Plasma atomized metal powder manufacturing method and system

The method addresses the challenge of high yields and low costs in plasma atomization by optimizing the gas-to-metal ratio and alignment, producing spherical metal powders with 80% yield in the 0-106 micron range for applications like 3D printing and coating.

JP7572494B2Active Publication Date: 2024-10-23AP&C ADVANCED POWDERS & COATINGS
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023061454
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-11-05
Filing Date
2023-04-05
Publication Date
2024-10-23
Estimated Expiration
2036-07-06

AI Technical Summary

Technical Problem

Existing methods for producing metal powders via plasma atomization face challenges in achieving high yields of fine particle size distribution, particularly in the 0-106 micron range, while maintaining low production costs and reducing waste.

Method used

A method involving a gas-to-metal ratio of less than about 20, precise alignment of the metal source with the plasma source, and controlled atomization conditions to produce plasma atomized metal powder with at least 80% yield in the 0-106 micron range, using techniques such as induction heating and alignment systems to optimize the atomization process.

Benefits of technology

The method achieves high yields of spherical metal powders with a particle size distribution of 0-106 microns, reducing production costs and minimizing waste, suitable for applications like 3D printing and coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572494000007
    Figure 0007572494000007
  • Figure 0007572494000008
    Figure 0007572494000008
  • Figure 0007572494000009
    Figure 0007572494000009
Patent Text Reader

Abstract

To provide a method of producing a plasma-atomized metal powder allowing for obtaining spherical powder having a sufficient fine particle-size distribution with a reduced production cost, and a system therefor.SOLUTION: A method of producing a plasma-atomized metal powder includes: providing a heated metal source; and bringing the heated metal source into contact with a plasma of at least one plasma source under an effective condition for causing atomization of the heated metal source. Atomization may be carried out using a gas-to-metal ratio of nearly smaller than 20, thereby obtaining material metal powder having a 0-106 micron particle-size distribution yield of at least 80%. The present method may further include positioning the heated metal source with a plasma of the at least one plasma source. An atomization system may include a positioning system positioned upstream of the plasma source and adapted to adjust the orientation of the metal source to the at least one plasma source.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 193,622, filed July 17, 2015, and U.S. Provisional Application No. 62 / 251,476, filed November 5, 2015, which documents are incorporated by reference in their entireties.

[0002] The present disclosure relates to the field of production of spherical powders, such as metallic spherical powders. More specifically, the present disclosure relates to a method and an apparatus for preparing metallic powders by plasma atomization. [Background technology]

[0003] Typically, the desired characteristics of high quality reactive metal powders are a combination of high sphericity, density, purity, flowability and low amounts of gas-trapped porosity. Fine powders are useful in applications such as 3D printing, powder injection molding, hot isostatic pressing and coating. Such fine powders are used in aerospace, biomedical and industrial applications.

[0004] Various solutions have been proposed so far regarding methods and devices for preparing metal powders via plasma atomization, but the proposed solutions have some problems, for example, some of the proposed methods and devices are unable to obtain spherical powders with a sufficiently fine particle size distribution.

[0005] Moreover, the proposed solutions still involve high production costs and low production rates.

[0006] Some other challenges arise regarding the percentage of 0-106 micron particles in the produced raw metal powder. In fact, so far, there have not been many techniques that allow the production of raw metal powders with a high 0-106 micron particle size distribution yield. In fact, some techniques have only been able to produce particles with a size of 0-106 micron in very small quantities. For example, some techniques produce only 20-40% of 0-106 micron grade powder, while other techniques do not exceed about 60-70%. Therefore, those prior art techniques have not allowed the preparation of raw metal powders with a high 0-106 micron particle size distribution yield. The low yield significantly increases the production cost and generates a lot of waste. Moreover, typical methods such as the EIGA process may require very large amounts of atomizing gas to achieve a 70% yield of particles with a size of 0-106 micron. For example, the gas-to-metal ratio in the EIGA process may reach about 33. This may further increase the production cost. Summary of the Invention

[0007] It would therefore be highly desirable to provide an apparatus, system or method that at least partially addresses the shortcomings of the existing technology. [Means for solving the problem]

[0008] In one aspect, the embodiments described herein include a method for producing plasma atomized metal powder, comprising the steps of: Providing a heated metal source; and contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source.

[0009] In another aspect, the embodiments described herein include a method of producing plasma atomized metal powder, comprising the steps of: Providing a heated metal source; contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source, thereby obtaining a raw metal powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214.

[0010] In another aspect, embodiments described herein provide a method of producing plasma atomized metal powder, comprising: providing a heated metal source; and contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source, wherein the atomization is carried out by using a gas to metal ratio of less than about 20, thereby obtaining a raw metal powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214.

[0011] In another aspect, embodiments described herein provide a method of producing plasma atomized metal powder comprising providing a heated metal source and contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source, wherein the atomization is carried out by using a gas to metal ratio of less than about 20, thereby obtaining a metal powder having at least 80% of a 0-106 micron distribution.

[0012] In another aspect, embodiments described herein provide a plasma atomization manufacturing method that includes providing a heated metal source, aligning the heated metal source with a plasma of at least one plasma source, and contacting the heated metal source with the plasma of the at least one plasma source under conditions effective to cause atomization of the heated metal source.

[0013] In yet another aspect, embodiments described herein provide an atomization system comprising: a delivery device for delivering a metal source; at least one heating system for heating the metal source; at least one plasma source configured to contact the metal source after heating with a plasma under conditions effective to cause atomization of the heated metal source; and an alignment system positioned upstream of the at least one plasma source, the alignment system adapted to adjust an orientation of the metal source relative to the at least one plasma source.

[0014] The following drawings represent non-limiting examples. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view of an atomization system according to a first exemplary embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram of an alignment system of an atomization system according to an exemplary embodiment of the present disclosure. [Diagram 3] FIG. 3 is a cross-sectional view of a guide of a guided atomization system according to an exemplary embodiment of the present disclosure. [Figure 4] FIG. 4 is a cross-sectional view of a guide having an induction heating element according to an exemplary embodiment of the present disclosure. [Diagram 5] FIG. 5 is a cross-sectional view of a guide having an electrode heating element according to another exemplary embodiment of the present disclosure. [Figure 6] FIG. 6 is a cross-sectional view of a guided atomization system according to a first exemplary embodiment of the present disclosure. [Figure 7] FIG. 7 is a cross-sectional view of a guided atomization system according to a second exemplary embodiment of the present disclosure. [Figure 8] FIG. 8 is a cross-sectional view of a guided atomization system according to a third exemplary embodiment of the present disclosure. [Figure 9]FIG. 9 is a SEM image at 250x magnification of an example atomized metal particle (Ti-6A1-4V) of the present disclosure. [Figure 10] FIG. 10 is a SEM image at 500x magnification of an example atomized metal particle (Ti-6A1-4V) of the present disclosure. [Figure 11] FIG. 11 is a SEM image at 2000x magnification of an example atomized metal particle (Ti-6A1-4V) of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The following examples are offered in a non-limiting manner.

[0017] The word "a" or "an," when used in conjunction with the term "comprising" in the claims and / or specification, may mean "one," but it is also consistent with the meanings of "one or more," "at least one," and "one or more," unless the content clearly dictates otherwise. Similarly, the word "another" may mean at least a second or more, unless the content clearly dictates otherwise.

[0018] As used in this specification and the claims, "comprising" (and any form of comprising, such as "comprise" and "comprises"), "having" (and any form of having, such as "have" and "has"), "including" (and any form of including, such as "include" and "includes"), or "containing" (and any form of containing, such as "contain" and "contains") are inclusive or expandable and do not exclude additional, unrecited elements or method steps.

[0019] As used herein, the expression "atomization zone", when referring to a method, apparatus or system for preparing metal powder, refers to a zone where material is atomized into droplets of material. A person skilled in the art will understand that the dimensions of the atomization zone will vary according to various parameters such as the temperature of the atomization means, the speed of the atomization means, the material of the atomization means, the power of the atomization means, the temperature of the material before entering the atomization zone, the nature of the material, the dimensions of the material, the electrical resistivity of the material, etc.

[0020] The phrase "metal powder having at least T% yield of particle size distribution of X to Y microns as measured according to ASTM B214" refers to a metal powder in which at least T% of the resulting powder has a particle size distribution of from about X to about Y microns, as measured according to the ASTM B214 standard.

[0021] The phrase "metal powder having a particle size distribution yield of at least 80% between 0 and 106 microns as measured according to ASTM B214" refers to a metal powder in which at least 80% of the resulting powder has a particle size distribution between about 0 and about 106 microns, as measured according to the ASTM B214 standard.

[0022] As used herein, the expression "gas to metal ratio" refers to the mass per unit time (Kg / s) of gas injected for the mass velocity (Kg / s) of the metal source into the atomization zone.

[0023] As used herein, the phrase "reactive metal powder" refers to metal powders that cannot be effectively prepared via classical gas atomization methods using close-coupled nozzles. For example, such reactive metal powders can be powders comprising at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals.

[0024] As used herein, the term "raw metal powder" refers to metal powder obtained directly from the atomization process without post-processing steps such as sieving or classification techniques.

[0025] Various exemplary embodiments described herein provide high yields of raw metal powder of a given distribution while maintaining low production costs. By minimizing waste and by reducing the gas flow rate (i.e., gas volume) used in the atomization process, production is improved. Costs are kept low, for example, the gas to metal ratio is less than 30 according to the methods and systems described herein.

[0026] According to various exemplary embodiments, a metal source is provided, from which a raw metal powder is formed, the metal source being preheated prior to entering the atomization zone.

[0027] In some exemplary embodiments, the metal source is already heated before being delivered to the atomization zone. However, the metal source is further heated immediately upstream of the atomization zone so that the metal source reaches a sufficient temperature before being atomized. Once at a sufficient temperature, the metal source is atomized by contacting it with a plasma from at least one plasma source under conditions effective to cause atomization of the heated metal source.

[0028] For example, the raw material can be melted in a water-cooled crucible (skull melting). The metal source is then further heated to contact the plasma from at least one plasma source to be atomized, resulting in a molten stream that is delivered to the atomization zone.

[0029] For example, the metal source may initially be delivered as a metal wire or rod. Prior to atomization, the metal wire or rod may be further heated by resistive heating, arc discharge, inductive heating, or any combination thereof. After being heated, the metal wire or rod is delivered to an atomization zone so as to contact the plasma from at least one plasma source to be atomized.

[0030] By sufficiently heating the metal source prior to atomization and proper alignment, a high yield of the raw metal powder to be atomized can be achieved. This high yield can be achieved without a significant increase in production costs compared to the energy costs of the plasma torch. For example, the temperature of the metal source prior to atomization can be near the melting point of the material. For example, the temperature can be about 75% to about 110% of the melting point temperature or about 85% to about 95% of the melting point temperature.

[0031] For example, high yields of fine powder are achieved for small amounts of very hot gas streams injected into the atomization zone. It will be appreciated that the injected gas is often an inert gas. Reducing the amount of injected gas can significantly reduce production costs, especially the cost of recycled gas.

[0032] According to various exemplary embodiments, to achieve the yields provided herein, the plasma from at least one plasma source must provide sufficient heating energy and momentum to the metal source during atomization. The plasma gas flow is typically greater than 100 slm per torch for a titanium mass feed rate of about 10 kg / h, more preferably greater than 150 slm for three focused plasma torches. The power per torch is about 25 kW, more preferably about 30 kW or more.

[0033] It will be understood that an increased amount of power and energy is required to provide the required amount of heat from at least one plasma source. According to various exemplary embodiments, it has been observed that the cost savings (yield) obtained from lowering the amount of gas injected during atomization greatly outweighs the increased cost from higher power consumption by at least one plasma source.

[0034] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas-to-metal ratio of less than about 20.

[0035] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas-to-metal ratio of about 5 to about 15.

[0036] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas-to-metal ratio of about 2 to about 10.

[0037] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas-to-metal ratio of about 5 to about 10.

[0038] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas-to-metal ratio of about 10 to about 20.

[0039] According to various exemplary embodiments, the raw metal powder may be formed from atomizing a metal source using a gas to metal ratio of about 10 to about 15.

[0040] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-106 micron particle size distribution yield of at least 80%.

[0041] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-106 micron particle size distribution yield of at least 85%.

[0042] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-106 micron particle size distribution yield of at least 90%.

[0043] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-75 micron particle size distribution yield of at least 85%.

[0044] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-45 micron particle size distribution yield of at least 50%.

[0045] According to various exemplary embodiments, the raw metal powder resulting from atomization has a 0-45 micron particle size distribution yield of at least 60%.

[0046] According to various exemplary plasma atomized metal powder production methods, a metal source delivered to an atomization zone is appropriately positioned relative to the plasma and at least one plasma source.

[0047] For example, the metal source and at least one plasma source fed into the atomization zone are positioned relative to each other such that the metal source contacts the plasma at an apex of the plasma source, which may be the geometric apex of the plasma source. It has been observed that the apex of the plasma source corresponds to the region where the atomization shear force of the plasma is greatest.

[0048] Proper relative positioning of the metal source and the at least one plasma source within the atomization zone may require placing a nozzle outlet of the plasma source in close proximity to the metal source within the atomization zone.

[0049] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 5 centimeters of the metal source.

[0050] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 3 centimeters of the metal source.

[0051] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 2.5 centimeters of the metal source.

[0052] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 2 centimeters of the metal source.

[0053] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 1.9 centimeters of the metal source.

[0054] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 1.75 centimeters of the metal source.

[0055] For example, the plasma source is positioned so that its nozzle exit is within a maximum of about 1.5 centimeters of the metal source.

[0056] According to various exemplary embodiments, the metal source is fed to the atomization zone as a vertical feed, which may be a molten stream, a metal rod, or a metal wire.

[0057] The at least one plasma source may be at least one plasma torch having at least one individual nozzle. If multiple individual nozzles are provided, the nozzles may be positioned at angles around the longitudinal feed of the metal source.

[0058] Alternatively, the at least one plasma source may include an annular nozzle extending around the periphery of the metal source longitudinal feed.

[0059] According to various exemplary embodiments, at least one nozzle of the at least one plasma source may be angled downward. For example, the at least one plasma source may emit a plasma jet oriented at an angle between about 10° and about 60° relative to a vertical axis.

[0060] For example, the at least one plasma source may emit a plasma jet oriented at an angle between about 20° and about 60° relative to the vertical axis.

[0061] For example, the at least one plasma source may emit a plasma jet oriented at an angle between about 20° and about 50° relative to the vertical axis.

[0062] For example, the at least one plasma source may emit a plasma jet oriented at about 20° to about 30° relative to the vertical axis.

[0063] For example, the at least one plasma source may emit a plasma jet oriented at about 25° to about 35° relative to the vertical axis.

[0064] According to various exemplary plasma atomized metal powder production methods, a metal source delivered to the atomization zone is aligned with the plasma of at least one plasma source. The alignment may include adjusting the orientation of the metal source as it is delivered to the atomization zone. The adjustment attempts to maintain a desired positioning of the metal source relative to the at least one plasma source and / or the plasma from the at least one plasma source over time.

[0065] It has been observed that the position of the metal source delivered to the atomization zone can vary spatially over time. This spatial variation can occur between separate atomization runs or within a single atomization run. So the orientation of the metal source as it is delivered to the atomization zone can be adjusted before starting an atomization run. The molten stream falling from the molten rod can move and not always contact the exact plasma jet apex (atomization point). Hot wires and small rods can bend and move away from the optimal atomization point.

[0066] Additionally or alternatively, the orientation of the metal source as it is delivered to the atomization zone may be repeatedly adjusted during the ongoing atomization process. Adjustments to the orientation of the metal source may be performed continuously or intermittently to maintain a desired alignment of the metal source with the plasma source and / or plasma from the at least one plasma source.

[0067] For example, during the atomization process, the orientation of the metal source delivered to the atomization zone may be visually monitored by a human operator, and if the operator perceives that the metal source has spatially varied and is no longer in the desired alignment, the operator may operate (manually or via input of a computerized command) an alignment correction mechanism to return the orientation of the metal source to the desired alignment.

[0068] Additionally or alternatively, the orientation of the metal source delivered to the atomization zone during the atomization process may be monitored by a computerized monitoring system. The computerized system may capture an image of the metal source relative to the plasma and / or at least one plasma source. By applying image analysis and / or processing techniques, the system identifies when the metal source has spatially shifted to no longer be in the desired alignment. The computerized system can further determine the amount of deviation and the correction required. The computer system can then issue a command to an alignment correction mechanism to return the orientation of the metal source to the desired alignment.

[0069] For example, the desired alignment may be the alignment of a metal source delivered to the atomization zone with an apex of a plasma jet from at least one plasma source.

[0070] For example, the method can include aligning a heated metal source with the plasma of the at least one plasma source, including positioning the heated metal source within up to 5 centimeters of an exit nozzle of the at least one plasma source.

[0071] For example, the method can include aligning a heated metal source with the plasma of the at least one plasma source, including positioning the heated metal source within a maximum of 2.5 centimeters of an exit nozzle of the at least one plasma source.

[0072] For example, the method can include aligning a heated metal source with the plasma of the at least one plasma source, including positioning the heated metal source within a maximum of 1.9 centimeters of an exit nozzle of the at least one plasma source.

[0073] 1, illustrated therein is a cross-sectional view of an atomization system 2 according to a first exemplary embodiment. The first atomization system 2 includes a vessel 8 that receives a metal source 16 from an upstream system. The vessel 8 may be a crucible. The metal source 16 within the vessel 8 may be heated using various techniques known in the art, such as the cold crucible technique (skull melting).

[0074] It will be appreciated that the heating of the metal source 16 within the vessel 8 corresponds to heating the metal source 16 prior to atomization. After being heated within the vessel 8, the metal source 16 is delivered through the vessel's outlet 24 to the atomization zone 32. For example, the heated metal source 16 exits through the outlet 24 under gravity.

[0075] The heated metal source 16 exits the vessel 8 and is delivered to the atomization zone 32 where it is immediately contacted with plasma from at least one plasma source 40 which is also used to heat the high pressure cold gas that creates the secondary atomization.

[0076] According to the illustrated example, the plasma source 40 includes at least one plasma torch. At least one angled nozzle 48 of the at least one plasma torch 40 is positioned at the center of the metal source feed. For example, a cross section of the nozzle 48 may be tapered toward the metal source feed to focus the plasma contacting the metal source feed. As described elsewhere herein, the nozzle 48 may be positioned such that an apex of the plasma contacts the metal source fed from the vessel 8. Contact of the metal source feed with the plasma from the at least one plasma source 40 results in atomization of the metal source.

[0077] When multiple plasma torches are provided, the nozzles of the torches are individual plasma torch nozzles 48 directed towards the metal source from the vessel 8. For example, the individual nozzles 48 are positioned such that the apex of the plasma output therefrom contacts the metal source from the vessel 8.

[0078] The atomization system 2 further includes a gas source that delivers a secondary high pressure gas toward the atomization zone. The secondary gas flow contacts the pre-atomized metal source feed immediately after it is formed from the plasma atomization. For example, the gas source (not shown) can deliver high pressure cooling gas. For example, Source? The gas delivered from the reactor is an inert gas.

[0079] The formed raw metal powder 64 exits the atomization zone 32 .

[0080] 2, illustrated therein is a schematic diagram of an adjustable guide system 100 of an atomization system according to various exemplary embodiments. The guide system includes a guide 108 that defines a through channel. The guide 108 is positioned upstream of the atomization zone 32. A metal source received from an upstream system is fed into an inlet 116 of the guide 108. The metal source is then displaced through the channel of the guide 108. The metal source exits the guide 108 at an outlet 124 located proximate to the atomization zone 32.

[0081] For example, the metal source 16 fed to the inlet 116 is in the form of a metal wire of a metal rod.

[0082] The orientation of the guide 108 is adjustable. By adjusting the orientation of the guide 108, the orientation of the metal source 16 exiting the guide 108 and delivered to the atomization zone 32 is also adjusted. Thus, the alignment of the metal source 16 delivered to the atomization zone relative to the plasma source (not shown in FIG. 2 ) can be adjusted via adjustments made to the guide 108.

[0083] According to one exemplary embodiment, as shown, the guide 108 is pivotally coupled about a pivot point 132. The guide 108 may be coupled to a fixed portion of the atomization system. By displacing the upper portion 140 of the guide 108, the lower portion 148 of the guide 108 is displaced in a corresponding manner about the pivot point 132.

[0084] The guide system 100 further includes an alignment correction mechanism operable to displace the guide 108. The displacement of the guide 108 in turn displaces the metal source 16.

[0085] According to one exemplary embodiment, as shown, the alignment correction mechanism comprises a displaceable member 156 coupled to the upper portion 140 of the guide 108. The displaceable member 156 is further coupled to at least one adjuster 164 capable of inducing a displacement of the displaceable member 156. For example, the adjuster 164 may be 4is an adjustment screw coupled to the displaceable member 156 via a threaded member 172. Rotation of the adjustment screw 164 causes displacement of the threaded member 172, which in turn causes displacement of the displaceable member 156 and the guide 108. For example, a number of differently oriented adjusters 164 may be used. 4 may be provided to displace the displaceable member 156 and the guide 108 in different directions.

[0086] Arrow 174 indicates possible directions of displacement of displaceable member 108 in the plane. Arrow 176 indicates possible displacement of displaceable member 156 to cause displacement of guide member 108 in the plane. It will be appreciated that the guide may be displaced in multiple directions.

[0087] 3, illustrated therein is a cross-sectional view of a guide 108 according to one exemplary embodiment. As previously discussed, the guide 108 defines a through channel 180 extending between its inlet 116 and outlet 124. An inner surface 188 of the through channel 180 may be lined with a material that will not contaminate the metal source 16 displaced through the channel 180.

[0088] It has been observed that the risk of contamination of the metal source 16 increases if the temperature of the inner surface 188 is elevated and / or if it is formed of a reactive material. For example, the inner surface 188 of the through channel 180 may be formed of a heat resistant material. For example, the inner surface 188 of the through channel 180 may be formed of an electrically insulating material. For example, the inner surface 188 is formed of a ceramic material. The ceramic material may be selected from alumina oxide, macor, zirconia, yttria, sialon, silicon oxide, and mixtures thereof.

[0089] According to various exemplary embodiments, the guide 108 may be formed from a heat resistant material.

[0090] According to various exemplary embodiments, the guide 108 may be formed from an electrically insulating material.

[0091] According to various exemplary embodiments, the guide 108 may be formed from a ceramic material.

[0092] According to various exemplary embodiments, as shown, the guide 108 includes a cooler to cool the guide and limit contamination of the metal source 16 displaced through the guide. For example, and as shown in FIG. 3, the guide 108 may have a cooling inlet 196 for receiving a cooling medium, such as a cooling gas or liquid. The guide 108 is also double-walled, with a cooling channel 204 defined between an inner wall 212 and an outer wall 218. The cooling channel 204 is in fluid communication with the cooling inlet 196. For example, the cooling channel 204 extends at an angle about the axis of the guide 108 and also extends over a substantial portion of the length of the guide 108. After flowing through the cooling channel 204, the cooling medium exits via a cooling outlet 220. Cooling the guide 108 may be important according to exemplary embodiments where the metal source is already heated before entering the guide 108 and / or where the metal source is heated as it displaces through the guide 108.

[0093] For example, as shown, the cooling inlet 196 is located downstream of the cooling outlet 220 along the displacement path of the metal source 16 through the guide 108. If the metal source 16 is heated, the metal source 16 at a downstream location, such as closer to the outlet 124, may be at a higher temperature than an upstream location, such as the inlet 116. By positioning the inlet 196 downstream of the cooling outlet 220, cooling of the portions closer to the inlet 196 is prioritized.

[0094] According to various exemplary embodiments, the bottom end 228 of the guide 108 may be removable and replaceable. It should be appreciated that the bottom end 228 is located within or proximate to the atomization zone. As such, the bottom end 228 may be exposed to higher temperatures than other portions of the guide 108. This higher temperature may result in faster wear and tear on the bottom end 228 than other portions of the guide 108, which may cause the bottom end 228 to be replaced more frequently than the guide 108 itself.

[0095] According to various exemplary embodiments, the metal source 16 may be heated as it is displaced through the guide 108 .

[0096] 4, illustrated therein is a cross-sectional view of a guide having at least one heating element. As illustrated, the heating element is a conductive coil 236 wound around a portion of the through channel 180. Current flowing through the conductive coil 236 generates a magnetic field, which further induces a current through the metal source 16 to flow through the channel 180. Due to the electrical properties of the metal source 16, the induced current through the metal source 16 causes the metal source 16 to heat. It will be appreciated that the metal source is heated via a form of induction heating. Furthermore, it will be appreciated that by providing the inner surface 188 and / or guide 108 to be electrically insulating, the magnetic field generated by the conductive coil 236 does not induce a current through the inner surface 188 and / or guide 108 that could cause heating.

[0097] 5, illustrated therein is a cross-sectional view of a guide having an electrode 244 for arc discharge heating. It will be understood that the guide 108 shown in FIG. 5 does not have a cooling mechanism (cooling inlet 196, cooling channel 204, and cooling outlet 220). However, in other exemplary embodiments, a cooling mechanism may be included in the guide 108. According to the illustrated example, the electrode 244 is placed in proximity to the metal source 16 as the metal source exits the outlet 124 of the guide 108. An electric arc 252 is formed between the electrode 244 and the metal source 16, and the electric arc discharge causes heating of the metal source 16.

[0098] According to other exemplary embodiments, the metal source 16 may be further heated by resistive heating before exiting. A first probe may contact the metal source 16 upstream of or within the guide 108. A second probe may contact the metal source 16 downstream of the guide 108 as an electrode 244. A power source connects the two probes, thereby forming an electrical circuit through the portion of the metal source 16 that extends between the two probes. Current flowing through this portion of the metal source 16 causes it to heat. It will be appreciated that the metal source is heated via resistive heating and arc discharge heating.

[0099] 6, illustrated therein is a guided atomization system 300 according to one exemplary embodiment. The metal source 16 extends through and is retained within a guide 108. The guide 108 is oriented such that the metal source 16 delivered to the atomization zone 32 is properly aligned with the plasma jet 49 exiting a nozzle 48 from the plasma source 40.

[0100] Arrow 308 displays exemplary degrees of freedom of movement of the guide 108 and the metal source 16. However, it will be understood that the metal source 16 and the guide 108 may be displaced in other directions as well. The orientation of the guide 108 may be adjusted to maintain proper alignment of the metal source 16 delivered to the atomization zone with the plasma source 40 and / or the plasma from the nozzle 48 of the plasma source.

[0101] The illustrated example shows the plasma source 40 as a plasma torch having a separate nozzle, however, in other exemplary embodiments, the plasma source 40 may emit plasma from an annular nozzle.

[0102] According to the illustrated example, the atomization system 300 includes a conductive coil 236 for inductively heating the metal source 16 as it is displaced through the guide 108 .

[0103] Continuing with reference to Figure 6, the atomization system 300 may further include a gas recovery system 316 that recovers gas present in the collection chamber 324 downstream of the atomization zone 32. The recovered gas may be returned to the atomization zone 32 as an atomization gas for the formed raw metal powder. The raw metal powder produced by the atomization system 300 may be further collected within the atomization system 300.

[0104] 7, illustrated therein is a guided atomization system 300 according to a modified exemplary embodiment. According to this modification, the guided atomization system 300 includes an electrode 244 positioned proximate to the atomization zone 300. The electrode 244 forms an electric arc with the metal source 16, passing an electric current through the metal source 16 to heat it. For example, a power source 324 is provided to provide the electric current and generate the electric arc.

[0105] 8, there is illustrated a guided atomization system 300 according to another alternative exemplary embodiment. According to this alternative, the guided atomization system 300 includes both a conductive coil 236 for inducing inductive heating of the metal source 16 and an electrode 244 for inducing arc discharge heating of the metal source.

[0106] According to various example methods and systems described herein, the heated molten source may comprise at least one member selected from titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals.

[0107] According to various exemplary methods and systems described herein, the metal source can be selected from titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals.

[0108] According to various exemplary methods and systems described herein, the melt source may be selected from titanium, titanium alloys, zirconium, zirconium alloys, aluminum, and aluminum alloys.

[0109] According to various exemplary methods and systems described herein, the melt source may be selected from a titanium alloy.

[0110] For example, the melt source may be a titanium alloy.

[0111] For example, the titanium alloy may be selected from Ti-6A-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminides.

[0112] For example, the melt source can be selected from unalloyed Ti grades (e.g., grades 1, 2, 3, or 4), Pd or Ru modified Ti alloys (e.g., grades 7, 11, 16, 17, 26, or 27), alpha and near alpha Ti alloys (e.g., grades 6, 9, 12, 18, 28), alpha-beta Ti alloys (e.g., grades 5, 23, or 29), near beta and beta Ti alloys (e.g., grades 19 or 20).

[0113] For example, plasma atomization can be performed with various types of plasma torches, such as a DC plasma torch, an AC plasma torch, an RF plasma torch, a microwave plasma torch or a three-phase plasma arc torch.

[0114] Example 1: Ti-6Al-4V atomization The plasma atomization run is accomplished using a 0.125 inch diameter wire of Ti-6Al-4V (gr.23) as the feedstock and three converging plasma jets oriented approximately 30° to the vertical axis. The plasma contacts the metal wire less than 2.5 centimeters from the plasma torch nozzle exit. Each plasma torch is operated at 30 kW power with 150 SLM argon gas flow.

[0115] A background sheath gas is also used to ensure proper transport of the metal droplets. The sheath gas flow rate is 550 SLM.

[0116] A direct current varying from 150 A to 180 A at a potential of 45 V is used to preheat the wire at a high temperature prior to atomization by the plasma jet, resulting in a wire feed rate varying from 8 to 13 kg / h.

[0117] The wire is fed through a gas-cooled, adjustable guide to allow continuous metal delivery right at the apex of the plasma torch jet. Batch sizes are typically 100 kg for each run.

[0118] The gas to metal ratio in these production runs varies, for example, from 8.7 to 12.9.

[0119] The resulting particle size distribution is determined according to ASTM B214.

[0120] The first batch (Batch 1) was produced using a gas to metal ratio of 8.7 and a plasma exit to atomization zone (contact point between the plasma and the metal source) of approximately 2.5 centimeters.

[0121] A second batch (Batch 2) was produced using a gas to metal ratio of 12.9 and a plasma exit to atomization zone (contact point between the plasma and the metal source) of approximately 1.9 centimeters.

[0122] The yield results for batches 1 and 2 are as follows: [Table 1]

[0123] It has been observed that low gas to metal ratios produce good yields of fine raw metal powder. For example, in batch 2, using a gas to metal ratio of 12.9, over 90% yield was obtained from 0 to 106 microns and nearly 60% yield from 0 to 45 microns.

[0124] It has been observed that the distance between the atomization zone and the nozzle exit is an important factor since gas velocity changes rapidly with distance.

[0125] Similar conditions to batch 2 were also tried, but with a higher throughput (i.e., a lower gas-to-metal ratio of 9-10). The resulting particle size distributions were very similar to the batch 2 results.

[0126] It will be appreciated that a high yield of fine feedstock metal powder by atomization is important to be able to provide large quantities of powder at a reasonable cost.

[0127] It has further been observed that the chemical composition of the raw metal powder produced by the plasma atomization process is very clean and free of contamination. Without being bound to any particular theory, this can be attributed to melting and atomizing the metal source without contacting contaminated surfaces.

[0128] A typical chemical composition obtained for the Ti-6Al-4V grade 23 powder is as follows: [Table 2]

[0129] The powders produced are very pure, spherical and contain a large proportion of fine particles that can be used for applications such as laser additive manufacturing and powder injection molding.

[0130] FIG. 9 is a scanning electron microscope (SEM) image at 250x magnification of the raw metal powder as formed in the example method (without sieving).

[0131] FIG. 10 is an SEM image at 500x magnification of the raw metal powder as is formed by the method of the example (without sieving).

[0132] FIG. 11 is an SEM image at 2000x magnification of the raw metal powder as formed in the example method (without sieving).

[0133] The presence of very fine particles (several microns in diameter) in Figures 9-11 is characteristic of the production of powders with a yield of 80% or more in the particle size range of 0-106 microns. These very fine particles are only weakly physically bound to the larger ones.

[0134] Example 2 - Ti-6Al-2Sn-4Zr-2Mo-0.08Si atomized The plasma atomization run is accomplished using a 0.125-inch diameter wire of Ti-6Al-2Sn-4Zr-2Mo-0.08Si as the feedstock and three converging plasma jets oriented at approximately 30° to the vertical axis. The plasma contacts the metal wire less than 2.0 centimeters from the plasma torch nozzle exit. Each plasma torch is operated at 30 kW power with an argon gas flow of 150 SLM.

[0135] A background sheath gas is also used to ensure proper transport of the metal droplets. The sheath gas flow rate is 550 SLM.

[0136] A direct current of 150 A at a potential of 45 V is used to preheat the wire to a high temperature prior to atomization by the plasma jet, resulting in a wire feed rate of 8.5 kg / h.

[0137] The wire is fed through a gas-cooled, adjustable guide to allow continuous metal delivery right at the apex of the plasma torch jet. Batch sizes are typically 100 kg for a run.

[0138] The gas to metal ratio in these production runs is, for example, about 12.6.

[0139] The resulting particle size distribution is determined according to ASTM B214.

[0140] The yield results are as follows: [Table 3]

[0141] A typical chemical composition obtained for the Ti-6Al-2Sn-4Zr-2Mo-0.08Si powder is as follows: [Table 4]

[0142] Example 3 - Zr atomization The plasma atomization operation is accomplished using a 0.080 inch diameter wire of zirconium as the feedstock and three converging plasma jets oriented at approximately 30° to the vertical axis. The plasma contacts the metal wire less than 2.0 centimeters from the plasma torch nozzle exit. Each plasma torch is operated at 30 kW power with 150 SLM argon gas flow.

[0143] A background sheath gas is also used to ensure proper transport of the metal droplets. The sheath gas flow rate is 550 SLM.

[0144] A direct current of 115 A at a potential of 45 V is used to preheat the wire to a high temperature prior to atomization by the plasma jet, resulting in a wire feed rate of 6.0 kg / h. The wire is gas-cooled and fed through adjustable guides to allow continuous metal delivery right at the apex of the plasma torch jet. Batch sizes are typically 50 kg for the run.

[0145] The gas to metal ratio in these production runs is, for example, about 17.8.

[0146] The resulting particle size distribution is determined according to ASTM B214.

[0147] The yield results are as follows: [Table 5]

[0148] A typical chemical composition obtained for the zirconium powder is as follows: [Table 6]

[0149] It will be understood that, for brevity and clarity of the diagrammatic description, where considered appropriate, reference numerals may be repeated among the figures to indicate corresponding or similar elements or steps. Additionally, numerous specific details are shown to provide a thorough understanding of the exemplary embodiments described herein. However, those skilled in the art will understand that the embodiments described herein may be practiced without these specific details. In other instances, well-known methods, procedures, and components have not been described in detail so as not to obscure the embodiments described herein. Furthermore, this description should in no way be considered as limiting the scope of the embodiments described herein, but merely as illustrating the implementation of various embodiments described herein. <Appendix 1> <Section 1> A method for producing plasma atomized metal powder, comprising the steps of: Providing a heated metal source; and contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source, wherein the atomization is carried out by using a gas to metal ratio of less than about 20, thereby obtaining a raw metal powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214. <Section 2> The manufacturing method described in <Item 1>, wherein the gas to metal ratio is less than about 17. <Section 3> The method according to <Item 1>, wherein the gas to metal ratio is about 5 to about 15. <Section 4> The method according to <Item 1>, wherein the gas to metal ratio is about 2 to about 10. <Section 5> The method for producing the present invention described in <Item 1>, wherein the gas to metal ratio is about 5 to about 10. <Section 6> The method according to <Item 1>, wherein the gas to metal ratio is about 10 to about 20. <Section 7> The method for producing the present invention described in <Item 1>, wherein the gas to metal ratio is about 10 to about 15. <Section 8> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of at least 90% from 0 to 106 microns as measured according to ASTM B214. <Section 9> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 75 microns of at least 85% as measured according to ASTM B214. <Section 10> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 50% as measured according to ASTM B214. <Section 11> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 60% as measured according to ASTM B214. <Section 12> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the heated metal source is in contact with the plasma at a vertex of the at least one plasma source. <Section 13> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 14> The manufacturing method described in any one of <Item 1> to <Item 11>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, and the individual nozzles are positioned at angles around the heated metal source. <Section 15> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 16> The manufacturing method according to any one of <Item 1> to <Item 15>, wherein the heated metal source is selected from a wire, a rod, and a molten stream. <Section 17> The manufacturing method according to any one of <Item 1> to <Item 16>, wherein the heated metal source is a wire heated by at least one of resistance heating, arc discharge, and induction heating. <Section 18> The manufacturing method according to any one of <Item 1> to <Item 16>, wherein the heated metal source is a rod heated by at least one of resistance heating, arc discharge, and induction heating. <Section 19> The manufacturing method according to any one of <Item 1> to <Item 16>, wherein the heated metal source is a heated molten stream obtained from a skull melt or a water-cooled crucible. <Section 20> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated molten source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals. <Section 21> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated melt source is selected from titanium, a titanium alloy, zirconium, a zirconium alloy, aluminum, and an aluminum alloy. <Section 22> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated melt source is selected from a titanium alloy. <Section 23> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated melt source is Ti-6Al-4V. <Section 24> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated melt source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 25> The heated melt source is selected from unalloyed Ti grades (e.g., grades 1, 2, 3, or 4), Pd or Ru modified Ti alloys (e.g., grades 7, 11, 16, 17, 26, or 27), alpha and near alpha Ti alloys (e.g., grades 6, 9, 12, 18, 28), alpha-beta Ti alloys (e.g., grades 5, 23, or 29), and near beta and beta Ti alloys (e.g., grades 19 or 20). The manufacturing method according to any one of <Item 1> to <Item 19>. <Section 26> The method according to any one of <Item 1> to <Item 19>, wherein the metal powder is a reactive metal powder. <Section 27> A method for producing plasma atomized metal powder, comprising the steps of: Providing a heated metal source; aligning the heated metal source with a plasma of at least one plasma source; and contacting the heated metal source with the plasma of the at least one plasma source under conditions effective to cause atomization of the heated metal source. <Section 28> The manufacturing method according to <Item 27>, wherein the heated metal source is one of a metal wire or a metal rod. <Section 29> The manufacturing method described in <Item 27> or <Item 28>, wherein the heated metal source is aligned with the apex of the plasma of the at least one plasma source. <Section 30> The manufacturing method described in any one of <Item 27> to <Item 29>, wherein aligning the heated metal source with the plasma of at least one plasma source includes positioning the heated metal source within a maximum of 5 centimeters of an exit nozzle of the at least one plasma source. <Section 31> A manufacturing method described in any one of <Item 27> to <Item 29>, wherein aligning the heated metal source with the plasma of at least one plasma source includes positioning the heated metal source within a maximum of 2.5 centimeters of an exit nozzle of the at least one plasma source. <Section 32> A manufacturing method described in any one of <Item 27> to <Item 29>, wherein aligning the heated metal source with the plasma of at least one plasma source includes positioning the heated metal source within a maximum of 1.9 centimeters of an exit nozzle of the at least one plasma source. <Section 33> The manufacturing method described in any one of <Item 27> to <Item 32>, wherein the alignment includes intermittently adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source. <Section 34> The manufacturing method described in <Item 33>, wherein the intermittent adjustment of the orientation of the heated metal source includes pivoting the heated metal source about a pivot point positioned upstream of and remote from the plasma of the at least one plasma source. <Section 35> The manufacturing method described in any one of <Item 27> to <Item 34>, wherein the alignment includes positioning a guide member defining a channel upstream of the plasma, and displacing the heated metal source through the channel of the guide member. <Section 36> The manufacturing method described in <Item 33> further comprises cooling the guide member by at least one of a gas source and a liquid source. <Section 37> The manufacturing method described in <Item 35> or <Item 36>, wherein the intermittent adjustment of the orientation of the heated metal source includes pivoting the heated metal source about a pivot point positioned upstream of and remote from the plasma of the at least one plasma source. <Section 38> The method for producing a semiconductor device according to any one of <Item 33> to <Item 36>, wherein an outlet of the channel is positioned in the vicinity of the plasma. <Section 39> The method for producing a metal source according to any one of <Item 33> to <Item 36>, wherein the guide member limits contamination of the heated metal source. <Section 40> The manufacturing method described in <Item 39>, wherein the inner surface of the guide member that defines the channel is formed of a non-contaminating material. <Section 41> The manufacturing method according to item 39 or 40, wherein the inner surface of the guide member that defines the channel is formed of an electrically insulating material. <Section 42> The manufacturing method according to any one of <Item 27> to <Item 41>, further comprising heating the heated metal source by at least one of resistance heating, arc discharge, and induction heating. <Section 43> The atomization is carried out by using a gas-to-metal ratio of less than about 20, thereby obtaining a metal powder having a 0-106 micron distribution yield of at least 80%. The manufacturing method according to any one of <Item 27> to <Item 41>. <Section 44> The manufacturing method according to <Item 43>, wherein the gas to metal ratio is less than about 17. <Section 45> The method according to <Item 43>, wherein the gas to metal ratio is about 5 to about 15. <Section 46> The method according to <Item 43>, wherein the gas to metal ratio is about 5 to about 10. <Section 47> The method according to <Item 43>, wherein the gas to metal ratio is about 2 to about 10. <Section 48> The method according to <Item 43>, wherein the gas to metal ratio is about 10 to about 20. <Section 49> The method according to <Item 43>, wherein the gas to metal ratio is about 10 to about 15. <Section 50> The method according to any one of <Item 43> to <Item 49>, wherein the obtained raw metal powder has a particle size distribution yield of 0 to 106 microns of at least 90% as measured according to ASTM B214. <Section 51> The method according to any one of <Item 43> to <Item 49>, wherein the obtained raw metal powder has a particle size distribution yield of 0 to 75 microns of at least 30% as measured according to ASTM B214. <Section 52> The method according to any one of <Item 43> to <Item 49>, wherein the obtained raw metal powder has a 0 to 45 micron distribution yield of at least 50% as measured according to ASTM B214. <Section 53> The method according to any one of <Item 43> to <Item 49>, wherein the obtained raw metal powder has a 0 to 45 micron distribution yield of at least 60% as measured according to ASTM B214. <Section 54> The manufacturing method according to any one of <Item 43> to <Item 53>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 55> The manufacturing method described in any one of <Item 43> to <Item 53>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 56> The manufacturing method according to any one of <Item 43> to <Item 53>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 57> The manufacturing method according to any one of <Item 27> to <Item 56>, wherein the heated molten source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals. <Section 58> The manufacturing method according to any one of <Item 27> to <Item 56>, wherein the heated melt source is selected from titanium, a titanium alloy, zirconium, a zirconium alloy, aluminum, and an aluminum alloy. <Section 59> The manufacturing method according to any one of <Item 26> to <Item 56>, wherein the heated melt source is selected from a titanium alloy. <Section 60> The manufacturing method according to any one of <Item 27> to <Item 56>, wherein the heated melt source is Ti-6Al-4V. <Section 61> The manufacturing method according to any one of <Item 27> to <Item 56>, wherein the heat melting source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 62> The heated melt source is selected from unalloyed Ti grades (e.g., grades 1, 2, 3, or 4), Pd or Ru modified Ti alloys (e.g., grades 7, 11, 16, 17, 26, or 27), alpha and near alpha Ti alloys (e.g., grades 6, 9, 12, 18, 28), alpha-beta Ti alloys (e.g., grades 5, 23, or 29), and near beta and beta Ti alloys (e.g., grades 19 or 20). The manufacturing method according to any one of <Item 27> to <Item 56>. <Section 63> The method according to any one of <Item 27> to <Item 56>, wherein the metal powder is a reactive metal powder. <Section 64> 1. An atomization system comprising: at least one heating system for heating the metal source; at least one plasma source configured to contact the metal source after heating with a plasma under conditions effective to cause atomization of the heated metal source; an alignment system positioned upstream of the at least one plasma source, the alignment system adapted to adjust an orientation of the metal source relative to the at least one plasma source. <Section 65> The atomization system described in <Item 64>, wherein the alignment system includes a guide member defining a channel upstream of the plasma, the channel further defining a displacement path of the metal source. <Section 66> The atomization system described in <Item 65>, wherein the alignment system further includes an inlet for receiving at least one of a gas source and a liquid source for cooling the guide member. <Section 67> An atomization system as described in <Item 65> or <Item 66>, wherein the outlet of the channel is positioned in proximity to the plasma. <Section 68> The atomization system according to any one of <Item 65> to <Item 67>, wherein the guide member limits contamination of the heated metal source. <Section 69> An atomizing system according to any one of <Item 65> to <Item 68>, wherein an inner surface of the guide member that defines the channel is formed of an electrically insulating material. <Section 70> The atomizing system according to any one of <Item 65> to <Item 69>, wherein the inner surface of the guide member is made of ceramic. <Section 71> The atomization system according to any one of <Item 65> to <Item 70>, wherein the guide member extends substantially between a feeding device for feeding the metal source and the plasma. <Section 72> An atomization system described in any one of <Item 64> to <Item 71>, wherein the alignment system comprises a displaceable member connected to the metal source, and displacement of the displaceable member causes a change in orientation of the metal source relative to the plasma. <Section 73> The atomization system described in <Item 72>, wherein the alignment system further comprises a pivot connected to the metal source, and the displacement of the displaceable member causes rotation of the metal source about the pivot, thereby causing the changing orientation of the metal source. <Section 74> The atomization system according to any one of <Item 64> to <Item 73>, wherein the at least one heating system is selected from resistance heating, arc discharge, and induction heating. <Section 75> The atomization system described in <Item 71>, wherein the at least one heating system is selected from resistance heating, arc discharge, and induction heating positioned around or within the guide member. <Section 76> The atomizing system according to any one of <Item 64> to <Item 75>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 77> An atomization system described in any one of <Item 64> to <Item 75>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 78> The atomization system according to any one of <Item 64> to <Item 75>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 79> A method for producing plasma atomized metal powder, comprising the steps of: Providing a heated metal source; and contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source, thereby obtaining a raw metal powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214. <Section 80> The manufacturing method according to <Item 79>, wherein the gas to metal ratio is less than about 20. <Section 81> The manufacturing method according to <Item 79>, wherein the gas to metal ratio is less than about 17. <Section 82> The method of claim 79, wherein the gas to metal ratio is about 5 to about 15. <Section 83> The method according to item 79, wherein the gas to metal ratio is about 2 to about 10. <Section 84> 80. The method of claim 79, wherein the gas to metal ratio is about 5 to about 10. <Section 85> The method of claim 79, wherein the gas to metal ratio is about 10 to about 20. <Section 86> The method of claim 79, wherein the gas to metal ratio is about 10 to about 15. <Section 87> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the raw metal powder has a particle size distribution yield of at least 90% from 0 to 106 microns, as measured according to ASTM B214. <Section 88> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the raw metal powder has a particle size distribution yield of at least 85% from 0 to 75 microns, as measured according to ASTM B214. <Section 89> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 50% as measured according to ASTM B214. <Section 90> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 60% as measured according to ASTM B214. <Section 91> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the heated metal source contacts the plasma at a vertex of the at least one plasma source. <Section 92> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 93> The manufacturing method described in any one of <Item 79> to <Item 86>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 94> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 95> The manufacturing method according to any one of <Item 79> to <Item 86>, wherein the heated metal source is selected from a wire, a rod, and a molten stream. <Section 96> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated metal source is a wire heated by at least one of resistance heating, arc discharge, and induction heating. <Section 97> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated metal source is a rod heated by at least one of resistance heating, arc discharge, and induction heating. <Section 98> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated metal source is a heated molten stream obtained from a skull melt or a water-cooled crucible. <Section 99> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated molten source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals. <Section 100> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated melt source is selected from titanium, titanium alloys, zirconium, zirconium alloys, aluminum, and aluminum alloys. <Section 101> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated melting source is selected from a titanium alloy. <Section 102> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated melt source is Ti-6Al-4V. <Section 103> The manufacturing method according to any one of <Item 79> to <Item 95>, wherein the heated melt source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 104> The heated melt source is selected from unalloyed Ti grades (e.g., grades 1, 2, 3, or 4), Pd or Ru modified Ti alloys (e.g., grades 7, 11, 16, 17, 26, or 27), alpha and near alpha Ti alloys (e.g., grades 6, 9, 12, 18, 28), alpha-beta Ti alloys (e.g., grades 5, 23, or 29), and near beta and beta Ti alloys (e.g., grades 19 or 20). The manufacturing method according to any one of <Item 79> to <Item 95>. <Section 105> The method according to any one of <Item 79> to <Item 95>, wherein the metal powder is a reactive metal powder. <Appendix 2> <Section 1> 1. A method for producing plasma atomized metal powder, comprising: Providing a heated metal source; aligning the heated metal source with the plasma of at least one plasma source, the aligning including positioning the heated metal source within a maximum of 5 centimeters of an exit nozzle of the at least one plasma source; and contacting the heated metal source with the plasma of the at least one plasma source under conditions effective to cause atomization of the heated metal source, wherein the atomization is carried out by using a total gas to metal mass ratio of less than about 20, thereby obtaining a raw metal powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214. <Section 2> The manufacturing method described in <Item 1>, wherein the total gas to metal mass ratio is less than about 17. <Section 3> The method according to <Item 1>, wherein the total gas to metal mass ratio is about 5 to about 15. <Section 4> The method according to <Item 1>, wherein the total gas to metal mass ratio is about 2 to about 10. <Section 5> The method according to <Item 1>, wherein the total gas to metal mass ratio is about 5 to about 10. <Section 6> The method according to <Item 1>, wherein the total gas to metal mass ratio is about 10 to about 20. <Section 7> The method according to <Item 1>, wherein the total gas to metal mass ratio is about 10 to about 15. <Section 8> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of at least 90% from 0 to 106 microns as measured according to ASTM B214. <Section 9> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 75 microns of at least 85% as measured according to ASTM B214. <Section 10> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 50% as measured according to ASTM B214. <Section 11> The manufacturing method according to any one of <Item 1> to <Item 7>, wherein the raw metal powder has a particle size distribution yield of 0 to 45 microns of at least 60% as measured according to ASTM B214. <Section 12> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the heated metal source is in contact with the plasma at a vertex of the at least one plasma source. <Section 13> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 14> The manufacturing method described in any one of <Item 1> to <Item 11>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, and the individual nozzles are positioned at angles around the heated metal source. <Section 15> The manufacturing method according to any one of <Item 1> to <Item 11>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 16> The manufacturing method according to any one of <Item 1> to <Item 15>, wherein the heated metal source is selected from a wire, a rod, and a molten stream. <Section 17> The manufacturing method according to any one of <Item 1> to <Item 15>, wherein the heated metal source is a wire heated by at least one of resistance heating, arc discharge, and induction heating. <Section 18> The manufacturing method according to any one of <Item 1> to <Item 15>, wherein the heated metal source is a rod heated by at least one of resistance heating, arc discharge, and induction heating. <Section 19> The manufacturing method according to any one of <Item 1> to <Item 15>, wherein the heated metal source is a heated molten stream obtained from a skull melt or a water-cooled crucible. <Section 20> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated metal source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals. <Section 21> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated metal source is selected from titanium, a titanium alloy, zirconium, a zirconium alloy, aluminum, and an aluminum alloy. <Section 22> The method for producing a metal source according to any one of <Item 1> to <Item 19>, wherein the heated metal source is selected from a titanium alloy. <Section 23> The method for producing a metal source according to any one of <Item 1> to <Item 19>, wherein the heated metal source is Ti-6Al-4V. <Section 24> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated metal source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 25> The manufacturing method according to any one of <Item 1> to <Item 19>, wherein the heated metal source is selected from non-alloyed Ti grades, Ti alloys modified with Pd or Ru, alpha and near alpha Ti alloys, alpha-beta Ti alloys, and near beta and beta Ti alloys. <Section 26> The method according to any one of <Item 1> to <Item 19>, wherein the metal powder is a reactive metal powder. <Section 27> The manufacturing method described in any one of <Item 1> to <Item 26>, wherein aligning the heated metal source with the plasma of at least one plasma source includes positioning the heated metal source within a maximum of 2.5 centimeters of the exit nozzle of the at least one plasma source. <Section 28> The manufacturing method described in any one of <Item 1> to <Item 26>, wherein aligning the heated metal source with the plasma of at least one plasma source includes positioning the heated metal source within a maximum of 1.9 centimeters of the exit nozzle of the at least one plasma source. <Section 29> 1. A method for producing plasma atomized metal powder, comprising: Providing a heated metal source; contacting the heated metal source with a plasma of at least one plasma source under conditions effective to cause atomization of the heated metal source; and aligning the heated metal source with a guide member that receives the heated metal source during the atomization, the alignment including adjusting an orientation of the guide with a displaceable member coupled to the guide to maintain alignment of the heated metal source with the plasma of the at least one plasma source. <Section 30> The manufacturing method according to <Item 29>, wherein the heated metal source is one of a metal wire or a metal rod. <Section 31> The manufacturing method according to item 29 or 30, wherein the heated metal source is aligned with the apex of the plasma of the at least one plasma source. <Section 32> A manufacturing method described in any one of <Item 29> to <Item 31>, wherein aligning the heated metal source with the plasma of the at least one plasma source includes positioning the heated metal source within a maximum of 5 centimeters of an exit nozzle of the at least one plasma source. <Section 33> A manufacturing method described in any one of <Item 29> to <Item 31>, wherein aligning the heated metal source with the plasma of the at least one plasma source includes positioning the heated metal source within a maximum of 2.5 centimeters of an exit nozzle of the at least one plasma source. <Section 34> A manufacturing method described in any one of <Item 29> to <Item 31>, wherein aligning the heated metal source with the plasma of the at least one plasma source includes positioning the heated metal source within a maximum of 1.9 centimeters of an exit nozzle of the at least one plasma source. <Section 35> The manufacturing method described in <Item 29> or <Item 34>, wherein the adjusting of the orientation of the heated metal source includes pivoting the heated metal source about a pivot point positioned upstream of and remote from the plasma of the at least one plasma source. <Section 36> The alignment may include: positioning a guide member upstream of the plasma to define a channel; and displacing the heated metal source through the channel of the guide member. <Section 37> The manufacturing method described in <Item 36> further comprises cooling the guide member by at least one of a gas source and a liquid source. <Section 38> The alignment may include: positioning a guide member upstream of the plasma to define a channel; displacing the heated metal source through the channel of the guide member; The manufacturing method described in <Item 29>, wherein the outlet of the channel is positioned in the vicinity of the plasma. <Section 39> The manufacturing method according to any one of <Item 34> to <Item 37>, wherein the guide member limits contamination of the heated metal source. <Section 40> The manufacturing method described in <Item 39>, wherein the inner surface of the guide member that defines the channel is formed of a non-contaminating material. <Section 41> The manufacturing method described in <Item 39>, wherein the inner surface of the guide member that defines the channel is formed of an electrically insulating material. <Section 42> The manufacturing method according to any one of <Item 29> to <Item 41>, further comprising heating the heated metal source by at least one of resistance heating, arc discharge, and induction heating. <Section 43> The atomization is carried out by using a total gas to metal mass ratio of less than about 20, thereby obtaining a metal powder having a 0 to 106 micron distribution yield of at least 80%. The manufacturing method according to any one of <Item 29> to <Item 41>. <Section 44> The manufacturing method according to <Item 43>, wherein the total gas to metal mass ratio is less than about 17. <Section 45> The method according to <Item 43>, wherein the total gas to metal mass ratio is about 5 to about 15. <Section 46> The method according to <Item 43>, wherein the total gas to metal mass ratio is about 5 to about 10. <Section 47> The method according to <Item 43>, wherein the total gas to metal mass ratio is about 2 to about 10. <Section 48> The method according to <Item 43>, wherein the total gas to metal mass ratio is about 10 to about 20. <Section 49> The method according to <Item 43>, wherein the total gas to metal mass ratio is about 10 to about 15. <Section 50> The method according to any one of <Item 43> to <Item 49>, wherein the obtained metal powder has a particle size distribution yield of at least 90% from 0 to 106 microns, as measured according to ASTM B214. <Section 51> The method according to any one of <Item 43> to <Item 49>, wherein the obtained metal powder has a particle size distribution yield of 0 to 75 microns of at least 30% as measured according to ASTM B214. <Section 52> The method according to any one of <Item 43> to <Item 49>, wherein the obtained metal powder has a 0 to 45 micron distribution yield of at least 50% as measured according to ASTM B214. <Section 53> The method according to any one of <Item 43> to <Item 49>, wherein the obtained metal powder has a 0 to 45 micron distribution yield of at least 60% as measured according to ASTM B214. <Section 54> The manufacturing method according to any one of <Item 43> to <Item 53>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 55> The manufacturing method described in any one of <Item 43> to <Item 53>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 56> The manufacturing method according to any one of <Item 43> to <Item 53>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 57> The manufacturing method according to any one of <Item 29> to <Item 56>, wherein the heated metal source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, tungsten alloys, oxygen-reactive metals, and nitrogen-reactive metals. <Section 58> The manufacturing method according to any one of <Item 29> to <Item 56>, wherein the heated metal source is selected from titanium, a titanium alloy, zirconium, a zirconium alloy, aluminum, and an aluminum alloy. <Section 59> The manufacturing method according to any one of <Item 28> to <Item 56>, wherein the heated metal source is selected from a titanium alloy. <Section 60> The method according to any one of <Item 29> to <Item 56>, wherein the heated metal source is Ti-6Al-4V. <Section 61> The manufacturing method according to any one of <Item 29> to <Item 56>, wherein the heating metal source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 62> The manufacturing method according to any one of <Item 29> to <Item 56>, wherein the heated metal source is selected from non-alloyed Ti grades, Ti alloys modified with Pd or Ru, alpha and near alpha Ti alloys, alpha-beta Ti alloys, and near beta and beta Ti alloys. <Section 63> The method according to any one of <Item 29> to <Item 56>, wherein the metal powder is a reactive metal powder. <Section 64> 1. An atomization system comprising: at least one heating system for heating the metal source; at least one plasma source configured to contact the heated metal source after heating with a plasma under conditions effective to cause atomization of the heated metal source; an alignment system positioned upstream of the at least one plasma source to cause a change in orientation of the heated metal source relative to the plasma during the atomization, the alignment system comprising a displaceable member connected to the heated metal source and a pivot point connected to the heated metal source, wherein displacement of the displaceable member causes the heated metal source to rotate about the pivot point. <Section 65> The atomization system described in <Item 64>, wherein the alignment system includes a guide member defining a channel upstream of the plasma, the channel further defining a displacement path of the heated metal source. <Section 66> The atomization system described in <Item 65>, wherein the alignment system further includes an inlet for receiving at least one of a gas source and a liquid source for cooling the guide member. <Section 67> An atomization system as described in <Item 65> or <Item 66>, wherein the outlet of the channel is positioned in proximity to the plasma. <Section 68> The atomization system according to any one of <Item 65> to <Item 66>, wherein the guide member limits contamination of the heated metal source. <Section 69> An atomizing system according to any one of <Item 65> to <Item 68>, wherein an inner surface of the guide member that defines the channel is formed of an electrically insulating material. <Section 70> The atomizing system according to any one of <Item 65> to <Item 68>, wherein the inner surface of the guide member is made of ceramic. <Section 71> The atomization system according to any one of <Item 65> to <Item 70>, wherein the guide member extends substantially between a feeding device for feeding the metal source and the plasma. <Section 72> The atomization system according to any one of <Item 64> to <Item 71>, wherein the at least one heating system is selected from resistance heating, arc discharge, and induction heating. <Section 73> The atomization system described in <Item 71>, wherein the at least one heating system is selected from resistance heating, arc discharge, and induction heating positioned around or within the guide member. <Section 74> The atomizing system according to any one of <Item 64> to <Item 73>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 75> An atomization system described in any one of <Item 64> to <Item 73>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 76> The atomization system according to any one of <Item 64> to <Item 73>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 77> 1. A method for producing plasma atomized metal powder, comprising: providing a heated metal source comprising at least one member selected from titanium and titanium alloys; aligning the heated metal source with the plasma of at least one plasma source, the aligning including positioning the heated metal source within a maximum of 2.5 centimeters of an exit nozzle of the at least one plasma source; and contacting the heated metal source with the plasma of the at least one plasma source under conditions effective to cause atomization of the heated metal source, wherein the atomization is carried out by using a total gas to metal mass ratio of less than about 20, thereby obtaining a raw titanium-containing powder having a 0-106 micron particle size distribution yield of at least 80% as measured in accordance with ASTM B214. <Section 78> The manufacturing method described in <Item 77>, wherein the total gas to metal mass ratio is less than about 20. <Section 79> The manufacturing method according to <Item 77>, wherein the total gas to metal mass ratio is less than about 17. <Section 80> The manufacturing method described in <Item 77>, wherein the total gas to metal mass ratio is about 5 to about 15. <Section 81> The manufacturing method according to <Item 77>, wherein the total gas to metal mass ratio is about 2 to about 10. <Section 82> The manufacturing method described in <Item 77>, wherein the total gas to metal mass ratio is about 5 to about 10. <Section 83> The manufacturing method described in <Item 77>, wherein the total gas to metal mass ratio is about 10 to about 20. <Section 84> The manufacturing method described in <Item 77>, wherein the total gas to metal mass ratio is about 10 to about 15. <Section 85> The method according to any one of <Item 77> to <Item 84>, wherein the raw titanium powder has a particle size distribution yield of 0 to 106 microns of at least 90% as measured according to ASTM B214. <Section 86> The manufacturing method according to any one of <Item 77> to <Item 84>, wherein the raw titanium powder has a 0 to 75 micron particle size distribution yield of at least 85% as measured according to ASTM B214. <Section 87> The method according to any one of <Item 77> to <Item 84>, wherein the raw titanium powder has a 0 to 45 micron particle size distribution yield of at least 50% as measured according to ASTM B214. <Section 88> The method according to any one of <Item 77> to <Item 84>, wherein the raw titanium powder has a 0 to 45 micron particle size distribution yield of at least 60% as measured according to ASTM B214. <Section 89> The manufacturing method according to any one of <Item 77> to <Item 84>, wherein the heated metal source contacts the plasma at a vertex of the at least one plasma source. <Section 90> The manufacturing method according to any one of <Item 77> to <Item 84>, wherein the plasma is emitted from at least one individual nozzle of the at least one plasma source. <Section 91> The manufacturing method described in any one of <Item 77> to <Item 84>, wherein the plasma is emitted from a plurality of individual nozzles of the at least one plasma source, the individual nozzles being positioned at angles around the heated metal source. <Section 92> The manufacturing method according to any one of <Item 77> to <Item 84>, wherein the plasma is emitted from an annular nozzle of the at least one plasma source. <Section 93> The manufacturing method according to any one of <Item 77> to <Item 84>, wherein the heated metal source is selected from a wire, a rod, and a molten stream. <Section 94> The manufacturing method according to any one of <Item 77> to <Item 92>, wherein the heated metal source is a wire heated by at least one of resistance heating, arc discharge, and induction heating. <Section 95> The manufacturing method according to any one of <Item 77> to <Item 92>, wherein the heated metal source is a rod heated by at least one of resistance heating, arc discharge, and induction heating. <Section 96> The manufacturing method according to any one of <Item 77> to <Item 92>, wherein the heated metal source is a heated molten stream obtained from a skull melt or a water-cooled crucible. <Section 97> The manufacturing method according to any one of <Item 77> to <Item 93>, wherein the heated metal source is a titanium alloy. <Section 98> The manufacturing method according to any one of <Item 77> to <Item 93>, wherein the heated metal source is selected from a titanium alloy. <Section 99> The manufacturing method according to any one of <Item 77> to <Item 93>, wherein the heated metal source is Ti-6Al-4V. <Section 100> The manufacturing method according to any one of <Item 77> to <Item 93>, wherein the heated metal source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminide. <Section 101> The manufacturing method according to any one of <Item 77> to <Item 93>, wherein the heated metal source is selected from non-alloyed Ti grades, Ti alloys modified with Pd or Ru, alpha and near alpha Ti alloys, alpha-beta Ti alloys, and near beta and beta Ti alloys. <Section 102> The method according to any one of <Item 77> to <Item 93>, wherein the metal powder is a reactive metal powder. <Section 103> A manufacturing method described in any one of <Item 77> to <Item 102>, wherein the heated metal source is positioned within a maximum of 1.9 centimeters of the exit nozzle of the at least one plasma source. <Section 104> The alignment may include: A manufacturing method described in any one of <Item 77> to <Item 103>, comprising intermittently adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source. <Section 105> The manufacturing method described in <Item 104>, wherein the intermittent adjustment of the orientation of the heated metal source includes pivoting the heated metal source about a pivot point positioned remotely upstream of the plasma of the at least one plasma source. <Section 106> The alignment may include: positioning a guide member upstream of the plasma to define a channel; and displacing the heated metal source through the channel of the guide member. <Section 107> The manufacturing method described in <Item 106> further comprises cooling the guide member with at least one of a gas source and a liquid source. <Section 108> The manufacturing method according to item 25, item 62 or item 101, wherein the heated metal source is unalloyed Ti of grade 1, 2, 3 or 4. <Section 109> The manufacturing method according to item 25, item 62 or item 101, wherein the heated metal source is a Ti alloy modified with Pd or Ru of grade 7, 11, 16, 17, 26 or 27. <Section 110> The manufacturing method according to item 25, item 62 or item 101, wherein the heated metal source is an alpha and near alpha Ti alloy of grade 6, 9, 12, 18 or 28. <Section 111> The manufacturing method according to item 25, item 62 or item 101, wherein the heated metal source is an alpha-beta Ti alloy of grade 5, 23 or 29. <Section 112> The manufacturing method according to item 25, item 62 or item 101, wherein the heated metal source is a grade 19 or 20 near beta and beta Ti alloy.

Claims

1. 1. A method for producing plasma atomized metal powder, comprising: contacting a heated metal source with a plasma of at least one plasma source under conditions effective to cause plasma atomization of the heated metal source; supplying a secondary high pressure gas toward an atomization zone; and contacting the secondary high pressure gas with a metal source previously atomized in contact with the plasma to produce a secondary atomization; said plasma atomization under effective conditions being carried out with a mass per unit time (Kg / s) of gas injected relative to a mass velocity (Kg / s) of said metal source into an atomization zone of less than 17, to obtain a raw metal powder having a particle size distribution yield of 0-106 microns of at least 80% by weight, as measured according to ASTM B214-07(2011); 1. The method of claim 1, wherein the heated metal source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, aluminum, aluminum alloys, molybdenum, molybdenum alloys, tungsten, and tungsten alloys.

2. aligning the heated metal source with the plasma of the at least one plasma source; The method of claim 1 further comprising:

3. The method of claim 1 or 2, wherein the at least one plasma source comprises a plasma jet.

4. The method of any one of claims 1 to 3, wherein the at least one plasma source comprises a plurality of individual nozzles, the individual nozzles being positioned at angles around the heated metal source.

5. The method according to any one of claims 1 to 4, wherein the mass per unit time (Kg / s) of the gas injected relative to the mass velocity (Kg / s) of the metal source is 5 to 15.

6. The method of any one of claims 1 to 5, wherein the heated metal source is a wire, a rod, a molten stream, or a combination thereof.

7. The method of any one of claims 1 to 5, wherein the heated metal source is a molten stream.

8. The method of any one of claims 1 to 7, wherein the heated metal source is a wire heated by resistance heating, arc discharge, induction heating, or a combination thereof.

9. The method of any one of claims 1 to 8, wherein the raw metal powder has a 0 to 106 micron particle size distribution yield of at least 90% by weight as measured according to ASTM B214-07(2011).

10. 10. The method of any one of claims 1 to 9, wherein the heated metal source comprises at least one member selected from one of titanium, titanium alloys, zirconium, zirconium alloys, cobalt superalloys, nickel superalloys, magnesium, magnesium alloys, niobium, niobium alloys, molybdenum, molybdenum alloys, tungsten, and tungsten alloys.

11. The method of any one of claims 1 to 9, wherein the heated metal source comprises titanium, zirconium, magnesium, aluminum, or a combination thereof.

12. The method of any one of claims 1 to 9, wherein the heated metal source is a titanium alloy.

13. The method of any one of claims 1 to 9, wherein the heated metal source is selected from Ti-6Al-4V, Ti-6Al-2Sn-4Zr-2Mo, Ti-5Al-5V-5Mo-3Cr, and titanium aluminides.

14. The method of any one of claims 1 to 13, wherein aligning the heated metal source comprises adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source.

15. The method of any one of claims 1 to 13, wherein aligning the heated metal source comprises adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source, and the aligning further comprises moving the heated metal source to adjust its orientation.

16. aligning the heated metal source includes aligning the heated metal source by means of a guide member receiving the heated metal source through the guide member during plasma atomization; The method of any one of claims 1 to 15, wherein the aligning further comprises adjusting an orientation of the guide member to which a displaceable member is coupled, thereby adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source.

17. The method of any one of claims 1 to 16, wherein aligning the heated metal source comprises adjusting an orientation of the heated metal source, and adjusting the orientation of the heated metal source comprises intermittently adjusting an orientation of the heated metal source to maintain alignment of the heated metal source with the plasma of the at least one plasma source.

Citation Information

Patent Citations

  • Technological method and device for preparing high-purity spherical superfine / nanoscale powdered materials in plasma atomization mode

    CN103769594A

  • JP1974025554A

  • Method and apparatus for spraying molten liquid from nozzlesof adjacent arrangement system and product

    JP1985211003A

  • Apparatus for manufacturing metal powder

    JP1992168209A

  • Manufacturing apparatus and manufacturing method for metallic powder

    JP2001226704A