Composition for semiconductor processing, method for producing same, and method for producing semiconductor device using same
The composition for semiconductor processing, with specific zeta potential and pH-adjusted abrasive particles, addresses the challenges of CMP by ensuring stable distribution and preventing agglomeration, resulting in defect-free, high-performance polishing of semiconductor wafers.
Patent Information
- Application Number
- JP2023006751
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-20
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-01-19
AI Technical Summary
The increasing complexity and integration of semiconductor devices require high-resolution lithography and atomic-level planarization techniques in chemical mechanical polishing (CMP) processes, which are affected by minute differences in process parts and fluids, leading to varying polishing results and defects.
A composition for semiconductor processing is developed with abrasive particles having a zeta potential of -50 mV to -10 mV and a zeta potential change rate of 6 mV/pH to 30 mV/pH, produced by adjusting the pH of abrasive particles to 2 to 4 using an acidic solution and adding an organic component, preventing agglomeration and maintaining dispersibility.
The composition achieves excellent polishing performance with minimized defects, ensuring flatness and uniformity in semiconductor wafer polishing, particularly for tungsten and metal barrier films, by maintaining stable abrasive particle distribution and preventing agglomeration.
Smart Images

Figure 0007572470000003 
Figure 0007572470000004 
Figure 0007572470000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition applicable to semiconductor manufacturing and processing steps and a method for producing the same, and more specifically to a composition applicable to a polishing step in semiconductor manufacturing and processing and a method for producing the same. [Background technology]
[0002] Chemical mechanical polishing is a technique in which a polishing pad is rubbed against the surface of the object to be polished while an abrasive slurry is injected into the interface between the polishing pad and the object to be polished, thereby polishing the surface of the sample to the desired level.
[0003] As modern chemical mechanical polishing is applied to the manufacture of large-scale semiconductor integrated circuits, it is used as an essential technology for planarizing the surfaces of elements such as transistors and interlayer insulating films in multilayer wiring, and for forming tungsten and copper wiring.
[0004] As the integration density of semiconductor devices increases and the size of chips decreases year by year, the surface structure of semiconductor devices becomes more complex and the step of the interlayer film becomes larger. Therefore, high-resolution lithography and atomic level planarization technology are required for the Chemical Mechanical Polishing (CMP) process used in the manufacturing process of semiconductor devices.
[0005] The CMP process is a process that uses physical friction and chemical reactions simultaneously to planarize a film, and the polishing results can vary greatly depending on minute differences in the process parts and / or process solutions used.
[0006] Therefore, currently, the precision required for the manufacture and design of such process parts and / or process liquids is increasing to a higher level. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a composition for semiconductor processing, a method for producing the same, and a method for producing a semiconductor device using the same.
[0008] Another object of the present invention is to provide a composition for semiconductor processing that can be applied to a semiconductor process involving a polishing process of a semiconductor wafer, and can achieve excellent polishing performance, minimize defects, and achieve flat polishing results.
[0009] Another object of the present invention is to provide a method for preparing a composition for semiconductor processing, which has excellent dispersibility by minimizing pH shock of abrasive particles and preventing agglomeration between particles.
[0010] Another object of the present invention is to provide a method for manufacturing semiconductor devices with a minimized defect rate by applying a semiconductor processing composition to polishing a semiconductor wafer. [Means for solving the problem]
[0011] In order to achieve the above object, a composition for semiconductor processing according to one embodiment of the present invention includes abrasive particles, and the abrasive particles may have a zeta potential of -50 mV to -10 mV at pH 6, and a zeta potential change rate represented by the following formula 1 may be 6 mV / pH to 30 mV / pH:
[0012] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0013] wherein p6 is pH 6 and p5 is pH 5; The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0014] A method for producing a composition for semiconductor processing according to another embodiment of the present invention may include a step of adding an acidic solution to abrasive particles having a pH of 6 and a zeta potential of -50 mV to -10 mV to adjust the pH to 2 to 4, and a step of stirring the abrasive particles with the pH adjusted, and adding an organic component and an organic acid to the abrasive particles.
[0015] A method for manufacturing a semiconductor device according to another embodiment of the present invention includes the steps of: preparing a platen having a polishing pad with a polishing surface attached thereto; preparing a carrier containing an object to be polished; rotating the platen and the carrier while rotating the platen and the carrier in a state in which the polishing surface of the polishing pad and the surface to be polished of the object to be polished are in contact with each other; and supplying a composition for semiconductor processing onto the polishing surface, wherein the polishing composition for semiconductor processing may have a zeta potential change rate represented by the following formula 1 of 6 mV / pH to 30 mV / pH:
[0016] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0017] wherein p6 is pH 6 and p5 is pH 5;
[0018] The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5. Effect of the Invention
[0019] The present invention is applicable to semiconductor processes involving a polishing process of a semiconductor wafer, and can realize excellent polishing performance, minimize defects, and achieve flat polishing results.
[0020] In addition, by minimizing the pH shock of the abrasive particles, preventing the agglomeration phenomenon between particles, and applying a method for manufacturing semiconductor devices using a polishing composition for semiconductor processing that has excellent dispersibility, it is possible to manufacture semiconductor devices with a minimized defect rate. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a diagram illustrating a configuration for a semiconductor element. [Diagram 2] 3A to 3C are diagrams illustrating a configuration related to a manufacturing method of the semiconductor device. [Diagram 3] This relates to a change in zeta potential due to a change in pH of an abrasive particle according to one embodiment of the present invention. [Figure 4] FIG. 2 is a diagram showing a stabilized state of the abrasive particles. [Diagram 5] FIG. 2 is a diagram showing an unstable state of the abrasive particles. [Figure 6] FIG. 2 is a diagram showing a schematic diagram of the zeta potential of the abrasive particle and its relationship to the zeta potential of a semiconductor wafer. [Figure 7] FIG. 2 is a diagram showing a schematic diagram of the zeta potential of the abrasive particle and its relationship to the zeta potential of a semiconductor wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The advantages and features of the present invention, as well as the methods for achieving them, will become clear from the following examples. However, the present invention is not limited to the following examples, and may be realized in various different forms. The following examples are provided to fully disclose the present invention and to fully inform those skilled in the art of the scope of the invention. The present invention is defined by the scope of the claims.
[0023] In this specification, the words "comprise," "contain," or "have," unless otherwise specified, mean that other components may also be included.
[0024] In the drawings, the thicknesses of various layers and regions are exaggerated for clarity, and the thicknesses of some layers and regions are exaggerated for ease of explanation. The same reference numerals refer to the same elements throughout the specification.
[0025] In addition, in this specification, when a part such as a layer, film, region, plate, etc. is described as being "on" or "above" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between. Conversely, when a part is described as being "directly on" the other part, it means that there is no other part in between. Similarly, when a part such as a layer, film, region, plate, etc. is described as being "under" or "below" the other part, this includes not only the case where it is "directly below" the other part, but also the case where there is another part in between. Conversely, when a part is described as being "directly below" the other part, it means that there is no other part in between.
[0026] In the present invention, the abrasive particles are defined as inorganic particles or the like dispersed in a solvent such as water, and the pH of the abrasive particles means the pH in the state where they are dispersed in the solvent such as water.
[0027] The composition for semiconductor processing according to one embodiment of the present invention includes abrasive particles, and the abrasive particles may have a zeta potential of -50 mV to -10 mV at pH 6, and a zeta potential change rate represented by the following formula 1 may be 6 mV / pH to 30 mV / pH:
[0028] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0029] wherein p6 is pH 6 and p5 is pH 5; The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0030] The composition for semiconductor processing contains abrasive particles having a zeta potential change rate as shown in Formula 1, thereby preventing the agglomeration phenomenon between the abrasive particles in the composition and preventing the occurrence of defects such as defects that occur during the polishing process. When applied to semiconductor processes for polishing tungsten films and metal barrier films, the composition for semiconductor processing can achieve excellent polishing performance.
[0031] A semiconductor wafer to be polished using the composition for semiconductor processing of the present invention is as shown in Fig. 1. As shown in Fig. 1, a SiO2 oxide film 20, which is an interlayer insulating film, is formed on a silicon substrate 10, and the SiO2 oxide film 20 is etched to form contact holes.
[0032] Next, a metal barrier film 30 such as Ti / TiN (adhesion layer / diffusion prevention layer) is formed on the entire surface of the substrate including the contact hole, and a tungsten (W) film 40 is deposited on the top so that the contact hole is completely filled. Then, a semiconductor processing composition is used to polish the tungsten film 40 and the metal barrier film 30 on the SiO2 oxide film 20 in a chemical mechanical polishing process to form a tungsten plug.
[0033] In the manufacturing process of semiconductor devices as described above, the semiconductor processing composition generally contains abrasive particles and other additives, the abrasive particles being for mechanical polishing of the target film quality, and the other additives may be included to improve or complement the performance of the semiconductor processing composition.
[0034] When the value of Equation 1 satisfies the above range, the composition for semiconductor processing can provide a polishing composition in which the abrasive particles have a high level of dispersibility and the particle sizes are uniformly distributed.
[0035] Specifically, the composition for semiconductor processing of the present invention may have a polishing particle having a pH of 6 and a zeta potential of -50 mV to -10 mV. The polishing composition is prepared using a polishing particle having a zeta potential of -50 mV to -10 mV at pH 6. By preparing the polishing composition using weakly acidic abrasive particles, a polishing composition having excellent dispersibility can be prepared without performing a separate aging process. That is, as described below, the abrasive particle is surface-treated with an organic component. In order to surface-treat the abrasive particle as described above, the pH of the abrasive particle in a weakly acidic state can be adjusted to an acidic state and mixed with an organic component. The mixed organic component is bonded to the surface of the abrasive particle, so that the abrasive particle is surface-treated. Even if the pH of the abrasive particle in a weakly acidic state is changed to an acidic state during the surface treatment process, a pH shock does not occur due to the pH change, and no clumping phenomenon occurs between particles.
[0036] Conventionally, the abrasive particles contained in a composition for semiconductor processing are dispersed in a strong alkaline solution, and the pH of the abrasive particles in the strong alkaline state can be changed to a strong acidic state by mixing and stirring with an acidic solution during the preparation of the composition for semiconductor processing. When the process of mixing and stirring with the acidic solution is carried out, the abrasive particles undergo a pH shock due to the sudden pH change, which can cause clumping between particles.
[0037] The acidic solution is specifically an organic acid, and examples of the organic acid include nitric acid, acetic acid, formic acid, benzoic acid, nicotinic acid, picolinic acid, alanine, phenylalanine, valine, leucine, isoleucine, arginine, aspartic acid, citric acid, adipic acid, succinic acid, oxalic acid, glycine, glutamic acid, glutaric acid, and phthalic acid. The organic acid may include one selected from the group consisting of nitric acid, histidine, threonine, serine, cysteine, methionine, asparagine, tyrosine, diiodotyrosine, tryptophan, proline, oxyproline, ethylenediaminetetraacetic acid (EDTA), nitrotriacetic acid (NTA), iminodiacetic acid (IDA), and combinations thereof. In one embodiment, the organic acid may be nitric acid or acetic acid, but is not limited to the above examples, and any organic acid that can maintain the abrasive particles in a stable dispersed state in the solution and adjust the pH to a strong acidity can be used without limitation.
[0038] Specifically, Fig. 3 shows the change in zeta potential of the polishing particles according to one embodiment of the present invention due to the change in pH, Fig. 4 shows the case where the polishing particles are in a stabilized state, and Fig. 5 shows the phenomenon of agglomeration between the polishing particles when the polishing particles are in an unstable state.
[0039] FIG. 3 shows the change in zeta potential of abrasive particles depending on the pH. The zeta potential value of abrasive particles 200 and 300 changes from a negative value to a positive value due to a change in pH (210, 220, 310, 320), and the zeta potential value can be further changed (230, 330) by surface modification of the abrasive particles.
[0040] More specifically, looking at the change in zeta potential of abrasive particles 200 dispersed in a weakly acidic solution, abrasive particles 210 dispersed in an initial weakly acidic solution can exhibit a negative zeta potential value, while abrasive particles 220 dispersed in a solution whose pH has changed to strongly acidic by mixing with an acidic solution can change their zeta potential to a positive value.
[0041] In addition, when looking at the change in the zeta potential value of the abrasive particles 300 dispersed in a strong alkaline solution, the abrasive particles 310 initially dispersed in a strong alkaline solution can exhibit a negative zeta potential value, while the abrasive particles 320, whose pH has changed to strongly acidic by mixing with an acidic solution during preparation of the polishing composition, can have their zeta potential change to a positive value.
[0042] At this time, when the abrasive particles 310 dispersed in the strong alkaline solution are mixed with the acidic solution, the pH shock requires a long reaction time and a long time for the abrasive particles to stabilize.
[0043] The abrasive particles being in a stabilized state may refer to a state in which a repulsive force acts between the particles to maintain a certain distance, as shown in FIG. 4, and the unstable state between the abrasive particles may refer to an aggregated state.
[0044] When abrasive particles dispersed in a strong alkaline solution are mixed with an acidic solution, a pH shock occurs due to a sudden change in pH, which may result in a clumping phenomenon as shown in Figure 5. That is, an aging process is required to stabilize the abrasive particles due to the pH shock generated in the abrasive particles, which requires an additional process to prepare a composition for semiconductor processing, and the overall process time may increase.
[0045] In contrast, if abrasive particles 200, 210 in a weakly acidic environment are used as in the present invention, there is little change in pH even when mixed with an acidic solution in the manufacturing process of a composition for semiconductor processing, so that a pH shock does not occur in the abrasive particles and a stable state can be maintained between the abrasive particles. If a polishing composition is manufactured in a state in which the abrasive particles maintain a stable state as shown in Figure 4, a separate aging process for the abrasive particles can be omitted.
[0046] The abrasive particles of the present invention are characterized in that when they are prepared into a semiconductor processing composition, a stable state is maintained between the abrasive particles and the size is uniform within a certain range. Specifically, a semiconductor processing composition diluted to an initial concentration of 4,000 particles / ml, a minimum size of 0.56 μm, and a maximum size of 20 μm is injected at 15 ml / min using an accusizer Fx Nano (PSSA Co.), and the number of particles over 5 μm may be about 100 to about 700, about 100 to about 500, about 100 to about 450, or about 100 to about 400. The number of particles over 3 μm may be about 100 to about 1,100, about 200 to about 1,000, about 300 to about 900, or about 400 to about 900. The number of particles exceeding 1 μm may be about 1,000 to about 3,400, about 1,200 to about 3,000, about 1,300 to about 2,800, or about 1,500 to about 2,500. As described above, the results of the LPC measurement show that the composition for semiconductor processing of the present invention contains abrasive particles having a small diameter, and when used in a polishing process, it can prevent the occurrence of defects such as defects on the surface of a semiconductor wafer.
[0047] As described above, the abrasive particles of the present invention are not affected by pH change in stability, and are characterized in that the zeta potential change rate, represented by the following formula 1, is 6 mV / pH to 30 mV / pH:
[0048] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0049] wherein p6 is pH 6 and p5 is pH 5; The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0050] The zeta potential change rate according to the formula 1 may be 6mV / pH to 30mV / pH, 14mV / pH to 24mV / pH, 14mV / pH to 19mV / pH, or 14.5mV / pH to 18.5mV / pH. When a polishing composition is prepared using abrasive particles having a zeta potential change rate within the above range, the pH change is small when mixed with an acidic solution, so that a pH shock does not occur in the abrasive particles and a stable state can be maintained between the abrasive particles, thereby improving the production efficiency of the polishing composition. In addition, since a stable state is maintained between the abrasive particles, no clumping phenomenon occurs, and thus defects can be prevented from occurring when applied to a polishing process.
[0051] The zeta potential change rate is determined by confirming the zeta potential change rate in a weakly acidic pH state, and when the abrasive particles for producing the polishing composition are dispersed in an initial weakly acidic solution and mixed with an acidic solution, the zeta potential change rate may be about 14 mV / pH to about 30 mV / pH when the pH is changed from 6 to 5.
[0052] In addition, when the pH of the polishing particles of the present invention is changed from 5 to 4, the zeta potential change rate may be about 10 mV / pH to about 55 mV / pH, about 15 mV / pH to about 48 mV / pH, or about 16 mV / pH to about 44 mV / pH. When the pH of the polishing particles of the present invention is changed from 4 to 3, the zeta potential change rate may be about 0 mV / pH to about 10 mV / pH, about 0.5 mV / pH to about 6 mV / pH, or about 0.5 mV / pH to about 5 mV / pH. When the pH of the polishing particles of the present invention is changed from 3 to 2, the zeta potential change rate may be about -5 mV / pH to about 10 mV / pH, about -3 mV / pH to about 8 mV / pH, or about 1 mV / pH to about 7 mV / pH. The zeta potential change rate of the abrasive particles of the present invention may be about -5mV / pH to about 10mV / pH, about -3mV / pH to about 8mV / pH, or about -2mV / pH to about 6mV / pH when the pH is changed from 2 to 1. If the zeta potential change rate is satisfied, the abrasive particles in the composition for semiconductor processing are contained in a stabilized state without causing agglomeration, and thus not only can the composition provide excellent polishing performance when applied to a polishing process, but also can prevent the occurrence of defects during the polishing process.
[0053] The abrasive particles of the present invention are characterized in that the zeta potential change rate, represented by the following formula 2, is 14 mV / pH to 40 mV / pH:
[0054] [Formula 2] Zeta potential change rate = |(Z6-Z4) / (p6-p4)|
[0055] wherein p6 is pH 6 and p4 is pH 4; The Z6 is the zeta potential at pH 6, and the Z4 is the zeta potential at pH 4.
[0056] The rate of change in zeta potential according to the formula 2 may be about 14mV / pH to about 40mV / pH, about 20mV / pH to 38mV / pH, or about 22mV / pH to about 35mV / pH. As described above, the abrasive particles of the present invention are provided in a weakly acidic state and are prepared into a composition for semiconductor processing, so that when the pH changes due to the supply of an organic acid in the weakly acidic state, the zeta potential of the abrasive particles can also change. According to FIG. 3, the weakly acidic abrasive particles 210 have a pH of 6, and when prepared into a composition for semiconductor processing, the pH can change to 4 (220). Due to the pH change, the abrasive particles exhibit a change in zeta potential value, and the occurrence of a pH shock is determined depending on the degree of the change in the zeta potential value. As shown in FIG. 3, when the range of the formula 2 is satisfied, it can be said that the abrasive particles do not exhibit a separate pH shock due to the pH change. In addition, by satisfying the above range, the abrasive particles in the composition for semiconductor processing are contained in a stabilized state without agglomeration, and thus not only can provide excellent polishing performance when applied to a polishing process, but also can prevent the occurrence of defects during the polishing process.
[0057] As described above, the abrasive particles of the present invention are characterized in that the zeta potential change rate, represented by the following formula 3, is 8 mV / pH to 20 mV / pH:
[0058] [Formula 3] Zeta potential change rate = |(Z6-Z1) / (p6-p1)|
[0059] wherein p6 is pH 6 and p1 is pH 1; The Z6 is the zeta potential at pH 6, and the Z1 is the zeta potential at pH 1.
[0060] The zeta potential change rate according to the formula 3 may be about 8mV / pH to about 20mV / pH, about 8mV / pH to 18mV / pH, or about 8mV / pH to about 16mV / pH. The formula 3 relates to the zeta potential change rate due to the state change of weakly acidic polishing particles to strongly acidic polishing particles, and when it satisfies the above range, it can mean that both the abrasive particles in the weakly acidic state and the abrasive particles in the strongly acidic state have excellent dispersibility. When the degree of change in the zeta potential value of the abrasive particles in the weakly acidic state and the zeta potential value of the abrasive particles in the strongly acidic state is shown as in the above range, the dispersibility of the abrasive particles in the semiconductor processing composition is excellent, no clumps are generated between the particles, and the abrasive particles can maintain a stable state as described above and have a uniform size within a certain range.
[0061] As described above, the abrasive particles of the present invention are characterized in that the zeta potential change rate, represented by the following formula 4, is 9.5 mV / pH to 20 mV / pH:
[0062] [Formula 4] Zeta potential change rate = |(Z6-Z2) / (p6-p2)|
[0063] wherein p6 is pH 6 and p2 is pH 2; The Z6 is the zeta potential at pH 6, and the Z2 is the zeta potential at pH 2.
[0064] The zeta potential change rate according to the formula 4 may be about 9.5mV / pH to about 20mV / pH, about 9.5mV / pH to 19mV / pH, or about 9.5mV / pH to about 18mV / pH. When the weakly acidic abrasive particles are prepared into a strongly acidic abrasive particle to prepare a polishing composition, if the zeta potential change is within the range of the formula 4, a shock due to a pH change does not occur, and a separate process for preventing particle clumping is not required, simplifying the manufacturing process and increasing production efficiency, and a composition for semiconductor processing containing the abrasive particles has an excellent polishing rate for the target film quality and can prevent defects, etc., when used in a polishing process.
[0065] In addition, as described above, the abrasive particles of the present invention may have a zeta potential change of about 31 mV to about 75 mV, about 35 mV to about 68 mV, or about 35 mV to about 65 mV due to a pH change from pH 6 to pH 4 during the process. As described above, the abrasive particles of the present invention are used to prepare a composition for semiconductor processing by changing the pH to a weakly acidic state of pH 4 using abrasive particles in a weakly acidic state of pH 6, and the zeta potential changes depending on the degree of the change in pH, and this can change within the above range. This means a zeta potential change that can prevent the occurrence of a pH shock due to a pH change of the abrasive particles during the process for preparing a composition for semiconductor processing, and even when the zeta potential changes due to a pH change within the above range, the abrasive particles do not undergo a shock, and when provided to a composition for semiconductor processing, they can exhibit excellent dispersibility, and when applied to a polishing process, they can provide excellent polishing performance and prevent the occurrence of defects during the polishing process.
[0066] Specifically, when applied to the chemical mechanical polishing of semiconductor wafers, the composition not only achieves excellent effects in terms of polishing flatness, but also minimizes the occurrence of defects. When applied to the polishing process of semiconductor wafers, the composition for semiconductor processing can exhibit significantly improved polishing performance for tungsten films and metal barrier films.
[0067] That is, the composition for semiconductor processing of the present invention can prevent the occurrence of defects on semiconductor wafers including tungsten films and metal barrier films, while at the same time achieving a desired level of polishing performance.
[0068] The polishing particles according to one embodiment of the present invention may include particles that have been surface-treated so that the zeta potential value of the polishing particles in the semiconductor processing composition is positive (+). Specifically, the polishing particles are surface-treated so that the zeta potential has a positive (+) zeta potential value when the pH is 4, and the zeta potential may be about 10 mV to about 50 mV, preferably about 15 mV to about 45 mV, and more preferably about 20 mV to about 40 mV.
[0069] The abrasive particles contained in the semiconductor processing composition of the present invention described above are characterized by being surface-treated to have a positive (+) zeta potential value, and this characteristic makes it possible to prevent the occurrence of defects.
[0070] As shown in FIG. 5, a composition for semiconductor processing containing abrasive particles that have been surface-treated to have a positive (+) zeta potential value has excellent adhesion efficiency with semiconductor wafers and can improve polishing performance. Specifically, the surface of a semiconductor wafer has a negative (-) zeta potential value. As described above, if the surface of a semiconductor wafer exhibits a negative zeta potential and abrasive particles having a positive zeta potential are used, the adhesion efficiency between the semiconductor wafer and the abrasive particles can be improved by electrostatic attraction. The improved adhesion efficiency makes it easier for chemical bonds to be formed, which facilitates mechanical wear and makes it easier to remove the target film.
[0071] In addition, the abrasive particles that have been surface-treated to have a positive zeta potential value can easily bond to a semiconductor wafer that exhibits a negative zeta potential through electrostatic attraction, but such a bond can easily come apart due to the pressure and rotation of the semiconductor wafer and the polishing pad.
[0072] In contrast, a semiconductor processing composition containing abrasive particles having a negative (-) zeta potential value may generate electrostatic repulsion with a semiconductor wafer having a negative zeta potential value, as shown in Fig. 6. Therefore, the abrasive particles shown in Fig. 6 are not attracted to the semiconductor wafer, and therefore mechanical wear may not easily occur or the target film may not easily be removed.
[0073] More specifically, the abrasive particles can include inorganic particles, and the inorganic particles can include particles that have been surface treated with at least one organic component.
[0074] In one embodiment, the at least one organic component for surface treatment of the inorganic particles may include, for example, one selected from the group consisting of amino silane, alkoxy silane, ethoxy silane, epoxy silane, and combinations thereof. The organic component may be an aminosilane, which may more specifically be selected from the group consisting of 3-aminopropyltriethoxysilane (APTES), 3-aminopropyltrimethoxysilane (APTMS), 3-glycidoxypropyltrimethoxysilane (GPTMS), 3-glycidoxypropylmethyldimethoxysilane (GPDMS), 3-aminopropylmethyldiethoxysilane (APDES), 3-mercaptopropyltrimethoxysilane (MrPTMS), 3-mercaptopropyltrimethyldimethoxysilane (MrPDMS), 3-methacryloxypropyltrimethoxysilane (MPTMS), 3-methacryloxypropylmethyldimethoxysilane (MPDMS), and mixtures thereof.
[0075] In one embodiment, the inorganic particles include silica (Silica, SiO2), and at least one organic component applied to the surface treatment of the inorganic particles can include aminosilane or epoxysilane. The abrasive particles dispersed in the acidic solution are characterized by having a positive zeta potential value. As a result, the surface is easily adsorbed to the surface of a semiconductor wafer that exhibits a negative zeta potential, and mechanical wear is easy, which can increase the polishing rate for the target film quality.
[0076] The abrasive particles of the present invention contain about 0.01 parts by weight to about 1 part by weight of an organic component and about 0.01 parts by weight to about 1 part by weight of an organic acid, preferably about 0.05 parts by weight to about 0.8 parts by weight of an organic component and about 0.05 parts by weight to about 0.8 parts by weight of an organic acid, more preferably about 0.1 parts by weight to about 0.8 parts by weight of an organic component and about 0.05 parts by weight to about 0.5 parts by weight of an organic acid, relative to 100 parts by weight of the abrasive particles, in order to perform surface treatment with an organic component. By including the above range, the dispersibility is improved when adjusting the pH of the abrasive particles, and the abrasive particles can exhibit a positive zeta potential, and after preparing a composition for semiconductor processing, the polishing performance can be improved when applied to the manufacturing process of semiconductor devices, and the occurrence of defects such as defects can be prevented.
[0077] In other embodiments, the abrasive particles may include organic / inorganic composite particles, which may be, for example, particles having a core-shell structure consisting of a core including a polymeric resin; and a shell including an inorganic component disposed on the surface of the core.
[0078] The core of the organic / inorganic composite particle may include a polymer resin, such as polymethylmethacrylate (PMMA) resin, polystyrene (PS) resin, etc. The inorganic component of the shell may include, for example, silica, silica (SiO2), ceria (CeO2), alumina (Al2O3), titania (TiO2), zirconia (ZrO2), germania (GeO2), etc.
[0079] The particles contained in the abrasive may have an average particle size (D50) of, for example, about 5 nm to about 150 nm, for example, about 5 nm to about 100 nm, for example, about 5 nm to about 80 nm, for example, about 10 nm to about 80 nm, for example, about 30 nm to about 50 nm, for example, about 30 nm to about 45 nm, for example, about 34 nm to about 44 nm. By using abrasive particles of such a size, the semiconductor processing composition may be more advantageous in satisfying the condition of the formula 1.
[0080] For example, the abrasive particles may have a particle distribution having a 10% cumulative mass particle size distribution diameter (D10) of about 5 nm to about 50 nm, such as about 5 nm to about 35 nm, for example, about 10 nm to about 35 nm, for example, about 20 nm to about 35 nm, for example, about 23 nm to about 33 nm.
[0081] For example, the abrasive particles may have a particle distribution with a 90% cumulative mass particle size distribution diameter (D90) of about 40 nm to about 150 nm, such as about 40 nm to about 100 nm, for example, about 45 nm to about 80 nm, for example, about 45 nm to about 65 nm, for example, 50 nm to about 60 nm.
[0082] For example, the abrasive particles may have a particle distribution in which the 10% cumulative mass particle size distribution diameter (D10) is about 23 nm to about 33 nm, the 50% cumulative mass particle size distribution diameter (D50) is about 34 nm to about 44 nm, and the 90% cumulative mass particle size distribution diameter (D90) is about 50 nm to about 60 nm.
[0083] The abrasive particles may satisfy the condition of 1.10≦D90 / D50≦1.80, for example, 1.50≦D90 / D10≦2.70, for example, 1.00≦D50 / D10≦2.00, in terms of particle distribution. By using abrasive particles having such a particle distribution, it may be more advantageous for the semiconductor processing composition to satisfy the value of Equation 1 within a predetermined range, and it may be more advantageous to calculate a corresponding excellent polishing result.
[0084] The method for measuring the particle size distribution of the abrasive particles is not particularly limited, and the particle size distribution can be determined using any general-purpose device used in the art for particle size analysis of nano (nm) size level particle powders.
[0085] The composition for semiconductor processing may contain at least one additive in addition to the above-described abrasive particles. The at least one additive may play a role in adjusting the surface state of the object to be polished to be suitable for polishing mainly through a chemical reaction.
[0086] The at least one additive may include, for example, an organic acid. The organic acid may function as a complexing agent that traps metal ions such as tungsten ions. The complexing agent functions to chelate the metal oxide oxidized by the oxidizing agent. That is, the complexing agent may inhibit the metal oxide oxidized by the chelation reaction with the metal oxide from being re-adsorbed onto the metal film layer of the polishing target layer, thereby increasing the polishing speed for the metal film and reducing surface defects. For example, the organic acid may be acetic acid, formic acid, benzoic acid, nicotinic acid, picolinic acid, alanine, phenylalanine, valine, leucine, isoleucine, arginine, aspartic acid, citric acid, adipic acid, succinic acid, oxalic acid, glycine, glutamic acid, glutaric acid, phthalic acid, or the like. The organic acid may include one selected from the group consisting of glycine, histidine, threonine, serine, cysteine, methionine, asparagine, tyrosine, diiodotyrosine, tryptophan, proline, oxyproline, ethylenediaminetetraacetic acid (EDTA), nitrotriacetic acid (NTA), iminodiacetic acid (IDA), and combinations thereof. In one embodiment, the organic acid may include glycine.
[0087] The at least one additive may include, for example, a polyol. The polyol may suppress the occurrence of defects such as the adsorption of abrasive particles to the polished surface or scratches, and may improve the dispersibility in the composition for semiconductor processing. For example, the polyol may include one selected from the group consisting of polyvinyl alcohol, cellulose, sorbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, glycerin monomethyl ether, glycerin dimethyl ether, glycerin diethyl ether, glycerin triethyl ether, and combinations thereof. In one embodiment, the polyol may include sorbitol.
[0088] The at least one additive may be a fluorosurfactant. By including the fluorosurfactant, the composition for semiconductor processing can effectively prevent excessive adsorption of the abrasive particles to the surface to be polished before and / or during the application of the composition for semiconductor processing to the polishing process. In addition, by including fluorine, the composition for semiconductor processing can prevent the proliferation of bacteria and mold, and can improve long-term storage stability.
[0089] Specifically, the surfactant of the present invention is BNO-BS-BOH from BNOCHEM, tm The polishing agent may be selected from the group consisting of FS-30, FS-31, FS-34, ET-3015, ET-3150, ET-3050, Capstone FS-3100, and mixtures thereof, but is not particularly limited as long as it plays a role in preventing carbon residues from being excessively adsorbed on the surface of the semiconductor substrate during the polishing process.
[0090] The surfactant of the present invention may be a surfactant containing a nonionic fluorine-based polymer compound, which may be used alone as a nonionic surfactant, or may be used in combination with other nonionic surfactants.
[0091] The nonionic surfactants include polyethylene glycol, polypropylene glycol, polyethylene-propylene copolymer, polyalkyl oxide, polyoxyethylene oxide (PEO), polyethylene oxide, and polypropylene oxide. The fluorosurfactants include sodium sulfonate fluorosurfactant, phosphate ester fluorosurfactant, amine oxide fluorosurfactant, betaine fluorosurfactant, ammonium carboxylate fluorosurfactant, stearate ester fluorosurfactant, quaternary ammonium fluorosurfactant, ethylene oxide / propylene oxide fluorosurfactant, and polyoxyethylene fluorosurfactant. fluorosurfactants).
[0092] The at least one additive may further include a pH adjuster. The pH adjuster may include, for example, one selected from the group consisting of hydrochloric acid (HCl), phosphoric acid (H3PO4), sulfuric acid (H2SO4), nitric acid (HNO3), ammonium hydroxide (NH4OH), potassium hydroxide (KOH), sodium hydroxide (NaOH), and combinations thereof. When the at least one additive includes a pH adjuster, it may be included in an amount of about 0.01 wt % to about 5 wt % based on the weight of the entire semiconductor processing composition.
[0093] The composition for semiconductor processing may contain a solvent other than the above-mentioned components. The solvent may be, for example, water (H2O), and more specifically, ultrapure water may be used.
[0094] The composition for semiconductor processing contains about 1% by weight to 10% by weight of abrasive particles, about 0.5% by weight to about 5% by weight of polyol, about 0.01% by weight to 1% by weight of organic acid, and the remaining solvent, preferably about 1% by weight to 8% by weight of abrasive particles, about 0.5% by weight to about 4% by weight of polyol, about 0.01% by weight to 0.8% by weight of organic acid, and the remaining solvent, more preferably about 1% by weight to 5% by weight of abrasive particles, about 1% by weight to about 4% by weight of polyol, about 0.05% by weight to 0.8% by weight of organic acid, and the remaining solvent. When contained within the above range, it is possible to prevent the abrasive particles from being adsorbed on the polished surface, prevent the occurrence of defects, and is more advantageous in realizing the polishing speed, the dispersion stability of the composition for semiconductor processing, and excellent flatness on the polished surface.
[0095] The composition for semiconductor processing may have a solid content of about 5% by weight to about 20% by weight. If the solid content is too low, the polishing rate for silicon oxide film may not be sufficiently ensured, and if the solid content is too high, defects may occur due to aggregation of the abrasive particles. That is, if the composition for semiconductor processing contains each of the above-mentioned components and the solvent and satisfies the above range of solid content, it may be advantageous to inject the composition for semiconductor processing at a uniform flow rate when applied to a polishing process, and it may be advantageous to ensure uniform dispersion and storage stability during distribution and storage of the composition for semiconductor processing.
[0096] In another embodiment of the present invention, a method for producing a composition for semiconductor processing includes the steps of adding an acidic solution to abrasive particles having a pH of 6 and a zeta potential of -50 mV to -10 mV to adjust the pH to 2 to 4, and stirring the abrasive particles whose pH has been adjusted, and adding an organic component and an organic acid to the abrasive particles. The abrasive particles may have a zeta potential change rate of 6 mV / pH to 30 mV / pH, as represented by the following formula 1:
[0097] [Formula 1]
[0098] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0099] wherein p6 is pH 6 and p5 is pH 5;
[0100] The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0101] In order to prepare the composition for semiconductor processing of the present invention, abrasive particles dispersed in a weakly acidic solution are used as described above. The abrasive particles may have a zeta potential of about -50mV to about -10mV, about -40mV to about -12mV, about -35mV to about -19mV, or about -20.5mV to about -30mV at a weakly acidic pH of 6. Abrasive particles having a zeta potential value within the above range can be prepared into a polishing composition in a stabilized state without pH shock of the abrasive particles even if the pH changes due to mixing with an acidic solution.
[0102] Specifically, the zeta potential change rate according to the formula 1 may be 6mV / pH to 30mV / pH, 14mV / pH to 24mV / pH, 14mV / pH to 19mV / pH, or 14.5mV / pH to 18.5mV / pH. As described above, the value of formula 1 satisfies the range of the present invention, which means that the stable state between the abrasive particles is maintained even when mixed with an acidic solution, and when it is within the range, there is little change in pH even when mixed with an acidic solution in the manufacturing process of the polishing composition, so that no pH shock occurs in the abrasive particles, and the stable state between the abrasive particles can be maintained, thereby improving the manufacturing efficiency of the polishing composition. In addition, since the stable state is maintained between the abrasive particles, no clumping phenomenon occurs, and therefore, when applied to the polishing process, the occurrence of defects can be prevented.
[0103] The abrasive particles are subjected to a stirring process, and at the same time, an organic acid is added to lower the pH to a strong acidity of 2 to 4. Thereafter, the stirring process is continued, and an organic component and an organic acid are added so that the organic component can be bonded to the surface of the abrasive particles.
[0104] In order to maintain the stabilized state between the abrasive particles and to bond the organic component to the surface of the particles, the stirring step is carried out at a speed of 1,500 rpm to 2,000 rpm, preferably 1,600 rpm to 1,900 rpm, and more preferably 1,600 rpm to 1,800 rpm. By carrying out the stirring step rapidly within the above range, the stabilized state between the particles can be maintained by the zeta potential of the abrasive particles, and the organic component can be easily bonded to the surface of the particles. In addition, as described above, the stabilized state between the abrasive particles can be maintained, thereby exhibiting excellent dispersion characteristics.
[0105] The abrasive particles having the amine-based surface binder bonded thereto are separated through an ion exchange membrane, and the separated abrasive particles having the amine-based surface binder bonded thereto can be manufactured into a composition for semiconductor processing.
[0106] The abrasive particles can be mixed with at least one additive to prepare a composition for semiconductor processing. The at least one additive can adjust the surface condition of the object to be polished to be suitable for polishing mainly through a chemical reaction.
[0107] The one or more additives may include an organic acid, a polyol, a fluorosurfactant, and a solvent, as described above, and may further include a pH adjuster, an azole compound, a phosphoric acid compound, etc.
[0108] The above-mentioned description of the additives can be equally applied to the method for manufacturing a composition for semiconductor processing.
[0109] In another embodiment of the present invention, a method for manufacturing a semiconductor device includes the steps of: preparing a platen having a polishing pad with a polishing surface attached thereto; preparing a carrier containing an object to be polished; rotating the platen and the carrier while rotating the platen and the carrier in a state in which the polishing surface of the polishing pad and the surface to be polished of the object to be polished are arranged to be in contact with each other; and supplying a composition for semiconductor processing onto the polishing surface, the polishing composition for semiconductor processing including abrasive particles; and at least one additive, the abrasive particles may have a zeta potential change rate of 6 mV / pH to 30 mV / pH, as represented by the following formula 1:
[0110] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0111] wherein p6 is pH 6 and p5 is pH 5; The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0112] All matters relating to the composition for semiconductor processing and formula 1 are the same as those described above for the composition for semiconductor processing.
[0113] 2 is a schematic diagram illustrating a configuration of a method for manufacturing a semiconductor device according to an embodiment of the present invention. Referring to FIG. 2, the method for manufacturing a semiconductor device may include a step of preparing a platen 120 on which a polishing pad 110 having a polishing surface is mounted, and a step of preparing a carrier 160 containing a polishing target 130.
[0114] In the method for manufacturing a semiconductor device, the polishing target 130 may be a semiconductor wafer having a structure as shown in Fig. 1. Specifically, a SiO2 oxide film, which is an interlayer insulating film, is formed on a silicon substrate, and the SiO2 oxide film is etched to form contact holes.
[0115] Next, a metal barrier film such as Ti / TiN (adhesion layer / diffusion prevention layer) is formed on the entire surface of the substrate including the contact hole, and a tungsten (W) film is deposited on the top so that the contact hole is completely filled in. Then, the tungsten film and the metal barrier film on the SiO2 oxide film are polished using a semiconductor processing composition in a chemical mechanical polishing process to form a tungsten plug.
[0116] The composition for semiconductor processing of the present invention is applied to the polishing process to polish the tungsten film and the metal barrier film on the SiO2 oxide film to form a tungsten plug, and has excellent polishing performance for the tungsten film and the metal barrier film, and can minimize the occurrence of defects.
[0117] 1 and 2, the polishing target 130 may be a semiconductor wafer having a tungsten film 40 and a metal barrier film 30, and the semiconductor wafer may include a substrate 10, a SiO2 oxide film 20, a metal barrier film 30 such as Ti / TiN (adhesion layer / diffusion barrier layer) on the SiO2 oxide film, and a tungsten film 40 on the metal barrier film. The SiO2 oxide film 20 is formed on the substrate 10 to a thickness of 1,000 to 2,000 Å, and the SiO2 oxide film 20 is etched to form contact holes.
[0118] Referring to FIG. 2, the method for manufacturing the semiconductor device may include a step of rotating the platen 120 and the carrier 160 while positioning the polishing surface of the polishing pad 110 and the polished surface of the object to be polished 130 in contact with each other.
[0119] The polishing pad 110 is mounted on the platen 120 with its polishing surface at the top, and the polished object 130 is accommodated in the carrier 160 with its surface to be polished at the bottom, so that the polishing surface and the surface to be polished are arranged to abut against each other. The abutment of the polishing surface and the surface to be polished is interpreted to include not only a case where they are in direct physical contact, but also a case where they are indirectly contacted via the abrasive particles in the semiconductor processing composition.
[0120] As the platen 120 rotates, the polishing pad 110 also rotates at substantially the same trajectory and speed, and as the carrier 160 rotates, the polishing target 130 also rotates at substantially the same trajectory and speed. The platen 120 and the carrier 160 may rotate in the same direction as each other, or in different directions.
[0121] In one embodiment of the present invention, the rotation speed of the platen 120 and the carrier 160 may be about 10 rpm to about 500 rpm, for example, about 30 rpm to about 200 rpm. When the platen 120 and the carrier 160 rotate at a rotation speed within the above range, the friction behavior of the polishing surface and the surface to be polished due to the centrifugal force is mutually linked with the composition for semiconductor processing supplied onto the polishing surface, so that the polishing flatness of the surface to be polished is ensured.
[0122] In one embodiment of the present invention, the rotation speed of the carrier 160 is higher than the rotation speed of the platen 120. By rotating the carrier 160 at a higher speed than the platen 120, it may be advantageous for ensuring polishing stability and for the polished surface of the polishing object 130 to be polished without defects.
[0123] In one embodiment of the present invention, the method for manufacturing semiconductor devices can rotate the platen 120 and the carrier 160 and rotate them under pressure conditions against the polishing surface of the carrier 160. By pressing the carrier 160 against the polishing surface under a predetermined pressure condition, excellent polishing performance can be achieved both when the surface to be polished of the object to be polished 130 is directly contact-polished with the polishing surface of the polishing pad 110 and when the surface is indirectly contact-polished with the composition for semiconductor processing 150 interposed therebetween. For example, the load with which the carrier 160 is pressed against the polishing surface may be about 0.01 psi to about 20 psi, for example, about 0.1 psi to about 15 psi.
[0124] 2, the method for manufacturing a semiconductor device may further include a step of supplying a semiconductor processing composition 150 onto the polishing surface. More specifically, the semiconductor processing composition 150 is supplied onto the polishing surface through a supply nozzle 140.
[0125] In one embodiment of the present invention, the flow rate of the semiconductor process composition 150 sprayed through the supply nozzle 140 may be about 10 mL / min to about 1,000 mL / min, for example, about 10 mL / min to about 800 mL / min, for example, about 50 mL / min to about 500 mL / min. When the semiconductor process composition 150 is supplied onto the polishing surface at a flow rate within the above range, the friction behavior between the polishing surface and the polished surface with the composition interposed therebetween may be more advantageous in improving the polishing performance of the polished surface. More specifically, the polishing performance is excellent in the polishing result for the polishing surface including the tungsten film and the metal barrier film depending on the structure of the semiconductor wafer, and the occurrence of defects such as defects can be prevented.
[0126] The composition for semiconductor processing may include abrasive particles; and at least one additive, and the matters related to the abrasive particles and the at least one additive are the same as those described for the composition for semiconductor processing. That is, all the specific examples and technical advantages of the abrasive particles and the at least one additive described above for the composition for semiconductor processing can be integrated and applied to the composition for semiconductor processing applied to the semiconductor manufacturing method, and can have advantageous interactions in terms of achieving technical objectives in relation to other configurations of the semiconductor manufacturing method, such as the structure and drive of the platen and the carrier.
[0127] Referring to FIG. 2, in one embodiment, the method for manufacturing a semiconductor device may further include a step of processing the polishing surface of the polishing pad 110 through a conditioner 170. The polishing surface of the polishing pad 110 is chemically affected as the semiconductor process composition 150 is continuously supplied, and at the same time, is physically affected by physical contact with the surface to be polished of the object to be polished 130. If the state of the polishing surface is deformed by such chemical / physical effects, it may be difficult to uniformly maintain the polishing performance for the surface to be polished. The step of processing the polishing surface through the conditioner 170 may contribute to the polishing surface constantly maintaining a state suitable for polishing.
[0128] For example, the conditioner 170 may roughen the polishing surface while rotating at a predetermined speed. The rotation speed of the conditioner 170 may be, for example, about 10 rpm to about 500 rpm, for example, about 50 rpm to about 500 rpm, for example, about 100 rpm to about 500 rpm, for example, about 200 rpm to about 500 rpm, for example, more than about 200 rpm and less than about 400 rpm.
[0129] The conditioner 170 can rotate while being pressed at a predetermined pressure against the polishing surface of the polishing pad 110. For example, the pressure of the conditioner 170 against the polishing surface may be about 1 psi to about 20 psi, for example, about 1 psi to about 15 psi, for example, about 5 psi to about 15 psi, for example, about 5 psi to about 10 psi.
[0130] By performing surface treatment using the conditioner 170 under the above-mentioned process conditions, the polishing surface can maintain an optimal surface condition throughout the polishing process, and the polishing life can be extended under the application conditions of the semiconductor processing composition 150.
[0131] Specific examples of the present invention are presented below. However, the examples described below are merely intended to specifically illustrate or explain the present invention, and should not be construed as limiting the scope of the present invention, which is defined by the claims.
[0132] Manufacturing Example 1 Production of abrasive particles (Example 1) Weakly acidic colloidal silica can be produced by using water glass as a precursor and KOH as a catalyst. Specifically, KOH was added to water glass to adjust the pH to a basic condition of 10. Under the basic condition, SiO was formed to form seeds, which then grew into particles. Then, a small amount of nitric acid was added, and unnecessary metal ions were removed using deionization as an ion exchange resin to produce weakly acidic colloidal silica. The weakly acidic colloidal silica had a pH of 6, a zeta potential of -24 mV, and an average particle size (D50) of 41 nm.
[0133] While stirring the weakly acidic colloidal silica at 1,700 rpm, acetic acid and aminosilane 3-aminopropyltriethoxysilane (APTES) were added little by little at a rate of 100 ml / min to prepare a weakly acidic surface-modified colloidal silica having a pH of 3.8.
[0134] Examples 2 to 3 Weakly acidic surface-modified colloidal silica was produced according to Production Example 1, except that the amounts of the weakly acidic colloidal silica, aminosilane, and acetic acid were as shown in Table 1 below.
[0135] Comparative Example 1 A strongly basic colloidal silica having a pH of 9 and a zeta potential of -52 mV was prepared. The strongly basic colloidal silica was stirred at 1,700 rpm, and nitric acid was added to produce a strongly acidic colloidal silica having a pH of 2.3. The acetic acid was rapidly added at 50 ml / sec.
[0136] The strongly acidic colloidal silica was stirred at 1,700 rpm, and aminosilane 3-aminopropyltriethoxysilane (APTES) and nitric acid were added little by little to prepare a surface-modified colloidal silica.
[0137] Comparative Example 2 The same preparation as in Comparative Example 1 was carried out, except that when adding acetic acid to the strong base colloidal silica, the addition rate was maintained at 1 ml / sec.
[0138] Comparative Example 3 Colloidal silica was prepared by dispersing it in a neutral solution having a pH of 6 and a zeta potential of -12 mV. The neutral colloidal silica was stirred at high speed, and in this state, nitric acid was added to the neutral colloidal silica to produce strongly acidic colloidal silica having a pH of 2.3.
[0139] The strongly acidic colloidal silica was stirred at high speed, and aminosilane 3-aminopropyltriethoxysilane (APTES) and nitric acid were gradually added to the strongly acidic colloidal silica while stirring at high speed, to prepare a surface-modified colloidal silica.
[0140] Comparative Example 4 Colloidal silica was prepared by dispersing it in a strong base solution having a pH of 9 and a zeta potential of -52 mV. The neutral colloidal silica was stirred at 1,700 rpm, and nitric acid was added thereto to produce strongly acidic colloidal silica having a pH of 2.3.
[0141] The strongly acidic colloidal silica was stirred at 1,700 rpm, and aminosilane 3-aminopropyltriethoxysilane (APTES) and nitric acid were added little by little to prepare a surface-modified colloidal silica.
[0142] The zeta potential values according to the contents of the components and pH for producing the surface-modified colloidal silica of the examples and comparative examples are shown in Table 1. The value according to the following formula 1 was also derived from the measured zeta potential values.
[0143] [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)|
[0144] wherein p6 is pH 6 and p5 is pH 5; The Z6 is the zeta potential at pH 6, and the Z5 is the zeta potential at pH 5.
[0145] Using the same method as in Equation 1, values for Equations 2 to 4 were also derived as follows.
[0146] [Formula 2] Zeta potential change rate = |(Z6-Z4) / (p6-p4)|
[0147] wherein p6 is pH 6 and p4 is pH 4; The Z6 is the zeta potential at pH 6, and the Z4 is the zeta potential at pH 4.
[0148] [Formula 3] Zeta potential change rate = |(Z6-Z1) / (p6-p1)|
[0149] wherein p6 is pH 6 and p1 is pH 1; The Z6 is the zeta potential at pH 6, and the Z1 is the zeta potential at pH 1.
[0150] [Formula 4] Zeta potential change rate = |(Z6-Z2) / (p6-p2)|
[0151] wherein p6 is pH 6 and p2 is pH 2; The Z6 is the zeta potential at pH 6, and the Z2 is the zeta potential at pH 2.
[0152] The following zeta potential change rates were calculated using the formula 1. Specifically, the change rates of 1 to 2 were calculated as (zeta potential at pH 1 - zeta potential at pH 2) / (pH2-pH1), and other values were calculated using the same formula.
[0153] JPEG0007572470000001.jpg150163
[0154] Manufacturing Example 2 Manufacture of compositions for semiconductor processing The abrasive particles prepared in Example 1 to Comparative Example 6 were mixed with glycine (Glycine, Yunwoo Chemical Co., A3-10), sorbitol (Sorbitol, Yunwoo Chemical Co., GC-30) and a fluorosurfactant (Chemours, FS-30). Specifically, 3 wt% of the abrasive particles, 0.1 wt% of glycine, 2 wt% of sorbitol solution, 0.0025 wt% of the fluorosurfactant, and the remaining ultrapure water solvent were mixed to prepare a composition for semiconductor processing.
[0155] Experimental Method (1) LPC measurement Each sample was prepared in 100 ml portions and aged for 2 hours to remove bubbles. Before measuring the samples, the entire line of the device was washed with ultrapure water. Using the device and conditions below, the diluted samples were measured five or more times and the average value was calculated.
[0156] Device name: accusizer Fx Nano (PSSA) Flow rate: 15ml / min Number of channels: 32 Light Extinction collection time: 60 seconds Initial concentration: 4000 pieces / ml Minimum size: 0.56μm Maximum size: 20μm
[0157] (2) Defect measurement Referring to FIG. 1, a wafer was prepared, which includes an SiO2 oxide film as an interlayer insulating film on a silicon substrate 10, a contact hole formed by etching the interlayer insulating film, a metal barrier film 30 such as Ti / TiN (adhesive layer / diffusion prevention layer) on the entire surface of the substrate including the contact hole, and a tungsten (W) film formed on the upper part so that the contact hole is completely filled. As shown in FIG. 2, the patterned wafer was placed in a carrier 160 as a polishing target 130 so that the polished surface faces downward. The carrier 160 was positioned so that the polished surface faces upward and the polishing surface abutted against a platen 120 on which a polishing pad 110 was mounted, and then the carrier 160 was operated for 60 seconds at a pressure of 3.0 psi on the polishing surface, a rotation speed of 93 rpm for the carrier 160, and a rotation speed of 87 rpm for the platen 120, and the polishing was performed while applying the semiconductor process composition of each of the examples and the comparative examples to the polishing surface at a flow rate of 300 ml / min. After polishing, a cleaning process was carried out by spraying cleaning solution at 2,000cc / min for 60 seconds with a brush rotation speed of 500rpm. The pattern wafer after the cleaning process was sealed in a wafer foup and the total defect count was measured using an AIT-XP+ device owned by SKC. The thickness after polishing under the above polishing conditions was measured to calculate the polishing rate (Å / min).
[0158] JPEG0007572470000002.jpg86163
[0159] The large difference in the number of defects can be compared with the results of LPC analysis. Example 1 had 284 particles over 5 μm and 630 particles over 3 μm, Example 2 had 143 particles over 5 μm and 423 particles over 3 μm, and Example 3 had 344 particles over 5 μm and 821 particles over 3 μm, whereas Comparative Example 1 had 724 particles over 5 μm and 2,423 particles over 3 μm, Comparative Example 2 had 435 particles over 5 μm and 1,872 particles over 3 μm, Comparative Example 3 had 921 particles over 5 μm and 3,114 particles over 3 μm, and Comparative Example 4 had 587 particles over 5 μm and 1,142 particles over 3 μm, showing a large difference in particle size.
[0160] In addition, the polishing rates of the oxide film were measured to be 1,824 Å / min in Example 1, 1,632 Å / min in Example 2, and 1,845 Å / min in Example 3. In the cases of Comparative Examples 1 to 4, the polishing rates were 1,823 Å / min, 1,722 Å / min, 1,813 Å / min, and 1,532 Å / min, respectively, confirming no significant difference.
[0161] This means that, compared to the abrasive particles contained in conventional semiconductor processing compositions, the semiconductor processing composition containing the abrasive particles of the present invention has the same or better polishing performance and can reduce the occurrence of defects and other imperfections.
[0162] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention. [Explanation of symbols]
[0163] 10: Substrate 20: SiO2 oxide film 30: Metal barrier film 40: Tungsten film D1: Via diameter D2: diameter of the conductor charging electrode T1: Thickness of the second silicon nitride film 21: First silicon nitride film 22: Second silicon nitride film 110: Polishing pad 120: Fixed plate 130: Polishing target 140: Supply nozzle 150: Composition for semiconductor processing 160: Career 170: Conditioner 200: Change in zeta potential of colloidal silica dispersed in weakly acidic solution 210: Colloidal silica dispersed in weakly acidic solution 220: Colloidal silica dispersed in a strongly acidic solution 230: Surface-modified colloidal silica dispersed in a strongly acidic solution 300: Change in zeta potential of colloidal silica dispersed in strong base solution 310: Colloidal silica dispersed in a strong base solution 320: Colloidal silica dispersed in a strongly acidic solution 330: Surface-modified colloidal silica dispersed in a strongly acidic solution 400: Abrasive particles that have been surface-treated to have a positive (+) zeta potential value 410: Abrasive particles that have been surface-treated to have a negative zeta potential value
Claims
1. Contains abrasive particles, The abrasive particles have a zeta potential of -50 mV to -10 mV at pH 6, a zeta potential change rate represented by the following formula 1 of 14 mV / pH to 19 mV / pH, and a zeta potential change rate represented by the following formula 2 of 16.5 mV / pH to 40 mV / pH. Semiconductor processing compositions: [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)| [Formula 2] Zeta potential change rate = |(Z6-Z4) / (p6-p4)| wherein p6 is pH 6, p5 is pH 5, and p4 is pH 4; The Z6 is the zeta potential at pH 6, the Z5 is the zeta potential at pH 5, and the Z4 is the zeta potential at pH 4.
2. The abrasive particles are surface-treated to have a positive (+) zeta potential value when the pH is between pH 2 and pH 4. The composition for semiconductor processing according to claim 1 .
3. The abrasive particles have a zeta potential of 10 mV to 50 mV. The composition for semiconductor processing according to claim 2 .
4. The abrasive particles are silica (SiO 2 ), Ceria (CeO 2 ), Alumina (Alumina, Al 2 O 3 ), zirconia (ZrO 2 ), and combinations thereof; The composition for semiconductor processing according to claim 1 .
5. The composition for semiconductor processing further comprises at least one additive selected from the group consisting of an organic acid, a polyol, a surfactant, and a combination thereof; The composition for semiconductor processing according to claim 1 .
6. adding an acidic solution to abrasive particles having a pH of 6 and a zeta potential of −50 mV to −10 mV to adjust the pH to 2 to 4; agitating the pH-adjusted abrasive particles and adding an organic component and an organic acid to the abrasive particles; The abrasive particles have a zeta potential change rate represented by the following formula 1 of 14 mV / pH to 19 mV / pH, and a zeta potential change rate represented by the following formula 2 of 16.5 mV / pH to 40 mV / pH. Method for producing a composition for semiconductor processing: [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)| [Formula 2] Zeta potential change rate = |(Z6-Z4) / (p6-p4)| wherein p6 is pH 6, p5 is pH 5, and p4 is pH 4; The Z6 is the zeta potential at pH 6, the Z5 is the zeta potential at pH 5, and the Z4 is the zeta potential at pH 4.
7. The abrasive particles are stirred at 1,500 rpm to 2,000 rpm; A method for producing the composition for semiconductor processing according to claim 6.
8. The organic component is selected from the group consisting of amino silane, alkoxy silane, ethoxy silane, epoxy silane, and combinations thereof; A method for producing the composition for semiconductor processing according to claim 6.
9. The organic acids include nitric acid, acetic acid, formic acid, benzoic acid, nicotinic acid, picolinic acid, alanine, phenylalanine, valine, leucine, isoleucine, arginine, aspartic acid, citric acid, adipic acid, succinic acid, and oxalic acid. acid, glycine, glutamic acid, glutaric acid, phthalic acid, histidine, threonine, serine, cysteine, methionine, asparagine, tyrosine, diiodotyrosine, tryptophan, proline, oxyproline, ethylenediaminetetraacetic acid (EDTA), nitrotriacetic acid (NTA), iminodiacetic acid (IDA), and combinations thereof; A method for producing the composition for semiconductor processing according to claim 6.
10. A step of preparing a platen on which a polishing pad having a polishing surface is attached; Providing a carrier containing an object to be polished; rotating the platen and the carrier while the polishing surface of the polishing pad and the surface to be polished of the object to be polished are in contact with each other; providing a semiconductor processing composition on the polishing surface; The semiconductor processing composition comprises abrasive particles; and at least one additive, The abrasive particles have a zeta potential of -50 mV to -10 mV at pH 6, a zeta potential change rate represented by the following formula 1 of 14 mV / pH to 19 mV / pH, and a zeta potential change rate represented by the following formula 2 of 16.5 mV / pH to 40 mV / pH. Manufacturing method of semiconductor device: [Formula 1] Zeta potential change rate (mV / pH) = |(Z6-Z5) / (p6-p5)| [Formula 2] Zeta potential change rate = |(Z6-Z4) / (p6-p4)| wherein p6 is pH 6, p5 is pH 5, and p4 is pH 4; The Z6 is the zeta potential at pH 6, the Z5 is the zeta potential at pH 5, and the Z4 is the zeta potential at pH 4.
Citation Information
Patent Citations
Method for producing modified colloidal silica
JP2005162533A
Integrated chemical-mechanical polishing composition and process for single-platen processing