Duplex Stainless Steel Pipe
The duplex stainless steel pipe achieves high strength and pitting corrosion resistance by optimizing chemical composition and microstructure, ensuring a balanced austenite-ferrite ratio and controlled austenite width, addressing the limitations of previous technologies.
Patent Information
- Application Number
- JP2021007359
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-20
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-01-20
AI Technical Summary
Existing duplex stainless steel pipes struggle to achieve both high strength and excellent pitting corrosion resistance, particularly in chloride-containing environments, despite previous attempts to optimize chemical composition and processing methods.
A duplex stainless steel pipe with a specific chemical composition and microstructure, including 0.035% C, 0.15-0.55% Si, 0.30-1.20% Mn, 0.05-1.00% Cu, 5.00-9.00% Ni, 23.0-27.0% Cr, 2.00-6.00% Mo, 0.200-0.350% N, and a microstructure with an austenite area ratio of 45.0-65.0% and average austenite width of 4.00-10.00 μm, optimized through controlled hot working and solution treatment.
The solution results in a duplex stainless steel pipe with a tensile strength of 800 MPa or more and excellent pitting corrosion resistance, maintaining performance in humid chloride environments.
Smart Images

Figure 0007572623000003 
Figure 0007572623000004 
Figure 0007572623000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a duplex stainless steel pipe. [Background technology]
[0002] Duplex stainless steel pipes having a two-phase structure of ferrite and austenite have excellent corrosion resistance. Duplex stainless steel pipes are particularly excellent in corrosion resistance against pitting corrosion and / or crevice corrosion (hereinafter referred to as "pitting corrosion resistance"), which are problems in aqueous solutions containing chlorides. Therefore, duplex stainless steel pipes are widely used in wet environments containing chlorides, such as seawater. In wet environments containing chlorides, duplex stainless steel pipes are used, for example, for flow line pipes, umbilical tubes, and heat exchangers.
[0003] When duplex stainless steel pipes are used in the above mentioned applications in wet chloride-containing environments, the pipes require not only good pitting corrosion resistance but also high strength.
[0004] Duplex stainless steel materials that attempt to combine excellent corrosion resistance and high strength have been proposed in JP 2003-171743 A (Patent Document 1), JP 2012-153953 A (Patent Document 2), JP 61-23713 A (Patent Document 3), and Patent No. 6358411 (Patent Document 4).
[0005] In Patent Document 1 and Patent Document 2, the element contents in the chemical composition are set within appropriate ranges to attempt to achieve both corrosion resistance and high strength of the duplex stainless steel material. Specifically, the duplex stainless steel material disclosed in JP 2003-171743 A (Patent Document 1) contains, by weight ratio, C: 0.020% or less, Si: 0.30 to 1.50%, Mn: 0.50 to 1.50%, P: 0.040% or less, S: 0.015% or less, Cu: 1.0 to 3.0%, Ni: 3.00 to 5.00%, Cr: 22.00 to 28.00%, Mo: 2.00 to 5.00%, N: 0.12 to 0.25%, W: 0.50% or less, Ca: 0.0100% or less, B: 0.0100% or less, with the balance being Fe and impurity elements. This duplex stainless steel material further has a two-phase structure of ferrite and austenite, with the area ratio of the ferrite phase in the two-phase structure being 40 to 70%.
[0006] The hot-rolled duplex stainless steel disclosed in JP 2012-153953 A (Patent Document 2) is a hot-rolled steel without solution treatment, and contains, by mass%, C: 0.03% or less, Si: 0.05-1.0%, Mn: 0.5-7.0%, P: 0.05% or less, S: 0.010% or less, Ni: 0.1-5.0%, Cr: 18.0-25.0%, N: 0.05-0.30%, Al: 0.001-0.05%, with the balance being Fe and unavoidable impurities. The chromium nitride precipitation temperature TN, which is an index of chromium nitride precipitation during hot rolling of this steel, is 960° C. or less, and the yield strength is 50 MPa or more higher than that of a hot-rolled steel that has been subjected to solution treatment. The steel material disclosed in this document has the content of each element in the chemical composition adjusted so that the chromium nitride precipitation temperature TN is 960° C. or less. This makes it possible to suppress the formation of chromium nitrides during the manufacturing process, and as a result, the document states that solution treatment can be omitted.
[0007] Patent Documents 3 and 4 attempt to achieve both corrosion resistance and high strength in duplex stainless steel materials by increasing the Cu content and carrying out aging precipitation after solution treatment. Specifically, the duplex stainless steel material disclosed in JP 61-23713 A (Patent Document 3) is produced by heating a Cu-containing duplex stainless steel to 1000°C or higher and hot working it, followed by quenching it from a temperature of 800°C or higher and then carrying out aging treatment. This document states that this makes it possible to achieve both corrosion resistance and high strength even without cold working.
[0008] The duplex stainless steel material disclosed in Japanese Patent No. 6358411 (Patent Document 4) has a composition containing, by mass%, C: 0.03% or less, Si: 1.0% or less, Mn: 0.10-1.5%, P: 0.030% or less, S: 0.005% or less, Cr: 20.0-30.0%, Ni: 5.0-10.0%, Mo: 2.0-5.0%, Cu: 2.0-6.0%, N: less than 0.07%, with the balance being Fe and unavoidable impurities. The structure of the duplex stainless steel material in this document has, by volume, 20-70% austenite phase and 30-80% ferrite phase, with the balance being 1% or less precipitates, and has a yield strength YS of 655 MPa or more. In this document, an attempt is made to increase the yield strength and achieve both corrosion resistance and high strength by increasing the Cu content and carrying out aging treatment after solution treatment. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2003-171743 A [Patent Document 2] JP 2012-153953 A [Patent Document 3] Japanese Patent Publication No. 61-23713 [Patent Document 4] Patent No. 6358411 Summary of the Invention [Problem to be solved by the invention]
[0010] In the above-mentioned Patent Documents 1 to 4, attempts are made to achieve both excellent corrosion resistance and high strength by appropriately adjusting the content of each element in the chemical composition (Patent Documents 1 and 2) or increasing the strength by precipitating Cu through aging treatment (Patent Documents 3 and 4). However, it may be possible to achieve both excellent pitting resistance and high strength by using techniques other than those disclosed in the above-mentioned Patent Documents 1 to 4.
[0011] An object of the present disclosure is to provide a duplex stainless steel pipe having excellent pitting corrosion resistance and high strength. [Means for solving the problem]
[0012] The duplex stainless steel pipe according to the present disclosure comprises: In mass%, C: 0.035% or less, Si: 0.15 to 0.55%, Mn: 0.30-1.20%, P: 0.035% or less, S: 0.0100% or less, Cu: 0.05-1.00%, Ni: 5.00~9.00%, Cr: 23.0-27.0%, Mo: 2.00-6.00%, N: 0.200~0.350%, W: 0 to 1.000%, Al: 0 to 0.050%, B: 0~0.0050%, Ca: 0 to 0.0100%, and the balance being Fe and impurities, When the longitudinal direction of the duplex stainless steel pipe is defined as the L direction and the wall thickness direction is defined as the T direction, in a microstructure of the duplex stainless steel pipe at a cross section including the L direction and the T direction, The austenite area fraction is 45.0 to 65.0%. The area ratio of the σ phase is 0 to 0.05%, The average width of the austenite in the T direction is 4.00 to 10.00 μm. Effect of the Invention
[0013] The duplex stainless steel pipe according to the present disclosure has excellent pitting corrosion resistance and high strength, with a tensile strength of 800 MPa or more. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a photographic image of the microstructure at a cross section including the longitudinal direction (L direction) and wall thickness direction (T direction) of the duplex stainless steel pipe of this embodiment. [Diagram 2] FIG. 2 is a schematic diagram for explaining a method for measuring the width of austenite in the microstructure photograph image shown in FIG. [Diagram 3] FIG. 3 is an enlarged view of a portion of line segment T0 in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventor first studied a duplex stainless steel pipe capable of achieving both pitting corrosion resistance and high strength from the viewpoint of chemical composition, and as a result, the present inventor considered that a chemical composition consisting of, in mass%, C: 0.035% or less, Si: 0.15-0.55%, Mn: 0.30-1.20%, P: 0.035% or less, S: 0.0100% or less, Cu: 0.05-1.00%, Ni: 5.00-9.00%, Cr: 23.0-27.0%, Mo: 2.00-6.00%, N: 0.200-0.350%, W: 0-1.000%, Al: 0-0.050%, B: 0-0.0050%, Ca: 0-0.0100%, and the balance being Fe and impurities, may be capable of achieving both pitting corrosion resistance and high strength.
[0016] Therefore, the present inventors further focused on the microstructure of a duplex stainless steel pipe having the above chemical composition and investigated the compatibility of pitting corrosion resistance and high strength. The microstructure of a duplex stainless steel pipe having the above chemical composition is a two-phase structure consisting of ferrite and austenite. When the microstructure of a duplex stainless steel pipe is biased toward either the ferrite or austenite phase (for example, when the ratio of either phase exceeds 65.0%), the distribution of element concentrations in each phase changes. In this case, the pitting corrosion resistance of the duplex stainless steel pipe decreases. If the austenite area ratio in a duplex stainless steel pipe having the above chemical composition is 35.0 to 65.0%, the pitting corrosion resistance of the duplex stainless steel pipe can be sufficiently ensured.
[0017] On the other hand, in the case of a duplex stainless steel pipe having the above-mentioned chemical composition, the strength of austenite is higher than the strength of ferrite. Therefore, higher strength can be obtained by increasing the austenite area fraction within a range in which the pitting corrosion resistance of the duplex stainless steel pipe can be ensured. As a result of investigation based on the above-mentioned idea, the present inventors have concluded that in a duplex stainless steel pipe having the above-mentioned chemical composition, if the austenite area fraction is set to 45.0 to 65.0%, high strength can be obtained while ensuring the pitting corrosion resistance of the duplex stainless steel pipe.
[0018] However, even if the austenite area fraction is 45.0% or more, the strength is high, but it is difficult to obtain a tensile strength of 800 MPa or more. Therefore, the present inventors further focused on the distribution of austenite and ferrite in the microstructure, in addition to the area fraction of austenite in the microstructure.
[0019] Fig. 1 is a photographic image of the microstructure of a duplex stainless steel pipe of this embodiment in a cross section parallel to the longitudinal and thickness directions. The L direction in Fig. 1 means the longitudinal direction (pipe axis direction) of the duplex stainless steel pipe. The T direction in Fig. 1 means the thickness direction of the duplex stainless steel pipe. In the following description, the longitudinal direction of the duplex stainless steel pipe is defined as the "L direction" and the thickness direction is defined as the "T direction". The L direction and the T direction are perpendicular to each other.
[0020] 1, as described above, the microstructure of the duplex stainless steel pipe is composed of austenite 10 (white region 10) and ferrite 20 (black region 20). In the microstructure of the duplex stainless steel pipe, the austenite 10 extending in the L direction and the ferrite 20 extending in the L direction are stacked in the T direction. In other words, the microstructure of the duplex stainless steel pipe of this embodiment is a lamellar structure. Hereinafter, the austenite 10 extending in the L direction will also be referred to as lamellar austenite 10. The ferrite 20 extending in the L direction will also be referred to as lamellar ferrite 20.
[0021] As described above, the strength of austenite 10 is higher than that of ferrite 20. Therefore, the present inventors focused on the width (length in the T direction) of each lamellar austenite 10 in the microstructure in a cross section including the L direction and the T direction. When the microstructure is a lamellar structure of ferrite and austenite as shown in FIG. 1, it is believed that if the width of the lamellar austenite is narrow, the austenite is generated finely. It is believed that the finer the austenite, the higher the strength.
[0022] Therefore, the present inventors have investigated and examined the relationship between the average width of lamellar austenite 10 in the microstructure and the tensile strength. As a result, it has been found that if the austenite area fraction is 45.0 to 65.0% and the average width of the lamellar austenite is 10.00 μm or less in the microstructure of a cross section including the L direction and the T direction of a duplex stainless steel pipe having the above-mentioned chemical composition, the tensile strength is 800 MPa or more and excellent pitting corrosion resistance is also obtained.
[0023] The duplex stainless steel pipe according to this embodiment, which has been completed based on the above findings, has the following configuration.
[0024] [1] A duplex stainless steel pipe, In mass%, C: 0.035% or less, Si: 0.15 to 0.55%, Mn: 0.30-1.20%, P: 0.035% or less, S: 0.0100% or less, Cu: 0.05-1.00%, Ni: 5.00~9.00%, Cr: 23.0-27.0%, Mo: 2.00-6.00%, N: 0.200~0.350%, W: 0 to 1.000%, Al: 0 to 0.050%, B: 0~0.0050%, Ca: 0 to 0.0100%, and the balance being Fe and impurities, When the longitudinal direction of the duplex stainless steel pipe is defined as the L direction and the wall thickness direction is defined as the T direction, in a microstructure of the duplex stainless steel pipe at a cross section including the L direction and the T direction, The austenite area fraction is 45.0 to 65.0%. The area ratio of the σ phase is 0 to 0.05%, The average width of the austenite in the T direction is 4.00 to 10.00 μm. Duplex stainless steel pipe.
[0025] [2] A duplex stainless steel pipe according to [1], W: 0.001 to 1.000%, Al: 0.001 to 0.050%, B: 0.0001 to 0.0050%, and Ca: 0.0001 to 0.0100%, Contains one or more elements selected from the group consisting of Duplex stainless steel pipe.
[0026] The duplex stainless steel pipe according to this embodiment will be described in detail below.
[0027] [Chemical composition] The chemical composition of the duplex stainless steel pipe according to this embodiment contains the following elements: "%" for each element means mass % unless otherwise specified.
[0028] C: 0.035% or less Carbon (C) is inevitably contained. That is, the C content is more than 0%. C forms Cr carbides at the grain boundaries and increases the corrosion susceptibility at the grain boundaries. As a result, the pitting corrosion resistance of the steel material decreases. If the C content exceeds 0.035%, the pitting corrosion resistance decreases significantly even if the contents of other elements are within the range of this embodiment. Therefore, the C content is 0.035% or less. The preferred upper limit of the C content is 0.033%, more preferably 0.030%, and even more preferably 0.028%. The C content is preferably as low as possible. However, excessive reduction of the C content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, the preferred lower limit of the C content is 0.001%, and even more preferably 0.005%.
[0029] Silicon: 0.15 to 0.55% Silicon (Si) deoxidizes steel. If the Si content is less than 0.15%, this effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Si content exceeds 0.55%, the low-temperature toughness and hot workability of the steel material will decrease even if the contents of other elements are within the range of this embodiment. Therefore, the Si content is 0.15 to 0.55%. The preferred lower limit of the Si content is 0.18%, more preferably 0.20%, and even more preferably 0.30%. The preferred upper limit of the Si content is 0.54%, more preferably 0.53%, and even more preferably 0.50%.
[0030] Mn: 0.30-1.20% Manganese (Mn) deoxidizes and desulfurizes steel. If the Mn content is less than 0.30%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Mn content exceeds 1.20%, the hot workability of the steel material decreases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Mn content is 0.30 to 1.20%. The lower limit of the Mn content is preferably 0.35%, and more preferably 0.40%. The upper limit of the Mn content is preferably 1.15%, and more preferably 1.10%.
[0031] P:0.035% or less Phosphorus (P) is an impurity. The P content may be 0%. P segregates at grain boundaries and reduces the hot workability of steel. If the P content exceeds 0.035%, the hot workability is significantly reduced even if the contents of other elements are within the range of this embodiment. Therefore, the P content is 0.035% or less. A preferred upper limit of the P content is 0.032%, more preferably 0.030%. It is preferable that the P content is as low as possible. However, excessive reduction of the P content significantly increases the refining cost in the steelmaking process. Therefore, in consideration of industrial production, a preferred lower limit of the P content is 0.001%, more preferably 0.003%.
[0032] S: 0.0100% or less Sulfur (S) is an impurity. The S content may be 0%. S segregates at grain boundaries and reduces the hot workability of steel. If the S content exceeds 0.0100%, the hot workability is significantly reduced even if the contents of other elements are within the range of this embodiment. Therefore, the S content is 0.0100% or less. A preferred upper limit of the S content is 0.0080%, more preferably 0.0050%. The S content is preferably as low as possible. However, excessive reduction of the S content significantly increases the refining cost of the steelmaking process. Therefore, in consideration of industrial production, a preferred lower limit of the S content is more than 0%, more preferably 0.0001%, and even more preferably 0.0003%.
[0033] Cu: 0.05-1.00% Copper (Cu) increases the strength of steel material by solid solution strengthening. Cu also increases the pitting corrosion resistance of steel material. If the Cu content is less than 0.05%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cu content exceeds 1.00%, Cu precipitates in the steel material, and the pitting corrosion resistance is rather reduced even if the contents of other elements are within the range of this embodiment. Therefore, the Cu content is 0.05 to 1.00%. The preferred lower limit of the Cu content is 0.10%, more preferably 0.15%, and more preferably 0.20%. The preferred upper limit of the Cu content is 0.90%, more preferably 0.85%, and more preferably 0.80%.
[0034] Ni: 5.00~9.00% Nickel (Ni) stabilizes the austenite structure of steel and increases the strength of the steel. That is, Ni is an element necessary for obtaining a stable two-phase structure of ferrite and austenite. Ni also increases the pitting corrosion resistance of the steel. If the Ni content is less than 5.00%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Ni content exceeds 9.00%, even if the contents of other elements are within the range of this embodiment, a proper balance between ferrite and austenite cannot be obtained, and a duplex stainless steel pipe cannot be stably produced. Therefore, the Ni content is 5.00 to 9.00%. The preferred lower limit of the Ni content is 5.20%, more preferably 5.30%, more preferably 5.40%, and more preferably 5.50%. The preferred upper limit of the Ni content is 8.80%, more preferably 8.50%, more preferably 8.20%, and more preferably 8.00%.
[0035] Cr: 23.0~27.0% Chromium (Cr) forms a passive film on the surface of the duplex stainless steel pipe as an oxide. The passive film inhibits corrosion factors from coming into contact with the surface of the duplex stainless steel pipe. As a result, the pitting corrosion resistance of the duplex stainless steel pipe is enhanced. Cr is also an element necessary for obtaining ferrite in the duplex stainless steel pipe. By obtaining a sufficient ferrite structure, stable pitting corrosion resistance can be obtained. If the Cr content is less than 23.0%, these effects cannot be obtained sufficiently even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content exceeds 27.0%, the hot workability of the duplex stainless steel pipe decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Cr content is 23.0 to 27.0%. The preferred lower limit of the Cr content is 23.2%, more preferably 23.5%, and more preferably 24.0%. The preferred upper limit of the Cr content is 26.8%, more preferably 26.5%, and more preferably 26.0%.
[0036] Mo: 2.00-6.00% Molybdenum (Mo) is contained in the passive film and further enhances the corrosion resistance of the passive film. As a result, the pitting corrosion resistance of the duplex stainless steel pipe is improved. If the Mo content is less than 2.00%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mo content exceeds 6.00%, the hot workability of the duplex stainless steel pipe is reduced even if the contents of other elements are within the range of this embodiment. Therefore, the Mo content is 2.00 to 6.00%. The preferred lower limit of the Mo content is 2.20%, more preferably 2.30%, and more preferably 2.50%. The preferred upper limit of the Mo content is 5.80%, more preferably 5.50%, and more preferably 5.00%.
[0037] N: 0.200~0.350% Nitrogen (N) stabilizes the austenite of the steel material to increase the strength of the steel material. That is, N is an element necessary for obtaining a stable two-phase structure of ferrite and austenite. N also increases the pitting corrosion resistance of the steel material. If the N content is less than 0.200%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the N content exceeds 0.350%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the N content is 0.200 to 0.350%. The preferable lower limit of the N content is 0.220%, more preferably 0.240%, and more preferably 0.260%. The preferable upper limit of the N content is 0.340%, more preferably 0.330%, and more preferably 0.320%.
[0038] The balance of the chemical composition of the duplex stainless steel pipe according to the present embodiment is Fe and impurities. Here, the impurities in the chemical composition refer to substances that are mixed in from raw materials such as ore and scrap, or the manufacturing environment, during industrial production of the duplex stainless steel pipe, and are permissible within a range that does not adversely affect the duplex stainless steel pipe according to the present embodiment.
[0039] [About optional elements] The chemical composition of the above-mentioned duplex stainless steel pipe may further contain one or more elements selected from the group consisting of W, Al, B, and Ca in place of a portion of Fe. These elements are optional elements.
[0040] W: 0~1.000% Tungsten (W) is an optional element and may not be contained. That is, the W content may be 0%. When W is contained, W is contained in the passive film like Mo, and further enhances the corrosion resistance of the passive film. As a result, the pitting corrosion resistance of the duplex stainless steel pipe is improved. Even if even a small amount of W is contained, this effect can be obtained to a certain extent. On the other hand, if the W content exceeds 1.000%, even if the contents of other elements are within the range of this embodiment, the sigma (σ) phase is likely to precipitate. The σ phase reduces the pitting corrosion resistance of the duplex stainless steel pipe. Therefore, the W content is 0 to 1.000%. The preferable lower limit of the W content is 0.001%, more preferably 0.003%, and more preferably 0.005%. The preferable upper limit of the W content is 0.800%, more preferably 0.700%, and more preferably 0.500%.
[0041] Al: 0 to 0.050% Aluminum (Al) is an optional element and may not be contained. That is, the Al content may be 0%. When it is contained, Al deoxidizes the steel in the steelmaking process in the manufacturing process of the steel material. If even a small amount of Al is contained, the above effect can be obtained to some extent. On the other hand, if the Al content exceeds 0.050%, even if the contents of other elements are within the range of this embodiment, coarse oxide-based inclusions are generated, which reduces the toughness of the duplex stainless steel pipe, or the coarse oxide-based inclusions become the starting point of corrosion, which reduces the pitting corrosion resistance of the duplex stainless steel pipe. Therefore, the Al content is 0 to 0.050%. The preferred lower limit of the Al content is 0.001%, and more preferably 0.002%. The preferred upper limit of the Al content is 0.040%, and more preferably 0.035%, and more preferably 0.030%. The Al content in this specification means the content of total Al (Total-Al).
[0042] B: 0~0.0050% Boron (B) is an optional element and may not be contained. In other words, the B content may be 0%. When contained, B fixes S in the steel material as sulfides to render it harmless, and improves the hot workability of the steel material. If even a small amount of B is contained, the above effect can be obtained to a certain extent. On the other hand, if the B content exceeds 0.0050%, boron nitride (BN) is generated even if the contents of other elements are within the range of this embodiment, and the toughness of the steel material decreases. Therefore, the B content is 0 to 0.0050%. The preferred lower limit of the B content is 0.0001%, more preferably 0.0005%, and more preferably 0.0010%. The preferred upper limit of the B content is 0.0040%, more preferably 0.0035%, and more preferably 0.0030%.
[0043] Ca: 0 to 0.0100% Calcium (Ca) is an optional element and may not be contained. In other words, the Ca content may be 0%. When contained, Ca fixes S in the steel material as sulfides to render it harmless and improves the hot workability of the steel material. If even a small amount of Ca is contained, the above effect can be obtained to a certain extent. On the other hand, if the Ca content exceeds 0.0100%, even if the contents of other elements are within the range of this embodiment, the oxides in the steel material become coarse and the toughness of the steel material decreases. Therefore, the Ca content is 0 to 0.0100%. The preferred lower limit of the Ca content is 0.0001%, more preferably 0.0003%, and more preferably 0.0005%. The preferred upper limit of the Ca content is 0.0090%, more preferably 0.0070%, and more preferably 0.0050%.
[0044] [About the microstructure] In the microstructure of the cross section including the L direction and the T direction of the duplex stainless steel pipe of this embodiment, the area fraction of austenite is 45.0 to 65.0%, the area fraction of σ phase is 0 to 0.05%, and the remainder is ferrite. This point will be described in detail below.
[0045] [Austenite area ratio] The microstructure of the duplex stainless steel pipe according to the present embodiment in a cross section including the L direction and the T direction is composed of ferrite and austenite. In this specification, "composed of ferrite and austenite" means that phases other than ferrite and austenite (including precipitates and inclusions) are negligibly small. For example, in the microstructure of the duplex stainless steel pipe according to the present embodiment, the area ratio of precipitates and inclusions is very small compared to the area ratios of ferrite and austenite.
[0046] In the microstructure of the duplex stainless steel pipe according to the present embodiment, the area ratio of austenite is 45.0 to 65.0% in the cross section including the L direction and the T direction. In the duplex stainless steel pipe having the chemical composition of the present embodiment, the strength of austenite is higher than that of ferrite. Therefore, the higher the area ratio of austenite in the microstructure, the higher the strength of the duplex stainless steel pipe. If the area ratio of austenite is less than 45.0%, the duplex stainless steel pipe cannot obtain sufficient strength. On the other hand, if the area ratio of austenite exceeds 65.0%, the balance between austenite and ferrite in the microstructure is lost, and the pitting corrosion resistance of the duplex stainless steel pipe is reduced. Therefore, the area ratio of austenite in the microstructure is 45.0 to 65.0%. The lower limit of the area ratio of austenite is preferably 47.0%, more preferably 50.0%, and even more preferably 52.0%. The upper limit of the area ratio of austenite is preferably 63.0%, and even more preferably 60.0%.
[0047] [Area ratio of σ phase] The area ratio of the σ phase in the microstructure of the cross section including the L direction and the T direction of the duplex stainless steel pipe of this embodiment is 0 to 0.05%. The smaller the area ratio of the σ phase, the more preferable, and it is most preferably 0%. The σ phase reduces the pitting corrosion resistance of the duplex stainless steel pipe. Therefore, the area ratio of the σ phase is 0 to 0.05%. The preferred upper limit of the area ratio of the σ phase is 0.04%, more preferably 0.03%, even more preferably 0.02%, even more preferably 0.01%, and most preferably 0% (0.00%).
[0048] [Average width of austenite] FIG. 1 is a microstructure photographic image of a cross section including the longitudinal direction (L direction) and wall thickness direction (T direction) of the duplex stainless steel pipe of this embodiment. As described above, in the microstructure of FIG. 1, the white region 10 is lamellar austenite. The black region 20 is lamellar ferrite. In the microstructure of the duplex stainless steel pipe of this embodiment, the lamellar austenite 10 and the lamellar ferrite 20 form a lamellar structure. That is, both the lamellar austenite 10 and the lamellar ferrite 20 extend in the L direction (longitudinal direction) of the duplex stainless steel pipe and are stacked in the T direction (wall thickness direction). In the microstructure, the T direction length perpendicular to the L direction of each lamellar austenite 10 extending in the L direction of the duplex stainless steel pipe is defined as the "width of austenite". In this case, the average width of austenite is 4.00 to 10.00 μm in the microstructure of the cross section including the L direction and T direction of the duplex stainless steel pipe.
[0049] The narrower the average width of austenite, the greater the number of lamellar austenite 10 and lamellar ferrite 20 layers per unit thickness. In other words, the narrower the average width of austenite, the denser the lamellar structure formed. If the average width of austenite is 10.00 μm or less, the lamellar austenite and lamellar ferrite are sufficiently dense, and as a result, sufficient strength can be obtained in the duplex stainless steel pipe, provided that the above-mentioned chemical composition and austenite area ratio are satisfied. Specifically, a tensile strength of 800 MPa or more can be obtained. On the other hand, the lower limit of the average width of austenite is not particularly limited, but considering the manufacturing process described later, the lower limit of the average width of austenite is 4.00 μm. Therefore, the average width of austenite is 4.00 to 10.00 μm. The preferred upper limit of the average width of austenite is 9.50 μm, more preferably 9.20 μm, more preferably 9.00 μm, and more preferably 8.70 μm. The lower limit of the average width of austenite is preferably 4.50 μm, more preferably 5.00 μm, still more preferably 5.50 μm, and still more preferably 6.00 μm.
[0050] [How to calculate the austenite area fraction, σ phase area fraction, and average austenite width] The austenite area fraction, σ phase area fraction, and average austenite width of the microstructure in a cross section including the L direction and T direction of the duplex stainless steel pipe of this embodiment are determined by the following method.
[0051] A test piece for microstructure observation was taken from the center of the wall thickness of the duplex stainless steel pipe. As described above, the longitudinal direction of the duplex stainless steel pipe is defined as the L direction, and the wall thickness direction is defined as the T direction.
[0052] Among the surfaces of the test piece taken from the center position of the wall thickness, the surface (cross section) including the L direction and T direction of the duplex stainless steel pipe is defined as the structure observation surface. The size of the test piece is not particularly limited. The test piece is taken so that the center position of the T direction of the structure observation surface approximately coincides with the center position of the wall thickness of the duplex stainless steel pipe.
[0053] The surface of the collected test piece to be observed is polished to a mirror finish. The polished surface is then electrolytically etched in a 20-30% sodium hydroxide solution to reveal the structure. Using an optical microscope at 400x magnification, 30 fields of view are selected from the surface to be observed.
[0054] In each field of view, the austenite 10, the ferrite 20, and the σ phase have different contrasts. Specifically, as shown in FIG. 1, the brightness of the austenite 10 is high, and the brightness of the ferrite 20 is low. Furthermore, the σ phase has a different brightness from the austenite 10 and the ferrite 20. Therefore, the austenite 10, the ferrite 20, and the σ phase in the field of view can be easily identified. In each field of view, the total area of the identified austenite 10 is obtained. Based on the point count method specified in ASTM E562 (2019), the austenite area ratio obtained in 25 lattices x 30 fields of view is defined as the austenite area ratio (%) of the duplex stainless steel pipe. Furthermore, the ratio of the total area of the σ phase to the total area of the 30 fields of view is defined as the area ratio (%) of the σ phase.
[0055] The average width of austenite is determined by the following method. Five fields of view are arbitrarily selected from the electrolytically etched microstructure observation surface described above using an optical microscope at 400x magnification. Figure 2 shows one of the selected fields of view. As shown in Figure 2, a line segment T0 extending in the T direction is drawn in each field of view. Then, the portion where the line segment T0 and the austenite 10 overlap is identified. Hereinafter, the portion where the line segment T0 and the austenite 10 overlap is referred to as the "overlap portion."
[0056] FIG. 3 is a schematic diagram of a portion of FIG. 2. Referring to FIG. 3, the line segment T0 overlaps with a plurality of austenite 10 in the field of view. Six austenite 10 overlapping with the line segment T0 are selected. Then, the lengths t1 to t6 of the overlapping portions of the six austenite 10 overlapping with the line segment T0 (i.e., the widths t1 to t6 of each austenite 10) are obtained. Using the above method, the widths (t1 to t6) of the six austenite 10 are measured in each field of view (a total of five fields of view). Then, the arithmetic average value of the widths of the 5 fields of view x 6 = 30 austenite 10 is defined as the average width (μm) of the austenite in the duplex stainless steel pipe.
[0057] [Strength of duplex stainless steel pipes] The duplex stainless steel pipe according to the present embodiment has a tensile strength of 800 MPa or more. The lower limit of the tensile strength is preferably 802 MPa, more preferably 804 MPa, more preferably 806 MPa, and even more preferably 810 MPa. The upper limit of the tensile strength of the duplex stainless steel pipe is not particularly limited. The upper limit of the tensile strength of the duplex stainless steel pipe is, for example, 1100 MPa.
[0058] The tensile strength of the duplex stainless steel pipe according to the present embodiment can be determined by the following method. Specifically, a tensile test is performed in air at room temperature (25°C) using a method in accordance with ASTM E8 (2016) to determine the tensile strength (MPa).
[0059] [Pitting corrosion resistance of duplex stainless steel pipes] The duplex stainless steel pipe according to this embodiment has a high tensile strength of 800 MPa or more, and also has excellent pitting corrosion resistance. Excellent pitting corrosion resistance can be defined as follows.
[0060] In accordance with ASTM G48-11 (2015) method E, a 24-hour immersion test is performed using a 6% FeCl3 + 1% HCl solution as the test liquid. The test piece is not particularly limited, but for example, a plate-shaped test piece with a width of 20 mm, a plate thickness of 2.0 mm, and a length of 50 mm. A test piece is prepared from the center of the wall thickness of a duplex stainless steel pipe. The test piece is immersed in the test liquid for 24 hours. After immersion for 24 hours, the test piece is removed from the test liquid and the depth of pitting corrosion that has occurred on the test piece is measured. If the maximum value of the measured pitting corrosion depth is 0.025 mm or less, it is considered to be a pass. If the maximum value exceeds 0.025 mm, it is considered to be a fail. If the result is a pass, a new test liquid 5°C higher than the previous test is prepared, and the above-mentioned immersion test is performed using a new test piece. The maximum temperature at which the result is a pass is defined as the critical pitting temperature (CPT: unit: °C).
[0061] In the duplex stainless steel pipe according to this embodiment, the critical temperature for pitting corrosion initiation in accordance with ASTM G48-11(2015) method E is 80°C or higher.
[0062] [Manufacturing method of duplex stainless steel pipe according to the present embodiment] A method for manufacturing a duplex stainless steel pipe according to the present embodiment will be described below. The method for manufacturing a duplex stainless steel pipe described below is merely one example of the method for manufacturing a duplex stainless steel pipe according to the present embodiment. Therefore, a duplex stainless steel pipe having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the duplex stainless steel pipe according to the present embodiment.
[0063] The method for manufacturing a duplex stainless steel pipe of this embodiment includes a step of preparing a raw material (a preparation step), a step of hot working the raw material to manufacture a mother pipe (a hot working step), and a step of solution treating the mother pipe after hot working (a solution treatment step). Each step will be described below.
[0064] [Preparation process] In the preparation step, a material having the above-mentioned chemical composition is prepared. The material may be supplied from a third party or may be manufactured. The material may be an ingot, a slab, a bloom, or a billet. When manufacturing the material, the material is manufactured by the following method. Molten steel having the above-mentioned chemical composition is manufactured. The manufactured molten steel is used to manufacture an ingot by an ingot casting method. The manufactured molten steel may be used to manufacture a slab, a bloom, or a billet by a continuous casting method. The manufactured ingot, slab, or bloom may be subjected to hot working to manufacture a billet. For example, the ingot may be subjected to hot forging to manufacture a cylindrical billet, and this billet may be used as the material.
[0065] [Hot processing process] In the hot working process, hot working is performed on the material prepared in the preparation process to produce a blank pipe. Specifically, a blank (cylindrical blank) is prepared. A through hole is formed along the central axis of the cylindrical blank by machining. The cylindrical blank with the through hole formed therein is subjected to hot extrusion, typically the Ugine-Séjournet process, to produce a blank pipe.
[0066] Instead of hot extrusion, piercing and rolling by the Mannesmann process may be performed to manufacture a mother pipe. In this case, a round billet is pierced and rolled by a piercing machine. When piercing and rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The pierced and rolled round billet is further hot rolled by a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative reduction in area in the hot working process is not particularly limited, but is, for example, 20 to 80%.
[0067] [Heating temperature before hot processing] In this embodiment, the heating temperature (° C.) before hot working is as follows. Heating temperature: 1150~1260℃
[0068] If the heating temperature before hot working is less than 1150°C, the hot workability of the material is low. In this case, cracks may occur in the material during hot working, or excessive load may be applied to the hot working equipment. On the other hand, if the heating temperature exceeds 1050°C, the ratio of austenite in the steel decreases and the ratio of ferrite increases with increasing heating temperature. That is, in the case of the chemical composition of this embodiment, if the heating temperature exceeds 1050°C, the austenite gradually transforms into ferrite with increasing heating temperature. And, if the heating temperature exceeds 1260°C, the area ratio of ferrite in the steel exceeds 65%. In this case, in the manufactured duplex stainless steel pipe (final product after solution treatment process), the area ratio of austenite, which is responsible for strength, is excessively reduced, and as a result, the strength is reduced.
[0069] If the heating temperature before hot working is 1150 to 1260°C, the ratio of austenite in the material can be increased while hot working is performed. Therefore, assuming that other manufacturing conditions are also satisfied, the austenite area ratio is 45.0 to 65.0% and the average width of austenite is 4.00 to 10.00 μm in the microstructure of the cross section including the L direction and T direction of the duplex stainless steel pipe, which is the final product after the solution treatment process.
[0070] The preferred lower limit of the heating temperature before hot working is 1160°C, more preferably 1170°C. The preferred upper limit of the heating temperature before hot working is 1255°C, more preferably 1250°C.
[0071] [Cooling of the blank pipe after hot working] The mother pipe after hot working is water-cooled. When hot working is performed using a material heated at the above-mentioned heating temperature, the microstructure of the mother pipe after hot working is a lamellar structure of ferrite and austenite, and the width of the lamellar austenite in the mother pipe is narrow. However, if the cooling rate of the mother pipe after hot working is slow, the temperature of the mother pipe gradually decreases. In this case, the width of the lamellar austenite increases as the temperature decreases. If the width of the lamellar austenite increases, the strength of the duplex stainless steel pipe decreases.
[0072] Therefore, in this embodiment, the mother pipe after the hot working is water-cooled instead of being naturally cooled. That is, the mother pipe immediately after the hot working is water-cooled at a cooling rate of 10°C / sec or more. This prevents the width of the lamellar austenite from increasing during cooling.
[0073] [Solution treatment process] After the hot working, the mother pipe is water-cooled and then subjected to a solution treatment under the following conditions. Solution temperature: 1050~1150℃ Holding time at solution temperature: 120 to 480 seconds
[0074] [About solution temperature] As described above, in this embodiment, the mother pipe after hot working is water-cooled to prevent the width of the lamellar austenite in the mother pipe after hot working from becoming wider. However, a small amount of σ phase is generated in the mother pipe. If the solution temperature is less than 1050°C, the σ phase generated in the hot working process is not fully dissolved. Therefore, in the microstructure of the cross section including the L direction and the T direction of the final product duplex stainless steel pipe, the area ratio of the σ phase exceeds 0.05%. Furthermore, the austenite area ratio may exceed 65.0%. In this case, the pitting corrosion resistance of the duplex stainless steel pipe is reduced. On the other hand, if the solution temperature exceeds 1150°C, the width of the lamellar austenite formed in the hot working process becomes wider. In this case, the strength of the duplex stainless steel pipe is reduced.
[0075] If the solution temperature is 1050 to 1150°C, the area ratio of the σ phase can be suppressed to 0 to 0.05%, the area ratio of austenite can be suppressed to 45.0 to 65.0%, and the average width of austenite can be suppressed to 10.00 μm or less in the microstructure of the cross section including the L direction and the T direction of the final product duplex stainless steel pipe, provided that other manufacturing conditions are satisfied. As a result, sufficient strength and pitting corrosion resistance can be obtained in the final product duplex stainless steel pipe. The preferred lower limit of the solution temperature is 1055°C, more preferably 1060°C, and more preferably 1065°C. The preferred upper limit of the solution temperature is 1145°C, more preferably 1140°C, and more preferably 1135°C.
[0076] [Holding time at solution temperature] As described above, in the present embodiment, in the hot working step, hot working is performed while increasing the austenite area ratio as much as possible, and narrow lamellar austenite is formed in the mother tube. If the holding time at the solution temperature is too long, the width of the lamellar austenite increases with time. Therefore, in the present embodiment, the holding time at the solution temperature is set to the minimum necessary time.
[0077] When the holding time at the solution temperature is less than 120 seconds, the σ phase in the steel material does not dissolve sufficiently. Therefore, in the microstructure of the cross section including the L direction and the T direction of the final product duplex stainless steel pipe, the area ratio of the σ phase exceeds 0.05%. In this case, the pitting corrosion resistance of the duplex stainless steel pipe is reduced. On the other hand, when the holding time at the solution temperature exceeds 480 seconds, in the microstructure of the cross section including the L direction and the T direction of the final product duplex stainless steel pipe, the average width of austenite exceeds 10.00 μm. In this case, the strength of the duplex stainless steel pipe is reduced.
[0078] If the holding time at the solution temperature of 1050 to 1150 ° C is 120 to 480 seconds, on the premise that other manufacturing conditions are satisfied, the area ratio of the σ phase can be suppressed to 0 to 0.05%, the area ratio of austenite can be suppressed to 45.0 to 65.0%, and the average width of austenite can be suppressed to 10.00 μm or less in the microstructure of the cross section including the L direction and the T direction of the final product duplex stainless steel pipe. As a result, sufficient strength and sufficient pitting corrosion resistance can be obtained in the duplex stainless steel pipe. The preferable lower limit of the holding time at the solution temperature is 130 seconds, more preferably 140 seconds, and more preferably 150 seconds. The preferable upper limit of the holding time is 400 seconds, more preferably 350 seconds, more preferably 300 seconds, and more preferably 280 seconds.
[0079] After the holding time has elapsed, the steel pipe is water-cooled to produce the duplex stainless steel pipe of this embodiment.
[0080] [About the cold processing process] In the manufacturing method of this embodiment, a cold working step is not performed after the hot working step and before the solution treatment. In other words, the cold working step is omitted in the manufacturing process of this embodiment. The duplex stainless steel pipe of this embodiment can obtain a tensile strength of 800 MPa or more even if the cold working step is omitted in the manufacturing process.
[0081] The duplex stainless steel pipe of this embodiment can be manufactured by the above steps. The above manufacturing method is one example of a method for manufacturing the duplex stainless steel pipe of this embodiment. Therefore, the manufacturing method for the duplex stainless steel pipe of this embodiment is not limited to the above manufacturing method. As long as the duplex stainless steel pipe has the above chemical composition, satisfies the above microstructure, and has a tensile strength of 800 MPa or more, the duplex stainless steel pipe of this embodiment is not limited to the above manufacturing method.
[0082] As described above, the duplex stainless steel pipe of the present embodiment has a chemical composition in which the contents of the elements fall within the above-mentioned numerical ranges, and the microstructure satisfies the above-mentioned ranges, and therefore has a high tensile strength of 800 MPa or more and excellent pitting corrosion resistance. EXAMPLES
[0083] A cylindrical material (round billet) having the chemical composition shown in Table 1 was prepared.
[0084] [Table 1]
[0085] In Table 1, "-" means that the corresponding element was below the detection limit. A through hole was formed along the central axis of the cylindrical material of each test number by machining. The cylindrical material with the through hole formed therein was heated at the heating temperature (°C) shown in Table 2. After heating, the cylindrical material was subjected to hot extrusion to produce a mother tube. In test numbers 1 to 17 and 19 to 24, the mother tube immediately after hot extrusion was water-cooled to room temperature. In test numbers 18 and 25, the mother tube after hot extrusion was allowed to stand to cool. [Table 2]
[0086] The mother pipe after the hot working process was subjected to a solution treatment, in which the mother pipe was held at the solution temperature (°C) for the holding time (seconds) shown in Table 2. After the holding time had elapsed, the mother pipe was water-cooled to produce a duplex stainless steel pipe.
[0087] [Evaluation test] The following evaluation tests were carried out on the duplex stainless steel pipes manufactured with each test number.
[0088] [Austenite area ratio, σ phase area ratio, and average austenite width measurement test] For the duplex stainless steel pipe of each test number, the austenite area fraction and the σ phase area fraction were determined by the following method.
[0089] A test piece for microstructural observation was taken from the center of the wall thickness of the duplex stainless steel pipe. Among the surfaces of the test piece taken from the center of the wall thickness, the surface (cross section) including the L direction (longitudinal direction) and T direction (wall thickness direction) of the duplex stainless steel pipe was defined as the microstructural observation surface. The test piece was taken so that the center position of the T direction of the microstructural observation surface almost coincided with the center position of the wall thickness of the duplex stainless steel pipe.
[0090] The surface of the specimen for microstructure observation was polished to a mirror finish. The polished surface for microstructure observation was electrolytically etched in a 30% sodium hydroxide etching solution to reveal the structure. Thirty fields of view were randomly selected from the surface for microstructure observation using an optical microscope at 400x magnification.
[0091] In each field, the austenite, ferrite, and σ phase have different contrasts. Therefore, the identified austenite was identified in each field and the total area of austenite was calculated. Based on the point count method specified in ASTM E562 (2019), the austenite area ratio obtained in 25 grids x 30 fields was defined as the austenite area ratio (%) of the duplex stainless steel pipe. Furthermore, the ratio of the total area of the σ phase to the total area of the 30 fields was defined as the area ratio of the σ phase (%).
[0092] Furthermore, the average width of the lamellar austenite in the microstructure was obtained by the following method. Five arbitrary fields of view were selected from the above-mentioned electrolytically etched structure observation surface using a 400x optical microscope. As shown in FIG. 2, a line segment T0 extending in the T direction was drawn in each field of view. Then, the overlapping portion of the line segment T0 and the austenite 10 was specified. As shown in FIG. 3, six austenite 10 overlapping with the line segment T0 were selected in each field of view. Then, the lengths t1 to t6 of the overlapping portions of the six austenite 10 overlapping with the line segment T0 (i.e., the widths t1 to t6 of each austenite 10) were obtained. The widths (t1 to t6) of the six austenite 10 were measured in each field of view (a total of five fields of view). Then, the arithmetic average value of the widths of the 30 austenite 10 (5 fields of view x 6) was defined as the average width (μm) of the austenite of the duplex stainless steel pipe.
[0093] [Tensile test] The tensile strength of the duplex stainless steel pipes of each test number was determined by the following method. Specifically, a tensile test was performed in air at room temperature (25°C) according to the method of ASTM E8 (2016), and the tensile strength (MPa) was determined.
[0094] [CPT Exam] The critical temperature CPT (℃) for pitting corrosion of the duplex stainless steel pipes of each test number was determined by the following method. In accordance with ASTM G48-11 (2015) method E, a 24-hour immersion test was conducted using a 6% FeCl3 + 1% HCl solution as the test liquid. The test pieces (plate-shaped test pieces) were 20 mm wide, 2.0 mm thick, and 50 mm long. The test pieces were prepared from the center of the wall thickness of the duplex stainless steel pipes. The test pieces were immersed in the test liquid for 24 hours. After immersion for 24 hours, the test pieces were removed from the test liquid and the depth of the pitting corrosion that occurred on the test pieces was measured. If the maximum value of the measured pitting corrosion depth was 0.025 mm or less, the test was considered to have passed. If the maximum value exceeded 0.025 mm, the test was considered to have failed. If the result was a pass, a new test liquid 5℃ higher than the previous test was prepared, and the above-mentioned immersion test was conducted using the new test pieces. The maximum temperature at which the result was acceptable was defined as the critical pitting temperature CPT (°C).
[0095] When the critical temperature for pitting corrosion initiation CPT was 80°C or higher, the pitting corrosion resistance was judged to be excellent (indicated as "E" (Excellent) in the "CPT test" column in Table 2). On the other hand, when the critical temperature for pitting corrosion initiation CPT was less than 80°C, the pitting corrosion resistance was judged to be poor (indicated as "B" (Bad) in the "CPT test" column in Table 2).
[0096] [Evaluation Results] The evaluation results are shown in Table 2. Referring to Table 2, the chemical compositions of test numbers 1 to 12 and 19 were appropriate. Furthermore, the heating temperature before hot working was appropriate, and water cooling was performed after hot working. Furthermore, the solution treatment temperature and holding time were appropriate. Therefore, in the microstructure of the cross section including the L direction and the T direction of the duplex stainless steel pipes of these test numbers, the austenite area fraction was 45.0 to 65.0%, and the average width of the lamellar austenite was within the range of 4.00 to 10.00 μm. Furthermore, the σ phase area fraction was 0 to 0.05%. As a result, the tensile strength of the duplex stainless steel pipes of these test numbers was 800 MPa or more, the pitting initiation critical temperature CPT was 80 ° C or more, and the pitting resistance was excellent.
[0097] On the other hand, in the test numbers 13 and 20, the heating temperature before hot working was high. Therefore, the austenite area ratio was less than 45.0%. Furthermore, the average width of austenite exceeded 10.00 μm. Therefore, the tensile strength of the duplex stainless steel material was less than 800 MPa.
[0098] In test numbers 14 and 21, the solution temperature was too high. Therefore, the average width of austenite exceeded 10.00 μm. Also, the austenite area ratio was less than 45.0%. Therefore, the tensile strength of the duplex stainless steel pipe was less than 800 MPa.
[0099] In test numbers 15 and 22, the solution temperature was too low. Therefore, the area fraction of the σ phase exceeded 0.05%. Furthermore, the area fraction of the austenite exceeded 65.0%. Therefore, the critical temperature CPT for pitting corrosion initiation of the duplex stainless steel pipe was less than 80°C, and the pitting corrosion resistance was low.
[0100] In test numbers 16 and 23, the solution temperature was appropriate, but the holding time at the solution temperature was short. As a result, the area ratio of the σ phase exceeded 0.05%. As a result, the critical temperature CPT for pitting corrosion initiation of the duplex stainless steel pipe was less than 80°C, and the pitting corrosion resistance was low.
[0101] In test numbers 17 and 24, the solution temperature was appropriate, but the holding time of the solution temperature was too long, so that the average width of austenite exceeded 10.00 μm, and the tensile strength of the duplex stainless steel pipe was less than 800 MPa.
[0102] In test numbers 18 and 25, water cooling after hot working was not performed, and the raw pipe after hot working was allowed to cool to room temperature. As a result, the average width of austenite exceeded 10.00 μm, and the tensile strength of the duplex stainless steel pipe was less than 800 MPa.
[0103] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. [Industrial Applicability]
[0104] The duplex stainless steel pipe of this embodiment is widely applicable to low-temperature environments where low-temperature toughness is required. The duplex stainless steel pipe of this embodiment is particularly suitable for oil well applications. Duplex stainless steel pipes for oil well applications include line pipes, casings, tubing, and drill pipes. [Explanation of symbols]
[0105] 10 Austenite 20 Ferrite
Claims
1. A duplex stainless steel pipe, In mass percent, C: 0.035% or less, Si: 0.15-0.55%, Mn: 0.30-1.20%, P: 0.035% or less, S: 0.0100% or less, Cu: 0.05-1.00%, Ni: 5.00-9.00%, Cr: 23.0-27.0%, Mo: 2.00-6.00%, N: 0.200-0.350%, W: 0-1.000%, Al: 0 to 0.050%, B: 0 to 0.0050%, Ca: 0 to 0.0100%, and The balance is Fe and impurities, When the longitudinal direction of the duplex stainless steel pipe is defined as an L direction and the wall thickness direction is defined as a T direction, in a microstructure of the duplex stainless steel pipe at a cross section including the L direction and the T direction, The austenite area fraction is 45.0 to 65.0%, The area ratio of the σ phase is 0 to 0.05%, The average width of the austenite in the T direction is 4.00 to 10.00 μm; Duplex stainless steel pipe.
2. 2. The duplex stainless steel pipe of claim 1, W: 0.001-1.000%, Al: 0.001-0.050%, B: 0.0001 to 0.0050%, and Ca: 0.0001-0.0100%, Contains one or more elements selected from the group consisting of Duplex stainless steel pipe.
Citation Information
Patent Citations
Near-net shaping preparation method of super double-phased stainless steel thin strip
CN107829043A
Production of high-strength two phase stainless steel
JP1986023713A
Stepping type lens barrel driving device
JP1988058411A
Duplex stainless steel having excellent strength, toughness and seawater resistance, and production method therefor
JP2003171743A
Alloying element-saving hot rolled duplex stainless steel material, and method for production thereof
JP2012153953A