Novel unsaturated group-containing epoxy carboxylate compound, its derivative, photosensitive resin composition containing the same, and cured product thereof
A resin composition with monocarboxylic acid and reactive epoxycarboxylate compounds addresses curing inefficiencies and developability issues, enabling fine pattern formation and high insulation in high-density printed wiring boards.
Patent Information
- Application Number
- JP2021070517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-19
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-04-19
AI Technical Summary
Existing solder resist materials require high doses of active energy rays for curing, have poor developability with dilute alkaline solutions, and struggle with forming fine patterns and vias in high-density printed wiring boards, leading to inefficiencies in manufacturing.
A resin composition containing monocarboxylic acid compounds with ethylenically unsaturated groups and reactive epoxycarboxylate compounds, which are reacted with polybasic acid anhydrides to create a photosensitive resin with improved sensitivity, developability, and high insulation and adhesion properties.
The resin composition achieves excellent photosensitivity, allowing for fine pattern formation with dilute alkaline solutions, high insulation, and heat resistance, enhancing manufacturing efficiency in high-density printed wiring boards.
Smart Images

Figure 0007572290000001 
Figure 0007572290000002 
Figure 0007572290000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel unsaturated group-containing epoxy carboxylate compound, a derivative thereof, a photosensitive resin composition containing the same, and a cured product thereof. [Background technology]
[0002] In recent years, there has been a demand for printed wiring boards with higher precision and density in order to make portable devices smaller and lighter and to improve communication speeds. Accordingly, the demands on the solder resist that covers the circuits themselves are also becoming increasingly stringent. Compared to conventional demands, solder resists are now required to have better heat resistance and thermal stability while still providing adhesion to the substrate, high insulation properties, and excellent developability, and there is a demand for film-forming materials with tougher curing properties.
[0003] In general, excellent properties such as heat resistance and thermal stability are achieved by introducing many reactive groups into a main chain having a rigid skeleton and imparting a high crosslink density. Such resins have been suitably used in applications such as ordinary solder resists, color resists for displays, and hard coats.
[0004] As one of these materials, Patent Document 1 discloses a carboxylate resin obtained by reacting acrylic acid and a polybasic acid anhydride together, which has an epoxy resin having a polycyclic hydrocarbon group of a specific structure as a basic skeleton, as a material having excellent insulating properties and heat resistance (Patent Document 1).
[0005] However, this carboxylate resin has low curability with active energy rays, and requires a large amount of irradiation with active energy rays to cure sufficiently. In addition, the developability with a dilute alkaline aqueous solution is poor, which causes a problem that a pattern of the required shape cannot be obtained.
[0006] On the other hand, the build-up method is a conventional method for manufacturing printed circuit boards. This build-up method alternates between stacking interlayer insulating layers and conductor layers on the conductor layers of an inner circuit board, and forms via holes in the interlayer insulating layers to enable connections between the layers. Laser processing is the mainstream method for forming vias in the interlayer insulating layers (Patent Document 2).
[0007] However, as the density of printed wiring boards increases, the diameter of vias needs to be further reduced, and the reduction in diameter achieved by laser irradiation using a laser processing machine is reaching its limit. Furthermore, when forming vias using a laser processing machine, each via hole needs to be formed one by one, and when a large number of vias are provided due to high density, it takes a long time to form the vias, resulting in poor manufacturing efficiency. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 5-214048 [Patent Document 2] Japanese Patent Application Publication No. 7-304931 Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a resin composition which has excellent photosensitivity to active energy rays, is capable of forming a fine pattern by development with a dilute aqueous alkali solution, and is capable of forming a film having high insulating properties, adhesion and heat resistance, and a cured product thereof. [Means for solving the problem]
[0010] Means for Solving the Problems The present inventors have conducted intensive research in order to solve the above-mentioned problems, and as a result have found that a reactive epoxy carboxylate compound obtained by reacting a monocarboxylic acid compound having one or more ethylenically unsaturated groups in a specific molecule with a compound having a hydroxyl group and a carboxy group in one molecule, if necessary, and an unsaturated group-containing polycarboxylic acid compound obtained by reacting the reactive epoxy carboxylate compound with a polybasic acid anhydride, and a resin composition containing them are excellent in photosensitivity and developability, and further, the cured product thereof has excellent heat resistance and insulating reliability, thereby completing the present invention.
[0011] That is, the present invention includes the following. (1) A reactive epoxy carboxylate compound (A) obtained by reacting an epoxy resin (a) represented by the following general formula (1), in which the total content of an epoxy compound represented by the following formula (2) and an epoxy compound represented by the following formula (3) is 1 area % or more and less than 70 area % in the total amount of all epoxy compounds represented by n=1 in the epoxy resin, in terms of HPLC area percentage, with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, a compound (c) having a hydroxyl group and a carboxy group in one molecule.
[0012] [ka] (In formula (1), G represents a substituted or unsubstituted glycidyl group. p and q each exist independently and represent a real number of 1 or 2. n represents a real number of 1 to 20.)
[0013] [ka] (In formula (2), G represents a substituted or unsubstituted glycidyl group.)
[0014] [ka] (In formula (3), G represents a substituted or unsubstituted glycidyl group.) (2) The epoxy resin (a) according to (1) above has an epoxy equivalent of 200 g / eq. or more and less than 230 g / eq. (A) containing an unsaturated group. (3) A reactive epoxy carboxylate compound (A) obtained by reacting an epoxy compound (a) represented by the following formula (2) or (3) with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, a compound (c) having a hydroxyl group and a carboxyl group in one molecule:
[0015] [ka] (In formula (2), G represents a substituted or unsubstituted glycidyl group.)
[0016] [ka] (In formula (3), G represents a substituted or unsubstituted glycidyl group.) (4) An unsaturated group-containing polycarboxylic acid compound (B) obtained by reacting the reactive epoxy carboxylate compound (A) according to any one of (1) to (3) with a polybasic acid anhydride (d). (5) The unsaturated group-containing polycarboxylic acid resin (B) according to any one of (1) to (3), having an acid value of the solid content of 40 to 160 mg·KOH / g. (6) A photosensitive resin composition comprising the unsaturated group-containing epoxy carboxylate compound (A) or the unsaturated group-containing polycarboxylic acid resin (B) according to any one of (1) to (4), a photopolymerization initiator (C) and a crosslinking agent (D). (7) The photosensitive resin composition according to (6), further comprising a curing agent (E). (8) The photosensitive resin composition according to (6) or (7), which is a film-forming material. (9) The photosensitive resin composition according to (6) or (7), which is a material for a permanent resist. (10) A cured product of the photosensitive resin composition according to any one of (6) to (9). Effect of the Invention
[0017] According to the present invention, it is possible to provide a resin composition and a cured product thereof which have excellent photosensitivity to active energy rays, and which are capable of forming patterns of fine images and vias by development with a dilute alkaline aqueous solution, and which are capable of forming a film having high insulating properties, adhesion, and heat resistance.
[0018] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The following embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out with appropriate modifications within the scope of its gist.
[0019] The epoxy resin (a) is an epoxy resin represented by the following general formula (1), and is characterized in that the total content of the epoxy compound represented by the following formula (2) and the epoxy compound represented by the following formula (3) is 1 area % or more and less than 70 area % in the total amount of all epoxy compounds represented by n=1 in the epoxy resin.
[0020] [ka] (In formula (1), G represents a substituted or unsubstituted glycidyl group. p and q each exist independently and represent a real number of 1 or 2. n represents a real number of 1 to 20.)
[0021] [ka] (In formula (2), G represents a substituted or unsubstituted glycidyl group.)
[0022] [ka] (In formula (3), G represents a substituted or unsubstituted glycidyl group.)
[0023] In the above formula (1), G is a substituted or unsubstituted glycidyl group, and the substituent is preferably an alkyl group, particularly preferably a methyl group. In the formula (1), when p and q are 2, the orientation of the glycidyl ether group may be any of the ortho, meta, and para positions relative to one glycidyl ether group, but is preferably the meta position.
[0024] In the formula (1), the value of n can be calculated from the number average molecular weight of the epoxy resin determined by gel permeation chromatography (GPC, detector: RI) or the area ratio of each separated peak. n is usually a real number of 1 to 20, preferably 1 to 10, and more preferably 1 to 5.
[0025] The epoxy equivalent of the epoxy resin is preferably 190 g / eq. or more and less than 230 g / eq., more preferably 200 g / eq. or more and less than 230 g / eq., even more preferably 210 g / eq. or more and less than 230 g / eq., and particularly preferably 220 g / eq. or more and less than 228 g / eq. When the epoxy equivalent is 190 g / eq. or more, a high elastic modulus is obtained, and when it is 230 g / eq. or less, heat resistance is good.
[0026] The epoxy resin has a resinous form having a softening point. The softening point is preferably 50 to 90°C, more preferably 60 to 75°C, and even more preferably 60 to 68°C. A softening point of 50°C or higher means that the molecular weight distribution is appropriate or that there is no residual solvent, etc., and the heat resistance is good, and problems such as poor curing and voids during molding can be suppressed. A softening point of 90°C or lower provides good handling when kneading with other resins.
[0027] The melt viscosity is preferably 0.05 Pa·s or more and 1.0 Pa·s or less (ICI melt viscosity (150°C) cone plate method), more preferably 0.06 Pa·s or more and 0.2 Pa·s or less, and even more preferably 0.07 Pa·s or more and 0.1 Pa·s or less. A viscosity of 0.05 Pa·s or more results in an appropriate molecular weight distribution and good solubility in solvents. A melt viscosity of 1.0 Pa·s or less results in good handling when kneaded with other resins.
[0028] In the above formula (1), when n=1, one of p and q is 1 and the other is 2, the epoxy compound is represented by the above formula (2) or (3).
[0029] In the formulas (2) and (3), G is a substituted or unsubstituted glycidyl group, and the substituent is preferably an alkyl group, particularly preferably a methyl group. Furthermore, when a benzene ring has two substituted or unsubstituted glycidyl ether groups, the orientation may be any of the ortho, meta, and para positions relative to one glycidyl ether group, but is preferably the meta position.
[0030] The total content of the epoxy compound represented by the formula (2) and the epoxy compound represented by the formula (3) can be determined by an analytical method using two techniques, namely, gel permeation chromatography analysis and high performance liquid chromatography analysis.
[0031] ·GPC (gel permeation chromatography) analysis Manufacturer:Waters Column: Guard column SHODEX GPC KF-601 (2 columns), KF-602 KF-602.5, KF-603 Flow rate: 1.23ml / min. Column temperature: 25℃ Solvent used: THF (tetrahydrofuran) Detector: RI (Differential Refraction Detector)
[0032] High performance liquid chromatography analysis Shimadzu Corporation Liquid Delivery Unit LC-20AD Shimadzu Corporation Photodiode array detector SPD-M20A Shimadzu Corporation Column Oven CTO-20A Column: Intersil ODS-2, 5 μm, 4.6 × 250 mm, 40 °C MobilPhaseA: Acetonitrile (AN) MobilPhaseB: Water (W) Time Program: 0-28min.AN / W=30% / 70%→100% / 0% 28-40min.AN / W=100% / 0% Flow Rate: 1.0mL / min. Detection: UV274nm, PDA
[0033] The content ratio (α) of the n=1 component in the epoxy resin represented by the formula (1) can be determined by gel permeation chromatography analysis, and the content ratio (β2) of the epoxy compound represented by the formula (2) contained in the n=1 component and the content ratio (β3) of the epoxy compound represented by the formula (3) can be determined by high performance liquid chromatography analysis. For example, the product of α and β2 is the content ratio of the epoxy compound represented by the formula (2) contained in the epoxy compound represented by the formula (1). The content ratios of the epoxy compound represented by the formula (2) and the epoxy compound represented by the formula (3) contained in the epoxy resin represented by the formula (1) are expressed as α×(β2+β3). Specifically, the content ratio of the epoxy compound of formula (2) and the epoxy compound of formula (3) in the epoxy resin of formula (1) is expressed as "(GPC area % of the epoxy compound represented by n=1 in the epoxy resin of formula (1) × (HPLC area % of the epoxy compound represented by formula (2) relative to the total epoxy compounds represented by n=1) + (HPLC area % of the epoxy compound represented by formula (3) relative to the total epoxy compounds represented by n=1 as determined by HPLC analysis)."
[0034] In this embodiment, the total content of the epoxy compound represented by formula (2) and the epoxy compound represented by formula (3) is, in terms of HPLC area percentage, 1 area % or more and less than 70 area %, preferably 1 area % or more and less than 30 area %, more preferably 3 area % or more and less than 20 area %, and particularly preferably 5 area % or more and 15 area % or less, in the total amount of the epoxy resin represented by formula (1) (n=1). When the ratio is 70 area % or less, a high elastic modulus is obtained, and when it is 1 area % or more, it is preferable because the heat resistance is good.
[0035] The total content of the epoxy compound represented by the formula (2) and the epoxy compound represented by the formula (3) in the epoxy resin represented by the formula (1) is preferably 1 area% or more and 20 area% or less, more preferably 3 area% or more and 15 area% or less, and particularly preferably 5 area% or more and 10 area% or less. When the ratio is 20 area% or less, a high elastic modulus is obtained, and when it is 1 area% or more, heat resistance is good, so this is preferable. Here, the "area%" is the product of the above-mentioned GPC area% and HPLC area%.
[0036] In the epoxy resin of the present embodiment, p and q in the formula (1) are both 1 or 2. By controlling p and q, the crosslink density of the cured product can be adjusted to obtain a cured product with excellent heat resistance and mechanical properties. When p and q are both 1 or 2, the crosslink density is higher than when p and q are both 1, and therefore the heat resistance is excellent. In addition, when p and q are both 2, that is, when the functional group density is increased, the mechanical strength is superior and the increase in water absorption is suppressed. By suppressing the increase in water absorption, it is possible to suppress adverse effects such as a significant decrease in strength after absorbing moisture. This not only suppresses the deterioration of properties due to the polarity of the epoxy group by suppressing the epoxy group density from becoming too high, but also avoids problems such as epoxy groups not reacting well with the curing agent when they are close to each other and remaining unreacted, or problems such as crosslinking within the molecule and not improving heat resistance much.
[0037] The epoxy resin represented by the above formula (1) can be obtained by reacting a phenol resin represented by the following formula (4) with epihalohydrin.
[0038] [ka]
[0039] (In formula (4), p and q each exist independently and represent a real number of 1 or 2. n represents a real number of 1 to 20.)
[0040] The preferred ranges of n, p and q in the formula (4) are the same as those in the formula (1).
[0041] In the synthesis method of the phenol resin represented by the formula (4) above, when dicyclopentadiene is reacted (condensed) with a phenol, the amount of the phenol is preferably in the range of 3 to 20 moles, particularly preferably 5 to 15 moles, per mole of dicyclopentadiene.
[0042] Examples of phenols include disubstituted phenols such as catechol, resorcinol, and hydroquinone, and monosubstituted phenols such as phenol. These may be used alone or in combination of two or more kinds.
[0043] In the above condensation reaction, it is preferable to use an acid catalyst, and as the acid catalyst, Lewis acids such as boron trifluoride, anhydrous aluminum chloride, zinc chloride, sulfuric acid, titanium chloride, etc. are preferable, and in particular, ether complexes and phenol complexes of the above Lewis acids are preferable. These acid catalysts may be used alone or in combination of two or more kinds.
[0044] The amount of these acid catalysts used is not particularly limited, but can be selected in the range of 0.001 to 0.1 moles relative to the amount of dicyclopentadiene used. When these acid catalysts are added to the reaction system, they can be added in advance to a heated melt of a phenol or diluted in a suitable solvent and then gradually added.
[0045] The condensation reaction in the presence of these acid catalysts is preferably carried out in the range of 40 to 180°C, particularly preferably in the range of 80 to 165°C, and the reaction time can usually be selected in the range of 0.5 to 10 hours. These reactions can also be carried out in the presence of a solvent inert to the reaction, such as nitrobenzene, diphenyl ether, dichlorobenzene, carbon disulfide, etc. Furthermore, the reaction product thus obtained is neutralized so that the system becomes neutral, or repeatedly washed with water in the presence of a solvent, and the water is separated and drained, and then the solvent and unreacted materials are removed under heating and reduced pressure to obtain the phenolic resin represented by the above formula (4).
[0046] The hydroxyl equivalent of the phenolic resin represented by the formula (4) is preferably in the range of 120 g / eq. or more and less than 160 g / eq., more preferably 135 g / eq. or more and less than 160 g / eq., even more preferably 140 g / eq. or more and less than 160 g / eq., and particularly preferably 145 g / eq. or more and less than 155 g / eq. When the hydroxyl equivalent is 120 g / eq. or more and 160 g / eq. or less, the hydroxyl equivalent is appropriate, and therefore the heat resistance of the cured product can be improved without causing a decrease in mechanical strength.
[0047] The softening point of the phenol resin represented by the formula (4) is preferably in the range of 90 to 140° C., and more preferably 100 to 130° C. When the softening point is in the above range, the resins do not block each other at room temperature, resulting in excellent handleability.
[0048] Next, the reaction for obtaining the epoxy resin (a) will be described. The epoxy resin of the present embodiment can be obtained, for example, by reacting a phenol resin represented by the above formula (4) with epihalohydrin.
[0049] The epihalohydrin is easily available on the market. The amount of epihalohydrin used is usually 4.0 to 10 moles, preferably 4.5 to 8.0 moles, more preferably 5.0 to 7.0 moles per mole of hydroxyl groups in the raw phenol mixture. During epoxidation, the generated epoxy resin reacts with the unreacted phenolic hydroxyl groups to generate an epoxy resin having a glycerin ether moiety. The more glycerin ether moieties, the higher the toughness of the epoxy resin cured product, which is preferable. In addition, since the increase in the melt viscosity due to the increase in the molecular weight of the epoxy resin, which occurs when there are many glycerin ether moieties, can be suppressed, the amount of epihalohydrin used must be in accordance with the design. Using an excess of epihalohydrin relative to the hydroxyl groups of the raw phenol resin can suppress the intermolecular reaction during epoxidation, and an epoxy resin with a low viscosity can be obtained, which is preferable.
[0050] In the above reaction, an alkali metal hydroxide can be used as a catalyst for promoting the epoxidation step. Examples of alkali metal hydroxides that can be used include sodium hydroxide, potassium hydroxide, etc., and a solid or an aqueous solution thereof can be used. In this embodiment, however, it is particularly preferable to use a solid formed into a flake shape from the standpoint of solubility and handling. The amount of the alkali metal hydroxide used is usually 0.90 to 1.5 mol, preferably 0.95 to 1.25 mol, and more preferably 0.99 to 1.15 mol, per mol of hydroxyl groups in the raw material phenol mixture.
[0051] In order to promote the reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may be added as a catalyst. The amount of the quaternary ammonium salt used is usually 0.1 to 15 g, preferably 0.2 to 10 g, per mole of hydroxyl groups in the raw material phenol mixture.
[0052] The reaction temperature is usually 30 to 90° C., preferably 35 to 80° C. In particular, in this embodiment, for higher purity epoxidation, a temperature of 50° C. or higher is preferred, and particularly 60° C. or higher is preferred. The reaction time is usually 0.5 to 10 hours, preferably 1 to 8 hours, and particularly preferably 1 to 3 hours. If the reaction time is too short, the reaction will not proceed to completion, and if the reaction time is too long, by-products will be produced, which is undesirable. The reaction product of these epoxidation reactions is washed with water or heated under reduced pressure to remove epihalohydrin and solvent. Furthermore, in order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the recovered epoxy resin can be dissolved in a ketone compound having 4 to 7 carbon atoms (e.g., methyl isobutyl ketone, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc.) as a solvent, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to carry out the reaction to ensure ring closure. In this case, the amount of the alkali metal hydroxide used is usually 0.01 to 0.3 mol, preferably 0.05 to 0.2 mol, per mol of hydroxyl group in the raw material phenol mixture used in the epoxidation. The reaction temperature is usually 50 to 120°C, and the reaction time is usually 0.5 to 2 hours.
[0053] After the reaction is completed, the salt formed is removed by filtration, washing with water, or the like, and the solvent is then distilled off under heating and reduced pressure to obtain the epoxy resin of the present embodiment.
[0054] Next, the carboxylation step will be described. In this reaction, the obtained epoxy resin (a) is reacted with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, and, if necessary, a compound (c) having a hydroxyl group and a carboxyl group in one molecule to obtain a reactive carboxylate compound (A).
[0055] Examples of the monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule used in the carboxylation step include acrylic acids, crotonic acid, α-cyanocinnamic acid, cinnamic acid, or a reaction product of a saturated or unsaturated dibasic acid and an unsaturated group-containing monoglycidyl compound. Examples of the acrylic acids include (meth)acrylic acid, β-styrylacrylic acid, β-furfurylacrylic acid, half esters which are equimolar reactants of a saturated or unsaturated dibasic acid anhydride and a (meth)acrylate derivative having one hydroxyl group in one molecule, and half esters which are equimolar reactants of a saturated or unsaturated dibasic acid and a monoglycidyl (meth)acrylate derivative, and the like. In terms of sensitivity when made into a photosensitive resin composition, (meth)acrylic acid, a reaction product of (meth)acrylic acid and ε-caprolactone, or cinnamic acid are particularly preferred.
[0056] Specific examples of the monocarboxylic acid compound (d) having at least two hydroxyl groups in the molecule used in the carboxylation step include polyhydroxycarboxylic acids such as dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolacetic acid, dimethylolbutyric acid, dimethylolvaleric acid, dimethylolcaproic acid, etc. Particularly preferred examples include dimethylolpropionic acid, dimethylolbutanoic acid, etc.
[0057] The reaction of the epoxy resin (a) with the monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, the compound (c) having a hydroxyl group and a carboxyl group in one molecule can be carried out in a solventless or organic solvent, specifically, for example, ketones such as acetone, ethyl methyl ketone, and cyclohexanone, aromatic hydrocarbons such as benzene, toluene, xylene, and tetramethylbenzene, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, triethylene glycol dimethyl ether, and the like. The copolymer can be obtained by reacting the copolymer in an organic solvent, such as glycol ethers such as triethylene glycol diethyl ether, ethyl acetate, butyl acetate, methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, propylene glycol monomethyl ether acetate, dialkyl glutarate, dialkyl succinate, dialkyl adipate, and other esters, cyclic esters such as γ-butyrolactone, petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, or a crosslinking agent (D) described below, either alone or in a mixture of such organic solvents.
[0058] In the reaction of obtaining a reactive epoxy carboxylate compound (A) by reacting an epoxy resin (a) with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, a compound (c) having a hydroxyl group and a carboxyl group in one molecule, the addition ratio of the monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule is preferably 0.8 to 1.2 equivalents per equivalent of the epoxy compound (a) having two or more glycidyl groups in the molecule. If the ratio is outside this range, gelation may occur during the reaction, or the thermal stability of the finally obtained unsaturated group-containing polycarboxylic acid resin (B) may be reduced.
[0059] During the reaction, it is preferable to add a thermal polymerization inhibitor to suppress the thermal polymerization reaction, and the amount of the thermal polymerization inhibitor is 0.1 to 10 parts by mass per 100 parts by mass of the total amount of the reaction mixture including the epoxy compound (a) having two or more glycidyl groups in the molecule, the monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, and optionally the monocarboxylic acid compound (d) having at least two hydroxyl groups in the molecule, and the solvent. Examples of the thermal polymerization inhibitor include hydroquinone, 2-methylhydroquinone, hydroquinone monomethyl ether, and 2,6-di-tert-butyl-p-cresol.
[0060] In addition, it is preferable to use a catalyst during the reaction to promote the reaction, and the amount of the catalyst used is 0.1 to 10 parts by mass per 100 parts by mass of the total amount of the reaction mixture including the epoxy resin (a), the monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, and the compound (c) having a hydroxyl group and a carboxyl group in one molecule as necessary, and the solvent. The reaction temperature is 60 to 150°C, and the reaction time is preferably 3 to 60 hours. Examples of the catalyst used in this reaction include dimethylaminopyridine, triethylamine, benzyldimethylamine, triethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium iodide, triphenylphosphine, triphenylstibine, methyltriphenylstibine, chromium 2-ethylhexanoate, chromium octanoate, zinc 2-ethylhexanoate, zinc octanoate, zirconium octanoate, dimethylsulfide, and diphenylsulfide.
[0061] The reaction is preferably allowed to proceed until the acid value (solid acid value) is 3mg·KOH / g or less. The solid acid value is the amount (mg) of potassium hydroxide required to neutralize the acidity of the carboxylic acid in 1g of resin, and the acid value is the amount (mg) of potassium hydroxide required to neutralize 1g of a solution containing the resin, and is measured by a normal neutralization titration method in accordance with JIS K0070. In addition, if the concentration of the resin in the solution is known, the solid acid value can also be calculated from the acid value of the solution.
[0062] The preferred molecular weight range of the reactive epoxy carboxylate compound (A) obtained by reacting an epoxy resin (a) with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, a compound (c) having a hydroxyl group and a carboxyl group in one molecule is, in terms of polystyrene, a weight average molecular weight measured by GPC of 500 to 50,000, more preferably 500 to 30,000, and particularly preferably 500 to 10,000.
[0063] Next, the acid addition step will be described in detail. The acid addition step is carried out for the purpose of introducing a carboxyl group into the reactive epoxy carboxylate compound (A) obtained in the previous step as necessary to obtain an unsaturated group-containing polycarboxylic acid compound (B). That is, the hydroxyl group generated by the carboxylation reaction is subjected to an addition reaction with a polybasic acid anhydride (d), thereby introducing a carboxyl group via an ester bond.
[0064] Specific examples of the polybasic acid anhydride (d) include, for example, any compound having an acid anhydride structure in the molecule, and particularly preferred are succinic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, itaconic anhydride, 3-methyl-tetrahydrophthalic anhydride, 4-methyl-hexahydrophthalic anhydride, trimellitic anhydride, and maleic anhydride, which are excellent in alkaline aqueous solution developability, heat resistance, hydrolysis resistance, and the like.
[0065] The reaction of adding the polybasic acid anhydride (d) can be carried out by adding the polybasic acid anhydride (d) to the carboxylation reaction liquid. The amount of the polybasic acid anhydride added should be appropriately changed depending on the application.
[0066] For example, when the polycarboxylic acid compound (B) of the present invention is used as an alkali development resist, the amount of polybasic acid anhydride (d) added is preferably calculated so that the solid acid value (based on JIS K5601-2-1:1999) of the finally obtained reactive polycarboxylic acid compound (B) is 40 to 120 mg KOH / g, more preferably 60 to 110 mg KOH / g. When the solid acid value is within this range, the photosensitive resin composition of the present invention exhibits good developability in an aqueous alkaline solution. That is, there is good patterning property, a wide control range for overdevelopment, and no excess acid anhydride remains.
[0067] During the reaction, it is preferable to use a catalyst to promote the reaction, and the amount of the catalyst used is 0.1 to 10 parts by weight based on the total amount of the reactants, i.e., the epoxy compound (a), the carboxylate compound obtained from the carboxylic acid compound (b), and the polybasic acid anhydride (d), and optionally the solvent and other components. The reaction temperature is 60 to 150°C, and the reaction time is preferably 5 to 60 hours. Specific examples of catalysts that can be used include triethylamine, benzyldimethylamine, triethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium iodide, triphenylphosphine, triphenylstibine, methyltriphenylstibine, chromium octanoate, zirconium octanoate, and the like.
[0068] The acid addition step can be carried out without a solvent or diluted with a solvent. When a solvent is used, the solvent is not particularly limited as long as it is an inert solvent in the acid addition reaction. When a solvent is used in the preceding urethane formation step, the acid addition reaction can be carried out without removing the solvent if the solvent is inert in both reactions.
[0069] The amount of the solvent used should be adjusted appropriately depending on the viscosity and use of the resin obtained, but it is preferable to use the solvent so that the solid content is 90 to 40% by weight, more preferably 80 to 40% by weight. As the solvent, the same solvents as those exemplified in the carboxylation step may be used.
[0070] In the photosensitive resin composition of the present invention, a photopolymerization initiator (C) can be used as necessary. Specific examples of the photopolymerization initiator (C) include radical type photopolymerization initiators and cationic type photopolymerization initiators. Examples of the radical type photopolymerization initiator include benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, and benzoin isobutyl ether; acetophenones such as acetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-phenylpropan-1-one, diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one; 2-ethylanthraquinone, 2 thioxanthones such as 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone; ketals such as acetophenone dimethyl ketal, benzyl dimethyl ketal; benzophenones such as benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 4,4'-bismethylaminobenzophenone; and phosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0071] Examples of the cationic photopolymerization initiator include diazonium salts of Lewis acids, iodonium salts of Lewis acids, sulfonium salts of Lewis acids, phosphonium salts of Lewis acids, other halides, triazine-based initiators, borate-based initiators, and other photoacid generators.
[0072] Examples of the diazonium salt of a Lewis acid include p-methoxyphenyldiazonium fluorophosphonate, N,N-diethylaminophenyldiazonium hexafluorophosphonate (San-Aid SI-60L / SI-80L / SI-100L, etc., manufactured by Sanshin Chemical Industry Co., Ltd.), and the like. Examples of iodonium salts of Lewis acids include diphenyliodonium hexafluorophosphonate, diphenyliodonium hexafluoroantimonate, and the like. Examples of sulfonium salts of Lewis acids include triphenylsulfonium hexafluorophosphonate (Cyracure UVI-6990 manufactured by Union Carbide, etc.), triphenylsulfonium hexafluoroantimonate (Cyracure UVI-6974 manufactured by Union Carbide, etc.), and the like. An example of the phosphonium salt of a Lewis acid is triphenylphosphonium hexafluoroantimonate.
[0073] Other examples of halides include 2,2,2-trichloro-[1-4'-(dimethylethyl)phenyl]ethanone (e.g., Trigonal PI manufactured by AKZO), 2,2-dichloro-1-(4-phenoxyphenyl)ethanone (e.g., Sandray 1000 manufactured by Sandoz), and α,α,α-tribromomethylphenyl sulfone (e.g., BMPS manufactured by Seitetsu Kagaku Co., Ltd.). Examples of triazine initiators include 2,4,6-tris(trichloromethyl)triazine, 2,4-bis(trichloromethyl)-6-(4'-methoxyphenyl)triazine (Triazine A manufactured by Panchim, etc.), 2,4-bis(trichloromethyl)-6-(4'-methoxystyryl)triazine (Triazine PMS manufactured by Panchim, etc.), 2,4-bis(trichloromethyl)-6-piperonyltriazine (Triazine PP manufactured by Panchim, etc.), 2,4-bis(trichloromethyl)-6-(4'-methoxynaphthyl)triazine (Triazine PP manufactured by Panchim, etc.), and B, etc.), 2-[2'-(5''-methylfuryl)ethylidene]-4,6-bis(trichloromethyl)-s-triazine (manufactured by Sanwa Chemical Co., Ltd., etc.), and 2-(2'-furylethylidene)-4,6-bis(trichloromethyl)-s-triazine (manufactured by Sanwa Chemical Co., Ltd.).
[0074] Examples of the baureate initiator include NK-3876, NK-3881, and the like (both manufactured by Nippon Kanko Shikiso). Other examples of photoacid generators include 9-phenylacridine, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2-biimidazole (e.g., Biimidazole manufactured by Kurogane Chemical Industries, Ltd.), 2,2-azobis(2-amino-propane) dihydrochloride (e.g., V50 manufactured by Wako Pure Chemical Industries, Ltd.), 2,2-azobis[2-(imidazolin-2yl)propane] dihydrochloride (e.g., VA044 manufactured by Wako Pure Chemical Industries, Ltd.), [eta-5-2-4-(cyclopentadecyl)(1,2,3,4,5,6,eta)-(methylethyl)benzene]iron(II) hexafluorophosphonate (Irgacure manufactured by Ciba Geigy), 261, etc.), bis(eta-5-cyclopentadienyl)bis[2,6-difluoro-3-(1H-pyridin-1-yl)phenyl]titanium (CGI-784, manufactured by Ciba Geigy, etc.), and the like.
[0075] Furthermore, an azo-based initiator such as azobisisobutyronitrile, a heat-sensitive peroxide-based radical initiator such as benzoyl peroxide, etc. may be used in combination. In addition, both radical and cationic initiators may be used in combination, and one type of each initiator may be used alone, or two or more types may be used in combination.
[0076] Among these, taking into consideration the application of the present invention, the radical type photopolymerization initiators are particularly preferred.
[0077] In the photosensitive resin composition of the present invention, a crosslinking agent (D) can be used as necessary. Specific examples of the crosslinking agent (D) include compounds such as radical reaction type acrylates, cationic reaction type epoxy compounds, radical reaction type maleimide compounds, and vinyl compounds that react with both of them.
[0078] Examples of radical reaction type acrylates include monofunctional (meth)acrylates and polyfunctional (meth)acrylates.
[0079] Examples of the monofunctional (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate monomethyl ether, phenylethyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.
[0080] Examples of the polyfunctional (meth)acrylates include butanediol di(meth)acrylate, hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(meth)acryloyloxyethyl isocyanurate, polypropylene glycol di(meth)acrylate, adipate epoxy di(meth)acrylate, bisphenol ethylene oxide di(meth)acrylate, hydrogenated bisphenol ethylene oxide di(meth)acrylate, bisphenol di(meth)acrylate, ) acrylate, di(meth)acrylate of an ε-caprolactone adduct of hydroxypivalic acid neopentyl glycol, poly(meth)acrylate of a reaction product of dipentaerythritol and ε-caprolactone, dipentaerythritol poly(meth)acrylate, trimethylolpropane tri(meth)acrylate, triethylolpropane tri(meth)acrylate or an ethylene oxide adduct thereof, pentaerythritol tri(meth)acrylate or an ethylene oxide adduct thereof, pentaerythritol tetra(meth)acrylate or an ethylene oxide adduct thereof, dipentaerythritol hexa(meth)acrylate or an ethylene oxide adduct thereof, and the like.
[0081] The cationic reaction type epoxy compounds are not particularly limited as long as they are compounds having an epoxy group, including the epoxy compound (i). Examples of the epoxy compounds include glycidyl (meth)acrylate, methyl glycidyl ether, ethyl glycidyl ether, butyl glycidyl ether, bisphenol-A diglycidyl ether, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (e.g., "Cyracure UVR-6110" manufactured by Union Carbide), 3,4-epoxycyclohexylethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide (e.g., "ELR-4206" manufactured by Union Carbide), limonene diamine, and the like. oxide (Daicel Chemical Industries, Ltd.'s "Celloxide 3000", etc.), allylcyclohexene dioxide, 3,4-epoxy-4-methylcyclohexyl-2-propylene oxide, 2-(3,4-epoxycyclohexyl-5,5-spiro-3,4-epoxy)cyclohexane-m-dioxane, bis(3,4-epoxycyclohexyl)adipate (Union Carbide Corporation's "Cyracure UVR-6128", etc.), bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxycyclohexyl)ether, bis(3,4-epoxycyclohexylmethyl)ether, bis(3,4-epoxycyclohexyl)diethylsiloxane, and the like.
[0082] Examples of the radical reaction type maleimide compounds include N-phenylmaleimide, N-cyclohexylmaleimide, N-hydroxyphenylmaleimide, N-anilinophenylmaleimide, N-carboxyphenylmaleimide, N-(4-carboxy-3-hydroxyphenyl)maleimide, 6-maleimidohexanoic acid, 4-maleimidobutyric acid, bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, 4,4-diphenylmethane bismaleimide, bis(3,5-dimethyl-4- maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, phenylmethanemaleimide, o-phenylenebismaleimide, m-phenylenebismaleimide, p-phenylenebismaleimide, o-phenylenebiscitraconimide, m-phenylenebiscitraconimide, p-phenylenebiscitraconimide, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4 -Diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,2-bismaleimidoethane, 1,4-bismaleimidobutane, 1,5-bismaleimidopentane, 1,5-bismaleimido-2-methylpentane, 1,6-bismaleimidohexane, 1,6-bismaleimido-(2,2,4-trimethyl)hexane, 1,8-bismaleimido-3,6-dioxaoctane, 1,11-bismaleimido-3,6,9-trioxaundecane, 1,3-bis(maleimidomethyl)cyclohexane, 1,4-bis (maleimidomethyl)cyclohexane, 4,4-diphenylether bismaleimide, 4,4-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, 4,4-diphenylmethane biscitraconimide, 2,2-bis[4-(4-citraconimidophenoxy)phenyl]propane, bis(3,5-dimethyl-4-citraconimidophenyl)methane, bis(3-ethyl-5-methyl-4-citraconimidophenyl)methane, bis(3,5-diethyl-4-citraconimidophenyl)methane, polyphenylmethane maleimide, polyphenylmethane maleimide, etc.
[0083] Examples of the vinyl compounds include vinyl ethers, styrenes, and other vinyl compounds. Examples of the vinyl ethers include ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether. Examples of the styrenes include styrene, methylstyrene, and ethylstyrene. Examples of other vinyl compounds include triallyl isocyanurate and trimethallyl isocyanurate.
[0084] In the photosensitive resin composition of the present invention, a crosslinking agent (E) can be used as necessary. Specific examples of the crosslinking agent (E) include, for example, epoxy compounds, and among them, epoxy compounds containing two or more epoxy groups in one molecule are preferred. This is because a stronger cured product can be obtained than when a monofunctional epoxy compound is used. In addition, the epoxy equivalent of these epoxy compounds is preferably in the range of 150 to 450 g / eq, more preferably 180 to 350 g / eq. If the epoxy equivalent is smaller than this, the obtained cured product tends to be brittle, and if it is larger than this, the crosslinking sites are reduced, and the obtained cured product tends to be soft.
[0085] The epoxy compound is selected according to the intended use of the cured product and the required properties, and any known epoxy compound can be used.
[0086] Examples of the monofunctional epoxy compound include phenyl glycidyl ether and glycidyl (meth)acrylate.
[0087] Examples of epoxy compounds having two or more epoxy groups in the molecule include phenol novolac type epoxy resins, cresol novolac type epoxy resins, trishydroxyphenylmethane type epoxy resins, dicyclopentadiene phenol type epoxy resins, bisphenol-A type epoxy resins, bisphenol-F type epoxy resins, biphenol type epoxy resins, bisphenol-A novolac type epoxy resins, naphthalene skeleton-containing epoxy resins, glyoxal type epoxy resins, and heterocyclic epoxy resins.
[0088] Examples of the phenol novolac type epoxy resin include Epicron N-770 (manufactured by DIC Corporation), DEN438 (manufactured by Dow Chemical Company), jER154 (manufactured by Japan Epoxy Resins Co., Ltd.), EPPN-201, and RE-306 (all manufactured by Nippon Kayaku Co., Ltd.). Examples of the cresol novolac type epoxy resin include Epicron N-695 (manufactured by DIC Corporation), EOCN-102S, EOCN-103S, EOCN-104S (all manufactured by Nippon Kayaku Co., Ltd.), UVR-6650 (manufactured by Union Carbide Corporation), and ESCN-195 (manufactured by Sumitomo Chemical Co., Ltd.).
[0089] Examples of the trishydroxyphenylmethane type epoxy resin include EPPN-503, EPPN-502H, EPPN-501H (all manufactured by Nippon Kayaku Co., Ltd.), TACTIX-742 (manufactured by The Dow Chemical Company), jER E1032H60 (manufactured by Japan Epoxy Resins Co., Ltd.), and the like. Examples of the dicyclopentadiene phenol type epoxy resin include Epicron EXA-7200 (manufactured by DIC Corporation) and TACTIX-556 (manufactured by The Dow Chemical Company).
[0090] Examples of the bisphenol type epoxy resin include bisphenol-A type epoxy resins such as jER828, jER1001 (both manufactured by Japan Epoxy Resins Co., Ltd.), UVR-6410 (manufactured by Union Carbide Corporation), DER-331 (manufactured by Dow Chemical Co., Ltd.), YD-8125 (manufactured by Tohto Kasei Co., Ltd.), NER-1202, NER-1302 (all manufactured by Nippon Kayaku Co., Ltd.), and bisphenol-F type epoxy resins such as UVR-6490 (manufactured by Union Carbide Corporation), YDF-8170 (manufactured by Tohto Kasei Co., Ltd.), NER-7403, NER-7604 (all manufactured by Nippon Kayaku Co., Ltd.).
[0091] Examples of the biphenol type epoxy resin include biphenol type epoxy resins such as NC-3000, NC-3000-H, and NC-3000-L (all manufactured by Nippon Kayaku Co., Ltd.), bixylenol type epoxy resins such as YX-4000 (manufactured by Japan Epoxy Resins Co., Ltd.), and YL-6121 (manufactured by Japan Epoxy Resins Co., Ltd.). Examples of the bisphenol A novolac type epoxy resin include Epicron N-880 (manufactured by DIC Corporation) and jER E157S75 (manufactured by Japan Epoxy Resins Co., Ltd.).
[0092] Examples of the naphthalene skeleton-containing epoxy resin include NC-7000 (manufactured by Nippon Kayaku Co., Ltd.) and EXA-4750 (manufactured by DIC Corporation). An example of the glyoxal type epoxy resin is GTR-1800 (manufactured by Nippon Kayaku Co., Ltd.). Examples of the alicyclic epoxy resin include EHPE-3150 (manufactured by Daicel Corporation), etc. Examples of the heterocyclic epoxy resin include TEPIC (manufactured by Nissan Chemical Industries, Ltd.), etc.
[0093] Among these, bisphenol type epoxy resins and biphenol type epoxy resins are particularly effective in terms of flexibility and heat resistance, and for example, bisphenol-A type epoxy resins, bisphenol-F type epoxy resins, NC-3000, NC-3000-H, NC-3000-L, etc. are most preferred.
[0094] When the epoxy compound is contained, the preferred blending amount is about 5 to 80% by weight, more preferably about 10 to 70% by weight, of the solid content of the photosensitive resin composition of the present invention. If the blending amount is less than this amount, the obtained cured product is likely to be weak, and if it is too much, it may have an adverse effect on the curability, etc. due to a problem of balance with the epoxy curing agent described below.
[0095] Other additives that may be contained in the photosensitive resin composition of the present invention include, for example, a thermosetting catalyst such as melamine, a thixotropy-imparting agent such as Aerosil, a silicone-based or fluorine-based leveling agent or defoaming agent, a polymerization inhibitor such as hydroquinone or hydroquinone monomethyl ether, a stabilizer, an antioxidant, and a flame retardant for imparting flame retardancy. In particular, when used as a film-forming material for electrical insulation, it is preferable to use it in combination with a flame retardant.Preferred flame retardants include known general flame retardants, such as halogen-based flame retardants such as brominated epoxy resins and bromodiphenyl ether, phosphazene resins, phosphoric acid ester resins such as triphenyl phosphate, organic phosphorus-based flame retardants such as dihydro-9-oxa-phosphaphenanthrene-10-oxide derivatives, metal hydroxide-based flame retardants such as magnesium hydroxide, and inorganic flame retardants such as red phosphorus and antimony trioxide.
[0096] The pigment material that may be contained in the photosensitive resin composition of the present invention includes coloring pigments intended for coloring and extender pigments not intended for coloring. Examples of the color pigment include organic pigments such as phthalocyanine, azo and quinacridone pigments, and inorganic pigments such as carbon black and titanium oxide. Examples of the extender pigment include talc, barium sulfate, calcium carbonate, magnesium carbonate, barium titanate, aluminum hydroxide, silica, clay, and the like.
[0097] Furthermore, it may contain resins that are not reactive to active energy rays (so-called inert polymers).These resins may include, for example, epoxy resins other than the epoxy resins used as the curing agent, phenolic resins, urethane resins, polyester resins, ketone formaldehyde resins, cresol resins, xylene resins, diallyl phthalate resins, styrene resins, guanamine resins, natural and synthetic rubbers, acrylic resins, polyolefin resins, and modified products thereof, which may be contained in the active energy ray curable resin composition of the present invention.These resins are preferably used in the active energy ray curable resin composition in an amount of up to 40% by weight.
[0098] The volatile solvent that may be contained in the photosensitive resin composition of the present invention may be added to the resin composition in an amount of up to 50% by weight, more preferably up to 35% by weight, for the purpose of adjusting the viscosity depending on the intended use.
[0099] The photosensitive resin composition of the present invention is easily cured by active energy rays. Examples of active energy rays include ultraviolet rays, visible light rays, infrared rays, electromagnetic waves such as X-rays, gamma rays, and laser beams, and particle rays such as alpha rays, beta rays, and electron beams. In consideration of the preferred applications of the present invention, among these, ultraviolet rays, laser beams, visible light, and electron beams are preferred.
[0100] The present invention also includes the use of the photosensitive resin composition as a film-forming material for coating the surface of a substrate, for example, ink materials such as gravure ink, flexo ink, silk screen ink, offset ink, etc., coating materials such as hard coat, top coat, overprint varnish, clear coat, etc., adhesive materials such as adhesives and pressure sensitive adhesives for lamination and optical disks, etc., resist materials such as solder resist, etching resist, resist for micromachine, etc. Furthermore, a so-called dry film, in which a film-forming material is temporarily applied to a peelable substrate to form a film, and then the film is attached to the intended substrate to form a film, also falls under the category of film-forming material.
[0101] The present invention also includes the use of the photosensitive resin composition as a material for forming a film for the purpose of electrical insulation, namely, a solder resist material for a circuit board, an insulating molding material, an interlayer insulating material, a semiconductor protective film material, a wiring coating material, and other materials that require electrical insulation.
[0102] The present invention also includes the use of the active energy ray-curable resin composition as an active energy ray-sensitive resist material for forming a coating layer of the composition on a substrate, then partially irradiating the substrate with active energy rays such as ultraviolet rays, and utilizing the difference in physical properties between the irradiated and unirradiated portions to perform drawing. That is, the active energy ray-curable resin composition is used for the purpose of removing the irradiated or unirradiated portions by some method, for example, dissolving the irradiated or unirradiated portions with a solvent or an alkaline solution, and then performing drawing.
[0103] The present invention also includes the photosensitive resin composition used in a material for a permanent resist. A permanent resist is one of the resist materials described above that is not intended to be peeled off after drawing, but rather is one that maintains its purpose and function without being peeled off until the substrate is actually used.
[0104] The photosensitive resin composition for resists of the present invention can be applied to various materials requiring patterning, and is particularly useful as a solder resist material, an interlayer insulating material for a build-up method, and can also be used as an optical waveguide in electrical / electronic / optical substrates such as printed wiring boards, optoelectronic boards, and optical boards.
[0105] Particularly suitable applications include a wide range of applications requiring a resin composition, such as photosensitive films, photosensitive films with supports, insulating resin sheets such as prepregs, circuit boards (for laminates, multilayer printed wiring boards, etc.), solder resists, underfill materials, die bonding materials, semiconductor encapsulants, hole-filling resins, and component-embedding resins, taking advantage of the properties of good heat resistance and developability. Among these, it is preferable to use the resin composition as a resin composition for an insulating layer of a multilayer printed wiring board (a multilayer printed wiring board in which a cured product of a photosensitive resin composition is used as an insulating layer), a resin composition for an interlayer insulating layer (a multilayer printed wiring board in which a cured product of a photosensitive resin composition is used as an interlayer insulating layer), and a resin composition for plating (a multilayer printed wiring board in which plating is formed on a cured product of a photosensitive resin composition). Furthermore, it exhibits good developability even at high pigment concentrations, and can be suitably used as a color resist, a resist material for a color filter, and particularly as a black matrix material.
[0106] Furthermore, taking advantage of the characteristics of good developability and ability to give a cured product having excellent heat resistance and insulating properties, the composition can be used in solder resist applications and interlayer insulating layer applications that require insulating reliability, which are suitable applications in which the effects of the present invention can be maximized.
[0107] The method for forming the coating is not particularly limited, and any of various coating methods can be used, including intaglio printing methods such as gravure, letterpress printing methods such as flexography, stencil printing methods such as silk screen printing, lithographic printing methods such as offset printing, and methods using a roll coater, knife coater, die coater, curtain coater, spin coater, etc.
[0108] The present invention also includes a cured product obtained by curing the above-mentioned photosensitive resin composition by irradiating it with active energy rays. EXAMPLES
[0109] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples. Various analytical methods used in the examples are described below.
[0110] Various analytical methods were carried out under the following conditions. Epoxy equivalent It is measured according to the method described in JIS K-7236, and the unit is g / eq. ·Softening point The measurement was performed according to JIS K-7234 and the unit is °C. Melt Viscosity ICI melt viscosity (150°C) measured by the cone-plate method, the unit is Pa·s.
[0111] Hydroxyl equivalent It is measured by the following method, and the unit is g / eq. The phenolic resin is reacted with an excess of acetic anhydride and the amount of free acetic acid is measured by titration with a 0.5N ethanolic KOH solution using a potentiometer. Reagents: acetic anhydride, triphenylphosphine, pyridine Solvent: Tetrahydrofuran, propylene glycol monomethyl ether Automatic titration device: COM-1600 manufactured by Hiranuma Co., Ltd. Burette: Hiranuma Corporation B-2000
[0112] ·GPC (gel permeation chromatography) analysis Manufacturer:Waters Column: Guard column SHODEX GPC KF-601 (2 columns), KF-602 KF-602.5, KF-603 Flow rate: 1.23ml / min. Column temperature: 25℃ Solvent used: THF (tetrahydrofuran) Detector: RI (Differential Refraction Detector)
[0113] High performance liquid chromatography analysis Shimadzu Corporation Liquid Delivery Unit LC-20AD Shimadzu Corporation Photodiode array detector SPD-M20A Shimadzu Corporation Column Oven CTO-20A Column: Intersil ODS-2, 5 μm, 4.6 × 250 mm, 40 °C MobilPhaseA: Acetonitrile (AN) MobilPhaseB: Water (W) Time Program: 0-28min.AN / W=30% / 70%→100% / 0% 28-40min.AN / W=100% / 0% Flow Rate: 1.0mL / min. Detection: UV 274nm, PDA
[0114] Synthesis Example 1-1 Into a four-neck flask equipped with a thermometer, a stirrer, a dropping funnel, and a condenser, 1035 parts (11 mol) of phenol, 88 parts (0.8 mol) of resorcinol, and 65 parts (0.7 mol) of toluene were charged, and azeotropic dehydration was carried out at 170°C for 2 hours while purging with nitrogen gas. The oil bath was then cooled to 100°C, and when the internal temperature was stabilized at 100°C, 2.1 parts (0.01 moles) of boron trifluoride diphenol complex was added, and 112 parts (0.8 moles) of dicyclopentadiene was further added using a dropping funnel over a period of 3 hours to cause a reaction. After the dropwise addition was completed, the mixture was further reacted at 120°C for 2 hours and at 145°C for 3 hours. After the reaction was completed, 6 parts of sodium tripolyphosphate and 555 parts of methyl isobutyl ketone were added and stirred, and the mixture was repeatedly washed with warm water to neutralize the system. The oil layer was then distilled off at 180°C using an evaporator to obtain 250 parts of phenolic resin P-1. The softening point of the obtained resin was 109°C, and the hydroxyl equivalent was 152g / eq. The proportion of the component in which one of p and q is 1 and the other is 2 in the n=1 component in the obtained phenolic resin was 15.8% by HPLC area percentage.
[0115] Synthesis Example 1-2 Next, 228 parts of the phenol resin P-1 obtained in Synthesis Example 1-1, 555 parts of epichlorohydrin, 139 parts of dimethyl sulfoxide, and 22 parts of water were added to a four-neck flask equipped with a stirrer and a reflux condenser while purging with nitrogen, and the water bath was heated to 65 ° C. When the internal temperature stabilized at 65 ° C., 63 parts of flake-shaped sodium hydroxide were added in portions over 90 minutes, and the reaction was further carried out at 65 ° C. for 2 hours and at 70 ° C. for 1 hour. After the reaction was completed, the reaction was washed with water, and the oil layer was distilled at 125 ° C. under reduced pressure using a rotary evaporator to remove excess solvents such as epichlorohydrin. 720 parts of methyl isobutyl ketone was added to the residue and dissolved, and the temperature was raised to 75 ° C. 18 parts of a 30 wt % aqueous sodium hydroxide solution was added under stirring, and the reaction was carried out for 1 hour, followed by washing with water, and it was confirmed that the washing water was neutral with a pH test paper. The resulting solution was distilled under reduced pressure at 180°C using a rotary evaporator to remove methyl isobutyl ketone and other components, yielding 295 parts of epoxy resin (EP1). The epoxy equivalent of the resulting epoxy resin was 226 g / eq., the softening point was 63°C, and the ICI melt viscosity was 0.08 Pa·s (150°C). The resin properties are shown in Table 1. In Table 1, the area % in column A is the GPC area %, the area % in column B is the HPLC area %, and the area % in column C is the product of the above GPC area % and the above HPLC area %. In the n=1 component in the resulting epoxy resin, the proportion of components in which one of p and q is 1 and the other is 2 in the total amount was 13.1%.
[0116] Synthesis Example 2-1 The reaction was carried out in the same manner as in Synthesis Example 1-1, except that 231 parts (2.1 moles) of resorcinol was used, to obtain 245 parts of phenolic resin P-2. The softening point of the obtained resin was 120°C, and the hydroxyl equivalent was 140 g / eq. The proportion of the component in which one of p and q was 1 and the other was 2 in the total amount of n=1 components in the obtained phenolic resin was 29.7% by HPLC area percentage.
[0117] Synthesis Example 2-2 Synthesis was performed in the same manner as in Example 1-2, except that the phenol resin was changed to 209 parts of P-2 obtained in Synthesis Example 2-1, and 282 parts of epoxy resin (EP2) were obtained. The epoxy equivalent of the obtained epoxy resin was 215 g / eq., the softening point was 70°C, and the ICI melt viscosity was 0.17 Pa s (150°C). The resin properties are shown in Table 1. The proportion of components in which one of p and q was 1 and the other was 2 in the total amount of n=1 components in the obtained epoxy resin was 24.8%.
[0118] [Table 1]
[0119] Synthesis Example 3-1 In a four-neck flask equipped with a thermometer, stirrer, and cooler, 46.50 parts of propylene glycol 1-monomethyl ether 2-acetate as a reaction solvent, 81.67 parts of the epoxy resin (EP1) obtained in Synthesis Example 1-2, 26.83 g of acrylic acid (molecular weight: 72.06) as a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, 0.33 g of 2,6-di-tert-butyl-p-cresol as a thermal polymerization inhibitor, and 0.33 g of triphenylphosphine as a reaction catalyst were charged and reacted at a temperature of 120°C until the acid value of the reaction solution became 3 mg KOH / g or less, to obtain a solution of reactive acetoxylate compound (A-1). The reaction time was 10 hours.
[0120] Synthesis Example 3-2 21.08 parts of THPA (1,2,3,6-tetrahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) and 23.27 parts of propylene glycol 1-monomethyl ether 2-acetate were added as polybasic acid anhydride (d) to 155.64 g of the reactive epoxy carboxylate compound (A-1) solution obtained in Synthesis Example 3-1, and the mixture was reacted at a temperature of 100°C for 4 hours to obtain a resin solution containing 65% of the unsaturated group-containing polycarboxylic acid compound of the present invention. The acid value of the resin solution was 39.6 mg KOH / g (solid acid value: 60.9 mg KOH / g), and the molecular weight of the unsaturated group-containing polycarboxylic acid compound was 1,400. This resin solution is designated as B-1.
[0121] Synthesis Example 4-1 In a four-neck flask equipped with a thermometer, stirrer, and cooler, 46.50 parts of propylene glycol 1-monomethyl ether 2-acetate as a reaction solvent, 80.65 parts of the epoxy resin (EP2) obtained in Synthesis Example 1-2, 27.85 g of acrylic acid (molecular weight: 72.06) as a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, 0.33 g of 2,6-di-tert-butyl-p-cresol as a thermal polymerization inhibitor, and 0.33 g of triphenylphosphine as a reaction catalyst were charged and reacted at a temperature of 120°C until the acid value of the reaction solution became 3 mg KOH / g or less, to obtain a solution of reactive ethoxycarboxylate compound (A-2). The reaction time was 10 hours.
[0122] Synthesis Example 4-2 To 155.64 g of the reactive epoxy carboxylate compound (A-2) solution obtained in Synthesis Example 4-1, 21.08 parts of THPA (1,2,3,6-tetrahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) as the polybasic acid anhydride (d) and 23.27 parts of propylene glycol 1-monomethyl ether 2-acetate were added, and the mixture was reacted at a temperature of 100°C for 4 hours to obtain a resin solution containing 65% of the unsaturated group-containing polycarboxylic acid compound of the present invention. The acid value of the resin solution was 39.1 mg KOH / g (solid acid value: 60.2 mg KOH / g), and the molecular weight of the unsaturated group-containing polycarboxylic acid compound was 1,600. This resin solution is designated as B-2.
[0123] Synthesis Example 5-1 In a four-neck flask equipped with a thermometer, stirrer, and cooler, 46.50 parts of propylene glycol 1-monomethyl ether 2-acetate as a reaction solvent, 80.03 parts of the epoxy resin (EP1) obtained in Synthesis Example 1-2, 23.71 g of acrylic acid (molecular weight: 72.06) as a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in a molecule, 4.75 parts of dimethylolpropionic acid as a compound (c) having a hydroxyl group and a carboxyl group in one molecule, 0.33 g of 2,6-di-tert-butyl-p-cresol as a thermal polymerization inhibitor, and 0.33 g of triphenylphosphine as a reaction catalyst were charged and reacted at a temperature of 120°C until the acid value of the reaction solution became 3 mg·KOH / g or less, and a solution of reactive ethoxycarboxylate compound (A-3) was obtained. The reaction time was 10 hours.
[0124] Synthesis Example 5-2 21.08 parts of THPA (1,2,3,6-tetrahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) and 23.27 parts of propylene glycol 1-monomethyl ether 2-acetate were added to 155.64 g of the reactive epoxy carboxylate compound (A-1) solution obtained in Synthesis Example 3-1 as the polybasic acid anhydride (d), and the mixture was reacted at a temperature of 100°C for 4 hours to obtain a resin solution containing 65% of the unsaturated group-containing polycarboxylic acid compound of the present invention. The acid value of the resin solution was 39.5 mg KOH / g (solid acid value: 60.8 mg KOH / g), and the molecular weight of the unsaturated group-containing polycarboxylic acid compound was 1,600. This resin solution is designated as B-3.
[0125] Synthesis Example 6-1 In a four-neck flask equipped with a thermometer, stirrer, and cooler, 46.50 parts of propylene glycol 1-monomethyl ether 2-acetate as a reaction solvent, 83.80 parts of XD-1000 (dicyclopentadiene type epoxy resin, epoxy equivalent 252g / eq., the ratio of components in which one of p and q is 1 and the other is 2 in the total amount of n=1 components in the epoxy resin is 0.0%), 24.69g of acrylic acid (molecular weight: 72.06) as a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, 0.33g of 2,6-di-tert-butyl-p-cresol as a thermal polymerization inhibitor, and 0.33g of triphenylphosphine as a reaction catalyst were charged and reacted at a temperature of 120℃ until the acid value of the reaction solution became 3mg·KOH / g or less, and a solution of reactive exicarboxylate compound (A-4) was obtained. The reaction time was 10 hours.
[0126] Synthesis Example 6-2 To 155.64 g of the reactive epoxy carboxylate compound (A-4) solution obtained in Synthesis Example 6-1, 21.08 parts of THPA (1,2,3,6-tetrahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) as the polybasic acid anhydride (d) and 23.27 parts of propylene glycol 1-monomethyl ether 2-acetate were added, and the mixture was reacted at a temperature of 100°C for 4 hours to obtain a resin solution containing 65% of the unsaturated group-containing polycarboxylic acid compound of the present invention. The acid value of the resin solution was 40.4 mg KOH / g (solid acid value: 62.2 mg KOH / g), and the molecular weight of the unsaturated group-containing polycarboxylic acid compound was 1,500. This resin solution is designated as B-4.
[0127] Synthesis Example 7-1 In a four-neck flask equipped with a thermometer, stirrer, and cooler, 46.50 parts of propylene glycol 1-monomethyl ether 2-acetate as a reaction solvent, 79.75 parts of NC-3500 (resorcin-containing biphenol-type epoxy resin, epoxy equivalent 206g / eq.) as an epoxy resin, 28.74g of acrylic acid (molecular weight: 72.06) as a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule, 0.33g of 2,6-di-tert-butyl-p-cresol as a thermal polymerization inhibitor, and 0.33g of triphenylphosphine as a reaction catalyst were charged and reacted at a temperature of 120°C until the acid value of the reaction solution became 3mg·KOH / g or less, to obtain a solution of reactive ethoxycarboxylate compound (A-5). The reaction time was 10 hours.
[0128] Synthesis Example 7-2 To 155.64 g of the reactive epoxy carboxylate compound (A-5) solution obtained in Synthesis Example 7-1, 21.08 parts of THPA (1,2,3,6-tetrahydrophthalic anhydride, manufactured by New Japan Chemical Co., Ltd.) as the polybasic acid anhydride (d) and 23.27 parts of propylene glycol 1-monomethyl ether 2-acetate were added, and the mixture was reacted at a temperature of 100°C for 4 hours to obtain a resin solution containing 65% of the unsaturated group-containing polycarboxylic acid compound of the present invention. The acid value of the resin solution was 40.0 mg KOH / g (solid acid value: 61.5 mg KOH / g), and the molecular weight of the unsaturated group-containing polycarboxylic acid compound was 3,000. This resin solution is designated as B-5.
[0129] Examples 1 to 3 and Comparative Examples 1 and 2 The resin solution obtained in the synthesis examples 3-2, 4-2, 5-2, 6-2, and 7-2 was mixed with 10.00 parts of B-1 to B-5, 0.42 parts of Irgacure 907 (manufactured by Ciba Specialty Chemicals) as a photopolymerization initiator (C), and 0.02 parts of Kayacure DETX-S (manufactured by Nippon Kayaku Co., Ltd.), 1.95 parts of DPCA-20 (trade name: manufactured by Nippon Kayaku Co., Ltd.) as a crosslinking agent (D), 0.02 parts of TPP as a heat curing catalyst, and 3.81 parts of propylene glycol 1-monomethyl ether 2-acetate as a concentration adjusting solvent, and the solid content concentration was adjusted to 60%. Then, 2.06 parts of bisphenol A type epoxy resin (trade name: YD-134, manufactured by Nippon Steel & Sumitomo Metal Corporation) was added as a curing agent (E) and dispersed uniformly to obtain a resist resin composition.
[0130] Each evaluation item will be described in detail.
[0131] Photosensitivity evaluation (abbreviation in table: photosensitivity) The resist resin composition was applied to rolled copper foil BHY-82F-HA-V2 (manufactured by JX Metals Co., Ltd.) with an applicator to a thickness of 20 μm, and the coating was dried for 30 minutes in a hot air dryer at 80° C. A step tablet (manufactured by Stouffer: 21 steps) was placed on the dried coating, and the amount of irradiation was adjusted using an ultraviolet irradiator (manufactured by USHIO (ultra-high pressure mercury lamp)) to perform curing. Thereafter, spray development was performed using a 1% aqueous sodium carbonate solution as the developer. The amount of irradiation when the step tablet was used to cure up to the 7th step was used to evaluate the photosensitivity. ○ 150mJ / cm 2 below × 150mJ / cm 2 End
[0132] Developability evaluation (abbreviation in table: developability) The resist resin composition was applied to rolled copper foil BHY-82F-HA-V2 (manufactured by JX Metals Co., Ltd.) with an applicator to a thickness of 20 μm, and the coating was dried for 30 minutes in a hot air dryer at 80° C. Then, spray development was performed using a 1% aqueous sodium carbonate solution as a developer. The time until the coating was completely dissolved, the so-called break time, was used to evaluate the developability (unit: seconds). × Swelling peeling
[0133] Glass transition temperature measurement (abbreviation in table: Tg) The resist resin composition was applied to rolled copper foil BHY-82F-HA-V2 (manufactured by JX Metals Co., Ltd.) with an applicator to a thickness of 20 μm, and the coating was dried in a hot air dryer at 80 ° C for 30 minutes, and then irradiated with ultraviolet light at an energy of 500 mJ / cm2 using an ultraviolet irradiator (manufactured by GS YUASA: CS 30L-1). Next, the coating was cured in an oven at 150 ° C for 30 minutes to obtain a cured product. The copper foil was removed with iron (III) chloride 45 ° Baume (manufactured by Junsei Chemical Co., Ltd.). DMA measurement (manufactured by TA Instruments: RSA-G2) was performed on the sample from which the cured product was produced, and the temperature at which tangent δ was maximized was determined.
[0134] Thermal decomposition resistance evaluation (abbreviation in table: thermal decomposition resistance) The resist resin composition was applied to rolled copper foil BHY-82F-HA-V2 (manufactured by JX Metals Co., Ltd.) with an applicator to a thickness of 20 μm, and the coating was dried in a hot air dryer at 80 ° C for 30 minutes, and then irradiated with ultraviolet light at an energy of 500 mJ / cm2 using an ultraviolet irradiator (manufactured by GS YUASA: CS 30L-1). Next, the coating was cured in an oven at 150 ° C for 30 minutes to obtain a cured product. The copper foil was removed with iron (III) chloride 45 ° Pome (manufactured by Junsei Chemical Co., Ltd.). The temperature at which the weight of the sample of 3 mg of the cured product was reduced by 5% was measured using a METTLER TGA / DSC1 in an air flow of 100 ml per minute.
[0135] Ion migration evaluation (abbreviation in table: insulation) Each composition was applied to a thickness of 25 μm on an ESPANEX M series (manufactured by Nippon Steel Chemical Co., Ltd.: base imide thickness 25 μm, Cu thickness 18 μm) on which a comb-shaped pattern of L / S=100 μm / 100 μm was formed, and the coating was dried in an oven at 80° C. for 30 minutes. Next, an ultraviolet exposure device (manufactured by GS YUASA: CS 30L-1) was used to apply 500 mJ / cm 2The coating was exposed to light at 400 K and cured, and then dried in an oven at 150° C. for 1 hour to obtain a test substrate for evaluation. The electrodes of the obtained substrate were wired with solder, placed in an environment of 130° C. / 85% RH, and a voltage of 100 V was applied to evaluate the occurrence of migration and the maximum insulation resistance value. Migration: ○ 100 hours or more × Less than 50 hours
[0136] [Table 2]
[0137] From the above results, it was confirmed that the coating films obtained from the resin compositions containing the unsaturated group-containing polycarboxylic acid compound (B) of the present invention obtained in Synthesis Examples 3-2 and 4-2 have excellent sensitivity and developability, and the cured products thereof also have excellent heat resistance. In addition, in the ion migration evaluation, it was confirmed that the coating films have excellent copper adhesion because they have high resistance values and excellent insulation reliability without causing migration.
[0138] From the above, the photosensitive resin composition using the reactive epoxy carboxylate compound and the unsaturated group-containing polycarboxylic acid compound of the present invention is suitable for molding materials, film-forming materials, and resist materials. In particular, since it has excellent sensitivity and developability while also having excellent heat resistance and insulation reliability, it is suitable for a photosensitive material composition for printed wiring boards.
Claims
1. An epoxy resin represented by the following general formula (1): the total amount of all epoxy compounds represented by n=1 in the epoxy resin is 45.3 area % or more in the epoxy resin, an epoxy resin (a), in which the total content of an epoxy compound represented by the following formula (2) and an epoxy compound represented by the following formula (3) is 1 area % or more and less than 70 area % in the total amount of all epoxy compounds represented by n=1 in the epoxy resin, A reactive epoxy carboxylate compound (A) obtained by reacting a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule with a compound (c) having a hydroxyl group and a carboxyl group in one molecule, as required. 【Chemistry 1】 In formula (1), G represents a substituted or unsubstituted glycidyl group. p and q each independently exist and represent a real number of 1 or 2. When multiple q's are present, each q independently can be 1 or 2. n represents a real number from 1 to 20.) 【Chemistry 2】 (In formula (2), G represents a substituted or unsubstituted glycidyl group.) 【Chemistry 3】 (In formula (3), G represents a substituted or unsubstituted glycidyl group.)
2. The epoxy resin (a) according to claim 1, wherein the epoxy equivalent of the unsaturated group-containing epoxy carboxylate compound (A) is 200 g / eq. or more and less than 230 g / eq.
3. A reactive epoxy carboxylate compound (A) obtained by reacting an epoxy compound (a) represented by the following formula (2) or (3) with a monocarboxylic acid compound (b) having one or more ethylenically unsaturated groups in the molecule and, if necessary, a compound (c) having a hydroxyl group and a carboxy group in one molecule. 【Chemistry 4】 (In formula (2), G represents a substituted or unsubstituted glycidyl group.) 【Chemistry 5】 (In formula (3), G represents a substituted or unsubstituted glycidyl group.)
4. An unsaturated group-containing polycarboxylic acid compound (B) obtained by reacting the reactive epoxy carboxylate compound (A) according to any one of claims 1 to 3 with a polybasic acid anhydride (d).
5. The unsaturated group-containing polycarboxylic acid resin (B) according to any one of claims 1 to 3, wherein the acid value of the solid content is 40 to 160 mg·KOH / g.
6. A photosensitive resin composition comprising the unsaturated group-containing epoxy carboxylate compound (A) or the unsaturated group-containing polycarboxylic acid resin (B) according to any one of claims 1 to 4, a photopolymerization initiator (C) and a crosslinking agent (D).
7. The photosensitive resin composition according to claim 6 , further comprising a curing agent (E).
8. The photosensitive resin composition according to claim 6 or 7, which is a film-forming material.
9. The photosensitive resin composition according to claim 6 or 7, which is a material for a permanent resist.
10. A cured product of the photosensitive resin composition according to any one of claims 6 to 9.
Citation Information
Patent Citations
Photocurable resin composition and photocurable resin composition for solder resist
JP1993214048A
Thermosetting resin composition, multilayered printed wiring board, and preparation thereof
JP1995304931A