Powder high-speed tool steel

The Fe-based alloy composition with optimized C, Mn, Cr, Mo, V, Co, Si, and Al content, along with indices I(1) and I(2), addresses the toughness issues in powder high-speed tool steels, enhancing their performance in molding complex plastics and rolling high-strength metals.

JP7572215B2Active Publication Date: 2024-10-23SANYO SPECIAL STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020184678
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-10-23
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Existing powder high-speed tool steels exhibit insufficient toughness, leading to mold breakage during molding of small plastic products with complex shapes and inadequate performance in rolling high-strength metals, where large loads are applied.

Method used

An Fe-based alloy composition with specific ranges of C, Mn, Cr, Mo, V, Co, Si, and Al, along with indices I(1) and I(2) to optimize carbide formation and suppress solid solution C, enhancing toughness and workability.

Benefits of technology

The resulting powder high-speed tool steel demonstrates excellent toughness, extending tool life and enabling successful molding of complex plastic products and rolling of high-strength metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572215000003
    Figure 0007572215000003
  • Figure 0007572215000004
    Figure 0007572215000004
  • Figure 0007572215000005
    Figure 0007572215000005
Patent Text Reader

Abstract

To provide a powder high-speed steel having excellent toughness.SOLUTION: A powder high-speed steel is made up of an Fe-based alloy. The Fe-based alloy contains C: more than 1.0 mass% and 1.8 mass% or less, Mn: 0.10 mass% or more and 1.5 mass% or less, Cr: 6.0 mass% or more and 9.0 mass% or less, Mo: 2.0 mass% or more and 6.0 mass% or less, V: 1.0 mass% or more and 4.0% or less, Co: 1.0 mass% or more and 5.0 mass% or less, and inevitable impurities. The Fe-based alloy further contains Si: more than 1.0 mass% and 2.0 mass% or less and / or Al: 0.10 mass% or more and 1.5 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder high-speed tool steel suitable for use in dies, rolling rolls, and the like. [Background technology]

[0002] High-speed tool steel contains C, Cr, Mn, Mo, V, etc. In general, high-speed tool steel has high hardness and excellent corrosion resistance, wear resistance, and toughness. High-speed tool steel is also called "high-speed steel".

[0003] Powder metallurgy is known as a method for producing high-speed tool steel. High-speed tool steel obtained by powder metallurgy is called "powdered high-speed tool steel". Powdered high-speed tool steel is also called "powdered high-speed steel" and "sintered high-speed tool steel". Since powdered high-speed tool steel is obtained through sintering, the carbides are fine and the segregation of the carbides is small.

[0004] This powdered high-speed tool steel is used for various applications. JP 2004-27354 A discloses a powdered high-speed tool steel suitable for dies for plastic molding. JP 2005-213630 A discloses a powdered high-speed tool steel suitable for rolls used in rolling metals. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-27354 A [Patent Document 2] JP 2005-213630 A Summary of the Invention [Problem to be solved by the invention]

[0006] When molding small plastic products, localized stress is applied to the mold. When molding plastic products having complex shapes, localized stress is also applied to the mold. Concentration of stress leads to damage to the mold. The toughness of the powdered high-speed tool steel disclosed in JP 2004-27354 A is insufficient. A mold made of this powdered high-speed tool steel is prone to damage. A mold with even higher toughness is desired.

[0007] In recent years, high-strength high-tensile steels are becoming more widespread. In rolling high-strength metals such as high-tensile steels, a large load is placed on the rolls. Even in rolling to obtain thin products, a large load is placed on the rolls. A large load on the rolls hinders normal rolling. The toughness of the powdered high-speed tool steel disclosed in JP 2005-213630 A is insufficient. Rolls made of this powdered high-speed tool steel are not suitable for rolling under a large load. Rolls with even higher toughness are desired.

[0008] High toughness is also desired for tools other than dies and rolling rolls. An object of the present invention is to provide a powder high-speed tool steel having excellent toughness. [Means for solving the problem]

[0009] The powder high-speed tool steel according to the present invention is made of an Fe-based alloy. C: More than 1.0% by mass and less than 1.8% by mass Mn: 0.10 mass% or more and 1.5 mass% or less Cr: 6.0 mass% or more and 9.0 mass% or less Mo: 2.0 mass% or more and 6.0 mass% or less V: 1.0 mass% or more and 4.0% or less Co: 1.0 mass% or more and 5.0 mass% or less and Inevitable impurities The Fe-based alloy further comprises Si: More than 1.0 mass% and less than 2.0 mass% and / or Al: 0.10 mass% or more and 1.5 mass% or less Contains:

[0010] Preferably, the Fe-based alloy has an index I(1) calculated by the following formula (1) of 0.8 or greater and 2.0 or less. I(1) = (MSi + MAl) / MC (1) In this formula, MSi represents the mass content of Si, MAl represents the mass content of Al, and MC represents the mass content of C.

[0011] Preferably, the Fe-based alloy has an index I(2) calculated by the following formula (2) of 2.0 or greater and 6.5 or less. I(2) = PC + 1.5 × (ASi + AAl - 2.7) 2 (2) In this formula, PC represents the area ratio (%) of carbide, ASi represents the atomic content of Si, and AAl represents the atomic content of Al. Effect of the Invention

[0012] The powdered high-speed tool steel according to the present invention has excellent toughness, and tools obtained from this powdered high-speed tool steel have a long life. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a graph showing the relationship between the Si content and the Charpy impact value for examples of the present invention and comparative examples. [Diagram 2] FIG. 2 is a graph showing the relationship between the Al content and the Charpy impact value for the examples of the present invention and the comparative examples. [Diagram 3] FIG. 3 is a graph showing the relationship between the index I(1) and the Charpy impact value for the examples of the present invention and the comparative examples. [Figure 4] FIG. 4 is a graph showing the relationship between the index I(2) and the Charpy impact value for the examples of the present invention and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The powdered high-speed tool steel according to the present invention is obtained by sintering powder. In other words, this powdered high-speed tool steel is a sintered body. The powder is typically obtained by atomization. This powdered high-speed tool steel can be subjected to heat treatment. Typical heat treatments are quenching and tempering. The metal structure of the powdered high-speed tool steel after quenching and tempering includes a matrix (martensite phase) and a large number of metal carbides. These carbides are dispersed in the matrix.

[0015] [composition] The powder high-speed tool steel according to the present invention is made of an Fe-based alloy. C: More than 1.0% by mass and less than 1.8% by mass Mn: 0.1 mass% or more and 1.5 mass% or less Cr: 6.0 mass% or more and 9.0 mass% or less Mo: 2.0 mass% or more and 6.0 mass% or less V: 1.0 mass% or more and 4.0% or less Co: 1.0 mass% or more and 5.0 mass% or less and Inevitable impurities This Fe-based alloy further contains Si: More than 1.0 mass% and less than 2.0 mass% and / or Al: 0.1% by mass or more and 1.5% by mass or less Contains:

[0016] Preferably, the balance in this Fe-based alloy, excluding C, Mn, Cr, Mo, V, Co, Si and Al, is Fe and unavoidable impurities. The role of each element in this powder high-speed tool steel will be described in detail below.

[0017] [Carbon (C)] C dissolves in the matrix by quenching. The dissolved C can contribute to the hardness and strength of the powdered high-speed tool steel. C combines with Cr, V or Mo to form carbides. The carbides contribute to the wear resistance of the powdered high-speed tool steel. From these viewpoints, the C content is preferably more than 1.0 mass%, more preferably 1.1 mass% or more, and particularly preferably 1.2 mass% or more. Excess C causes excessive precipitation of carbides, which inhibits the toughness of the powdered high-speed tool steel. From the viewpoint of toughness, the C content is preferably 1.8 mass% or less, more preferably 1.5 mass% or less, and particularly preferably 1.4 mass% or less.

[0018] [Manganese (Mn)] Mn contributes to deoxidation in the steelmaking process. Mn also contributes to the hardenability of the powdered high-speed tool steel. From these viewpoints, the Mn content is preferably 0.10 mass% or more, more preferably 0.15 mass% or more, and particularly preferably 0.20 mass% or more. Excess Mn inhibits the workability of the powdered high-speed tool steel. From the viewpoint of workability, the Mn content is preferably 1.5 mass% or less, more preferably 0.8 mass% or less, and particularly preferably 0.5 mass% or less.

[0019] Chromium Cr combines with C to form carbides. These carbides contribute to the wear resistance of the powdered high-speed tool steel. Cr can also dissolve in the matrix. The dissolved Cr contributes to the corrosion resistance of the powdered high-speed tool steel. From these viewpoints, the Cr content is preferably 6.0 mass% or more, more preferably 6.5 mass% or more, and particularly preferably 7.0 mass% or more. Excessive Cr leads to the precipitation of excessive carbides. Excessive carbides impair the toughness and seizure resistance of the powdered high-speed tool steel. The surroundings of the carbides can become the starting point of crevice corrosion. Therefore, excessive carbides impair the corrosion resistance of the powdered high-speed tool steel. From these viewpoints, the Cr content is preferably 9.0 mass% or less, more preferably 8.5 mass% or less, and particularly preferably 8.3 mass% or less.

[0020] [Molybdenum (Mo)] Mo combines with C to form fine carbides. These carbides contribute to the strength of the powdered high-speed tool steel. From the viewpoint of strength, the Mo content is preferably 2.0 mass% or more, more preferably 2.5 mass% or more, and particularly preferably 3.0 mass% or more. Excess Mo leads to the precipitation of excessive carbides. Excessive carbides impair the toughness of the powdered high-speed tool steel. From the viewpoint of toughness, the Mo content is preferably 6.0 mass% or less, more preferably 5.5 mass% or less, and particularly preferably 5.0 mass% or less.

[0021] [Vanadium (V)] V combines with C to form fine carbides. These carbides contribute to the strength of the powdered high-speed tool steel. From the viewpoint of strength, the V content is preferably 1.0 mass% or more, more preferably 1.3 mass% or more, and particularly preferably 1.5 mass% or more. Excess V leads to the precipitation of excessive carbides. Excessive carbides impair the toughness of the powdered high-speed tool steel. From the viewpoint of toughness, the V content is preferably 4.0 mass% or less, more preferably 3.5 mass% or less, and particularly preferably 3.0 mass% or less.

[0022] [Cobalt (Co)] Co substitutes into the matrix and forms a solid solution. The dissolved Co contributes to the hardenability and strength of the powdered high-speed tool steel. From these viewpoints, the Co content is preferably 1.0 mass% or more, more preferably 1.5 mass% or more, and particularly preferably 2.0 mass% or more. Excess Co leads to high costs for the powdered high-speed tool steel. From the viewpoint of cost, the Co content is preferably 5.0 mass% or less, more preferably 4.0 mass% or less, and particularly preferably 3.0 mass% or less.

[0023] [Silicon (Si) and Aluminum (Al)] Si and Al are very important elements that characterize the powdered high-speed tool steel according to the present invention. In the powdered high-speed tool steel, carbides contribute to wear resistance. The addition of C is essential for the formation of carbides. However, C dissolves in the matrix and inhibits the toughness of the powdered high-speed tool steel. Powdered high-speed tool steels to which a large amount of C is added with emphasis on wear resistance are inferior in toughness. Si and Al promote the formation of carbides and inhibit the dissolution of C in the matrix. In the powdered high-speed tool steel containing Si or Al together with C, excellent wear resistance due to the carbides and excellent toughness due to the matrix are both achieved. The material of the powdered high-speed tool steel may be an alloy containing Si but not Al. The material of the powdered high-speed tool steel may be an alloy containing Al but not Si. The material of the powdered high-speed tool steel may be an alloy containing both Si and Al.

[0024] [Silicon (Si)] Si dissolves in the matrix. The dissolved Si contributes to the strength of the powdered high-speed tool steel. As described above, Si promotes the formation of carbides and inhibits the dissolution of C in the matrix. From these viewpoints, the Si content is preferably 1.0 mass% or more, more preferably 1.2 mass% or more, and particularly preferably 1.3 mass% or more. Excessive Si leads to the precipitation of intermetallic compounds containing Fe and Si. These intermetallic compounds inhibit the workability of the powdered high-speed tool steel. From the viewpoint of workability, the Si content is preferably 2.0 mass% or less, more preferably 1.8 mass% or less, and particularly preferably 1.6 mass% or less.

[0025] [Aluminum (Al)] Al dissolves in the matrix. The dissolved Al contributes to the strength of the powdered high-speed tool steel. As described above, Al promotes the formation of carbides and inhibits the dissolution of C in the matrix. From these viewpoints, the Al content is preferably 0.10 mass% or more, more preferably 0.15 mass% or more, and particularly preferably 0.20 mass% or more. Excessive Al leads to the precipitation of intermetallic compounds containing Fe and Al. These intermetallic compounds inhibit the workability of the powdered high-speed tool steel. From the viewpoint of workability, the Al content is preferably 1.5 mass% or less, more preferably 1.2 mass% or less, and particularly preferably 1.0 mass% or less.

[0026] [Iron (Fe)] As described above, the powder high-speed tool steel is made of an Fe-based alloy. Therefore, the main component of this powder high-speed tool steel is Fe. This powder high-speed tool steel has excellent toughness. From the viewpoint of toughness, the Fe content is preferably 60 mass% or more, more preferably 70 mass% or more, and particularly preferably 75 mass% or more.

[0027] [impurities] Powdered high-speed tool steel contains unavoidable impurities. A typical impurity is N. N causes the carbides to become coarse. The coarse carbides impair the toughness of the powdered high-speed tool steel. From the viewpoint of toughness, the N content (by mass) is preferably 300 ppm or less, and particularly preferably 200 ppm or less.

[0028] Another representative impurity is O. O causes the formation of inclusions (oxides). The inclusions can become the starting point of fracture. From the viewpoint of suppressing fracture, the O content (by mass) is preferably 300 ppm or less, and particularly preferably 200 ppm or less.

[0029] The Fe-based alloy may contain metallic impurities.

[0030] [Metal structure] As mentioned above, the metal structure of powdered high-speed tool steel after quenching and tempering contains a matrix and a large number of carbides (primary metal carbides and secondary metal carbides) dispersed in this matrix. The base of the matrix is ​​Fe. In this matrix, other elements are dissolved in Fe as a solid solution. The carbides are compounds of C and metal elements. By selecting the quenching temperature and tempering temperature suitable for the alloy composition, an appropriate metal structure can be obtained.

[0031] [Index I(1)] In the present invention, the index I(1) is calculated by the following formula (1). I(1) = (MSi + MAl) / MC (1) In this formula, MSi represents the mass content (mass%) of Si, MAl represents the mass content (mass%) of Al, and MC represents the mass content (mass%) of C.

[0032] The index I(1) is preferably 0.8 or more and 2.0 or less. According to the findings of the present inventors, in a powdered high-speed tool steel having an index I(1) of 0.8 or more, the solid solution of C in the matrix is ​​suppressed. This powdered high-speed tool steel has excellent toughness. From the viewpoint of toughness, the index I(1) is more preferably 1.0 or more, and particularly preferably 1.2 or more. According to the findings of the present inventors, in a powdered high-speed tool steel having an index I(1) of 2.0 or less, the formation of intermetallic compounds is suppressed. This powdered high-speed tool steel has excellent workability. From the viewpoint of workability, the index I(1) is more preferably 1.8 or less, and particularly preferably 1.6 or less.

[0033] [Index I(2)] In the present invention, the index I(2) is calculated by the following formula (2). I(2) = PC + 1.5 × (ASi + AAl - 2.7) 2 (2) In the formula, PC represents the area ratio (%) of carbide, ASi represents the atomic content (at%) of Si, and AAl represents the atomic content (at%) of Al.

[0034] The carbide area ratio PC is measured based on a structural photograph taken with an optical microscope. Picral solution is used as a corrosive liquid for this photograph. From this structural photograph, the area ratio PC is calculated using image analysis software. The ratio (%) of the total area of ​​all carbides contained in the measurement zone to the total area of ​​the measurement zone is the area ratio PC.

[0035] The index I(2) is preferably 2.0 or more and 6.5 or less. According to the findings of the present inventors, in a powdered high-speed tool steel having an index I(2) of 2.0 or more and 6.5 or less, the dissolution of C in the matrix and the formation of intermetallic compounds are suppressed. This powdered high-speed tool steel is excellent in toughness and workability. According to the findings of the present inventors, in a powdered high-speed tool steel having an index I(2) of 2.0 or more and 6.5 or less, the formation of excessive carbides is suppressed. In this powdered high-speed tool steel, crevice corrosion originating from the periphery of carbides is also suppressed. From these viewpoints, the index I(2) is more preferably 2.5 or more, and particularly preferably 3.0 or more.

[0036] [Powder metallurgy method] The high-speed tool steel according to the present invention can be obtained by powder metallurgy. In powder metallurgy, metal powder is first produced by atomization, pulverization, or the like. This powder is made up of a large number of particles. The material of these particles is as follows: C: More than 1.0% by mass and less than 1.8% by mass Mn: 0.10 mass% or more and 1.5 mass% or less Cr: 6.0 mass% or more and 9.0 mass% or less Mo: 2.0 mass% or more and 6.0 mass% or less V: 1.0 mass% or more and 4.0% or less Co: 1.0 mass% or more and 5.0 mass% or less and Inevitable impurities and further comprising Si: More than 1.0 mass% and less than 2.0 mass% and / or Al: 0.10 mass% or more and 1.5 mass% or less Preferably, the balance in this Fe-based alloy, excluding C, Mn, Cr, Mo, V, Co, Si and Al, is Fe and unavoidable impurities.

[0037] Examples of atomization methods include gas atomization, water atomization, and disk atomization. Gas atomization and disk atomization are preferred from the viewpoint of preventing impurities from being mixed into the powder. Gas atomization is preferred from the viewpoint of mass production. Atomization in an inert gas atmosphere is preferred from the viewpoint of preventing impurities from being mixed into the alloy.

[0038] The metal powder is pressed in a high-temperature atmosphere to solidify, and a compact is obtained. A preferred pressing method is hot isostatic pressing. In hot isostatic pressing, the powder is pressed at a high temperature of several hundred degrees Celsius to 2000 degrees Celsius with an isotropic pressure of several tens to several hundred MPa. Preferably, an inert gas such as argon gas or helium gas is used as the pressurizing medium. The use of an inert gas suppresses oxidation of the metal powder.

[0039] This formed body is subjected to hot working. This formed body is subjected to heat treatment (annealing). Furthermore, this formed body is subjected to quenching and tempering under predetermined conditions. A preferable metal structure is formed by quenching and tempering. In other words, this formed body has a metal structure obtained by quenching and tempering.

[0040] [Application] The present invention is also directed to a tool. The material of the tool according to the present invention is a powder high-speed tool steel. This powder high-speed tool steel is C: More than 1.0% by mass and less than 1.8% by mass Mn: 0.10 mass% or more and 1.5 mass% or less Cr: 6.0 mass% or more and 9.0 mass% or less Mo: 2.0 mass% or more and 6.0 mass% or less V: 1.0 mass% or more and 4.0% or less Co: 1.0 mass% or more and 5.0 mass% or less and Inevitable impurities and further comprising Si: More than 1.0 mass% and less than 2.0 mass% and / or Al: 0.10 mass% or more and 1.5 mass% or less The Fe-based alloy preferably contains C, Mn, Cr, Mo, V, Co, Si and Al, and the remainder of the Fe-based alloy is Fe and unavoidable impurities. The powder high-speed tool steel has an index I(1) calculated by the above formula (1) of 0.8 or more and 2.0 or less. The powder high-speed tool steel has an index I(2) calculated by the above formula (2) of 2.0 or more and 6.5 or less.

[0041] A specific example of a tool is a mold for molding plastics. The powdered high-speed tool steel according to the present invention is suitable for molds for small plastic products. The powdered high-speed tool steel according to the present invention is also suitable for molds for plastic products having complex shapes.

[0042] Another application of the powdered high-speed tool steel is a roll for a metal product. The powdered high-speed tool steel according to the present invention is suitable for a roll for a metal product made of high-strength high-tensile steel. The powdered high-speed tool steel according to the present invention is also suitable for a roll for a thin metal product. EXAMPLES

[0043] The effects of the present invention will be clarified by the following examples, but the present invention should not be construed as being limited based on the description of these examples.

[0044] [Example 1] The molten metal was gas atomized to obtain a powder. The powder was filled into a cylindrical steel can with a diameter of 180 mm and a length of 100 mm. The steel can was vacuum degassed and then sealed. In an argon gas atmosphere, hot isostatic pressing was performed for 6 hours under conditions of a pressure of 100 MPa and a temperature of 1150°C to obtain a compact. The steel can-derived portion was removed from the compact. The compact was forged, rolled, and hot extruded at a temperature of 1100-1200°C to obtain a diameter of 50 mm. The compact was held at a temperature of 800-950°C for 0.5-3.0 hours and slowly cooled at a rate of 15°C / h (annealing). The composition of the compact is shown in Table 1 below. In addition to the elements shown in Table 1, the compact contains unavoidable impurities.

[0045] [Examples 2-20 and Comparative Examples 1-10] Molded articles of Examples 2-20 and Comparative Examples 1-10 were obtained in the same manner as in Example 1, except that the compositions were as shown in Tables 1 and 2 below.

[0046] [Specific wear rate] Plate-shaped test pieces measuring 10 mm x 25 mm x 50 mm were obtained from the compacts. These test pieces were quenched at temperatures of 1050-1200°C and then tempered. The tempering conditions were selected from the following ranges so that the Rockwell hardness of the test pieces was 64-65HRC. Tempering temperature: 450-600℃ Tempering time: 1-3 hours The test piece was subjected to a finishing process. The test piece was set in an Ohkoshi type abrasion tester, and the specific abrasion rate was measured under the following measurement conditions. Mating material: SCM420 Wear rate: 0.2m / sec Wear distance: 200m Final load: 61.8N Lubrication: None Temperature: room temperature The wear scar width obtained in the test was measured, and the wear volume was calculated. The wear volume was divided by the product of the wear distance and the final load to calculate the specific wear rate. The average values ​​of the results of three measurements are shown in Tables 1 and 2 below. The unit of the specific wear rate in Tables 1 and 2 is "10 -8 (mm 3 / Nmm).

[0047] [Charpy impact value] Test pieces (size: 10mm x 10mm x 50mm, notch: 10RC) were obtained from the compacts. These test pieces were quenched at temperatures of 1050-1200℃ and then tempered. The tempering conditions were selected from the following ranges so that the Rockwell hardness of the test pieces was 64-65HRC. Tempering temperature: 450-600℃ Tempering time: 1-3 hours The test pieces were subjected to a Charpy impact test to measure the impact value. The results are shown in the following Tables 1 and 2 and Figures 1 to 4. In Figures 3 and 4, "Example (AB)" represents the powdered high-speed tool steel with an overall rating of "A" or "B" in Tables 1 and 2, "Example (C)" represents the powdered high-speed tool steel with an overall rating of "C" in Tables 1 and 2, and "Example (D)" represents the powdered high-speed tool steel with an overall rating of "D" in Tables 1 and 2.

[0048] [comprehensive evaluation] The powdered high speed tool steels were graded based on the following criteria: A: Ogoshi abrasion test is 0.30×10 -8 mm 3 / Nmm or less, and the Charpy impact value is 55J / cm 2 That's all. B: Ogoshi abrasion test is 0.30×10 -8 mm 3 / Nmm or less, and the Charpy impact value is 50J / cm 2 More than 55J / cm 2 is less than. C: Ogoshi abrasion test is 0.30×10 -8 mm 3 / Nmm or less, and the Charpy impact value is 45J / cm 2 More than 50J / cm 2 is less than. D: Ogoshi abrasion test is 0.30×10 -8 mm 3 / Nmm or less, and the Charpy impact value is 40J / cm 2 More than 45J / cm 2 is less than. F: Ogoshi abrasion test is 0.30×10 -8 mm 3 / Nmm or less, and the Charpy impact value is 40J / cm 2 is less than. The results are shown in Tables 1 and 2 below.

[0049] [Table 1]

[0050] [Table 2]

[0051] As shown in Tables 1 and 2, the wear resistance of the powdered high-speed tool steels of the Examples is equivalent to that of the powdered high-speed tool steels of the Comparative Examples. Furthermore, as is clear from Tables 1 and 2 and Figures 1 to 4, the powdered high-speed tool steels of the Examples are excellent in toughness. From the above evaluation results, the superiority of the present invention is clear. [Industrial Applicability]

[0052] The powdered high-speed tool steel according to the present invention can be used for various applications such as dies, rollers, machine tools, hand tools, injection molding machine parts, die caps, punches, and blades.

Claims

1. The material is C: more than 1.0 mass% and not more than 1.8 mass% Mn: 0.10% by mass or more and 1.5% by mass or less Cr: 6.0% by mass or more and 9.0% by mass or less Mo: 2.0% by mass or more and 6.0% by mass or less V: 1.0% by mass or more and 4.0% by mass or less and Co: 1.0% by mass or more and 5.0% by mass or less and further comprising Si: more than 1.0 mass% and not more than 2.0 mass% and / or Al: 0.10% by mass or more and 1.5% by mass or less It contains The remainder of the powder high-speed tool steel is an Fe-based alloy containing Fe and unavoidable impurities.

2. 2. The powder metallurgical high-speed tool steel according to claim 1, wherein an index I(1) calculated by the following mathematical formula (1) is 0.8 or more and 2.0 or less: I(1) = (MSi + MAl) / MC (1) (In the above formula, MSi represents the mass content of Si, MAl represents the mass content of Al, and MC represents the mass content of C.)

3. 3. The powder metallurgical high-speed tool steel according to claim 1, wherein an index I(2) calculated by the following mathematical formula (2) is 2.0 or more and 6.5 or less: I(2) = PC + 1.5 × (ASi + AAl - 2.7) 2 (2) (In the above formula, PC represents the area ratio (%) of carbide, ASi represents the atomic content of Si, and AAl represents the atomic content of Al.)

4. The material is C: more than 1.0 mass% and not more than 1.8 mass% Mn: 0.10% by mass or more and 1.5% by mass or less Cr: 6.0% by mass or more and 9.0% by mass or less Mo: 2.0% by mass or more and 6.0% by mass or less V: 1.0% by mass or more and 4.0% by mass or less Co: 1.0% by mass or more and 5.0% by mass or less Si: 2.0% by mass or less and Al: 0.10% by mass or more and 1.5% by mass or less It contains The remainder of the powder high-speed tool steel is an Fe-based alloy containing Fe and unavoidable impurities.

Citation Information

Patent Citations

  • Wearable high-speed steel

    CN103789651A

  • High-speed tool steel having superior toughness

    JP1988118054A

  • Steel for plastic molding having excellent corrosion resistance and wear resistance and molded part

    JP2004027354A

  • Powder high speed tool steel for mill roll having excellent wear resistance and toughness

    JP2005213630A

  • Powdered high-speed steel

    JP2021147638A