Forging heat treatment method for case hardening steel
The forging heat treatment method for case hardened steel addresses miniaturization and distortion issues by controlling cooling rates and performing retention transformation, enhancing tool life and reducing environmental impact.
Patent Information
- Application Number
- JP2023021332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2043-02-15
AI Technical Summary
Conventional methods for producing case hardened steel parts face challenges in miniaturization, increased hardness leading to shortened tool life, and carburizing and quenching distortion, which increase carbon dioxide emissions and complicate the manufacturing process while decreasing mechanical properties due to austenite grain coarsening.
A forging heat treatment method involving hot forging, controlled cooling, and retention transformation treatment is employed, with specific temperature and cooling rate controls to suppress austenite grain coarsening and reduce quenching distortion.
The method reduces carburizing and quenching distortion, suppresses austenite grain growth, and shortens production time, contributing to environmental sustainability and cost reduction while maintaining mechanical properties.
Smart Images

Figure 0007572740000003 
Figure 0007572740000001 
Figure 0007572740000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a forging and heat treatment method for case hardening steel, in which case hardening steel is used as a raw material and hot forging and heat treatment are performed. [Background technology]
[0002] Conventionally, in the manufacture of mechanical parts such as continuously variable transmissions (hereinafter referred to as "CVTs"), mission gears, and differential gears, case hardening steel is used to be hot forged, then heat treated to soften the steel, and machined to form the final part shape. After that, the steel is carburized and quenched, and finally finished to obtain the final part.
[0003] In recent years, from the perspective of global environmental issues, there has been a trend toward making these parts smaller and lighter, and to achieve this, the shapes of these parts have become more complex. There is also a demand for optimizing the manufacturing process to reduce CO2 emissions. That is, (1) in order to make these parts smaller, they need to be stronger, but the hardness of the forging material increases, shortening the tool life during machining, and (2) because parts with complex shapes are carburized and quenched, the carburizing and quenching distortion is also increasing. In order to address this problem, (1) attempts have been made to improve tool life by performing normalizing treatment after forging to soften the forged parts, and (2) normalizing treatment or normalizing + tempering treatment has been performed after hot forging in order to reduce carburizing and quenching distortion (see, for example, Patent Document 1). However, these methods not only increase the cost of forged parts and CO2 emissions, and make the process more complicated, but in some cases they can also lead to a deterioration in the mechanical properties of the forged parts due to the coarsening of austenite grains during carburizing, so there was a need to optimize these processes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6765551 Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above-mentioned problems associated with the conventional manufacture of forged parts, the present invention has been made based on various considerations regarding simplification of the process, and has an object to provide a forging heat treatment method for case hardening steel that enables softening before machining, can suppress coarsening of austenite grains during carburization, and can also reduce carburization-quenching distortion in-line. [Means for solving the problem]
[0006] In order to achieve the above object, the forging heat treatment method of case hardening steel of the present invention is characterized in that (1) hot forging and heat treatment are continuous, and (2) the cooling rate after forging is controlled and then a retained transformation treatment is carried out. More specifically, case hardening steel is used as a raw material, and hot forging and heat treatment are carried out in the following steps (1) to (4). (1) A process in which the material is heated to 1100~1280°C and then forged at a temperature of 950~1200°C. (2) A process in which the forged material is cooled at least once in cooling equipment at a cooling rate of 1 to 30°C / s immediately after forging, and the cooling and reheating are repeated at least once. (3) The surface temperature after the final reheating is controlled to the target cooling stop temperature between 600 and 750°C, and then the material is loaded into a holding furnace. (4) The material is held at 600-700°C in a holding furnace for 15-60 minutes, and then removed from the furnace.
[0007] Here, the term "case hardening steel" refers to "case hardening steel" as defined in JIS G 4052 or JIS G 4053. Moreover, the "cooling rate" refers to the average cooling rate between 800 and 500°C. In addition, after the final cooling, the surface of the forged part will heat up due to internal heat, and the maximum surface temperature after the heat recovery is defined as the "cooling stop temperature."
[0008] In this case, the material may be case hardening steel containing one or more of Al: 0.010-0.060 wt%, Nb: 0.015-0.060 wt%, N: 0.010-0.025 wt%, and Ti: 0.0015-0.050 wt%. Effect of the Invention
[0009] The forging heat treatment method of case hardening steel of the present invention can be provided as a manufacturing method for carburized parts used in drive system components of automobiles and construction and industrial machinery, particularly mechanical components used as CVTs, transmission gears, differential gears, etc., that contributes to (1) environmental considerations (energy saving, CO2 reduction), (2) reduction in carburized quenching distortion, (3) suppression of abnormal grain growth of austenite grains during carburizing, and (4) shortening of construction time and reducing costs. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing a schematic diagram of the steps of the forging heat treatment method for case hardening steel of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the forging heat treatment method for case hardening steel of the present invention will be described.
[0012] The forging heat treatment method for case hardening steel of the present invention is a method that can be carried out in-line by combining hot forging and heat treatment to soften the steel before machining, suppress coarsening during carburizing, reduce carburizing and quenching distortion, etc.
[0013] 1. Material: Steel Generally, carburized parts used in automobiles and construction and industrial machinery are manufactured by carburizing and quenching using case hardening steels specified in JIS G 4052 and JIS G 4053. Case hardening steel is specifically defined as low carbon steel and low carbon alloy steel, and is primarily defined as steel that is surface hardened by carburizing and quenching, and is used for carburized parts.
[0014] Here, the case hardening steel used as the raw material may contain one or more of Al: 0.010 to 0.060 weight%, Nb: 0.015 to 0.060 weight%, N: 0.010 to 0.025 weight%, and Ti: 0.0015 to 0.050 weight%, which makes it possible to suppress coarsening of austenite grains during carburization.
[0015] The reasons for specifying the amounts of Al, Nb, N and Ti added are as follows. [Al:0.010~0.060wt%] Al reacts with N in steel to form AlN, which has the effect of preventing the coarsening of austenite grains during carburization. If the Al content is less than 0.010% by weight, the effect of adding it is poor, while if the Al content exceeds 0.060% by weight, the effect of preventing the coarsening of crystal grains becomes saturated. Therefore, the above range is specified. [N:0.010~0.0250wt%] N is an element necessary for reacting with Al in steel to precipitate AlN, and has the effect of improving toughness. If the N content is less than 0.010% by weight, the effect of adding it is poor, while if the N content exceeds 0.0250% by weight, the effect of preventing grain coarsening becomes saturated. Also, adding excessive N causes blowholes to occur and reduces strength. Therefore, the above range is specified. [Nb: 0.015-0.060% by weight] Nb is an element required to combine with carbon (C) and nitrogen (N) in steel to produce Nb carbide and Nb carbonitride, and has the effect of preventing the coarsening of austenite grains during carburization. If the amount of Nb added is less than 0.015% by weight, the effect of preventing grain coarsening is poor. As the amount of Nb added increases, the temperature at which grains begin to coarsen also becomes higher, but if the amount of Nb added exceeds 0.060% by weight, the effect saturates and the hardness increases due to precipitation hardening, worsening machinability, so the upper limit is set at 0.060% by weight. [Ti:0.0015~0.050wt%] Like Nb, Ti is an element required to combine with carbon (C) and nitrogen (N) in steel to form Ti carbide and Ti carbonitride, or NbTi carbide and NbTi carbonitride, and has the effect of preventing the coarsening of austenite grains during carburization. If the amount of Ti added is less than 0.015% by weight, the effect of preventing grain coarsening is poor. As the amount of Ti added increases, the temperature at which grains begin to coarsen also becomes higher, but if the amount of Ti added exceeds 0.050% by weight, the effect saturates and the hardness increases due to precipitation hardening, worsening machinability, so the upper limit is set at 0.050% by weight.
[0016] 2. Forging heat treatment FIG. 1 shows a schematic diagram of the steps of the forging heat treatment method for case hardening steel of the present invention.
[0017] 2.1 Configuration of this manufacturing method The present invention consists of four processes: (1) hot forging, (2) controlled cooling, (3) charging into a holding furnace, and (4) holding treatment. The constraints on the manufacturing conditions set for each process are explained below.
[0018] (1) Hot forging (a) Heating time In the case of hot forging, for example, the material steel is heated from room temperature to a specified temperature by high-frequency heating and then forged, and the heating time is generally 10 to 120 seconds. Since this varies depending on the capacity of the equipment and the size of the material, only a guideline is given here. (b) Heating temperature (1100~1280℃) Considering the forging load, it is preferable to heat to 1100°C or higher. However, if heated to above 1280°C, not only will the effect saturate, but the possibility of decarburization and burning cannot be eliminated, so the range is set to 1100 to 1280°C. (c) Forging temperature (950~1200℃) Hot forging is often performed for the purpose of hot forming and refining the structure. Refining the forged structure is done by utilizing recrystallization caused by processing, but it is preferable to perform it at 950 ° C or higher. In addition, when hot forging is performed at a temperature of 950 ° C or lower, depending on the added elements, (i) it may be processed in the non-recrystallized region, so that grain refinement may not be possible, and (ii) such processing in the low-temperature γ region causes relatively large processing-induced precipitation of precipitates such as AlN, Nb (CN), and NbTi (CN), so that it becomes impossible to maintain the micro-alloy elements such as Al, Nb, and Ti in a solid solution state, and it becomes impossible to maintain the solid solution amount of these elements necessary to precipitate fine carbonitrides that have a pinning effect during carburizing during retention treatment. On the other hand, if forging is performed at a temperature above 1200°C, although no precipitates are formed, the grains grow extremely fast after forging, and the effect of inhibiting grain growth by cooling cannot be exerted. Even if recrystallization is achieved by hot working, there are cases in which the grains cannot be refined. Therefore, the forging temperature was set to 950°C to 1200°C.
[0019] (2) Controlled cooling (d) Cooling rate In order to refine the structure after forging, recrystallization by processing is utilized, but even if recrystallization is performed, the grains cannot be refined unless the subsequent grain growth is suppressed. To achieve this, it is necessary to suppress grain growth by cooling at a cooling rate of 1°C / s or more as early as possible after forging. However, if the cooling rate exceeds 30°C / s, not only will the effect saturate, but the equipment cost for the cooling equipment will only become excessive. Therefore, the cooling rate is set to 1 to 30°C / s. In addition, precipitates such as AlN, Nb(CN), and NbTi(CN), which have the effect of suppressing the coarsening of austenite grains during carburizing due to the pinning effect, may lose their effect if they precipitate in the γ region after forging, so it is necessary to cool as early as possible after forging to suppress their precipitation. The number of cooling times is set to one or more. This is intended to make the temperature difference formed in the thickness direction uniform by utilizing cooling and reheating (interrupting cooling to raise the temperature on the surface side by the heat inside the forged part). For this purpose, it is preferable to perform cooling multiple times. Furthermore, cooling two or three times is most preferable in practice. Cooling after forging has the effect of reducing temperature variation in the forged parts, and can reduce distortion caused by delay in transformation due to the γ / α transformation sites during the cooling process after forging, resulting in reduced carburizing and quenching distortion. Here, liquids such as water, or mist or gas thereof are used for cooling. In addition, lubricants, rust inhibitors, etc. can be added to the refrigerant used for cooling depending on the application. (e) Cooling stop temperature (600~750℃) After hot forging, it is necessary to suppress deformation in the holding furnace by reducing the temperature difference between the surface temperature and the center temperature by cooling at least once, preferably multiple times. It has been confirmed that there is no deformation in the holding furnace if the difference is 150 ° C or less. On the other hand, the purpose of the holding treatment is to pre-precipitate fine precipitates that have the effect of inhibiting the grain growth of austenite grains during carburizing treatment, and quenching by cooling to a temperature of up to 600 ° C is effective in maintaining the solid solution of elements such as Al, Nb, and Ti, and enables fine precipitation during the later holding treatment. However, although the solid solution of these elements can be achieved by stopping cooling at a temperature above 750 ° C, it is not possible to precipitate fine precipitates that can fully exert the effect of inhibiting the grain growth of austenite grains during carburizing treatment in the later holding treatment. On the other hand, if cooling is performed to a cooling stop temperature significantly below 600 ° C, the heating time is required to raise the temperature to the holding treatment temperature, and the meaning of making it continuous is weakened.
[0020] (3) Holding furnace charging As soon as the cooling stop temperature of 600 to 750 ° C is reached, the forged parts are charged into the holding furnace. It is preferable that the charging temperature into the holding furnace (almost the cooling stop temperature) is lower than the holding temperature. To finely precipitate AlN, Nb (CN), NbTi (CN), etc., holding after heating is more suitable for fine precipitation than isothermal treatment. The charging temperature is preferably in the range of 550 to 700 ° C.
[0021] (4) Retention process The reason for holding treatment at 600-700℃ for 15-60min is that this temperature range (i) has the effect of releasing residual stress remaining in the forged parts, (ii) has the effect of finely precipitating fine precipitates such as AlN, Nb(CN), NbTi(CN) etc. that have the effect of inhibiting the grain growth of austenite grains during the subsequent carburizing treatment, and (iii) has a sufficient softening effect, so as soon as the target cooling stop temperature is reached, the forged parts are loaded into a holding furnace and held at the specified temperature for the specified time. However, in this case, the forged parts may be removed from the furnace after cooling in the furnace, or may be air-cooled and treated at the specified temperature for the specified time and then removed from the furnace as is. EXAMPLES
[0022] The effects of the present invention will be described below with reference to more specific examples.
[0023] Table 1 shows the chemical composition of the steel used in the demonstration test.
[0024] [Table 1]
[0025] The steel material was melted in a vacuum melting furnace, cast into a mold, and then demolded and hot forged into a round bar with a diameter of 80 mm.Then, the bar was peeled to obtain a round bar with a diameter of 70 mm, and used as a prototype to demonstrate the effects of the present invention.
[0026] Table 2 shows specific examples of forging heat treatment prototypes.
[0027] [Table 2]
[0028] The present invention involves four steps: (1) hot forging, (2) controlled cooling, (3) charging into a holding furnace, and (4) holding treatment. Since the process consists of four steps, the specific implementation conditions are listed for each step. To enable a relative comparison, this prototype used material steel with a diameter of 70 mm and a length of 130 mm, which was forged and heat-treated into a round bar with a diameter of 52 mm under the conditions shown in Table 2, and then machined on a lathe to a test piece with a diameter of 50 mm and a length of 250 mm, which was then carburized and quenched, and the energy consumption, carburizing distortion, grain coarsening, and machinability were evaluated. Here, the carburizing and quenching were carried out under the following conditions: carburizing treatment at 950°C for 6 hours in an atmosphere of Cp = 1.1, diffusion treatment at 850°C for 30 minutes in an atmosphere of Cp = 0.80, oil quenching at 140°C, and tempering at 180°C for 3 hours. In addition, (i) the energy consumption was evaluated by taking the energy consumption per production ton when hot forging was followed by normalizing and carburizing as 100% (excluding the energy consumption of carburizing), and the energy consumption in this prototype was calculated and expressed as a percentage. (ii) The carburizing distortion was evaluated by measuring the runout in the center of the longitudinal direction while rotating after centering both ends of the carburized and quenched test piece. Specifically, the average runout (μm) + 3σ value measured with 20 pieces was 100μm or less, which was considered to be pass (○), and the value exceeding 150μm was considered to be fail (×). The value of 100 to 150μm was considered to be the same (-). (iii) The evaluation of grain coarsening was based on the criterion of "mixed grain" as defined in JIS G 0551 Steel - Microscopic test method for grain size, and the area ratio of grains with grain size numbers differing by 3 or more was considered to be fail (×) or more, and the rest was considered to be pass (○). (iv) For the evaluation of machinability, a blank with a diameter of 100 mm and a thickness of 35 mm was manufactured from a round bar with a diameter of 70 mm under the conditions shown in Table 2. After rough machining, the blank was machined with a carbide hob cutter into a gear with 52 teeth, a twist of 23°, and a tooth width of 35 mm, and the amount of tool wear at that time was measured. The machining conditions with the carbide hob cutter were a speed of 200 m / min., a feed of 2.4 mm / rev., and dry cutting. The machinability was evaluated as passing (○) when the amount of wear was smaller than that when the same machining was performed after normalizing treatment (920°C x 70 min. air cooling) after forging, and failing (×) when the amount of wear was equal to or smaller than that when the same machining was performed. The evaluation results are shown in Table 2.
[0029] Table 2 will be explained below. Table 2(a) shows examples of the present invention, and Table 2(b) shows comparative examples. The comparative example shown in trial product number 1 in Table 2(b) is an example in which test steel 4 was used for forging and then normalized, followed by carburizing and quenching, which is a conventional manufacturing method. Based on this, the examples of the present invention in Table 2(a) will be explained first. Test steels 2, 4, 5, and 6, which have a composition system that takes into consideration coarsening during carburizing, are used in the examples of the present invention. Here, test steel 1 is a general carbon steel, and test steel 3 is a chromium steel. It can be confirmed that manufacturing according to the method of the present invention can reduce energy consumption, suppress carburizing distortion and coarsening, and improve machinability, as shown in the evaluation results of the examples in Table 2(a). On the other hand, in the case of the steels produced by the method of the present invention, even though the steels had such effects, as shown in the test samples 5, 11, 13, and 15, if cooling after forging was not performed (5, 11, 15) or the cooling stop temperature was incorrect (11, 15), the carburizing distortion was inferior (5, 11) or did not improve (11, 13). In other words, these test results show the effectiveness of the method of the present invention. On the other hand, when test samples were produced using steels (test sample steels 1 and 3) that did not take into account grain coarsening during carburizing (16 and 17), the targets for both carburizing distortion and grain coarsening could not be achieved. As has been discussed in the past, case hardening steels basically need to have a composition that takes into account grain coarsening during carburizing, and it goes without saying that the method of the present invention is effective for producing steels with a composition that takes into account the composition. Here, test sample 4 was classified as a comparative example because it was not forged.
[0030] The forging heat treatment method for case hardening steel according to the present invention has been described above based on its embodiment, but the present invention is not limited to the configurations described in the above examples, and the configurations can be changed as appropriate within the scope of the invention. [Industrial Applicability]
[0031] The forging and heat treatment method of the case hardening steel of the present invention is (1) capable of continuously performing hot forging and heat treatment, and (2) ) By controlling the cooling rate after forging and subsequently carrying out a constant transformation treatment, it is possible to soften the material before machining, suppress the coarsening of austenite grains during carburizing, and also achieve in-line reduction of carburizing quench distortion. Therefore, this method is suitable for use in the manufacture of carburized parts used in drive system components for automobiles and construction and industrial machinery, in particular mechanical components used as CVTs, transmission gears, differential gears, etc.
Claims
[Claim 1] A forging heat treatment method for case hardening steel, characterized in that case hardening steel containing one or more of Al: 0.010 to 0.060 wt%, Nb: 0.015 to 0.060 wt%, and Ti: 0.0015 to 0.050 wt%, and N: 0.010 to 0.025 wt%, is used as a material, and hot forging and heat treatment are performed in the following steps (1) to (4). (1) A process in which the material is heated to 1100-1280°C and then forged at a temperature of 950-1200°C. (2) A process in which the forged material is cooled at least once at a cooling rate of 1 to 30°C / s in cooling equipment immediately after forging, and the cooling and reheating are repeated at least once. (3) The surface temperature after the final reheating is controlled to the target cooling stop temperature between 600 and 750°C, and then the material is loaded into a holding furnace. (4) A process of holding the material at a temperature of 600 to 700°C in a holding furnace for 15 to 60 minutes, and then removing the material from the furnace.
Citation Information
Patent Citations
Manufacturing method of hot-forged component for high-temperature carburization and hot-forged component for high-temperature carburization manufactured through the same
JP2004300519A
High strength bainite type nitrided component and its production method
JP2006022350A
Forging and production method thereof
JP2014155944A
Method of producing forged material for carburization
JP2017078193A
Case-hardened steel forged and heat-treated products
JP6765551B2