Manufacturing method for RTB sintered magnets
The method enhances R-T-B sintered magnets' magnetic properties by adjusting composition and heat treatment conditions, achieving high Br and HcJ while minimizing Dy usage.
Patent Information
- Application Number
- JP2019174668
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-20
- Filing Date
- 2019-09-25
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2039-09-25
AI Technical Summary
Existing R-T-B sintered magnets face challenges in maintaining high coercive force (HcJ) and residual magnetic flux density (Br) while minimizing the use of heavy rare earth elements like Dy, which are scarce and volatile in supply.
A manufacturing method for R-T-B sintered magnets involving specific compositions and heat treatment conditions, including a heat treatment temperature of 400°C to 600°C for 10 seconds to 30 minutes, with a composition of R: 27.0% to 35.0% by mass, B: 0.80% to 0.93% by mass, Ga: 0.15% to 1.0% by mass, and T: 61.5% to 70.0% by mass, and adhering to the formula 14[B]/10.8<[T]/55.85, to enhance magnetic properties.
This method achieves high Br and HcJ in R-T-B sintered magnets with reduced Dy content, optimizing magnetic properties by balancing composition and heat treatment time.
Smart Images

Figure 0007572775000001 
Figure 0007572775000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing an RTB based sintered magnet. [Background technology]
[0002] R2T 14 RTB sintered magnets with a B-type compound as the main phase (R is a rare earth element containing at least one selected from the group consisting of Nd, Pr and Ce; T is Fe or Fe and Co, and 90% or more by mass of T is Fe) are known as the highest performance magnets among permanent magnets, and are used in various motors for hybrid cars, electric cars and home appliances.
[0003] RTB sintered magnets have a coercive force H cJ (Hereafter, simply "H cJ ") decreases, and irreversible thermal demagnetization occurs. Therefore, when used in motors for hybrid and electric vehicles, it is necessary to have a high H cJ is required to be maintained.
[0004] Conventionally, H cJ To improve the residual magnetic flux density B r (Hereinafter, simply "B r For this reason, in recent years, heavy rare earth elements have been diffused from the surface to the inside of RTB sintered magnets to concentrate the heavy rare earth elements in the outer periphery of the main phase crystal grains, thereby improving the B r While suppressing the decline of cJ A method has been adopted to obtain
[0005] However, due to the limited production areas, Dy has problems such as unstable supply and price fluctuations. For this reason, it is recommended to use as little heavy rare earth elements as possible (use as little as possible) to produce RTB sintered magnets with H. cJ There is a demand for technologies that can improve this.
[0006] Patent Document 1 describes a method for producing an R2T alloy by lowering the B content compared to conventional RTB alloys and adding at least one metal element M selected from Al, Ga, and Cu. 17 The R2T 17 Transition metal-rich phase (R6T 13 By ensuring a sufficient volume fraction of Dy, the coercive force H cJ It is described that an RTB sintered magnet with high mechanical properties can be obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2013 / 008756 Summary of the Invention [Problem to be solved by the invention]
[0008] Further improvements in magnetic properties have been sought for RTB sintered magnets with low Dy content as described in Patent Document 1. The present disclosure aims to achieve high B while suppressing the Dy content. r and high H cJ The object of the present invention is to provide a method for producing an RTB based sintered magnet having the above-mentioned properties. [Means for solving the problem]
[0009] Aspect 1 of the present invention is Contains at least R, B, Ga and T; R: 27.0% by mass or more and 35.0% by mass or less, R is a rare earth element and includes at least one selected from the group consisting of Nd, Pr, and Ce; B: 0.80% by mass or more and 0.93% by mass or less; Ga: 0.15% by mass or more and 1.0% by mass or less, preparing an RTB based sintered magnet material having T of 61.5 mass % or more and 70.0 mass % or less (T is Fe or Fe and Co, and 90 mass % or more of T is Fe) and satisfying the following formula (1); 14[B] / 10.8<[T] / 55.85 (1) ([B] is the content of B in mass%, and [T] is the content of T in mass%) and a heat treatment step of heat treating the RTB based sintered magnet material by holding the heat treatment temperature at 400°C or higher and 600°C or lower for a holding time of 10 seconds or higher and less than 30 minutes.
[0010] Aspect 2 of the present invention is Aspect 2 is a method for producing an RTB based sintered magnet according to aspect 1, wherein the holding time in the heat treatment step is from 10 seconds to 10 minutes.
[0011] Aspect 3 of the present invention is 3. The method for producing an RTB based sintered magnet according to aspect 1 or 2, wherein the holding time in the heat treatment step is from 10 seconds to 3 minutes. Effect of the Invention
[0012] According to the manufacturing method of the present disclosure, it is possible to obtain a high B while suppressing the Dy content. r and high H cJ It is possible to provide a method for producing an RTB based sintered magnet having the above-mentioned properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] RTB sintered magnets can be made into H by heat treatment after sintering. cJ It is generally known that the H cJ It was thought that in order to maximize the value of H, it was necessary to hold the heat treatment temperature at this temperature for at least 1.5 to 3 hours after the optimum temperature had been reached. cJIn order to fully utilize the effect of B, the heat treatment was usually performed with a holding time of 1.5 hours or more. r and H cJ Therefore, the shorter the retention time (e.g., 5 min), the greater the B r Although the value of H cJ The value of H drops significantly. And when the holding time is increased (e.g., 3 hours), cJ The value of H cJ With the improvement of B r The value of decreases.
[0014] However, as a result of intensive research by the present inventors, it was found that the B content in the R2T 14 Surprisingly, in the case of RTB sintered magnets containing Ga and a smaller amount of B than the stoichiometric composition ratio, the heat treatment is performed for an extremely short time of less than 30 minutes. cJ It was found that the B r and H cJ In other words, the B content decreased with increasing R2T 14 In the case of an RTB sintered magnet containing Ga and having a lower than stoichiometric composition ratio of the B compound, when the holding time is less than 30 minutes (preferably 10 minutes or less, more preferably 3 minutes or less), B r and H cJ Based on this knowledge, the present inventors have completed the method for producing an RTB based sintered magnet according to the present invention.
[0015] The manufacturing method according to the embodiment of the present invention will be described in detail below. In the present invention, a material in a stage before completion of heat treatment under specific conditions (heat treatment held at a temperature of 400°C or higher and 600°C or lower for a holding time of 10 seconds or longer and less than 30 minutes) is referred to as an "R-T-B sintered magnet material" or simply a "sintered magnet material". An R-T-B sintered magnet material after performing the heat treatment under the above specific conditions is referred to as an "R-T-B sintered magnet" or simply a "sintered magnet". That is, in this specification, a material before performing the heat treatment under the above specific conditions and a material during the heat treatment are referred to as "R-T-B sintered magnet materials".
[0016] <Manufacturing Method of R-T-B Sintered Magnet> The manufacturing method of the R-T-B sintered magnet according to the present invention will be described. The manufacturing method of the R-T-B sintered magnet includes a step of preparing an R-T-B sintered magnet material having a predetermined composition, and a heat treatment step of heat-treating the R-T-B sintered magnet material under specific conditions. Hereinafter, each step will be described.
[0017] (1) Step of preparing an R-T-B sintered magnet material The R-T-B sintered magnet material in the present disclosure contains at least R, B, Ga, and T, and their compositions satisfy the following regulations.
[0018] (Content of R: 27.0 mass% or more and 35.0 mass% or less) R is a rare earth element and contains at least one selected from the group consisting of Nd, Pr, and Ce. The content of R is 27.0 mass% or more and 35.0 mass% or less. If the content of R is less than 27.0 mass%, densification during sintering may be difficult, and if it exceeds 35.0 mass%, the main phase ratio may decrease and it may be impossible to obtain a high B r There is a risk. The content of R is preferably 29.5 mass% or more and 33.0 mass% or less. If R is in such a range, a higher B r Can be obtained.
[0019] (Content of B: 0.80 mass% or more and 0.93 mass% or less) The content of B in the sintered magnet material is 0.80 mass % or more and 0.93 mass % or less, and satisfies the formula (1) described below. 17 Phase is generated and high H cJ If the content exceeds 0.93 mass%, the amount of RT-Ga phase produced is too small, and high H cJ The content of B is more preferably 0.88 mass% or more and 0.90 mass% or less, and a higher H cJ The improvement effect is obtained.
[0020] (Ga content: 0.15 mass% or more and 1.0 mass% or less) The Ga content is 0.15 mass% or more and 1.0 mass% or less. If the Ga content is less than 0.15 mass%, the amount of RT-Ga phase generated is too small, and the R2T 17 The phase cannot be eliminated, and high H cJ If it exceeds 1.0 mass%, unnecessary Ga will be present, and the main phase ratio will decrease, resulting in a decrease in B. r The Ga content is preferably 0.2% by mass or more and 0.8% by mass or less, and more preferably 0.3% by mass or more and 0.6% by mass or less. r and high H cJ can be obtained.
[0021] (T content: 61.5% by mass or more and 70.0% by mass or less) T is Fe or Fe and Co, and 90 mass% or more of T is Fe. The inclusion of Co can improve corrosion resistance, but if the amount of Co substituted exceeds 10 mass% of T, high B r The content of T is 61.5 mass% or more and 70.0 mass% or less, and satisfies the above formula (1). If the content of T is less than 61.5 mass%, B is significantly reduced. r There is a risk that it will decline.
[0022] The content of T in the sintered magnet material and the content of B satisfy the following formula (1). 14[B] / 10.8<[T] / 55.85 (1) By satisfying formula (1), the B content is less than that of a typical RTB sintered magnet. A typical RTB sintered magnet contains R2T, which is the main phase. 14 In addition to the B phase, there is a soft magnetic phase, R2T 17 In order to prevent the formation of any phase, the composition is set such that [T] / 55.85 (atomic weight of Fe) is less than 14[B] / 10.8 (atomic weight of B) ([T] is the content of T in mass %). Unlike typical RTB based sintered magnets, the RTB based sintered magnet of the present invention is specified by formula (1) such that [T] / 55.85 is greater than 14[B] / 10.8. Note that since the main component of T in the RTB based sintered magnet of the present invention is Fe, the atomic weight of Fe is used.
[0023] (remainder) In one preferred embodiment of the sintered magnet material, the balance is T and unavoidable impurities. In other words, as long as T satisfies formula (1), T and unavoidable impurities may constitute the balance. Inevitable impurities may include Cr, Mn, Si, La, Ce, Sm, Ca, Mg, etc., which are usually contained in didymium alloy (Nd-Pr), electrolytic iron, ferroboron, etc. Furthermore, examples of inevitable impurities in the manufacturing process include O (oxygen), N (nitrogen), and C (carbon).
[0024] In still another preferred embodiment of the sintered magnet material, any other element may be further contained within the scope of achieving the object of the present invention. Examples of other elements that can be selectively contained in this way are listed below.
[0025] (Cu: more than 0 mass%, 1.0 mass% or less) By including an appropriate amount of Cu, H cJ can be further improved. Cu may be contained in an amount of 1.0 mass% or less. The Cu content is preferably 0.05 to 0.50 mass%. When Cu is contained in an amount of 0.05 to 0.50 mass%, H cJ can be further improved.
[0026] (Al: more than 0 mass%, 1.0 mass% or less) By including an appropriate amount of Al, H cJ can be further improved. Al may be contained in an amount of 1.0 mass% or less. The content of Al is preferably 0.05 to 0.50 mass%. When Al is contained in an amount of 0.50 mass% or less, H cJ It is possible to further improve the above. Although Al may be contained in an amount of 0.05% by mass or more as an unavoidable impurity in the manufacturing process, the total amount of the unavoidable impurities and the amount intentionally added may be 1.0% by mass or less. The Al content is more preferably 0.05% by mass or more and 0.5% by mass or less.
[0027] (Other elements) In addition to the elements mentioned above, the sintered magnet material may contain one or more other elements (elements added intentionally other than unavoidable impurities). For example, such elements may contain small amounts (about 0.1% by mass each) of Ag, Zn, In, Sn, Ti, Ge, Y, H, F, P, S, V, Ni, Mo, Hf, Ta, W, Nb, Zr, etc. Furthermore, the elements listed as the unavoidable impurities above may be intentionally added. Such elements may be contained in a total amount of, for example, about 1.0% by mass. At this level, it is possible to obtain a high H cJ It is quite possible to obtain an RTB based sintered magnet having the above properties.
[0028] The RTB based sintered magnet material having the above composition can be prepared by the following steps (i) to (iii). That is, the process for preparing the sintered magnet material can include the following steps (i) to (iii). Note that steps (i) to (iii) are merely examples of how the sintered magnet material can be produced, and the present invention is not limited thereto. Furthermore, the process of preparing the sintered magnet material may further include a high-temperature heating step (step (iv)) and a diffusion step (step (v)) in addition to steps (i) to (iii).
[0029] (i) preparing an alloy powder Metals or alloys of the respective elements are prepared so as to obtain the above composition, and these are then subjected to strip casting or the like to produce alloy flakes. The obtained alloy flakes are subjected to hydrogen pulverization to obtain a coarsely pulverized powder having a size of, for example, 1.0 mm or less. The coarsely pulverized powder is then finely pulverized by a jet mill or the like to obtain a finely pulverized powder (alloy powder) having a particle size D50 (a value (median diameter) obtained by a laser diffraction method using an airflow dispersion method) of, for example, 3 to 7 μm. A known lubricant may be used as an auxiliary agent in the coarsely pulverized powder before the jet mill pulverization, and in the alloy powder during and after the jet mill pulverization.
[0030] (ii) Molding process The obtained alloy powder is subjected to compaction in a magnetic field to obtain a compact. The compaction in a magnetic field may be performed by any known method including a dry compaction method in which dried alloy powder is inserted into a cavity of a die and compacted while a magnetic field is applied, and a wet compaction method in which a slurry in which the alloy powder is dispersed is poured into a cavity of a die and compacted while the dispersion medium of the slurry is discharged.
[0031] (iii) Sintering process The green body obtained in the molding step is sintered to obtain an RTB sintered magnet material. The green body can be sintered by a known method (for example, a sintering temperature of 1000°C to 1090°C and a sintering time of about 1 hour to 10 hours). In order to prevent oxidation due to the atmosphere during sintering, the sintering is preferably carried out in a vacuum atmosphere or in an inert gas. The inert gas used is preferably an inert gas such as helium or argon.
[0032] (iv) High temperature heating process The sintered magnet material obtained in the sintering step may be further subjected to a high-temperature heating step in which the material is heated at a relatively high temperature of 700°C or higher and lower than the sintering temperature. cJ It is preferable that the heating time in the high-temperature heating step is 1.5 hours or more.
[0033] (v) Diffusion process The sintered magnet material obtained in the sintering step or the sintered magnet material after the high-temperature heating step may be further subjected to a diffusion step. The diffusion step can be performed using a known diffusion source and diffusion method. For example, JP 2008-147634 A discloses a method in which a powder containing Dy, Tb, etc. is present on the surface of a sintered body (the surface of an RTB-based sintered magnet material) and heated at a temperature lower than the sintering temperature to diffuse Dy, Tb, etc. from the powder into the sintered body. In addition, WO2018 / 143230 discloses a method in which at least a part of an R-Ga alloy is brought into contact with at least a part of the surface of an RTB-based sintered magnet material, and a first heat treatment is performed at a temperature of 700°C or more and 950°C or less to diffuse R and Ga into the magnet.
[0034] The RTB based sintered magnet material after the sintering step (or after the high-temperature heating step and / or the diffusion step) may be machined and then subjected to a heat treatment step.
[0035] (2) Heat treatment process The sintered magnet material obtained in the process of preparing the sintered magnet material is subjected to a heat treatment for the purpose of improving its magnetic properties. The heat treatment temperature is 400°C or higher and 600°C or lower. If the heat treatment temperature is lower than 400°C or higher than 600°C, H cJ and B. r The improvement effect of the above is not obtained. A preferred method for measuring the heat treatment temperature is to bring a thermocouple into contact with the RTB based sintered magnet material in the heat treatment furnace to measure the temperature. Alternatively, a simpler method may be to simultaneously measure the temperature in the heat treatment furnace and the temperature of another RTB based sintered magnet material placed in the heat treatment furnace in advance using a thermocouple to investigate the correspondence between the temperature in the heat treatment furnace and the temperature of the RTB based sintered magnet material in the heat treatment furnace, and then read the temperature of the RTB based sintered magnet material in the heat treatment furnace from the temperature in the heat treatment furnace based on the correspondence.
[0036] After the RTB based sintered magnet material reaches the heat treatment temperature, it is held at that heat treatment temperature for a period of at least 10 seconds and less than 30 minutes. The manufacturing method according to this embodiment is characterized in that this holding time is much shorter than conventional methods.
[0037] As mentioned above, by heat treating the sintered magnet material obtained by sintering, the H of the RTB sintered magnet as the final product can be obtained. cJ It has been known for some time that the H cJ It was thought that in order to maximize the value of B, it was necessary to hold the material at the optimum heat treatment temperature for 1.5 to 3 hours or more. r reaches a maximum value at a holding time of about 10 seconds, and as the holding time is increased, H cJ It was thought that the retention time would decrease with the increase in H cJ Therefore, heat treatment was conventionally performed with a holding time of 1.5 hours or more.
[0038] However, as a result of extensive investigation by the present inventors, it was found that the B content of R2T 14 In RTB sintered magnet materials that contain less B than the stoichiometric composition ratio of the B compound and Ga, the retention time during heat treatment is extremely short, resulting in a high B r and high H cJ It was found that an RTB based sintered magnet having the above-mentioned H of the RTB based sintered magnet can be obtained. cJ It was found that the holding time at which the maximum value is reached exists in the range of 10 seconds or more and less than 30 minutes. Therefore, in this embodiment, the holding time during the heat treatment is set to 10 seconds or more and less than 30 minutes. The retention time is preferably from 10 seconds to 25 minutes, more preferably from 10 seconds to 10 minutes, even more preferably from 10 seconds to 5 minutes, and even more preferably from 10 seconds to 3 minutes. cJ It is possible to produce an RTB based sintered magnet having the above structure.
[0039] In order to suppress oxidation due to oxygen in the atmosphere during the heat treatment process, it is preferable to carry out the heat treatment in a vacuum atmosphere or an inert gas atmosphere, such as helium or argon.
[0040] The obtained sintered magnet may be subjected to machining such as grinding in order to obtain the final product shape. In this case, the heat treatment may be performed before or after the machining. Furthermore, the obtained sintered magnet may be subjected to a surface treatment. The surface treatment may be any known surface treatment, such as Al vapor deposition, Ni electric plating, or resin paint.
[0041] The RTB sintered magnets obtained in this way have high H cJ and B. r The composition of the RTB based sintered magnet is substantially the same as that of the above-mentioned RTB based sintered magnet material. EXAMPLES
[0042] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited thereto.
[0043] Each element was weighed so that the composition of the RTB sintered magnet would be approximately the composition of No. 1 to No. 3 in Table 1 (with regard to No. 2, the composition after diffusion would be approximately the same as No. 2), and the alloy was cast by strip casting to produce a quenched alloy. The quenched alloy thus obtained was subjected to hydrogen embrittlement in a pressurized hydrogen atmosphere, and then to a dehydrogenation treatment in which the alloy was heated to 550°C in a vacuum and cooled, to obtain a coarsely pulverized powder. Next, 0.04% by mass of zinc stearate was added to the coarsely pulverized powder thus obtained as a lubricant relative to 100% by mass of the coarsely pulverized powder, and the mixture was then dry-pulverized in a nitrogen stream using an airflow pulverizer (jet mill device) to obtain a particle size D 50 A finely pulverized powder (alloy powder) with a median diameter of 4 μm was obtained.
[0044] The obtained alloy powder was mixed with a dispersion medium to prepare a slurry. Normal dodecane was used as the solvent, and methyl caprylate was mixed as the lubricant. The concentration of the slurry was 70% by mass of alloy powder, 30% by mass of dispersion medium, and 0.16% by mass of lubricant relative to 100% by mass of alloy powder. The slurry was molded in a magnetic field to obtain a compact. The magnetic field during molding was a static magnetic field of 0.8 MA / m, and the pressure was 5 MPa. The molding device used was a so-called perpendicular magnetic field molding device (horizontal magnetic field molding device), in which the magnetic field application direction and the pressure direction are perpendicular to each other.
[0045] The obtained green bodies were sintered in a vacuum at 1000°C to 1090°C (a temperature at which sufficient densification by sintering occurs was selected for each sample) for 4 hours, cooled to room temperature, and then subjected to a high-temperature heat treatment in a vacuum at 800°C for 2 hours, after which they were rapidly cooled to room temperature to obtain RTB sintered magnet materials (Nos. 1' to 3'). The density of the obtained RTB sintered magnet materials was 7.5 Mg / m 3 That was all.
[0046] Next, the No. 2' RTB sintered magnet material was subjected to a diffusion treatment. First, a diffusion alloy was prepared. The raw materials of each element were weighed so that the composition of the diffusion alloy was approximately 80% by mass of Pr, 10% by mass of Tb, 5% by mass of Ga, and 5% by mass of Cu, and the raw materials were melted and a ribbon or flake-shaped alloy was produced by a single-roll super-quenching method (melt spinning method). The obtained alloy was pulverized in an argon atmosphere using a mortar, and then passed through a sieve with a mesh size of 425 μm to prepare a diffusion alloy (PrTbGaCu alloy). The components of the obtained diffusion alloy were measured using inductively coupled plasma optical emission spectroscopy (ICP-OES), and the composition was almost as intended (80% by mass of Pr, 10% by mass of Tb, 5% by mass of Ga, and 5% by mass of Cu). Next, the diffusion alloy was sprayed on the surface (entire surface) of the No. 2' RTB sintered magnet material. The amount of dispersion was 3.3% by mass relative to 100% by mass of the RTB based sintered magnet material. After that, a diffusion treatment was carried out by heating at a temperature of 900°C for 3 hours in reduced pressure argon controlled at 50 Pa. In this way, an RTB based sintered magnet material (No. 2'') that had undergone the diffusion process was prepared.
[0047] Next, the RTB based sintered magnet materials No. 1', 2'' and 3' were subjected to heat treatment under the conditions shown in Table 2 to obtain RTB based sintered magnets. The heat treatment temperature was measured by contacting a thermocouple with the RTB based sintered magnet material in the heat treatment furnace.
[0048] The components of the obtained RTB sintered magnet are shown in Table 1. The components in Table 1 were measured using inductively coupled plasma optical emission spectroscopy (ICP-OES). Table 1 also shows whether formula (1) was satisfied. Here, "○" means that formula (1) was satisfied, and "×" means that formula (1) was not satisfied. The B of the obtained RTB sintered magnet r and H cJ The values of B are shown in Table 2. r and H cJ The value of was measured by machining the RTB sintered magnet to a sample of 7 mm x 7 mm x 7 mm using a BH tracer.
[0049] In Table 2, the values that were judged to have high magnetic properties are underlined. r is 1.40(T) or more, and H cJ If satisfies 1500(kA / m), B r Value and H cJ Both values are underlined. r and H cJ If any of the above criteria was not met, no value was underlined.
[0050] [Table 1]
[0051] [Table 2]
[0052] With regard to the examples of the present invention and the comparative examples shown in Table 2, a comparison between the five sintered magnets in No. 1, a comparison between the five sintered magnets in No. 2, a comparison between the two sintered magnets in No. 4, a comparison between the two sintered magnets in No. 5, and a comparison between the two sintered magnets in No. 6 shows that by setting the holding time in the heat treatment within the range of the present invention, r and H cJ In contrast, for the RTB sintered magnet No. 3, whose composition is outside the compositional range of the present invention (the amount of B and formula (1) are outside the range), the retention time of the present invention (5 minutes) is 5 minutes, and the H cJ On the other hand, for No. 3 with the same composition, when the holding time was increased (180 min), H cJ Although the improvement is cJ With the improvement of B r In addition, as shown in Table 2, the higher B r and high H cJ To obtain this, the holding time in the heat treatment is preferably 10 minutes or less, more preferably 5 minutes or less, and even more preferably 3 minutes or less.
Claims
1. Contains at least R, B, Ga and T; R: 27.0% by mass or more and 35.0% by mass or less, R is a rare earth element and includes at least one selected from the group consisting of Nd, Pr, and Ce; B: 0.80% by mass or more and 0.93% by mass or less; Ga: 0.15% by mass or more and 1.0% by mass or less; preparing a sintered R-T-B based magnet material having T of 61.5 mass % or more and 70.0 mass % or less (T is Fe or Fe and Co, and 90 mass % or more of T is Fe) and satisfying the following formula (1); 14[B] / 10.8<[T] / 55.85 (1) ([B] is the content of B in mass%, and [T] is the content of T in mass%) and a heat treatment step of heat treating the sintered R-T-B based magnet material at a heat treatment temperature of 400°C or higher and 600°C or lower for a holding time of 3 minutes or higher and less than 30 minutes.
2. 2. The method for producing a sintered RTB based magnet according to claim 1, wherein the holding time in the heat treatment step is from 3 minutes to 10 minutes.
3. The step of preparing the R-T-B based sintered magnet material includes: Providing an alloy powder having the composition of claim 1; a compacting step of compacting the alloy powder in a magnetic field to obtain a compact; 3. The method for producing a sintered R-T-B based magnet according to claim 1, further comprising the step of sintering the compact to obtain a sintered magnet material.
4. The step of preparing the R-T-B based sintered magnet material further includes the steps of: The method for producing a sintered R-T-B based magnet according to claim 3, further comprising a high-temperature heating step of heating the sintered magnet material obtained in the step of obtaining the sintered magnet material at a temperature of 700° C. or higher and lower than a sintering temperature.
5. The step of preparing the R-T-B based sintered magnet material further includes the steps of: The method for producing a sintered R-T-B based magnet according to claim 4, further comprising a diffusion step of subjecting the sintered magnet material after the high-temperature heating step to a diffusion treatment.
Citation Information
Patent Citations
Method for manufacturing r-t-b based sintered magnet
JP2018018911A
Alloy for r-t-b-based rare earth sintered magnet, process for producing alloy for r-t-b-based rare earth sintered magnet, alloy material for r-t-b-based rare earth sintered magnet, r-t-b-based rare earth sintered magnet, process for producing r-t-b-based rare earth sintered magnet, and motor
WO2013008756A1