EUV Pellicle
A pellicle with a ruthenium oxysilicide layer anchors the metal layer to a silicon substrate, preventing dewetting and maintaining high EUV transmission, thus enhancing the pellicle's stability and throughput in EUV lithography.
Patent Information
- Application Number
- JP2023060543
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-03-29
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2038-11-06
AI Technical Summary
Existing pellicles in lithographic apparatuses, particularly those used in EUV lithography, suffer from thermal instability and dewetting issues due to metal films, leading to reduced EUV transmission and pellicle failure, which affects manufacturing throughput and pattern quality.
A pellicle design incorporating a metal oxysilicide layer, such as ruthenium oxysilicide, is used to anchor the metal layer to a silicon substrate, preventing dewetting and maintaining high EUV transmission by enhancing thermal emissivity.
The pellicle design significantly extends the pellicle's lifetime and maintains high EUV transmission, allowing for increased throughput and improved pattern quality by stabilizing the metal layer against dewetting.
Smart Images

Figure 0007572492000001
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS)
[0001] This application claims priority to European Application No. 17201126.4 filed November 10, 2017, and European Application No. 18165122.5 filed March 29, 2018, which applications are incorporated by reference in their entireties into this specification.
[0002] The present invention relates to a pellicle for a lithographic apparatus, a method for manufacturing a pellicle for a lithographic apparatus, as well as a lithographic apparatus comprising a pellicle and uses thereof. [Background technology]
[0003] A lithographic apparatus is a machine configured to apply a desired pattern onto a substrate. Lithographic apparatus can be used, for example, in the manufacture of integrated circuits (ICs). A lithographic apparatus may, for example, project a pattern from a patterning device (e.g. mask) onto a layer of radiation-sensitive material (resist) provided on the substrate.
[0004]
[0004] The wavelength of radiation used by a lithographic apparatus to project a pattern onto a substrate determines the minimum size of features that can be formed on the substrate. To form smaller features on a substrate than conventional lithographic apparatus (which may use electromagnetic radiation having a wavelength of, for example, 193 nm), lithographic apparatus may be used that use EUV radiation, which is electromagnetic radiation having a wavelength in the range of 4-20 nm.
[0005]
[0005] A lithographic apparatus includes a patterning device (e.g. a mask or reticle). Radiation is reflected through or from the patterning device to form an image on a substrate. A pellicle may be provided to protect the patterning device from airborne particles and other forms of contamination. Contamination on the surface of the patterning device may cause manufacturing defects in the substrate.
[0006]
[0006] Pellicles may also be provided to protect optical components other than the patterning device. Pellicles may also be used to provide a passage for lithographic radiation between mutually sealed areas of the lithographic apparatus. Pellicles may also be used as filters, such as spectral purity filters. The environment inside a lithographic apparatus, particularly an EUV lithographic apparatus, can sometimes be harsh, and pellicles are required to provide good chemical and thermal stability.
[0007]
[0007] Known pellicles may comprise free-standing membranes such as, for example, silicon membranes, silicon nitride, graphene or graphene derivatives, carbon nanotubes, or other membrane materials. A mask assembly may include a pellicle that protects a patterning device (e.g., a mask) from particle contamination. The pellicle may be supported by a pellicle frame to form a pellicle assembly. The pellicle may be attached to the frame, for example, by gluing a pellicle boundary area to the frame. The frame may be permanently or removably attached to the patterning device.
[0008]
[0008] During use, the temperature of a pellicle within a lithographic apparatus can rise to anywhere from about 500° C. to 1000° C. or more. These high temperatures can damage the pellicle, and therefore it is desirable to improve techniques for dissipating heat in order to reduce the operating temperature of the pellicle and improve pellicle life.
[0009] One approach to attempting this is by applying a thin metal film (coating layer) to the pellicle, such as a ruthenium film, which increases the rate at which heat radiates from the pellicle by increasing the emissivity of the pellicle, thereby lowering the equilibrium temperature at which the pellicle releases heat at the same rate it absorbs it.
[0010] However, metal films deposited on inert substrates at relatively low temperatures are in an energetically unfavorable state, and it is known that heating or annealing a thin metal film on a substrate leads to thermal instability at temperatures much lower than the melting point of the metal film. Thus, when the metal film is heated, sufficient energy is provided to cause the formation of holes in the metal film, which form by surface diffusion methods. The holes grow and eventually coalesce to form irregularly shaped islands. This process to break the film and form holes and eventually islands or droplets is known as dewetting. While this process may be beneficial in certain situations, such as for the formation of catalyst particles for carbon nanotube growth, it is highly unfavorable in other fields. For example, in the field of microelectronics, dewetting causes electrical interconnects to fail, and for pellicles such as EUV pellicles, dewetting changes the functionality of the emissive metal layer. Therefore, it is an object of the present invention to retard or prevent dewetting of metal films.
[0011]
[0011] The metal layer increases the thermal emissivity of the pellicle so that as the pellicle heats up, the metal film radiates and controls the temperature of the pellicle. When the metal film dewets and forms islands, the emissivity drops very rapidly to negligible values, resulting in significant temperature rise and associated pellicle failure.
[0012]
[0012] From the literature on thermal dewetting of metal films, it is known that the dewetting process always begins with the formation of holes in the metal film, unless holes already exist. The material forming the edge of the hole is subjected to capillary forces that tend to expand the hole, so that the edges of adjacent holes eventually merge to form strands of material. As the annealing proceeds and sufficient energy is applied, these strands of material break up into islands. The average size of the islands in the metal film is proportional to the initial thickness of the metal film. Also, the size of the islands increases with the duration of the anneal, with larger islands achieving larger sizes at the expense of smaller islands through atomic migration of metal species on the substrate. This description of dewetting generally applies to metal films of thickness from a few hundred nanometers to about 10 nm on inert substrates.
[0013]
[0013] SiO x N y In the case of Ru nanocoating of EUV pellicles with capping layers, this change in Ru morphology also holds if the Ru thickness is below a threshold thickness. The silicon oxynitride capping layer serves as a chemical etch retardation layer. Thus, below the threshold, with thicker Ru and longer annealing, the Ru layer breaks up into islands with progressively larger dimensions. The threshold thickness is not universal, and its exact value depends on several factors, among which are the mass density of the Ru layer and the SiO x N y The atomic composition of the cap layer is key. The threshold thickness is between 0 nm and 10 nm. In one case, the Ru threshold thickness was found to be about 4.5 nm, but as already mentioned, this is specific to the applied material preparation and annealing conditions. For Ru thicknesses above the threshold, the dewetting process is stopped at the hole formation stage or at the material strand formation stage, depending on the reached temperature of the pellicle. Ru on EUV pellicles tolerates significantly higher temperatures than the literature reports for dewetting on inert substrates until hole formation or islanding occurs. This shows that the atomic migration of metal species on the external pellicle surface is strongly weakened. This surprising realization is at the heart of the present invention.
[0014]
[0014] Although ruthenium films with thicknesses above a certain threshold thickness are stable under the operating conditions of an EUV lithography tool, the thickness of the metal layer causes the pellicle to absorb more of the incident EUV radiation, and therefore reduces the EUV transmittance of the pellicle. The reduction in the amount of EUV radiation that can pass through the pellicle means that longer exposure times are required, and therefore the throughput of the lithography tool is reduced. Of course, the EUV transmittance of the pellicle can be increased by reducing the thickness of the metal layer, but this will cause undesirable dewetting of the metal layer as mentioned above, resulting in overheating and eventual failure of the pellicle.
[0015]
[0015] It is therefore desirable to provide a method for manufacturing a pellicle that can withstand the operating conditions of a lithography tool, particularly an EUV lithography tool, and has sufficient EUV transmittance to allow a high scanner yield, i.e., the number of wafers exposed per hour. It is also desirable to provide a pellicle that is thermally and chemically stable and exhibits an acceptable EUV transmittance.
[0016]
[0016] Although this application refers to pellicles in the context of lithographic apparatus generally, and EUV lithographic apparatus in particular, it will be understood that the present invention is not limited to only pellicles and lithographic apparatus, and the subject matter of the present invention may be used in any other suitable apparatus or situation.
[0017]
[0017] For example, the method of the present invention may be equally applied to spectral purity filters, which are a type of pellicle. EUV radiation sources, such as those that use plasma to generate EUV radiation, in practice emit not only the desired "in-band" EUV radiation, but also undesired (out-of-band) radiation. This out-of-band radiation is particularly in the deep UV (DUV) radiation range (100 nm to 400 nm). Furthermore, for some EUV radiation sources, such as laser-produced plasma EUV radiation sources, the radiation from the laser, typically at 10.6 microns, may also form a significant source of undesired (out-of-band) infrared (IR) radiation.
[0018]
[0018] Spectral purity may be desirable in a lithographic apparatus for several reasons. One reason is that resist is sensitive to out-of-band wavelengths of radiation and therefore exposure of the resist to such out-of-band radiation may degrade the image quality of the exposure pattern applied to the resist. Also, out-of-band infrared radiation, for example the 10.6 micron radiation in some laser-produced plasma radiation sources, results in unwanted and unnecessary heating of the patterning device, substrate, and optical components in the lithographic apparatus. Such heating may lead to damage, reduced lifetime of these elements, and / or defects or distortions in the pattern projected and applied to the resist-coated substrate.
[0019]
[0019] A spectral purity filter may be formed, for example, from a silicon film coated with a reflective metal such as molybdenum or ruthenium. In use, a typical spectral purity filter will be exposed to high heat loads, for example from incident infrared and EUV radiation. This heat load can cause the temperature of the spectral purity filter to exceed 800°C, which will eventually result in delamination or dewetting of the coating. Delamination and degradation of the silicon film can be accelerated by the presence of hydrogen. Hydrogen is often used as a gas in the environment in which the spectral purity filter is used to suppress debris (such as molecular outgassing from the resist, or particulate debris) from entering or leaving certain parts of the lithographic apparatus. In this way, a spectral purity filter may be used as a pellicle, and vice versa. Thus, when referring to a "pellicle" in this application, reference is also made to a "spectral purity filter". Although reference is made primarily to pellicles in this application, all of the features may equally be applied to spectral purity filters. It is understood that a spectral purity filter is a type of pellicle.
[0020]
[0020] In a lithographic apparatus (and / or method), it is desirable to minimize losses in the intensity of the radiation being used to apply a pattern to a resist-coated substrate. One reason is that ideally as much radiation as possible should be available to apply a pattern to the substrate, for example to reduce exposure times and increase throughput. At the same time, it is desirable to minimize the amount of undesired radiation (e.g. out-of-band radiation) that passes through the lithographic apparatus and is incident on the substrate. Furthermore, it is desirable to ensure that a pellicle used in a lithographic method or apparatus has a sufficient lifetime and does not degrade rapidly over time as a result of the high thermal loads to which the pellicle may be exposed and / or hydrogen (or similar, such as free radical species including H* and HO*) to which the pellicle may be exposed. It is therefore desirable to provide improved (or alternative) pellicles, and pellicles suitable for use in, for example, lithographic apparatus and / or methods. Summary of the Invention
[0021]
[0021] The present invention has been made in consideration of the above-mentioned problems associated with known pellicles and known pellicle manufacturing methods.
[0022] According to a first aspect of the present invention there is provided a pellicle for a lithographic apparatus, the pellicle comprising a metal oxysilicide layer, the metal oxysilicide layer being capable of acting as an external surface atomic migration attenuator.
[0023]
[0023] The pellicle may comprise a silicon layer or a silicon substrate. The silicon layer or silicon substrate may act as a core layer to provide mechanical pretension and robustness. Silicon may be used as the substrate, since self-supporting silicon wafers can be manufactured using known techniques. It is also possible to manufacture silicon wafers large enough to be used as pellicles. The advantage of using silicon in an EUV lithography apparatus is that silicon absorbs very little of the EUV radiation that passes through the pellicle. However, silicon has a lower emissivity than other materials, so although silicon does not highly absorb EUV radiation, it radiates heat relatively slowly and therefore heats up when EUV radiation passes through it.
[0024]
[0024] The pellicle may include a metal layer, which may act as a thermal emissivity enhancing layer. The metal layer has a higher emissivity than silicon and therefore helps cool the silicon by increasing the rate at which heat radiates from the pellicle.
[0025]
[0025] A metal oxysilicide layer can be disposed between the silicon substrate and the metal layer. Without wishing to be bound by scientific theory, observations of dedicated laser annealing experiments on Ru-coated pellicles indicate that the presence of an interfacial metal oxysilicide layer helps to anchor the metal species to the silicon substrate and prevent dewetting of the metal layer.
[0026]
[0026] The metal of the metal oxysilicide interfacial layer may be the same as the metal of the metal layer. To maximize the interaction between the metal oxysilicide interfacial layer and the metal layer and the degree of anchoring of the metal layer, it is preferred to use the same metal in both of these two layers.
[0027]
[0027] The metal can be any suitable metal. A suitable metal is one that has a high emissivity, has low EUV absorption properties, does not easily oxidize, and if oxidized, is easily reduced back to the metallic state, or if oxidized but is not easily reduced back to the metallic state, has an oxide that at least provides emissivity. The metal can be selected from ruthenium, zirconium, hafnium, and / or combinations thereof. Preferably, the metal is ruthenium, since ruthenium is thermally conductive in both metallic and oxidized forms. The environment in which the pellicle is operated is at reduced pressure and contains primarily hydrogen gas, but due to the high temperature of the pellicle, the metal layer may react with oxygen present during use. For most metals, the oxide has a much lower emissivity than the metallic form, and therefore oxidation of the metal may reduce the performance of the pellicle. However, ruthenium oxide is thermally conductive and has good emissivity, so it can still radiate heat and the performance of the pellicle is maintained.
[0028]
[0028] The thickness of the metal layer may be about 6 nm or less, preferably about 5 nm or less, more preferably about 4.5 nm or less, and even more preferably about 3.5 nm or less. Metal layers with thicknesses greater than about 4.5 nm have been tested to be resistant to dewetting but exhibit lower EUV transmittance. A reduction in transmittance may be acceptable to allow the thickness of the metal layer to be increased to extend the life of the pellicle, while it is desirable to have a thinner metal layer while maintaining resistance to dewetting. The metal-oxysilicide interface layer stabilizes the metal layer, and surprisingly, it has been realized that thinner metal layers can be used without dewetting, i.e., for films with thicknesses of less than 4.5 nm.
[0029]
[0029] The metal layer may be on one side of the silicon substrate. It has been found that providing a metal layer on one side of the silicon substrate is sufficient to increase the emissivity of the pellicle while maintaining an acceptable EUV transmittance.
[0030]
[0030] The silicon substrate may comprise a silicon oxynitride capping layer. The silicon oxynitride capping layer may be capable of reacting with the metal layer to form a metal oxysilicide layer. Thus, the silicon oxynitride layer may be fully reacted to form a metal oxysilicide layer, or may only be partially reacted.
[0031]
[0031] In one embodiment, the pellicle may include molybdenum. The molybdenum is preferably disposed between the metal ruthenium layer and the silicon substrate. The molybdenum is preferably disposed at the interface between the metal ruthenium layer and the silicon oxynitride layer. The silicon oxynitride layer is preferably disposed on the surface of the silicon substrate. The molybdenum may be provided as a layer. The molybdenum may be provided on one or both sides of the pellicle. In particular, the silicon substrate may form a central core having two sides, each side may comprise a silicon oxynitride layer. The molybdenum layer may be provided on the silicon oxynitride layer. The molybdenum may be provided on one or both of the silicon oxynitride layers. If the molybdenum is provided on only one of the silicon oxynitride layers, in use the pellicle is oriented such that the side containing the molybdenum faces the reticle. It will be understood that the opposite orientation is also contemplated.
[0032]
[0032] Surprisingly, it has been found that the presence of molybdenum not only improves the reflectivity of the pellicle, but also acts as a barrier at the interface between the ruthenium layer and the silicon oxynitride layer and prevents oxidation and intermixing of the pellicle at operating temperatures. Pellicles with molybdenum at the interface between the ruthenium layer and the silicon oxynitride layer do not exhibit dewetting even after exposure to temperatures above 500°C. Also, the molybdenum may be at least partially oxidized, which prevents ruthenium from reacting with silicon to form ruthenium silicide (Ru2Si3). When tested under conditions similar to scanner conditions, it has been found that the pellicle according to the invention has a transmission loss of less than 1% after being used to image more than 10,000 wafers.
[0033]
[0033] Thus, in an embodiment there is provided a pellicle for a lithographic apparatus, the pellicle comprising a silicon oxynitride layer, a molybdenum layer and a ruthenium layer. The ruthenium layer and / or the molybdenum layer may be metallic.
[0034]
[0034] The molybdenum layer is located between the silicon oxynitride layer and the ruthenium layer. The silicon oxynitride layer is partially or completely reacted to provide a ruthenium oxysilicide layer. Thus, the silicon oxynitride layer may be at least partially converted to a ruthenium oxysilicide layer, and the pellicle may comprise a ruthenium oxysilicide layer instead of or in addition to the silicon oxynitride layer. The silicon oxynitride layer may be provided on a silicon substrate, which may be a polycrystalline silicon substrate. In summary, the pellicle of the present invention may comprise a ruthenium oxysilicide interface layer located between the silicon substrate and the metal ruthenium layer. The ruthenium oxysilicide interface layer helps to prevent dewetting of the metal ruthenium layer, thereby allowing a thinner ruthenium layer to be applied. This results in a more stable pellicle with increased EUV transmittance compared to known pellicles. In addition, the pellicle with the molybdenum layer is also resistant to dewetting when exposed to conditions to which the pellicle is exposed in use.
[0035] According to a second aspect of the present invention there is provided a method of manufacturing a pellicle for a lithographic apparatus, the method comprising providing a metal oxysilicide layer.
[0036]
[0036] Surprisingly, it has been found that a metal oxysilicide layer can prevent dewetting of an overlying metal layer, preventing premature failure of the metal layer and the pellicle, and allowing a thinner metal layer to be used, thus allowing a greater proportion of the incident EUV radiation to pass through the pellicle.
[0037]
[0037] The metal oxysilicide layer may be provided by any suitable means. For example, where the pellicle comprises a silicon substrate and a metal layer, the metal oxysilicide may be provided by heating the pellicle for a first period of time to a temperature below the temperature at which dewetting occurs. The silicon substrate is preferably provided with a silicon oxynitride capping layer.
[0038]
[0038] If the pellicle is heated to a temperature above the temperature at which dewetting occurs, the metal layer will dewet before reacting with the silicon substrate and / or silicon oxynitride capping layer. Thus, heating the pellicle to a temperature below the temperature at which dewetting occurs allows the formation of a metal oxysilicide layer. Once the metal oxysilicide layer is formed, it is possible to heat the pellicle to a temperature higher than would have caused dewetting otherwise, since the metal oxysilicide layer stabilizes the metal layer. In use, the pellicle heats up very quickly and exceeds the dewetting temperature shortly after the EUV radiation is turned on.
[0039]
[0039] The temperature at which dewetting occurs will depend on the thickness of the metal layer as well as the nature of the substrate to which it is attached. A person skilled in the art will be able to determine the dewetting temperature for any given combination of metal layer and substrate by heating the pellicle until dewetting is observed.
[0040]
[0040] The pellicle is preferably heated to a temperature below the dewetting temperature for a sufficient time to cause the metal oxysilicide layer to form. Because the metal oxysilicide layer takes time to form, the pellicle needs to be held at the required temperature for a sufficient period of time to cause the metal oxysilicide layer to form.
[0041]
[0041] Heating can be performed by any suitable means. Heating may be performed by placing the pellicle in a heating chamber, but is preferably performed by exposing the pellicle to laser radiation. Preferably, the power used is about 125 W. eq Here, 125W eq is defined as the equivalent power incident on a pellicle in a lithography tool operating at intermediate focus at 125 W, as described below.
[0042]
[0042] Following the reaction to form the metal oxysilicide, additional metal may be applied to the pellicle to account for or replace the metal that reacted to form the metal oxysilicide layer, so as to achieve the desired thickness of the metal layer.
[0043]
[0043] In an alternative embodiment, the metal oxysilicide layer is formed by sputtering. A metal target can be sputtered using known techniques to be deposited on a silicon substrate. The composition of the plasma used in sputtering can be changed to change the film properties. For example, the plasma can contain oxygen, which reacts with the metal and silicon to form the metal oxysilicide layer.
[0044]
[0044] Once the metal oxysilicide layer is formed, a metal layer may be formed on the metal oxysilicide layer. The metal layer may comprise ruthenium. A metal layer comprising molybdenum may be provided between the silicon oxynitride layer and the ruthenium layer.
[0045]
[0045] According to a third aspect of the present invention, there is provided an assembly for a lithographic apparatus comprising a pellicle according to the first or second aspect of the present invention, a frame supporting the pellicle, and a patterning device mounted on the frame.
[0046] According to a fourth aspect of the present invention there is provided the use of a pellicle according to the first or second aspect of the present invention in a lithographic apparatus.
[0047]
[0047] Features described with respect to any of these aspects may be combined with features described with respect to any of the other aspects of the invention, for example features of the pellicle according to the first aspect of the invention may be combined with any features according to the second aspect of the invention, and vice versa.
[0048]
[0048] The invention will now be described with reference to an EUV lithography apparatus, although it will be appreciated that the invention is not limited to pellicles and is equally applicable to spectral purity filters. [Brief description of the drawings]
[0049]
[0049] An embodiment of the present invention will now be described, by way of example only, with reference to the accompanying schematic drawings, in which:
[0050] [Figure 1] 1 depicts a lithography system comprising a lithographic apparatus and a radiation source according to an embodiment of the invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051]
[0050] Figure 1 shows a lithographic system including a pellicle 15 according to an embodiment of the invention manufactured according to the first aspect of the invention or according to a method according to the second aspect of the invention. The lithographic system comprises a radiation source SO and a lithographic apparatus LA. The radiation source SO is configured to generate an extreme ultraviolet (EUV) radiation beam B. The lithographic apparatus LA comprises an illumination system IL, a support structure MT configured to support a patterning device MA (e.g. a mask), a projection system PS and a substrate table WT configured to support a substrate W. The illumination system IL is configured to condition the radiation beam B before it is incident on the patterning device MA. The projection system is configured to project the radiation beam B (now patterned by the mask MA) onto the substrate W. The substrate W may include a previously formed pattern. In that case, the lithographic apparatus aligns the patterned radiation beam B with the pattern previously formed on the substrate W. In this embodiment, a pellicle 15 is illustrated in the path of the radiation to protect the patterning device MA. It will be appreciated that the pellicle 15 may be in any desired position and may be used to protect any of the mirrors within the lithographic apparatus.
[0052]
[0051] The radiation source SO, the illumination system IL, and the projection system PS may all be constructed and arranged such that they may be isolated from the external environment. A gas (e.g. hydrogen) at a pressure below atmospheric pressure may be provided in the radiation source SO. A vacuum may be provided in the illumination system IL and / or the projection system PS. A small amount of gas (e.g. hydrogen) at a pressure significantly below atmospheric pressure may be provided in the illumination system IL and / or the projection system PS.
[0053]
[0052] The radiation source SO shown in Fig. 1 is of a type that may be referred to as a laser-produced plasma (LPP) source. A laser 1, which may be, for example, a CO2 laser, is arranged to deposit energy via a laser beam 2 onto a fuel, such as tin (Sn), provided from a fuel emitter 3. Although reference is made to tin in the following description, any suitable fuel may be used. The fuel may be, for example, in the form of a liquid, and may be, for example, a metal or an alloy. The fuel emitter 3 may comprise a nozzle configured to direct the tin, for example in the form of droplets, along a trajectory towards a plasma formation region 4. The laser beam 2 is incident on the tin in the plasma formation region 4. The deposition of laser energy on the tin generates a plasma 7 in the plasma formation region 4. Radiation, including EUV radiation, is emitted from the plasma 7 during de-excitation and recombination of the ions of the plasma.
[0054]
[0053] The EUV radiation is collected and focused by a near normal incidence radiation collector 5 (sometimes more commonly referred to as a normal incidence radiation collector). Collector 5 may have a multi-layer structure arranged to reflect EUV radiation (e.g. EUV radiation having a desired wavelength such as 13.5 nm). Collector 5 may have an elliptical shape and have two elliptical foci. The first focus may be at the plasma formation region 4 and the second focus may be at an intermediate focus 6, as described below.
[0055]
[0054] The laser 1 may be separate from the radiation source SO. In that case, the laser beam 2 may be passed from the laser 1 to the radiation source SO with the aid of a beam delivery system (not shown), for example with suitable directing mirrors and / or beam expanders and / or other optical components. The laser 1 and the radiation source SO may together be considered as a radiation system.
[0056]
[0055] Radiation reflected by the collector 5 forms a radiation beam B. The radiation beam B is focused at a point 6 to form an image of the plasma formation region 4, which acts as a virtual radiation source for the illumination system IL. The point 6 at which the radiation beam B is focused may be referred to as an intermediate focus. The radiation source SO is positioned such that the intermediate focus 6 is at or near an aperture 8 of the source containing structure 9.
[0057]
[0056] From a radiation source SO, a radiation beam B enters an illumination system IL configured to condition the radiation beam. The illumination system IL may include a facetted field mirror device 10 and a facetted pupil mirror device 11. Together the facetted field mirror device 10 and the facetted pupil mirror device 11 provide a radiation beam B having a desired cross-sectional shape and a desired angular distribution. The radiation beam B passes through the illumination system IL and is incident on a patterning device MA, which is held by a support structure MT. The patterning device MA reflects and patterns the radiation beam B. The illumination system IL may include other mirrors or devices in addition to or instead of the facetted field mirror device 10 and the facetted pupil mirror device 11.
[0058]
[0057] Following reflection from the patterning device MA, the patterned radiation beam B enters a projection system PS. The projection system comprises a number of mirrors 13, 14 arranged to project the radiation beam B onto a substrate W held by a substrate table WT. The projection system PS may apply a demagnification factor to the radiation beam to form an image having smaller features than corresponding features on the patterning device MA. For example, a demagnification factor of 4 may be applied. In Figure 1 the projection system PS has two mirrors 13, 14, however the projection system may include any number of mirrors, for example six mirrors.
[0059]
[0058] The radiation source SO shown in Figure 1 may include components not shown. For example, the radiation source may be provided with a spectral filter. The spectral filter may be substantially transparent for EUV radiation but substantially blocking for radiation of other wavelengths, such as infrared radiation. In practice, the spectral filter may be a pellicle according to any aspect of the present invention.
[0060]
[0059] The term "EUV radiation" may be considered to encompass electromagnetic radiation having a wavelength in the range of 4 to 20 nm, for example in the range of 13 to 14 nm. EUV radiation may have a wavelength less than 10 nm, for example in the range of 4 to 10 nm, such as 6.7 nm or 6.8 nm.
[0061]
[0060] An exemplary pellicle according to one aspect of the present invention comprises a silicon substrate, a ruthenium oxysilicide interface layer, and a ruthenium metal layer. In another exemplary pellicle, a molybdenum layer may be provided between the layer of silicon oxynitride on the silicon substrate and the ruthenium metal layer. While the silicon substrate provides support and strength to the pellicle, the ruthenium metal layer helps to increase the emissivity of the pellicle, thereby extending the life of the pellicle and allowing the pellicle to operate at higher powers than known pellicles. The ruthenium oxysilicide layer helps to anchor the ruthenium metal and stops or at least reduces the tendency of the ruthenium metal to dewet. The molybdenum layer also increases the emissivity of the pellicle and acts as a barrier to further inhibit the dewetting of the ruthenium at high temperatures, thereby extending the life of the pellicle. This also allows the pellicle to be used at higher powers without performance degradation.
[0062]
[0061] Although specific reference may be made in the present text to embodiments of the invention in the context of a lithography apparatus, embodiments of the invention may be used in other apparatus. Embodiments of the invention may form part of a mask inspection apparatus, a metrology apparatus, or any apparatus that measures or processes an object such as a wafer (or other substrate) or a mask (or other patterning device). These apparatus may be generally referred to as lithography tools. Such lithography tools may utilise vacuum or atmospheric (non-vacuum) conditions.
[0063]
[0062] Although specific embodiments of the present invention have been described above, it will be understood that the present invention can be practiced otherwise than as described. The above description is intended to be illustrative and not limiting. Thus, it will be apparent to one skilled in the art that modifications of the present invention as described may be made without departing from the scope of the following claims.
Claims
1. 1. A spectral purity filter for a lithographic apparatus comprising: a silicon layer; a ruthenium layer; and a molybdenum layer disposed between the ruthenium layer and the silicon layer, the silicon layer comprising a silicon oxynitride capping layer.
2. 1. A spectral purity filter for a lithographic apparatus, comprising: a silicon layer, a ruthenium layer, a molybdenum layer disposed between the ruthenium layer and the silicon layer, and a metal oxysilicide layer.
3. 3. The spectral purity filter according to claim 1 or 2, wherein the thickness of the ruthenium layer is less than or equal to about 6 nm.
4. 3. The spectral purity filter of claim 1 or 2, wherein one or both of the molybdenum and ruthenium layers are metallic.
5. 2. The spectral purity filter of claim 1, wherein said molybdenum layer is disposed between said ruthenium layer and said silicon oxynitride capping layer.
6. 2. The spectral purity filter of claim 1, wherein said molybdenum layer is disposed at an interface between said ruthenium layer and said silicon oxynitride capping layer.
7. 3. The spectral purity filter of claim 2, wherein said metal oxysilicide layer is disposed between said silicon layer and said ruthenium layer.
8. 1. A pellicle for a lithographic apparatus comprising: a silicon layer; a ruthenium layer; and a molybdenum layer disposed between the ruthenium layer and the silicon layer, the silicon layer comprising a silicon oxynitride capping layer.
9. 1. A pellicle for a lithographic apparatus, comprising: a silicon layer; a ruthenium layer; a molybdenum layer disposed between the ruthenium layer and the silicon layer; and a metal oxysilicide layer.
10. 10. The pellicle of claim 8 or 9, wherein the ruthenium layer has a thickness of about 6 nm or less.
11. 10. The pellicle of claim 8 or 9, wherein the ruthenium layer has a thickness of about 4.5 nm or less.
12. 10. The pellicle of claim 8 or 9, wherein one or both of the molybdenum layer and the ruthenium layer are metallic.
13. 1. A method of manufacturing a spectral purity filter for a lithographic apparatus, the method comprising: providing a molybdenum layer between a silicon layer and a ruthenium layer; and providing a silicon oxynitride capping layer on the silicon layer.
14. 13. A method of manufacturing a spectral purity filter for a lithographic apparatus, the method comprising providing a molybdenum layer between a silicon layer and a ruthenium layer, and providing a metal oxysilicide layer.
15. 1. A method of manufacturing a pellicle for a lithographic apparatus, the method comprising: providing a molybdenum layer between a silicon layer and a ruthenium layer; and providing a silicon oxynitride capping layer on the silicon layer.
16. 1. A method of manufacturing a pellicle for a lithographic apparatus, the method comprising providing a molybdenum layer between a silicon layer and a ruthenium layer, and providing a metal oxysilicide layer.
Citation Information
Patent Citations
Pellicle and method of producing pellicle
JP2009271262A
Pellicle and pellicle production method
JP2014211474A
Pellicle for EUV mask
JP2016130789A
Pellicle inspection method and pellicle inspection device
JP2017053893A
Extreme ultraviolet lithography pellicle and method for manufacturing the same
JP2018151622A