000002 
Figure 0007572124000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a film formation method. [Background technology]
[0002] 2. Description of the Related Art A film formation method is known in which a silane-based gas, a nitriding gas, and an impurity-containing gas are supplied into a processing chamber capable of being evacuated to form an impurity-containing silicon nitride film on a surface of a wafer (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-270016 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique for forming a silicon nitride film having high etching resistance. [Means for solving the problem]
[0005] A film forming method according to one aspect of the present disclosure is a method for forming a silicon nitride film on a surface of a substrate, the method comprising the steps of: dissolving trisilylamine in a processing vessel containing the substrate; Process gas containing and forming a silicon nitride film on the surface of the substrate by intermittently supplying the gas. death , The step of forming the silicon nitride film is performed without supplying a nitriding agent for nitriding the trisilylamine, and in the step of forming the silicon nitride film, the temperature of the substrate is set to 450° C. or higher, and the silicon nitride film is formed while breaking the Si-H bond of the trisilylamine and eliminating hydrogen from the trisilylamine. . Effect of the Invention
[0006] According to the present disclosure, a silicon nitride film having high etching resistance can be formed. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic diagram illustrating an example of a processing apparatus according to an embodiment; [Diagram 2]A flowchart showing an example of a film forming method according to an embodiment. [Diagram 3] Comparison of refractive indices of silicon nitride films [Figure 4] Comparison of WER of silicon nitride films [Diagram 5] Comparison of silicon nitride film compositions [Figure 6] FIG. 1 shows the results of measuring the relationship between the hydrogen concentration in a silicon nitride film and the WER. [Figure 7] Comparison of hydrogen concentration and chlorine concentration in silicon nitride film [Figure 8] Comparison of cross-sectional shape and step coverage of silicon nitride films DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, non-limiting exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings. In all of the accompanying drawings, the same or corresponding members or parts are designated by the same or corresponding reference numerals, and duplicated descriptions will be omitted.
[0009] [Processing Device] An example of a processing apparatus capable of carrying out the film forming method of the embodiment will be described with reference to Fig. 1. As shown in Fig. 1, the processing apparatus 1 is a batch type apparatus that processes a plurality of substrates at once. The substrates may be, for example, semiconductor wafers (hereinafter simply referred to as "wafers W").
[0010] The processing apparatus 1 includes a processing vessel 10, a gas supply unit 30, an exhaust unit 40, a heating unit 50, a control unit 80, and the like.
[0011] The processing vessel 10 can have its interior depressurized and accommodates a wafer W. The processing vessel 10 has a cylindrical inner tube 11 with a ceiling and an open lower end, and a cylindrical outer tube 12 with a ceiling and an open lower end that covers the outside of the inner tube 11. The inner tube 11 and the outer tube 12 are made of a heat-resistant material such as quartz, and are arranged coaxially to form a double-tube structure.
[0012] The ceiling of the inner pipe 11 is, for example, flat. A storage section 13 for storing a gas nozzle is formed along the longitudinal direction (vertical direction) of the inner pipe 11 on one side. In this embodiment, a part of the side wall of the inner pipe 11 protrudes outward to form a convex section 14, and the inside of the convex section 14 is formed as the storage section 13.
[0013] A rectangular opening 15 is formed in the side wall of the inner tube 11 opposite the housing portion 13 along the longitudinal direction (vertical direction).
[0014] The opening 15 is a gas exhaust port formed so as to be able to exhaust gas from inside the inner tube 11. The length of the opening 15 is the same as the length of the wafer boat 16, or is formed so as to extend in the vertical direction longer than the length of the wafer boat 16.
[0015] The lower end of the processing vessel 10 is supported by a cylindrical manifold 17 made of, for example, stainless steel. A flange 18 is formed at the upper end of the manifold 17, and the lower end of the outer tube 12 is placed and supported on the flange 18. A seal member 19 such as an O-ring is interposed between the flange 18 and the lower end of the outer tube 12 to make the inside of the outer tube 12 airtight.
[0016] An annular support 20 is provided on the inner wall of the upper part of the manifold 17, and the lower end of the inner tube 11 is placed and supported on the support 20. A lid 21 is air-tightly attached to the opening at the lower end of the manifold 17 via a seal member 22 such as an O-ring, so as to air-tightly close the opening at the lower end of the processing vessel 10, i.e., the opening of the manifold 17. The lid 21 is made of, for example, stainless steel.
[0017] A rotating shaft 24 that rotatably supports the wafer boat 16 via a magnetic fluid seal 23 penetrates the center of the lid 21. A lower portion of the rotating shaft 24 is rotatably supported by an arm 25A of a lifting mechanism 25 that is a boat elevator.
[0018] A rotating plate 26 is provided at the upper end of the rotating shaft 24, and the wafer boat 16 holding the wafers W is placed on the rotating plate 26 via a quartz heat retention stand 27. Therefore, by raising and lowering the lifting mechanism 25, the lid 21 and the wafer boat 16 move up and down as a unit, so that the wafer boat 16 can be inserted into and removed from the processing vessel 10. The wafer boat 16 can be accommodated in the processing vessel 10, and holds a plurality of wafers W (e.g., 50 to 150 pieces) approximately horizontally with a gap between them in the vertical direction.
[0019] The gas supply unit 30 is provided in the manifold 17. The gas supply unit 30 introduces a process gas into the inner tube 11. In this embodiment, the process gas contains trisilylamine (TSA: (SiH3)3N) and an inert gas. Examples of the inert gas include nitrogen gas (N2) and argon gas (Ar). The gas supply unit 30 has a gas nozzle 31.
[0020] The gas nozzle 31 is made of, for example, quartz, and is provided in the inner tube 11 along the longitudinal direction thereof, and its base end is bent into an L-shape and supported so as to penetrate the manifold 17. The gas nozzle 31 has a plurality of gas holes 32 formed along the longitudinal direction thereof, and gas is discharged from the gas holes 32 in a horizontal direction. The plurality of gas holes 32 are arranged, for example, at intervals equal to the intervals between the wafers W supported by the wafer boat 16. The gas nozzle 31 is a nozzle that supplies gases such as a film forming gas, a cleaning gas, a purge gas, etc., and supplies the gases into the processing vessel 10 as necessary while controlling the flow rate.
[0021] 1, the gas supply unit 30 has one gas nozzle 31, but the form of the gas supply unit 30 is not limited thereto, and for example, the gas supply unit 30 may have a plurality of gas nozzles. In this case, TSA and N2 may be introduced into the inner tube 11 from the same gas nozzle, or may be introduced into the inner tube 11 from different gas nozzles.
[0022] The exhaust unit 40 exhausts gas that is discharged from the inner tube 11 through the opening 15 and then discharged from a gas outlet 41 through a space P1 between the inner tube 11 and the outer tube 12. The gas outlet 41 is formed in the side wall of the upper part of the manifold 17, above the support part 20. An exhaust passage 42 is connected to the gas outlet 41. A pressure adjustment valve 43 and a vacuum pump 44 are sequentially provided in the exhaust passage 42, so that the inside of the processing vessel 10 can be exhausted.
[0023] The heating unit 50 is provided around the outer tube 12. The heating unit 50 is provided, for example, on the base plate 28. The heating unit 50 has a cylindrical shape so as to cover the outer tube 12. The heating unit 50 includes, for example, a heating element, and heats the wafer W in the processing vessel 10.
[0024] The control unit 80 controls the operation of each part of the processing device 1. The control unit 80 may be, for example, a computer. A computer program for performing the operation of each part of the processing device 1 is stored in a storage medium 90. The storage medium 90 may be, for example, a flexible disk, a compact disk, a hard disk, a flash memory, a DVD, or the like.
[0025] [Film formation method] An example of a film forming method according to the embodiment will be described with reference to Fig. 2. In the following, a case where a silicon nitride film (SiN film) is formed in the above-mentioned processing apparatus 1 will be described as an example. The following film forming method is performed by a control unit 80 controlling the operation of each unit of the processing apparatus 1.
[0026] First, the wafer boat 16 carrying a plurality of wafers W is lifted up from below into the processing vessel 10. Next, the opening at the lower end of the manifold 17 is closed with the lid 21 to make the inside of the processing vessel 10 into an airtight space.
[0027] Next, the inside of the processing chamber 10 is evacuated to maintain the process pressure, and the power supplied to the heating unit 50 is controlled to raise the wafer temperature to the process temperature. The process temperature is set to a temperature at which the Si-H bond of the TSA is broken, for example, 450° C. or higher. After the wafer temperature is stabilized at the process temperature, the film formation process is started while rotating the wafer boat 16.
[0028] In the film formation process, TSA is intermittently supplied into the processing vessel 10 to form a silicon nitride film on the surface of the wafer W. In this embodiment, as shown in Fig. 2, a TSA supplying process S1 and an inert gas supplying process S2 are repeated until a set number of times set in a determining process S3 is reached, thereby forming a silicon nitride film on the surface of the wafer W.
[0029] In the TSA supplying step S1, TSA is supplied into the processing chamber 10 through the gas holes 32 of the gas nozzle 31. As a result, the TSA is adsorbed onto the surface of the wafer W, forming a silicon nitride layer. At this time, the wafer W is heated to a temperature at which the Si-H bond of the TSA is broken, for example, 450° C. or higher, so that the Si-H bond of the TSA is broken and H is desorbed from the TSA. In the TSA supplying step S1, the time for supplying the TSA is, for example, 5 to 10 seconds.
[0030] In the inert gas supplying step S2, N2 is supplied as an inert gas into the processing vessel 10 through the gas holes 32 of the gas nozzle 31. This causes the TSA remaining in the processing vessel 10 to be exhausted from the processing vessel 10. Also, H desorbed from the TSA in the TSA supplying step S1 is exhausted together with N2 from the processing vessel 10. In the inert gas supplying step S2, the time for supplying N2 is, for example, 20 to 60 seconds.
[0031] In the determination step S3, it is determined whether the number of times the TSA supply step S1 and the inert gas supply step S2 have been performed has reached a set number of times. If it is determined in the determination step S3 that the number of times the TSA supply step S1 and the inert gas supply step S2 have been performed has reached the set number of times, the film formation process is terminated. On the other hand, if it is determined in the determination step S3 that the number of times the TSA supply step S1 and the inert gas supply step S2 have been performed has not reached the set number of times, the process returns to the TSA supply step S1.
[0032] After the film formation process is completed, the wafer W is unloaded from the processing chamber 10 in the reverse order to the procedure in which the wafer W was loaded into the processing chamber 10 .
[0033] As described above, according to the film forming method of the embodiment, the TSA supplying step S1 and the inert gas supplying step S2 are repeated until the number of times set in the determining step S3 is reached, thereby forming a silicon nitride film on the surface of the wafer W. This makes it possible to form a silicon nitride film while breaking the Si-H bond of the TSA and removing H from the TSA. As a result, it is possible to form a silicon nitride film having a low hydrogen concentration in the film. As will be described later, in a silicon nitride film, the lower the hydrogen concentration in the film, the higher the wet etching resistance. Therefore, according to the film forming process of the embodiment, a silicon nitride film having a high wet etching resistance can be formed.
[0034] In the above embodiment, the TSA supplying process S1 and the inert gas supplying process S2 are alternately repeated to intermittently supply TSA into the processing vessel 10, but the present invention is not limited to this. For example, instead of the inert gas supplying process S2, a vacuum pumping process may be performed to evacuate the processing vessel 10 without supplying an inert gas into the processing vessel 10. That is, the TSA supplying process S1 and the vacuum pumping process may be alternately repeated to intermittently supply TSA into the processing vessel 10.
[0035] [Example] An example in which the film characteristics of a silicon nitride film formed by the film forming method of the above embodiment are evaluated will be described. In the example, a silicon nitride film is formed on the surface of a wafer W by alternately repeating the supply of TSA and the supply of N2, and the film characteristics of the silicon nitride film are evaluated. In addition, as a comparative example, a silicon nitride film is formed on the surface of a wafer W by alternately repeating the supply of dichlorosilane (DCS) and the supply of ammonia (NH3) activated by plasma, and the film characteristics of the silicon nitride film are evaluated.
[0036] Fig. 3 is a diagram comparing the refractive indexes of silicon nitride films. In Fig. 3, the horizontal axis indicates the wafer temperature [°C] when the silicon nitride film was formed, and the vertical axis indicates the refractive index of the silicon nitride film. In Fig. 3, the results of the working example are indicated by triangles, and the results of the comparative example are indicated by circles.
[0037] As shown in FIG. 3, in the embodiment, when the wafer temperature is 450° C. to 500° C., the refractive index of the silicon nitride film is about 3.5. On the other hand, in the comparative example, when the wafer temperature is 350° C. to 650° C., the refractive index of the silicon nitride film is about 2.0. This result shows that the embodiment can form a silicon nitride film having a higher refractive index than the comparative example. In addition, since the silicon nitride film has a higher silicon content as the refractive index increases, it is considered that the embodiment can form a silicon nitride film that is more silicon-rich than the comparative example. That is, it is considered that a silicon-rich silicon nitride film can be formed according to the film forming method in which the supply of TSA and the supply of N2 are alternately repeated.
[0038] Figure 4 is a graph comparing the WER of silicon nitride films. In Figure 4, the horizontal axis indicates the wafer temperature [°C] when the silicon nitride film was formed, and the vertical axis indicates the WER [Å / min], which is the etching rate when the silicon nitride film was etched with 0.5% dilute hydrofluoric acid (DHF). In Figure 4, the results of the working example are indicated by triangles, and the results of the comparative example are indicated by circles.
[0039] As shown in FIG. 4, in the embodiment, when the wafer temperature is 450°C to 500°C, the WER is about 4.0 Å / min. On the other hand, in the comparative example, when the wafer temperature is 550°C or less, the WER is 10 Å / min or more. This result shows that in the embodiment, a silicon nitride film with a low WER can be formed at a lower temperature (for example, 500°C or less) compared to the comparative example. In other words, it is considered that a silicon nitride film with a low WER can be formed at a low temperature by the film formation method in which the supply of TSA and the supply of N2 are alternately repeated.
[0040] FIG. 5 is a diagram comparing the compositions of silicon nitride films. FIG. 5 shows the compositions of silicon (Si), nitrogen (N) and hydrogen (H) contained in the silicon nitride film measured by the Rutherford Backscattering Spectrometry (RBS) / Hydrogen Forward-scattering Spectroscopy (HFS) method. In FIG. 5, the results of the comparative example are shown in graph A, and the results of the example are shown in graphs B to F. More specifically, graph A shows the film composition of a silicon nitride film formed by alternately repeating the supply of DCS and the supply of NH3 activated by plasma with the wafer temperature set to 500° C. Graph B shows the film composition of a silicon nitride film formed by alternately repeating the supply of TSA and the supply of N2 with the wafer temperature set to 450° C. Graphs C to F show the film composition of a silicon nitride film formed by alternately repeating the supply of TSA and the supply of N2 with the wafer temperature set to 500° C. Graphs B to F show the film compositions when the TSA supply time and N2 supply time (TSA / N2) were set to 10 sec / 60 sec, 10 sec / 60 sec, 5 sec / 60 sec, 10 sec / 20 sec, and 5 sec / 20 sec, respectively.
[0041] As shown in FIG. 5, in the embodiment, even if the wafer temperature or TSA / N2 is changed, the composition ratio of Si to N (Si:N) in the silicon nitride film is 3:1, and the H concentration is almost 0%. This result shows that the process margin is large in the embodiment. In addition, in the embodiment, when the wafer temperature is 450°C to 500°C, it is considered that the Si-H bond of the TSA is broken during the formation of the silicon nitride film, and H is desorbed from the TSA. On the other hand, in the comparative example, the composition ratio of Si to N to H (Si:N:H) in the silicon nitride film is 38.5:52.9:8.6. From this result, it is considered that H is less likely to be desorbed during the formation of the silicon nitride film in the comparative example.
[0042] Fig. 6 is a diagram showing the results of measuring the relationship between the hydrogen concentration in a silicon nitride film and the WER. In Fig. 6, the horizontal axis indicates the hydrogen concentration in the silicon nitride film [at%], and the vertical axis indicates the WER [Å / min] when the silicon nitride film is etched with 0.5% DHF. In Fig. 6, the results of the embodiment are indicated by triangles, and the results of the comparative example are indicated by circles.
[0043] As shown in Figure 6, there is a positive correlation between the hydrogen concentration in the silicon nitride film and the WER, and it can be seen that the lower the hydrogen concentration in the silicon nitride film, the lower the WER. From this result, it can be said that in order to form a silicon nitride film with high etching resistance, it is important to reduce the hydrogen concentration in the silicon nitride film.
[0044] FIG. 7 is a graph comparing the hydrogen (H) concentration and chlorine (Cl) concentration in a silicon nitride film. FIG. 7 shows the H concentration and Cl concentration in a silicon nitride film measured by secondary ion mass spectrometry (SIMS). The lower detection limit of Cl concentration by SIMS is 1×10 17 FIG. 7(a) shows the results of measuring the H concentration in the film, and FIG. 7(b) shows the results of measuring the Cl concentration in the film. In FIG. 7(a), the horizontal axis shows the wafer temperature [°C] when the silicon nitride film was formed, and the vertical axis shows the H concentration in the silicon nitride film [atoms / cm 3In FIG. 7(b), the horizontal axis represents the wafer temperature [°C] when the silicon nitride film was formed, and the vertical axis represents the Cl concentration in the silicon nitride film [atoms / cm 3 7(a) and 7(b), the results of the embodiment are indicated by triangles, and the results of the comparative example are indicated by circles.
[0045] As shown in Fig. 7(a), the H concentration in the film is one to two orders of magnitude lower in the example than in the comparative example. Also, as shown in Fig. 7(b), the Cl concentration in the film is at the detection limit in the example, and it is understood that Cl is not present in the silicon nitride film. This is believed to be because the example uses TSA, which is a precursor that does not contain halogen.
[0046] Fig. 8 is a diagram comparing the cross-sectional shape and step coverage of silicon nitride films, with the results of the embodiment shown on the left and the results of the comparative example shown on the right. More specifically, the left side of Fig. 8 shows the cross-sectional shape and step coverage of a silicon nitride film formed in a recess by alternately repeating the supply of TSA and the supply of N2 with the wafer temperature set to 500°C. The right side of Fig. 8 shows the cross-sectional shape and step coverage of a silicon nitride film formed in a recess by alternately repeating the supply of DCS and the supply of NH3 activated by plasma with the wafer temperature set to 550°C.
[0047] The cross-sectional shape was observed by a transmission electron microscope (TEM), and the step coverage was calculated based on the observed cross-sectional shape.
[0048] The step coverage means a ratio (%) of the film thickness of the silicon nitride film 120 at the lower part of the sidewall 111 of the recess 110 to the film thickness of the silicon nitride film 120 at the upper part of the sidewall 111 of the recess 110. That is, when the film thickness of the silicon nitride film 120 at the lower part of the sidewall 111 of the recess 110 is equal to the film thickness of the silicon nitride film 120 at the upper part of the sidewall 111 of the recess 110, the step coverage is 100%. When the film thickness of the silicon nitride film 120 at the lower part of the sidewall 111 of the recess 110 is relatively thinner than the film thickness of the silicon nitride film 120 at the upper part of the sidewall 111 of the recess 110, the step coverage is less than 100%. On the other hand, when the film thickness of the silicon nitride film 120 at the lower part of the sidewall 111 of the recess 110 is relatively thicker than the film thickness of the silicon nitride film 120 at the upper part of the sidewall 111 of the recess 110, the step coverage is greater than 100%.
[0049] 8, it can be seen that there is almost no difference in the cross-sectional shape and step coverage between the Example and the Comparative Example. This result shows that the embedding characteristics of the silicon nitride film in the recesses in the Example are equivalent to the embedding characteristics of the silicon nitride film in the recesses in the Comparative Example.
[0050] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.
[0051] In the above embodiment, the processing apparatus is a batch type apparatus that processes a plurality of wafers at once, but the present disclosure is not limited thereto. For example, the processing apparatus may be a single-wafer type apparatus that processes wafers one by one. Also, for example, the processing apparatus may be a semi-batch type apparatus that processes wafers by rotating a plurality of wafers arranged on a turntable in a processing vessel by the turntable, and passing the wafers through an area where a first gas is supplied and an area where a second gas is supplied in sequence. [Explanation of symbols]
[0052] 1 Processing equipment 10 Processing vessel W wafer
Claims
1. A method for forming a silicon nitride film on a surface of a substrate, comprising the steps of: The method includes a step of intermittently supplying a process gas containing trisilylamine into a process vessel containing a substrate, thereby forming a silicon nitride film on a surface of the substrate, the step of forming the silicon nitride film is carried out without supplying a nitriding agent that nitridizes the trisilylamine; In the step of forming the silicon nitride film, the temperature of the substrate is set to 450° C. or higher, and the silicon nitride film is formed while breaking the Si—H bond of the trisilylamine and eliminating hydrogen from the trisilylamine. Film formation method.
2. The step of forming the silicon nitride film includes: supplying the trisilylamine into the processing vessel; supplying an inert gas into the processing vessel; and alternately supplying trisilylamine into the treatment vessel. The film forming method according to claim 1 .
3. The inert gas is nitrogen gas. The film forming method according to claim 2 .
Citation Information
Patent Citations
Method of manufacturing silicon nitride film or silicon oxynitride film by thermal chemical vapor deposition method
JP2004119629A
Method and apparatus for film formation, and storage medium
JP2006049809A
Deposition apparatus, deposition method, and storage medium
JP2006179819A
Deposition method, deposition equipment and storage medium
JP2006270016A
Method for depositing silicon-containing films
JP2009500857A