An iron-based alloy designed for wear and corrosion resistance

Ferritic iron-based alloys with controlled compositions provide enhanced wear and corrosion resistance for brake discs, addressing industry challenges by reducing nickel and cobalt use and improving machining ease.

JP7572384B2Active Publication Date: 2024-10-23OERLIKON METCO (US) INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021576786
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-07-07
Publication Date
2024-10-23
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

The automotive industry faces challenges in achieving wear and corrosion resistance in brake discs, with existing materials being costly and regulatory pressures to reduce nickel and cobalt use, while current coatings do not adequately address particulate emissions and corrosion issues.

Method used

Development of ferritic iron-based alloys with controlled compositions, including specific weight percentages of elements like Cr, Nb, Ti, Mo, and C, forming a ferrite matrix with primary carbides, which are applied through processes like thermal spraying or laser cladding to provide enhanced wear and corrosion resistance.

Benefits of technology

The alloys offer improved wear resistance and corrosion resistance, maintaining low hardness for easier machining, while reducing the need for nickel and cobalt, and are suitable for various industrial applications including brake discs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572384000012
    Figure 0007572384000012
  • Figure 0007572384000013
    Figure 0007572384000013
  • Figure 0007572384000014
    Figure 0007572384000014
Patent Text Reader

Abstract

Disclosed herein are alloy embodiments configured to form coatings with two contrasting physical behaviors: 1) reduced hardness with the end result of an easily machinable coating, and 2) high wear resistance. Generally, lower hardness results in lower wear resistance. However, alloy embodiments described herein can maintain low hardness while exhibiting higher wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] INCORPORATION BY REFERENCE TO PRIORITY APPLICATIONS This application claims the benefit of U.S. Application No. 62 / 872,105, filed July 9, 2019, and entitled "Iron-Based Alloy Designed for Wear and Corrosion Resistance," and U.S. Application No. 62 / 952,668, filed December 23, 2019, and entitled "Corrosion and Wear Resistant Ferritic Alloy," each of which is incorporated by reference in its entirety herein.

[0002] FIELD OF THE DISCLOSURE Embodiments of the present disclosure generally relate to ferritic iron-based alloys having high wear resistance. [Background technology]

[0003] There is increasing interest in brake discs with improved wear and corrosion resistance compared to the standard grey cast iron commonly used in the automotive industry. Alternative technologies such as composite brake discs are often unattractive for mass production due to their high cost.

[0004] Two factors are driving this market trend. The first is increased pressure from regulators to reduce particulate emissions resulting from brake disc wear. The second is corrosion of cast iron brakes as a result of reduced use of friction brakes in vehicles capable of regenerative braking. Visible corrosion (rust) is an aesthetic issue and can reduce the effectiveness of the brakes. As a result, the alloys and coatings described in this disclosure are likely to provide improved brake disc performance that the market is interested in. Additionally, because the alloys of the present disclosure are iron-based, they have a competitive price compared to more expensive metals and composites.

[0005] In many coating applications, there are strong regulatory and safety pressures to reduce or eliminate the use of nickel and / or cobalt. Both of these materials are commonly used as the metallic phase in thermal spray and other coatings. The alloys of the present disclosure are iron-based, with particular limitations on cobalt and nickel, enhancing their attractiveness for many wear and corrosion applications.

[0006] Previous iterations of hardfacing coatings have focused on ferrous alloys with a martensite matrix, the hardest form of steel, to form hardfacing coatings. 431 Stainless Steel (SS) from Metco and others is the standard alloy used in this application. Additionally, U.S. Patent Nos. 7,491,910, 8,961,869, and 9,802,387, and U.S. Patent Application Publication No. 2005 / 013924, which are incorporated herein by reference in their entireties, teach reduced ferrite content, high martensite content to produce a material with high hardness. Summary of the Invention

[0007] Disclosed herein are embodiments of cladding feedstock that include Fe, about 10-about 26 wt. % Cr, about 2-about 12 wt. % Nb+Ti+V, and about 0.5-about 1.5 wt. % C.

[0008] In some embodiments, the feedstock comprises Fe, about 16-about 26 wt.% Cr, about 0.4-about 2.4 wt.% Ti, 0.8-3.6 wt.% Mo, about 4-about 6 wt.% Nb, and about 0.6-about 1.2 wt.% C.

[0009] In some embodiments, the feedstock comprises Fe, about 18-about 25 wt.% Cr, about 0.45-about 2.2 wt.% Ti, 0.9-3.3 wt.% Mo, about 4.5-about 5.5 wt.% Nb, and about 0.7-about 1.1 wt.% C.

[0010] In some embodiments, the feedstock further comprises 0.3-0.5 wt. % B.

[0011] Disclosed herein are embodiments of cladding feedstock that include Fe, about 10-about 25 wt.% Cr, up to 4 wt.% Ni, about 2-about 10 wt.% Nb+Ti+V, and about 0.5-about 1.5 wt.% C.

[0012] In some embodiments, the feedstock may include Fe, about 13.6 to about 20.4 wt.% Cr, about 1.2 to about 1.6 wt.% Ni, about 1.6 to about 2.4 wt.% Ti, about 4 to about 6 wt.% Nb, and about 0.8 to about 1.2 wt.% C. In some embodiments, the feedstock includes Fe, about 15.3 to about 18.7 wt.% Cr, about 1.35 to about 1.65 wt.% Ni, about 1.8 to about 2.2 wt.% Ti, about 4.5 to about 5.5 wt.% Nb, and about 0.9 to about 1.1 wt.% C.

[0013] In some embodiments, the feedstock is characterized under thermodynamic conditions as having a total ferrite phase mole fraction of about 50 mol% or greater at all temperatures below the solidus and above 500 K. In some embodiments, the feedstock is characterized under thermodynamic conditions as having a total ferrite phase mole fraction of about 60 mol% or greater at all temperatures below the solidus and above 500 K. In some embodiments, the feedstock is characterized under thermodynamic conditions as having a total ferrite phase mole fraction of about 70 mol% or greater at all temperatures below the solidus and above 500 K. In some embodiments, the feedstock is characterized under thermodynamic conditions as having a total ferrite phase mole fraction of about 90 mol% or greater at elevated elevated temperatures just below the solidus temperature.

[0014] In some embodiments, the feedstock may be characterized as having a primary carbide formation temperature, under thermodynamic conditions, between about 1750 K and about 2100 K. In some embodiments, the primary carbide formation temperature may be between about 1850 K and about 2000 K.

[0015] In some embodiments, the feedstock can have a total mole fraction of primary carbides of about 7.5 mol% at 1300 K under thermodynamic conditions. In some embodiments, the total mole fraction of primary carbides can be about 10 mol% at 1300 K.

[0016] In some embodiments, the feedstock may be formed by a gas atomization process.

[0017] In some embodiments, the coating can include a ferrite matrix and a plurality of primary carbides embedded within the ferrite matrix, the primary carbides being embedded in the ferrite matrix.

[0018] In some embodiments, the plurality of primary carbides can include at least one of Nb, Ti, and V. In some embodiments, the plurality of primary carbides can include isolated spheroidal morphologies.

[0019] In some embodiments, the coating may have a total volume fraction of primary carbides of at least about 5 vol.%. In some embodiments, the total volume fraction of primary carbides may be at least about 7.5 vol.%. In some embodiments, the total volume fraction of primary carbides may be at least about 10 vol.%. In some embodiments, the coating may have a ferritic matrix Cr content of at least about 12 wt.%. In some embodiments, the ferritic matrix Cr content may be at least about 15 wt.%. In some embodiments, the ferritic matrix Cr content is at least about 19 wt.%.

[0020] In some embodiments, the coating can have a hardness of about 450HV 0.3 or less. In some embodiments, the hardness can be about 400HV 0.3 or less. In some embodiments, the hardness can be about 350HV 0.3 or less.

[0021] In some embodiments, the coating is about 200 mm 3 The ASTM G65 Procedure A volume loss may be as follows: In some embodiments, the ASTM G65 Procedure A volume loss is about 150 mm 3 In some embodiments, the volume loss per ASTM G65 Procedure A may be less than or equal to about 100 mm 3 It can be the following:

[0022] In some embodiments, the coating can be configured to be formed by a deposition process, hi some embodiments, the coating can be configured to be formed by a process selected from the group consisting of thermal spraying, plasma transfer arc welding, laser cladding, and ultra-high speed laser cladding.

[0023] Also disclosed are embodiments that apply the materials as disclosed herein as a coating.

[0024] In some embodiments, the feedstock may be a powder. In some embodiments, the feedstock may be one or more wires.

[0025] Disclosed herein are embodiments of a thermal spray feedstock that includes Fe, about 14-35 wt. % Cr, about 0-16 wt. % Mo+W, and about 0.2 to about 2.8 wt. % B.

[0026] In some embodiments, the feedstock may further comprise about 20-about 34 wt% Cr, about 0-about 6 wt% Mo+W, about 0.8-about 1.8 wt% B, and about 1-about 4 wt% Nb+Ti. In some embodiments, the feedstock may further comprise about 15-about 34 wt% Cr, about 1-about 16 wt% Mo+W, about 0.3-about 2.7 wt% B, about 1-about 10 wt% Nb+Ti, and about 0-about 1.2 wt% C. In some embodiments, the feedstock may further comprise about 15-about 30 wt% Cr, about 0-about 6 wt% Mo+W, about 0.2-about 1.0 wt% B, and about 5-about 12% Nb+Ti, and about 0.4-about 1.4 wt% C.

[0027] In some embodiments, the feedstock contains less than about 1 wt% C. In some embodiments, the feedstock contains less than about 0.5 wt% C. In some embodiments, the feedstock contains less than about 0.25 wt% C. In some embodiments, the feedstock contains less than about 0.1 wt% C. In some embodiments, the feedstock contains less than about 5 wt% Ni. In some embodiments, the feedstock contains less than about 1 wt% Ni. In some embodiments, the feedstock contains less than about 0.1 wt% Ni.

[0028] In some embodiments, the raw material is a powder.

[0029] In some embodiments, the feedstock is configured to form a matrix and is characterized under thermodynamic equilibrium conditions as having a pitting resistance equivalent number greater than 17, as defined by the formula Cr+3.3*(Mo+0.5*W)+16*N or greater, less than 25 mol % intermetallic phases, about 7-about 35 mol % hard phases, about 2-about 25 mol % borides, about 1-about 15 mol % MC carbides, and a liquidus temperature less than 2000 K. In some embodiments, the feedstock is configured to form a matrix and is characterized under thermodynamic equilibrium conditions as having a pitting resistance equivalent number greater than 25, as defined by the formula Cr+3.3*(Mo+0.5*W)+16*N or greater, less than 8 mol % intermetallic phases, about 10-about 22 mol % hard phases, and a liquidus temperature less than 1900 K.

[0030] In some embodiments, the feedstock has the following composition by weight: Cr: about 20.1 wt%, Nb: about 5.6 wt%, Mo: about 2.1 wt%, B: about 0.44 wt%, C: about 0.81 wt%, Ti: about 1.6 wt%, Fe: balance.

[0031] Also disclosed herein are embodiments of coatings formed from the materials disclosed herein. In some embodiments, the coatings comprise a volume fraction of hard phase between about 5 and about 35% and a porosity of less than about 3%. In some embodiments, the coatings comprise a volume fraction of hard phase between about 10 and about 25% and a porosity of less than about 1%.

[0032] In some embodiments, the coating is applied to a brake disc.

[0033] Also disclosed herein are embodiments of methods for applying a metal coating onto a substrate, the methods including thermally spraying the feedstock materials disclosed herein onto the substrate.

[0034] Disclosed herein is an iron-based alloy feedstock comprising a matrix PREN of greater than 20 at 1300 K under equilibrium or near-equilibrium solidification conditions, a hard phase mole fraction of 5% to 25% at 1300 K under equilibrium or near-equilibrium solidification conditions, and a solidus of less than 2000 K under equilibrium or near-equilibrium solidification conditions.

[0035] In some embodiments, the alloy feedstock comprises between 1.0 and 10.0 wt.% niobium and titanium. In some embodiments, the matrix at 1300K has a Cr content greater than 15 wt.%. In some embodiments, the mole fraction of intermetallic phases at 800K is less than 25% under equilibrium or near equilibrium solidification conditions.

[0036] In some embodiments, the alloy is atomized to form a powder. In some embodiments, the alloy feedstock is deposited on a substrate to form a wear and corrosion resistant coating. In some embodiments, the arc-melted microstructure of the alloy feedstock comprises 8% to 30% by volume of hard phase. In some embodiments, the arc-melted ingot microstructure comprises a matrix PREN of greater than 20.

[0037] In some embodiments, the alloy feedstock is configured to be deposited via laser cladding or ultrafast laser cladding, hi some embodiments, the alloy feedstock is deposited on the wear surface of the brake disc.

[0038] In some embodiments, the alloy feedstock comprises a mole fraction of 3 to 26% borides under equilibrium solidification conditions at 1300 K. In some embodiments, the alloy feedstock comprises less than 10% FCC austenite under equilibrium conditions at 1300 K.

[0039] Further disclosed herein is a cladding feedstock comprising Fe and a ferritic matrix comprising greater than about 50% total ferrite mole fraction under thermodynamic conditions, at least about 12 wt. % CR, and greater than about 5% mole fraction of hard phases that precipitate from the liquid.

[0040] In some embodiments, the hard phase is a carbide. In some embodiments, the carbide is an FCC carbide. In some embodiments, the hard phase is a boride. In some embodiments, the hard phase includes both borides and carbides.

[0041] Also disclosed are embodiments of the coating as disclosed herein.

[0042] Also disclosed are embodiments of the feedstock as disclosed herein. [Brief description of the drawings]

[0043] [Figure 1] FIG. 1 illustrates an embodiment of a thermodynamic profile for an alloy of the present disclosure.

[0044] [Diagram 2] FIG. 2 shows the thermodynamic profile of 431 stainless steel.

[0045] [Diagram 3] FIG. 3 shows an embodiment of the microstructure of the alloy of the present disclosure as a PTA weld overlay coating.

[0046] [Figure 4] FIG. 4 illustrates an embodiment of a thermodynamic solidification diagram for an alloy of the present disclosure.

[0047] [Diagram 5] FIG. 5 illustrates an embodiment of a thermodynamic solidification diagram for an alloy of the present disclosure.

[0048] [Figure 6] FIG. 6 shows the microstructure of an arc-melted ingot of an alloy of the present disclosure.

[0049] [Figure 7] FIG. 7 shows the microstructure of an arc-melted ingot of an alloy of the present disclosure.

[0050] [Figure 8] FIG. 8 shows an embodiment of a Schaeffler diagram. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0051] Disclosed herein are embodiments of alloys that have a ferritic structure rather than a martensitic matrix, and as a result have a lower hardness than typical hardened products. However, embodiments of the present disclosure have excellent wear resistance, the wear resistance being provided in the form of hard carbides or hard borides, or a combination of both hard carbide and hard boride particles. Because of the ferritic structure, the coating can be ground and machined much more quickly than harder coatings known in the art, which is advantageous for many applications, including use on hydraulic rods. In some embodiments, the alloys described herein can be used as a hardbanding or hardened case layer or coating. In some embodiments, the alloys can be applied to hydraulic rods as a layer or coating. In some embodiments, the alloys can have high corrosion resistance, similar to that of 431 stainless steel, for example. This can be achieved, for example, by one or more of the following: in situ formation of a corrosion resistant matrix, a controlled percentage of hard phases, and a tough microstructure. Thus, embodiments of the present disclosure can be iron hardened case alloys that are resistant to corrosion and have high wear resistance.

[0052] In some embodiments, the hard layer can be a boride. This is beneficial from a design standpoint because boron has very low solid solution solubility with iron and iron alloys, which promotes precipitation of boride phases, even under the rapid cooling rates inherent in laser cladding and ultrafast laser cladding. In some embodiments, strong carbide formers can also be present to ensure precipitation during processing and minimal retained carbon in the matrix. The presence of these beneficial phases can reduce or eliminate detrimental phases. These include intermetallic phases such as sigma and Laves phases that can reduce the toughness and ductility of the alloy. The alloys of the present disclosure can specifically minimize the proportion of intermetallic phases. An additional consideration addressed in this disclosure relates to the manufacturability of the alloys by atomization by controlling the liquidus temperature of the alloys.

[0053] In some embodiments, the alloys described herein can be configured to form coatings with two contrasting physical behaviors: 1) reduced hardness with the end result of an easily machinable coating (e.g., faster grinding / honing times for clad coatings), and 2) high wear / abrasion resistance. Generally, lower hardness translates to lower wear resistance. However, embodiments of the alloys described herein can maintain low hardness while exhibiting higher wear resistance than typical iron-based materials. Other advantageous features described herein can include crack resistance, compatibility with gas atomization processes, compatibility with laser and PTA welding, and corrosion resistance.

[0054] The alloys disclosed herein can be produced in powder form using, for example, but not limited to, a gas atomization process, and other processes can be used as well. The powders can be used in a variety of deposition processes, such as thermal spray, high velocity oxygen fuel ("HVOF"), high velocity air fuel ("HVAF"), plasma spray, plasma transferred arc welding ("PTA"), laser cladding, and extreme high velocity laser cladding ("EHLA"), to form coatings with specific microstructural characteristics and performance properties.

[0055] As disclosed herein, the term alloy can refer to the chemical composition forming the powders disclosed therein, the powder itself, the feedstock itself, the wire, the wire containing the powder, the composition of the metallic components formed by heating, and / or the deposition of the powder (e.g., hardbanding layer / hardfacing layer), or other methodologies, and metal parts.

[0056] In some embodiments, alloys made into solid or cored wires (sheath containing powder) for welding or for use as a feedstock for another process may be described by the specific chemistries herein. For example, the wires may be used for thermal spraying. Additionally, the compositions disclosed below may be from a single wire or a combination of multiple wires (such as 2, 3, 4, or 5 wires).

[0057] In some embodiments, the alloys can be fully characterized by their composition ranges.

[0058] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr: 10-26 (or about 10-about 26); Nb+Ti+V: 2-10 (or about 2-about 10); Mo: up to 3 (or up to about 3); and C: 0.5-1.5 (or about 0.5-about 1.5).

[0059] In some embodiments, the composition may be nickel-free, hi some embodiments, the composition may include up to 4% nickel by weight.

[0060] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr: 10-26 (or about 10-about 26); Nb+Ti+V: 2-12 (or about 2-about 12); Mo: up to 3 (or up to about 3); and C: 0.5-1.5 (or about 0.5-about 1.5).

[0061] In some embodiments, the composition may be nickel-free, hi some embodiments, the composition may include up to 4% nickel by weight.

[0062] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr:16-26 (or about 16-about 26); Ti: 0.4-2.4 (or about 0.4-about 2.4); Mo: 0.8-3.6 (or about 0.8-about 3.6); Nb: 4-6 (or about 4 to about 6); and C: 0.6-1.2 (or about 0.6-about 1.2).

[0063] In some embodiments, the composition may be nickel-free. In some embodiments, the composition may include 1.2-1.6 (or about 1.2-about 1.6) weight percent nickel.

[0064] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr:18-25 (or about 18-about 25); Ti: 0.45-2.2 (or about 0.45-about 2.2) Mo: 0.9-3.3 (or about 0.9-about 3.3); Nb: 4.5-5.5 (or about 4.5-about 5.5); and C: 0.7-1.1 (or about 0.7-about 1.1).

[0065] In some embodiments, the composition may be nickel-free. In some embodiments, the composition may include 1.35-1.65 (or about 1.35-about 1.65) weight percent nickel.

[0066] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr: 16-24 (or about 13.6-about 20.4); Mo: 0.8-1.2 (or about 0.8-about 1.2); Ti: 0.4-2.4 (or about 0.4-about 2.4) Nb: 4-6 (or about 4 to about 6); and C: 0.8-1.2 (or about 0.8-about 1.2).

[0067] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr: 18-22 (or about 13.6-about 20.4); Mo: 0.9-1.1 (or about 0.8-about 1.2); Ti: 0.45-2.2 (or about 0.45-about 2.4) Nb: 4.5-5.5 (or about 4-about 6); and C: 0.9-1.1 (or about 0.8-about 1.2).

[0068] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr:16-26 (or about 16-about 26); Mo: 2-4 (or about 2-about 4); Ti: 0.4-2.4 (or about 0.4-about 2.4) Nb: 4-6 (or about 4-about 6); C: 0.6-0.9 (or about 0.6-about 0.9); and B:0.3-0.5(or about 0.3-about 0.5).

[0069] In some embodiments, the alloy may include, in weight percent: Fe: balance; Cr:18-24 (or about 18-about 24); Mo:2.5-3.5(or about 2.5-about 3.5); Ti: 0.4-2.2 (or about 0.4-about 2.2) Nb: 4.5-5.5 (or about 4.5-about 5.5); B: 0.35-0.45 (or about 0.35-about 0.45); and C: 0.65-0.85 (or about 0.65-about 0.85).

[0070] In some embodiments, the alloy may include, in weight percent: Fe; Cr: 14-35 (or about 14-about 35); Mo+W: 0-15 (or about 0-about 15); and B:0.2-2.8(or about 0.2-about 2.8).

[0071] In some embodiments, the alloy may include, in weight percent: Fe; Cr:20-34 (or about 20-about 34); Mo+W: 0-6 (or about 0-about 6); B: 0.8-1.8 (or about 0.8-about 1.8); and Nb+Ti: 1-4 (or about 1-about 4).

[0072] In some embodiments, the alloy may include, in weight percent: Fe; Cr:15-30 (or about 15-about 30); Mo+W: 0-6 (or about 0-about 6); B: 0.2-1.0 (or about 0.2-about 1.0); Nb+Ti: 5-12 (or about 5-about 12); and C: 0.4-1.4 (or about 0.4-about 1.4).

[0073] In some embodiments, the alloy may include, in weight percent: Fe; Cr: 15-34 (or about 15-about 34); Mo+W: 1-16 (or about 1-about 16); B: 0.3-2.7 (or about 0.3-about 2.7); Nb+Ti: 1-10 (or about 1-about 10); and C: 0-1.2 (or about 0-about 1.2).

[0074] In some embodiments, the alloy may include, in weight percent: Fe; Cr: 13.5-35 (or about 15-about 34); B+C: 0.8-2 (or about 0.8-about 2); and Nb+Ti+V: 0.5-8.5 (or about 0.5-8.5).

[0075] In some embodiments, the alloy may include, in weight percent: Fe; Cr:13.6-34.8 (or about 13.6-about 34.8); B+C: 0.8-1.92 (or about 0.8-about 1.92); Mo+W: 0-2.4 (or about 0-about 2.4); Ni: 0-1.6 (or about 0-about 1.6); and Nb+Ti+V: 0.8-8.4 (or about 0.8-about 8.4).

[0076] In some embodiments, the alloy may include, in weight percent: Fe; C: 0.8-1.2 (or about 0.8-about 1.2); B+C: 0.8-1.68 (or about 0.8-about 1.68); Cr: 13.6-24 (or about 13.6-about 24); Mo+W: 0-2.4 (or about 0-about 2.4); Ni: 0-1.6 (or about 0-about 1.6); Nb: 4-6 (or about 4-about 6); Ti: 1.6-2.4 (or about 1.6-about 2.4); and Nb+Ti+V: 4-8.4 (or about 4-about 8.4).

[0077] In any of the compositions disclosed herein, Mo+W may be greater than 1 wt.% (or greater than about 1 wt.%), or greater than 3 wt.% (or greater than about 3 wt.%).

[0078] In some embodiments, more preferably, the alloy can include 1.6 to 2.4 (or about 1.6 to about 2.4) weight % Mo+W. In some embodiments, the alloy can include 1.6 to 2.4 (or about 1.6 to about 2.4) weight % Mo. In some embodiments, the alloy can include 0.8 to 1.2 (or about 0.8 to about 1.2) weight % C. In some embodiments, the alloy can include 13.6 to 24 (or about 13.6 to about 24) weight % Cr. In some embodiments, the alloy can include 4 to 6 (or about 4 to about 6) weight % Nb. In some embodiments, the alloy has a Nb / C ratio of 4 to 6 (or about 4 to about 6). In some embodiments, the alloy has a Nb / C ratio of 4.5 to 5.5 (or about 4.5 to about 5.5).

[0079] In any of the above embodiments, the alloy can include 0.8 to 1.2 (or about 0.8 to about 1.2) by weight percent B. In any of the above embodiments, the alloy can include 0.3 to 0.5 (or about 0.3 to about 0.5) by weight percent B. In some embodiments, the alloy can include 1.6 to 2.4 (or about 1.6 to about 2.4) by weight percent Ti.

[0080] In some embodiments, the disclosed compositions can be wires / powder, coatings or other metal parts, or both.

[0081] In some embodiments, the disclosed alloys have modified chemistry by dilution with the substrate after deposition. In some embodiments, the substrate dilution can be between 0 and 50% by volume. The disclosed embodiments can be designed to handle dilution with substrates that have high levels of carbon, such as gray cast iron. For compositions, the carbon in the substrate will tend to form deleterious phases that reduce the Cr, Mo, and / or W content of the matrix, reduce corrosion performance, and / or reduce the toughness or wear performance of the alloy. As a result, the disclosed embodiments can work without dilution, diluted with low carbon steels, and diluted with high carbon iron alloys, such as gray cast iron, while maintaining good properties in all cases.

[0082] In some embodiments, the alloy can include less than 1% carbon by weight (or less than about 1% carbon). In some embodiments, the alloy can include less than 0.5% carbon by weight (or less than about 0.5% carbon). In some embodiments, the alloy can include less than 0.25% carbon by weight (or less than about 0.25% carbon). In some embodiments, the alloy can include less than 0.1% carbon by weight (or less than about 0.1% carbon).

[0083] Due to regulatory, environmental, and safety concerns, nickel may be restricted in all wear surfaces. Some embodiments of the present disclosure specifically limit the nickel content of the feedstock powder.

[0084] In some embodiments, the alloy can include less than 5% nickel (or less than about 5% nickel) by weight. In some embodiments, the alloy can include less than 2% nickel (or less than about 2% nickel) by weight. In some embodiments, the alloy can include less than 1% nickel (or less than about 1% nickel) by weight. In some embodiments, the alloy can include less than 0.5% nickel (or less than about 0.5% nickel) by weight. In some embodiments, the alloy can include less than 0.2% nickel (or less than about 0.2% nickel) by weight. In some embodiments, the alloy can include less than 0.15% nickel (or less than about 0.15% nickel) by weight. In some embodiments, the alloy can include less than 0.1% nickel (or less than about 0.1% nickel) by weight.

[0085] Table 1 shows some embodiments of arc melt alloy chemistries. Table 2 shows embodiments of laser cladding chemistries. [Table 1] [Table 2]

[0086] In some embodiments, titanium can be reduced by increasing Nb or including V. An exemplary composition is Fe: balance, C: 1, Cr: 20, Mo: 2, Nb: 5, Ti: 1.6, V: 4.8 (or Fe: balance, C: about 1, Cr: about 20, Mo: about 2, Nb: about 5, Ti: about 1.6, V: about 4.8), where Nb + Ti + V = 11.4 (or about 11.4). [Table 3] [Table 4]

[0087] The alloys disclosed herein may incorporate up to a total of 100 wt.% of the above-named elemental components. In some embodiments, the alloys may include, be limited to, or consist essentially of the above-named elements. In some embodiments, the alloys may contain impurities of 2 wt.% (or about 2 wt.%) or less, 1 wt.% (or about 1 wt.%) or less, 0.5 wt.% (or about 0.5 wt.%) or less, 0.1 wt.% (or about 0.1 wt.%) or less, or 0.01 wt.% (or about 0.01 wt.%) or less, or any range of these values. Impurities may be understood as elements or compositions that may be included in the alloy due to inclusion in the raw material components through their introduction into the manufacturing process. In some embodiments, the impurities may be Co, Mn, Mo, Ta, V, and / or W.

[0088] Additionally, the Fe content identified in all of the compositions above may be the balance of the composition, or, where Fe is provided as the balance, the balance of the composition may include Fe and other elements, in some embodiments the balance may consist essentially of Fe and may include incidental impurities.

[0089] thermodynamic criteria In some embodiments, the alloys can be completely characterized by their thermodynamic criteria.

[0090] The hardness of the alloy embodiments can be maintained at a relatively low level by engineering a stable ferritic phase. In most iron-based alloys, austenite appears at high temperatures. At a sufficiently fast cooling rate, austenite transforms into martensite. Martensite is the hardest metallic iron phase, and therefore is present in almost all case-hardened alloys. However, given a sufficiently low cooling rate, alloys classified as "martensitic steels" may form ferrite. Typical laser cladding conditions are fast enough that martensite usually forms in many iron alloys, with 431 stainless steel being a relevant example. The ferritic structure is thermodynamically stable at high temperatures, and its stability extends to low temperatures, so the alloy techniques described herein do not form martensite, even under rapid cooling conditions. Thus, in some embodiments, the alloy forms only a ferritic matrix with hard phases.

[0091] An example of the stability of the ferrite phase is shown in Figure 1, which shows a thermodynamic calculation of the alloy of the present disclosure. The figure plots the phase mole fraction as a function of temperature for a particular composition. As shown, the ferrite phase is present at 90 mole % at high temperatures just below the solidus temperature of the alloy. The ferrite phase is consistently present at greater than 70 mole % down to lower temperatures of 500K. Some austenite

[0104] and BCC Cr

[0105] are also present in this temperature range, but the majority of the phase composition is ferrite throughout the temperature window. In Figure 1,

[0101] shows the formation of a stable ferrite (BCC) matrix over the entire temperature range, and

[0102] shows the formation of Nb / Ti carbide hard phases at about 10% volume fraction. Under these conditions, the alloy forms ferrite under a variety of welding conditions, even at welding conditions with rapid cooling rates that tend to form martensite in iron-based alloys. Processes that exhibit rapid cooling conditions include thermal spraying, plasma transferred arc (PTA) welding, laser cladding, and extreme high speed laser cladding (EHLA).

[0092] For comparison, the thermodynamic profile of 431 stainless steel, a common case hardening alloy used in hydraulic rod applications, is shown in FIG. 2. In contrast to the alloys of FIG. 1, 431 stainless steel forms delta ferrite

[0201] at high temperatures, transitions to austenite

[0202] at low temperatures, and reverts to alpha ferrite

[0203] upon further cooling. 431 stainless steel forms ferrite, austenite, martensite, or some mixture, depending on the cooling rate of the process. 431 stainless steel is generally intended to form martensite in applications that provide high hardness for case hardening applications. 431 stainless steel can be made to form a ferritic structure under controlled slow cooling conditions or by heat treatment, but does not form a ferritic structure in related fast cooling processes such as PTA welding. The alloys of the present disclosure differ in their ferrite formation behavior in that ferrite forms even under rapid cooling conditions. This behavior is advantageous when it is desired to form low hardness coatings via such processes.

[0093] In some embodiments, at all temperatures below the solidus and above 500K, the ferrite phase fraction is 50 (or about 50) mole % or greater. In some embodiments, the ferrite phase fraction is 60 (or about 60) mole % or greater. In some embodiments, the ferrite phase fraction is 70 (or about 70) mole % or greater. For reference, the alloys of the present disclosure reach a minimum of 72.9 mole % within a given temperature window. 431 stainless steel reaches a minimum of 4.47 mole % ferrite.

[0094] In some embodiments, the alloy matrix can be 100% (or about 100%) ferritic at 1300K. In some embodiments, the alloy matrix can be greater than 95% (or greater than about 95%) ferritic at 1300K. In some embodiments, the alloy matrix can be greater than 90% (or greater than about 90%) ferritic at 1300K. In some embodiments, the alloy matrix can be greater than 80% (or greater than about 80%) ferritic at 1300K. This ferritic matrix can be maintained in the microstructure of the coating.

[0095] In some embodiments, there may be 0 mol% (or about 0 mol%) FCC austenite between 1000 and 1400K (or about 1000 and about 1400K). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 5 mol% (or less than about 5 mol%). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 10 mol% (or less than about 10 mol%). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 15 mol% (or less than about 15 mol%).

[0096] In some embodiments of the present disclosure, the alloy matrix chemistry at 1300K is in the ferritic region of the Schaeffler diagram shown in Figure 8. In some embodiments of the present disclosure, the alloy matrix chemistry at 1300K is in the ferritic region. The ferrite and martensite are in the Schaeffler diagram. In some embodiments of the present disclosure, the alloy matrix chemistry at 1300K is not in the austenite, austenite and martensite, or martensite regions of the Schaeffler diagram.

[0097] A second feature of the disclosed alloy is the formation of primary FCC carbides, also known as MC type carbides. Such carbides can provide enhanced wear resistance desired for applications despite their low hardness. Figure 1 shows the thermodynamic behavior of FCC carbides, where they form at relatively high temperatures

[0103] and ultimately form at about 10 mol% in the disclosed alloy. In some aspects, a high carbide formation temperature can be advantageous. This forces the carbide morphology to form isolated globular morphologies. Such morphologies provide wear resistance but do not significantly reduce the toughness of the coating. However, the formation temperature should not be too high as it would make the alloy incompatible with industrial gas atomization processes. The balance between maximizing the formation temperature for an idealized structure while minimizing it to avoid atomization difficulties was determined throughout the course of the inventive effort.

[0098] In some embodiments, the primary carbide formation temperature can be between 1750K and 2100K (or between about 1750K and about 2100K). In some embodiments, the primary carbide formation temperature can be between 1850K and 2000K (or between about 1850K and about 2000K).

[0099] In some embodiments, the measured primary carbide mole fraction at 1300K may be 5 (or about 5) mole % or greater. In some embodiments, the measured primary carbide mole fraction at 1300K may be 7.5 (or about 7.5) mole % or greater. In some embodiments, the measured primary carbide mole fraction at 1300K may be 10 (or about 10) mole % or greater. For reference, the alloys of the present disclosure form a 9.6 mole % primary carbide fraction, with the temperature of formation of primary carbides being 2000K. 431 stainless steel does not form primary carbides.

[0100] In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 1% and 15% (or between about 1% and about 15%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 1% and 6% (or between about 1% and about 6%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 5% and 15% (or between about 5% and about 15%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 7% and 12% (or between about 7% and about 12%).

[0101] The primary carbides of the disclosed alloys may include Nb and Ti as metallic species. It is possible to form FCC primary carbides with Nb, Ti, V, or any combination thereof. However, the ratio of such metallic species affects the formation temperature. Thus, in some embodiments, instead of forming niobium carbide, which has a very high formation temperature, other FCC carbide formers, such as titanium, may be added to lower the formation temperature of the carbides.

[0102] The thermodynamic properties of the alloy technology result in an advantageous microstructure with a ferritic matrix

[0301] with embedded primary carbides

[0302] as shown in Figure 3. Figure 3 shows a PTA coating of the alloy of the present disclosure using the parameters described later in this disclosure. Energy dispersive spectroscopy was used to measure the composition of the ferritic matrix itself with particular interest in the chromium content. The Cr content was measured to be 19 wt% in the PTA coating. It is generally advantageous to have a high Cr content in the ferritic matrix to provide high corrosion resistance.

[0103] In some embodiments, the Cr content of the ferritic matrix may be at least 12 (or about 12) wt%. In some embodiments, the Cr content of the ferritic matrix may be at least 15 (or about 15) wt%. In some embodiments, the Cr content of the ferritic matrix may be at least 19 (or about 19) wt%. It should be noted that the content of the ferritic matrix will often differ from the Cr composition of the alloy, and Cr in the form of Cr carbides or other phases does not improve the corrosion resistance of the alloy.

[0104] The corrosion performance of iron alloys can be predicted by the Pitting Resistance Equivalent Number (PREN). This number is calculated as PREN=Cr+3.3*(Mo+0.5*W)+16*N, where element values ​​are in weight percent. For common single-phase materials, such as most ferritic stainless steels, this number applies to the bulk alloy composition. Since the alloys of the present disclosure contain multiple phases, the PREN number can be calculated based on the equilibrium thermodynamic conditions of the matrix phase, purposely excluding the composition of other phases that may form, such as borides. The matrix phase is defined as an iron-rich metallic phase, either FCC or BCC. This allows the PREN value of the matrix to accurately predict the relative corrosion performance of multiphase materials. In some embodiments of the present disclosure, the matrix phase is BCC ferrite.

[0105] For the alloys of the present disclosure, as shown in Figure 4, the matrix PREN is calculated as 34.3 at 1300 K based on the chemistry of the BCC phase, which is the only matrix phase present under equilibrium solidification conditions

[0401] . For the alloys of the present disclosure, as shown in Figure 5, the matrix PREN is calculated as 27.0 at 1300 K based on the chemistry of the BCC phase

[0501] . See Table 5 below for all alloys produced by arc melting and the calculated PREN at 1300 K under equilibrium solidification conditions.

[0106] In some embodiments of the present disclosure, the matrix PREN at 1300K is greater than 17 (or greater than about 17). In some embodiments of the present disclosure, the matrix PREN at 1300K is greater than 20 (or greater than about 20). In some embodiments of the present disclosure, the matrix PREN at 1300K is greater than 23 (or greater than about 23). In some embodiments of the present disclosure, the matrix PREN at 1300K is greater than 25 (or greater than about 25).

[0107] Another way to predict the corrosion performance of ferrous alloys is by their chromium content, which can be calculated for the matrix phase under equilibrium solidification conditions and is further shown in Table 5.

[0108] In some embodiments at 1300K, the matrix can include, by weight, greater than 13% (or greater than about 13%) chromium. In some embodiments at 1300K, the matrix can include, by weight, greater than 15% (or greater than about 15%) chromium. In some embodiments at 1300K, the matrix can include, by weight, greater than 17% (or greater than about 17%) chromium. In some embodiments at 1300K, the matrix can include, by weight, greater than 18% (or greater than about 18%) chromium. In some embodiments at 1300K, the matrix can include, by weight, greater than 20% (or greater than about 20%) chromium. In some embodiments, the chromium discussed herein may be included in the final coating.

[0109] The formation of intermetallic phases in high Cr, Mo, and / or W stainless steels can result in a high percentage of intermetallic phases that correlate with reduced toughness and / or ductility. The alloys are configured to have minimal or no cracking after deposition by thermal spray or other processes, so minimizing the presence of embrittling phases can be advantageous. In this disclosure, the mole fraction of intermetallic phases is defined as the sum under equilibrium solidification conditions of all chi, sigma, and Laves phases. In some applications, such as brake discs, surfaces can reach 800K during extreme braking events, and as a result, it is important that intermetallic phases do not precipitate during use.

[0110] As shown in Figure 4, in the alloy of the present disclosure, the intermetallic phases present at 800K are sigma phase

[0402] and Laves phase

[0403] , so the fraction of intermetallic phases at 800K is calculated as 18.5%. Figure 5 shows that in the alloy of the present disclosure, both Laves phase

[0502] and sigma phase

[0503] are present, so the calculated total mole fraction is 8.6%.

[0111] In some embodiments at 800K, the alloy can include less than 25% (or less than about 25%) intermetallic phase by mole fraction. In some embodiments at 800K, the alloy can include less than 20% (or less than about 20%) intermetallic phase by mole fraction. In some embodiments at 800K, the alloy can include less than 15% (or less than about 15%) intermetallic phase by mole fraction. In some embodiments at 800K, the alloy can include less than 10% (or less than about 10%) intermetallic phase by mole fraction. In some embodiments at 800K, the alloy can include less than 8% (or less than about 8%) intermetallic phase by mole fraction.

[0112] The formation of hard phases such as borides, carbides, boron carbides, oxides, and nitrides can improve the wear resistance of an alloy. There is a practical limit to the proportion of hard phases that may cause cracking of the alloy after deposition of a hard layer with excessively high wear resistance values ​​or during its use, especially when exposed to cyclic and rapid temperature changes. Hard phases in this disclosure can be calculated as the sum of all borides, carbides, boron carbides, oxides, and / or nitrides under equilibrium solidification conditions.

[0113] In the disclosed alloy, there are two hard phases at 1300 K, M3B2 phase

[0405] and M2B phase

[0404] , the sum of these hard phases is 21.7 mole %. In the disclosed alloy, the hard phases present are M2B

[0504] and MC carbide (FCC_A1#2)

[0505] , so the mole fraction of hard phases at 1300 K is 15.1%.

[0114] In some embodiments of the present disclosure, the mole fraction of the hard phase under equilibrium or near equilibrium solidification conditions can be 7 to 35% (or about 7 to about 35%). In some embodiments of the present disclosure, the mole fraction of the hard phase can be 7 to 25% (or about 7 to about 25%). In some embodiments of the present disclosure, the mole fraction of the hard phase can be between 10 to 22% (or about 10 to about 22%). In some embodiments of the present disclosure, the mole fraction of the hard phase can be between 7 to 22% (or about 7 to about 22%).

[0115] In some embodiments, borides can be advantageously formed due to the low solid solution solubility of boron in iron, which improves precipitation of certain phases during rapid cooling rates such as those present in laser cladding and EHLA processes.

[0116] In some embodiments, the hard phase can be only borides or a combination of borides and carbides.

[0117] In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 2% and 25% (or about 2% and about 25%). In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 2% and 10% (or about 2% and about 10%). In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 2% and 6% (or about 2% and about 6%). In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 8% and 24% (or about 8% and about 24%). In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 8% and 16% (or about 8% and about 16%). In some embodiments, the molar fraction of boride under equilibrium or near-equilibrium solidification conditions may be between 10% and 22% (or about 10% and about 22%).

[0118] In some embodiments, MC type carbides, where M includes Nb and / or Ti, may be advantageously formed due to their advantageous low aspect ratio and isolated morphology, which may have relatively high crack resistance compared to hypoeutectic or eutectic morphologies present in other carbides and other hard phases.

[0119] In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 1% and 15% (or between about 1% and about 15%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 1% and 6% (or between about 1% and about 6%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 5% and 15% (or between about 5% and about 15%). In some embodiments, the mole fraction of MC carbides under equilibrium or near-equilibrium solidification conditions can be between 7% and 12% (or between about 7% and about 12%).

[0120] The formation of high temperature phases during melting and atomization can reduce the manufacturability of an alloy by limiting fluidity. Limited fluidity may require special equipment for melting, may reduce the yield of atomization, and / or may make industrial-scale production impossible. To ensure high fluidity, the liquidus temperature under equilibrium solidification conditions can be controlled, as a lower liquidus temperature correlates with improved fluidity during atomization.

[0121] The liquidus temperature is thermodynamically defined as the lowest temperature at which an alloy is 100% liquid. In one alloy of this disclosure, the liquidus temperature is 1950 K

[0506] , and in another alloy of this disclosure, the liquidus temperature is 1650 K

[0406] .

[0122] In some embodiments, the liquidus temperature of the alloy may be less than (or less than about) 2000 K. In some embodiments, the liquidus temperature of the alloy may be less than (or less than about) 1975 K. In some embodiments, the liquidus temperature of the alloy may be less than (or less than about) 1950 K. In some embodiments, the liquidus temperature of the alloy may be less than (or less than about) 1925 K. In some embodiments, the liquidus temperature of the alloy may be less than (or less than about) 1900 K.

[0123] In some embodiments of the present disclosure, it may be advantageous to have a ferritic matrix. In the alloys of the present disclosure, the matrix is ​​100% ferritic (BCC) at 1300K, and the composition is within the ferritic zone of the Schaeffler diagram.

[0124] In some embodiments of the present disclosure, the alloy matrix can be 100% ferritic at 1300K (or about 100%). In some embodiments of the present disclosure, the alloy matrix can be greater than 95% ferritic (or greater than about 95%) at 1300K. In some embodiments of the present disclosure, the alloy matrix can be greater than 90% (or greater than about 90%) ferritic at 1300K. In some embodiments of the present disclosure, the alloy matrix can be greater than 80% (or greater than about 80%) ferritic at 1300K. This ferritic matrix can be maintained in the microstructure of the coating.

[0125] In some embodiments, there may be 0 mol% (or about 0 mol%) FCC austenite between 1000 and 1400K (or about 1000 and about 1400K). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 5 mol% (or less than about 5 mol%). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 10 mol% (or less than about 10 mol%). In some embodiments, the maximum mole fraction of FCC austenite present between 1000 and 1400K (or about 1000 and about 1400K) is less than 15 mol% (or less than about 15 mol%).

[0126] In some embodiments of the present disclosure, the alloy matrix chemistry at 1300K is within the ferrite region of the Schaeffler diagram shown in Figure 8. The ferrite and martensite are in the Schaeffler diagram. In some embodiments of the present disclosure, the alloy matrix chemistry at 1300K is not in the austenite, austenite and martensite, or martensite regions of the Schaeffler diagram. [Table 5]

[0127] Thermodynamic properties after dilution If the alloys of the present disclosure can be deposited on a substrate containing high levels of carbon, such as gray cast iron or ductile iron, it may be advantageous to maintain good properties after dilution and the corresponding increase in carbon content in the overlay. The ferritic structure is advantageous in certain applications where austenite increases galling and / or martensite presents cracking and / or toughness issues. Certain embodiments of the present disclosure also describe maintaining the ferritic structure after dilution with the substrate. The substrate may be mild steel, HSLA steel, cast iron, ductile iron, white iron, or other iron-based substrates.

[0128] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.15% (or about 0.15%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.15% (or about 0.15%) carbon from substrate dilution.

[0129] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.20% (or about 0.20%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.20% (or about 0.20%) carbon from substrate dilution.

[0130] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.25% (or about 0.25%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.25% (or about 0.25%) carbon from substrate dilution.

[0131] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.30% (or about 0.30%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.30% (or about 0.30%) carbon from substrate dilution.

[0132] In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 20 (or about 20) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 23 (or about 23) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 17 (or about 17) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution.

[0133] When the alloys of the present disclosure are deposited on substrates containing high levels of carbon and silicon, such as grey cast iron or ductile cast iron, it can be advantageous to maintain good corrosion properties after dilution and a corresponding increase in carbon content in the overlay.

[0134] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.15% (or about 0.15%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.15% (or about 0.15%) carbon from substrate dilution.

[0135] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.20% (or about 0.20%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.20% (or about 0.20%) carbon from substrate dilution.

[0136] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.25% (or about 0.25%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.25% (or about 0.25%) carbon from substrate dilution.

[0137] In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 23 (or about 23) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.30% (or about 0.30%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value greater than 20 (or about 20) at 1300 K, and a matrix with greater than 90% (or about 90%) ferrite at 1300 K, after the addition of less than or equal to 0.30% (or about 0.30%) carbon from substrate dilution.

[0138] In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 20 (or about 20) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 23 (or about 23) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution. In some embodiments, the alloys of the present disclosure have a matrix PREN value of greater than 17 (or about 17) at 1300K and a matrix with greater than 90% (or about 90%) ferrite at 1300K after the addition of less than or equal to 0.35% (or about 0.35%) carbon from substrate dilution.

[0139] In some embodiments of the present disclosure, high levels of Nb and / or Ti can be present in the alloy. When the alloys of the present disclosure are coated onto a high carbon substrate, such as grey cast iron, Nb and / or Ti can bind to some of the carbon added via dilution in the substrate. This can increase the proportion of MC carbides, where M includes Nb and / or Ti, compared to the same level of dilution on a low carbon substrate. This formation of MC phases reduces the weight percent of carbon in the matrix, improving the stability of ferrite and providing beneficial properties. It also reduces the amount of M7C3 and M, which reduce PREN after deposition on high carbon substrates. 23 Chromium-containing carbides such as C6 are also suppressed.

[0140] In some embodiments of the present disclosure, the mole fraction MC after dilution with grey cast iron may be higher than the mole fraction that would be present given the same weight fraction diluted with low carbon steel.

[0141] In some embodiments, M7C3 and M 23The total mole fraction of C6 is 0% (or about 0%). In some embodiments, M7C3 and M 23 The total mole fraction of C6 is less than 2% (or about 2%). In some embodiments, M7C3 and M 23 The total mole fraction of C6 is less than 5% (or about 5%). [Table 6]

[0142] Microstructure and Performance In some embodiments of the present disclosure, the alloys may be fully described by their microstructural features. The microstructures of the alloy embodiments provide advantageous material properties.

[0143] As previously mentioned, the hardness of the disclosed alloy embodiments can remain relatively low. Hardness was measured using Vickers hardness, specifically HV0.3. Wear resistance was measured using ASTM G65 procedure A. PTA welding was used to compare the disclosed alloys to 431 SS using the following parameters to obtain a weld bead approximately 3 mm thick and 28 mm wide. Voltage: 28V Amperage: 120A Powder supply: 35g / min Traverse speed: 2.1 inches / min Plasma gas: 6 SCFH Carrier gas: 2.5 SCFH Shielding gas: 24 SCFH

[0144] Similar microstructures and coatings with similar performance characteristics can be produced using laser cladding and EHLA. [Table 7]

[0145] As shown in Table 7, the hardness of the disclosed alloy is lower than that of 431 SS. However, the wear resistance is higher for the disclosed alloy.

[0146] In some embodiments, the hardness of the disclosed alloys is less than or equal to 450 (or about 450) Vickers. In some embodiments, the hardness is less than or equal to 400 (or about 400) Vickers. In some embodiments, the hardness is less than or equal to 350 (or about 350) Vickers. This can include any type of coating, such as a PTA coating. As previously mentioned, a lower hardness improves the machinability of the coating.

[0147] In some embodiments, the alloy is 200 (or about 200) mm 3 In some embodiments, the alloy may have an ASTM G65 volume loss of 150 (or about 150) mm 3 In some embodiments, the alloy may have an ASTM G65 volume loss of 100 (or about 100) mm 3 It can have the following ASTM G65 volume loss: This can include any type of coating, such as a PTA coating.

[0148] Although the particular process is not limiting to the disclosure, it is also advantageous that the alloy be weldable crack-free under PTA, laser, and EHLA processes. Alloys of the disclosed alloys have demonstrated the ability to weld crack-free overlays under PTA and laser conditions.

[0149] The formation of hard phases such as borides, carbides, boron carbides, oxides, and nitrides can improve the wear resistance of the alloy. There are practical limits to the percentage of hard phases, where excessively high values ​​may cause cracking of the alloy after deposition or during service, especially when exposed to cyclic and rapid temperature changes. Hard phases in this disclosure can be calculated as the sum of all borides, carbides, hydrocarbons, oxides, and nitrides measured using quantitative metallographic techniques on arc-melted samples of the alloy.

[0150] Specifically, in some embodiments, the alloy may include an amount of primary carbides in a matrix. In some embodiments, a volume fraction of 5 (or about 5) vol. % of the primary carbides may be embedded in a matrix composed primarily of ferrite. In some embodiments, a volume fraction of 7.5 (or about 7.5) vol. % of the primary carbides may be embedded in a matrix composed primarily of ferrite. In some embodiments, a volume fraction of 10 (or about 10) vol. % of the primary carbides may be embedded in a matrix composed primarily of ferrite.

[0151] In other embodiments, the alloy may include borides in the microstructure. As shown in Figures 6-7, in the disclosed alloy, the volume fraction of hard phases is measured as the sum of all borides

[0301]

[0302] as 23%. In the disclosed alloy, the volume fraction of hard phases is measured as borides

[0401] and carbides

[0402] as 14%.

[0152] In some embodiments of the present disclosure, the volume fraction of all hard phases may be between 5 and 35% (or about 5 to about 35%). In some embodiments of the present disclosure, the volume fraction of all hard phases may be between 5 and 25% (or about 5 to about 25%). In some embodiments of the present disclosure, the volume fraction of all hard phases may be between 7 and 25% (or about 7 to about 25%). In some embodiments of the present disclosure, the volume fraction of all hard phases may be between 8 and 15% (or about 8 to about 15%). In some embodiments of the present disclosure, the volume fraction of all hard phases may be between 10 and 25% (or about 10 to about 25%).

[0153] The PREN of the matrix phase is a strong predictor of the corrosion performance of an alloy. PREN is calculated as [Cr+3.3*Mo+0.5*W)+16*N], where elemental values ​​are in weight percent. Elemental weight percent is measured using Energy Dispersive X-ray Spectroscopy (EDS) in a Scanning Electron Microscope (SEM).

[0154] In the alloys of the present disclosure, the PREN is calculated from the matrix phase

[0303] measured via EDS as 36.3.

[0155] In some applications, the alloys described in this disclosure can be deposited as coatings intended to provide corrosion resistance. When corrosive media, such as high chloride content water, are present, excessive coating porosity can allow the corrosive media to penetrate the substrate. If this penetration occurs, corrosion of the substrate can lead to surface discoloration, poor overlay performance, and / or delamination of the coating from the substrate. As a result, it can be advantageous to control the percentage of porosity in coatings deposited by thermal spray or other methods. Porosity is measured via ASTM E2109-01.

[0156] In some embodiments of the present disclosure, coatings formed from the described alloys can have a porosity of less than 3% (or about 3%). In some embodiments of the present disclosure, coatings formed from the described alloys can have a porosity of less than 2% (or about 2%). In some embodiments of the present disclosure, coatings formed from the described alloys can have a porosity of less than 1.5% (or about 1.5). In some embodiments of the present disclosure, coatings formed from the described alloys can have a porosity of less than 1% (or about 1%).

[0157] In some embodiments, 0 vol% (or about 0 vol%) FCC austenite may be present. In some embodiments, the maximum volume fraction of FCC austenite is less than 5 vol% (or less than about 5 vol%). In some embodiments, the maximum volume fraction of FCC austenite is less than 10 vol% (or less than about 10 vol%). In some embodiments, the maximum volume fraction of FCC austenite is less than 15 vol% (or less than about 15 vol%).

[0158] In some embodiments, the volume fraction of borides can be between 2% and 25% (or about 2% and about 25%). In some embodiments, the volume fraction of borides can be between 2% and 10% (or about 2% and about 10%). In some embodiments, the volume fraction of borides can be between 2% and 6% (or about 2% and about 6%). In some embodiments, the volume fraction of borides can be between 8% and 24% (or about 8% and about 24%). In some embodiments, the volume fraction of borides can be between 8% and 16% (or about 8% and about 16%). In some embodiments, the volume fraction of borides can be between 10% and 22% (or about 10% and about 22%).

[0159] In some embodiments, the volume fraction of MC carbides can be between 1% and 15% (or between about 1% and about 15%). In some embodiments, the volume fraction of MC carbides can be between 1% and 6% (or between about 1% and about 6%). In some embodiments, the volume fraction of MC carbides can be between 5% and 15% (or between about 5% and about 15%). In some embodiments, the volume fraction of MC carbides can be between 7% and 12% (or between about 7% and about 12%).

[0160] In some embodiments, the ferrite phase fraction is greater than or equal to 50% by volume. In some embodiments, the ferrite phase fraction is greater than or equal to 60% by volume. In some embodiments, the ferrite phase fraction is greater than or equal to 70% by volume.

[0161] In some embodiments, the alloy matrix may be 100% ferritic. In some embodiments of the present disclosure, the alloy matrix may be greater than (or greater than about) 95% ferritic. In some embodiments of the present disclosure, the alloy matrix may be greater than (or greater than about) 90% ferritic. In some embodiments of the present disclosure, the alloy matrix may be greater than (or greater than about) 90% ferritic. In some embodiments of the present disclosure, the alloy matrix may be greater than (or greater than about) 80% ferritic.

[0162] In some embodiments, the matrix may comprise, by weight, greater than 13% (or greater than about 13%) chromium. In some embodiments, the matrix may comprise, by weight, greater than 15% (or greater than about 15%) chromium. In some embodiments, the matrix may comprise, by weight, greater than 17% (or greater than about 17%) chromium. In some embodiments, the matrix may comprise, by weight, greater than 18% (or greater than about 18%) chromium. In some embodiments, the matrix may comprise, by weight, greater than 20% (or greater than about 20%) chromium.

[0163] In some embodiments, the alloy may include less than 25% (or less than about 25%) by volume of the intermediate metallic phase. In some embodiments, the alloy may include less than 20% (or less than about 20%) by volume of the intermediate metallic phase. In some embodiments, the alloy may include less than 15% (or less than about 15%) by volume of the intermediate metallic phase. In some embodiments, the alloy may include less than 10% (or less than about 10%) by volume of the intermediate metallic phase. In some embodiments, the alloy may include less than 8% (or less than about 8%) by volume of the intermediate metallic phase. Working Example Example 1:

[0164] The alloys of the present disclosure are deposited by a conventional laser cladding process using the parameters shown in Table 7. [Table 8]

[0165] The deposited coatings were then sectioned, mounted and polished for EDS chemical analysis. Using five measurements made by EDS on the matrix of the coating, the average Cr and Mo contents in the matrix of the coating are shown in Table 9. [Table 9]

[0166] Finally, the microhardness of the coating was measured using a Vickers hardness test at 300 gf. After 10 measurements averaged across the sample, the hardness of the alloy was found to be 283 HV300. Example 2:

[0167] The alloys of the present disclosure were deposited by a conventional laser cladding process to produce a coating approximately 25 mm x 75 mm and 3 mm thick. The coating was subjected to ASTM G65A testing and measured 92.3 mm. 3 A volume loss of 200 mm occurred. Additionally, the coating was sectioned, mounted, and polished for microhardness testing. The microhardness of the coating was performed using a Vickers hardness tester with a force of 300 g. After utilizing 10 measurements across the sample, the hardness of the alloy was measured to be 270 HV. 300 In comparison, a coating of 420 stainless steel was deposited by conventional laser cladding. The ASTM G65A abrasion resistance of the coating was 136.9 mm. 3 However, the microhardness of the coating was 570HV after 10 measurements on average. 300 was measured. [Table 10] Example 3:

[0168] The alloys of the present disclosure were deposited by a conventional laser cladding process along with the conventional material, 431 stainless steel, producing coatings approximately 3 mm thick. ASTM G65, G77, and Vickers microhardness were performed. [Table 11] Purpose

[0169] The alloys described in this patent are applicable in a variety of applications and industries. Some non-limiting examples of applications of use include:

[0170] Surface mining applications include the components listed below and coatings for the following components: wear resistant sleeves and / or wear resistant surfacing for slurry pipelines, mud pump parts or surfacing for mud pump parts including pump housings or impellers, or ore delivery chute parts including chute blocks or hardfacing for chute blocks, separating screens including but not limited to rotary breaker screens, banana screens, shaker screens, liners for autogenous and semi-autogenous crushers, ground engaging tools and teeth and hardfacing for ground engaging tools, shrouds and adapters, wear plates and rock boxes for bucket and dump truck liners, heel blocks and hardfacings for heel blocks on mining shovels, grader blades and hardfacings for grader blades, stacker reclaimers, sizer crushers, jaw crushers, ripper teeth, cutting edges, general wear packages for mining and other comminution components.

[0171] Downstream oil and gas applications include the components listed below and coatings of the following components: downhole casing and downhole casing, drill pipe and drill pipe coatings including hardbanding, mud management components, mud motors, fracking pump sleeves, fracking impellers, fracking blender pumps, stop collars, drill bits and drill bit components, directional drilling rigs and coatings for directional drilling rigs including stabilizers and centralizers, blowout preventers and blowout preventer components (including shear rams, oil country tubular products), sucker rods and couplings, lift plungers, knee-for rotors, artificial lift casing, ESP pump housings and impellers, flowline and subsea flowline coatings.

[0172] Upstream oil and gas applications include coatings of the components listed below and the following components: steam generators, amine vessels, distillation columns, cyclones, catalytic crackers, general refinery piping, process vessels and process vessel coatings including corrosion under insulation protection, sulfur recovery units, convection hoods, sour stripper lines, scrubbers, hydrocarbon drums, and other refinery equipment and vessels.

[0173] Pulp and paper applications include coatings for the components listed below and for rolls used in paper machines including Yankee dryers, air dryers, and other dryers, calendar rolls, machine rolls, press rolls, take-up rolls, digesters, pulp mixers, pulpers, pumps, boilers, shredders, tissue machines, roll and bale handling machines, deflector blades, doctor blades, evaporators, pulp mills, headboxes, wire parts, press parts, fiber guidance systems such as MG cylinders, pope reels, winders, vacuum pumps, deflakers, and other paper pulp equipment.

[0174] Power generation applications include coatings for the components listed below: boiler tubes, precipitators, fireboxes, turbines, generators, cooling towers, condensers, chutes and troughs, augers, baghouses, ducts, ID fans, coal piping, and other power generation components.

[0175] Agricultural applications include the components listed below and coatings for the following components: chutes, base cutter blades, sugarcane harvesting knives, hammers, troughs, primary fan blades, secondary fan blades, augers, components common to mining applications, and other agricultural applications.

[0176] Construction applications include the components listed below and coatings for the following components: cement chutes, cement piping, bag houses, mixing equipment and other construction applications.

[0177] Machine element applications include coatings for the components listed below and for the rebuilding, general remanufacturing and dimensional restoration of shaft journals, hydraulic cylinders, paper rolls, gearboxes, drive rollers, impellers, engine decks, propeller shafts and other shafts; applications involving the restoration of cast iron, especially grey iron and ductile iron parts, and other machine element applications.

[0178] Steel applications include the following components and coatings for the following components: cold rolling mills, hot rolling mills, wire rod mills, galvanizing lines, continuous pickling lines, continuous casting rolls and other steel mill rolls, and other steel applications.

[0179] Automotive applications include coatings for valves and valve seats, cylinders and other components of internal combustion engines, brake discs and pads, as listed below. The alloys described in this patent can be effectively manufactured and / or deposited by a variety of techniques. Some non-limiting examples of processes are:

[0180] Thermal spray processes include wire-based, such as twin-wire arc spray, high velocity arc spray, and combustion spray, and powder-based, such as high velocity oxy-fuel, high velocity air, plasma spray, implosion gun spray, and cold spray. Wire feedstocks can be in the form of metal-cored wire, solid wire, or flux-cored wire. Powder feedstocks are either a single homogenous alloy or a combination of multiple alloy powders that, when melted together, provide the desired chemistry.

[0181] Welding processes include, but are not limited to, wire-based processes such as metal inert gas (MIG) welding, tungsten inert gas (TIG) welding, arc welding, submerged arc welding, open arc welding, bulk welding, laser cladding, and powder-based processes such as laser cladding, extreme high speed laser cladding (EHLA), and plasma transferred arc welding. Wire feedstock can be in the form of metal cored wire, solid wire, or flux cored wire. Powder feedstocks are either a single homogenous alloy or a combination of multiple alloy powders that, when melted together, result in the desired chemistry.

[0182] Casting processes representative of cast iron production include, but are not limited to, sand casting, permanent casting, chill casting, investment casting, lost foam casting, die casting, centrifugal casting, glass casting, slip casting, and the like, and also include typical manufacturing processes for molten steel products, including continuous casting processes.

[0183] Post-treatment steps include, but are not limited to, surface treatments such as rolling, forging, carburizing, nitriding, and carbonitriding, and heat treatments such as, but not limited to, austenitizing, normalizing, annealing, stress relieving, tempering, aging, quenching, low temperature treating, flame hardening, induction hardening, differential quenching, case hardening, decarburization, machining, grinding, cold working, work hardening, and welding.

[0184] From the foregoing, it will be appreciated that the present ferritic alloys and methods of use are disclosed. Although certain components, techniques, and aspects have been described with a degree of particularity, it will be apparent that many modifications can be made to the specific designs, constructions, and methodologies described hereinabove without departing from the spirit and scope of the present disclosure.

[0185] Certain features described in this disclosure in the context of separate implementations may also be implemented in combination in a single implementation. Conversely, various features described in the context of a single implementation may also be implemented in multiple implementations separately or in any suitable subcombination. Furthermore, although features may be described above as acting in a particular combination, one or more features from a claimed combination may, in some cases, be carved out of the combination, and the combination may be claimed as any subcombination or any variation of any subcombination.

[0186] Additionally, although methods may be described in a particular order in the drawings or specification, such methods need not be performed in the particular order or sequential order shown, and not all methods need be performed to achieve desirable results. Other methods not shown or described may be incorporated into the exemplary methods and processes. For example, one or more additional methods may be performed before, after, simultaneously with, or between any of the described methods. Additionally, methods may be rearranged or reordered in other implementations. Also, the separation of various system components in the above implementations should not be understood as requiring such separation in all implementations, and it should be understood that the described components and systems may generally be integrated together in a single product or packaged in multiple products. Additionally, other implementations are within the scope of this disclosure.

[0187] Conditional language such as "can," "could," "might," or "may," unless specifically stated to the contrary or otherwise understood within the context in which it is used, is generally intended to convey that a particular embodiment includes or does not include a particular feature, element, and / or step. Thus, such conditional language is generally not intended to imply that a feature, element, and / or step is in any way required for one or more embodiments.

[0188] Conjunctions such as the phrase "at least one of X, Y, and Z" are understood otherwise in the context in which they are commonly used to convey that an item, term, etc. can be either, unless specifically stated to the contrary. Thus, such conjunctions are not generally intended to imply that a particular embodiment requires the presence of at least one X, at least one Y, and at least one Z.

[0189] As used herein, degree terms such as the terms "approximately," "about," "generally," and "substantially" refer to a value, amount, or characteristic that is close to the stated value, amount, or characteristic and performs a desired function or achieves a desired result. For example, the terms "approximately," "about," "generally," and "substantially" may be within 10%, 5%, 1%, 0.1%, or 0.01% of the stated quantity. When the stated quantity is zero (e.g., not present, not having), the ranges described above are specific ranges, not within a specific % of the value. For example, they may be within 10%, 5%, 1%, 0.1%, or 0.01% by weight / volume of the stated quantity. Additionally, all values ​​in tables within this disclosure are understood to be the stated value or to be about the stated value.

[0190] Any particular features, aspects, methods, properties, qualities, attributes, elements, etc. disclosed herein in connection with various embodiments can be used in all other embodiments described herein. Furthermore, it will be recognized that any method described herein may be implemented using any device suitable for performing the recited steps.

[0191] Although several embodiments and variations thereof have been described in detail, other modifications and methods of use thereof will be apparent to those skilled in the art. It is therefore to be understood that various applications, modifications, materials, and substitutions of equivalents may be made without departing from the scope of the unique invention disclosed herein or the claims.

Claims

1. Fe, 18-25 wt.% Cr; 0.45-2.2 wt.% Ti; 0.9-3.3 wt.% Mo; 4.5-5.5 wt.% Nb; 2-12% by weight of Nb+Ti+V; 0.7-1.1 wt.% C; 5 wt.% or less of Ni; 2% by weight or less of impurities; The elemental composition is A clad feedstock having a total ferrite phase mole fraction of 50 mole % or greater at all temperatures below the solidus and above 500K.

2. The clad feedstock of claim 1, containing 2-10% by weight of Nb+Ti+V.

3. Fe, 18-25 wt.% Cr; 0.45-2.2 wt.% Ti; 0.9-3.3 wt.% Mo; 4.5-5.5 wt.% Nb; 2-12% by weight of Nb+Ti+V; 0.7-1.1 wt.% C; 5 wt.% or less of Ni; 0.3-0.5 wt.% B; 2% by weight or less of impurities; The elemental composition is A clad feedstock having a total ferrite phase mole fraction of 50 mole % or greater at all temperatures below the solidus and above 500K.

4. 4. The clad feedstock of claim 1, wherein the total ferrite phase mole fraction is 60 mole % or more at all temperatures below the solidus and above 500K.

5. 4. The clad feedstock of claim 1 or 3, wherein the clad feedstock has a primary carbide formation temperature between 1750K and 2100K.

6. 4. The clad material according to claim 1, wherein the clad material has a total primary carbide molar fraction of 5 mol % or more at 1300K.

7. A coating formed from the cladding material of claim 1 or 3.

8. A ferrite matrix; a plurality of primary carbides embedded within the ferrite matrix; The coating of claim 7 comprising:

9. The coating of claim 8 , wherein the plurality of primary carbides comprises at least one of Nb, Ti, and V.

10. The coating of claim 8 , wherein the plurality of primary carbides comprises isolated globular morphologies.

11. 8. The coating of claim 7, wherein the coating has a total primary char volume fraction of at least 5 volume percent.

12. The coating of claim 8, wherein the ferritic matrix has a Cr content of at least 12 wt.%.

13. 8. The coating of claim 7, wherein the coating has a hardness of 450 HV0.3 or less.

14. The coating has a volume loss of 200 mm according to ASTM G65 Procedure A. 3 8. The coating of claim 7, wherein:

15. A method for producing a coating formed from a clad feedstock according to claim 1 or 3 through a deposition process.

16. A method for applying the cladding material of claim 1 or 3 to a coating.

17. 4. The feedstock of claim 1 or 3, wherein the clad feedstock is a powder or the clad feedstock is one or more wires.

18. The ferrite matrix comprises at least 12 wt. % Cr, The clad material according to claim 1 or 3, wherein the molar fraction of the hard phase precipitated from the liquid is 5% or more.

19. The clad feedstock of claim 18, wherein the hard phase comprises carbides.

20. A clad raw material as described in claim 1 or 3, wherein the impurities are 1 weight % or less.

21. A clad raw material as described in claim 1 or 3, wherein the impurities are incidental impurities.

22. The clad raw material of claim 1 or 3, wherein the impurities are selected from the group consisting of Co, Mn, Ta, W and combinations thereof.

Citation Information

Patent Citations

  • New high-chromium alloy cast iron surfacing material

    CN102335798A

  • Composite wire for build-up welding

    JP1986283489A

  • Stainless steel weld overlays with enhanced wear resistance

    US20070187458A1

  • Corrosion resistant hardfacing alloy

    US20150147591A1

  • Crack resistant hardfacing alloys

    US20150354036A1