Cerium-iron-boron permanent magnet material and preparation method thereof

Through the dual alloy powder mixing method and grain boundary diffusion technology, the content of praseodymium-neodymium alloy and metal trace elements is adjusted to form a rare earth magneto-hardened shell, which solves the problem of low magnetic performance caused by excessive cerium content in cerium-ferroboron permanent magnets, and improves the The intrinsic coercive force of magnets meets the performance requirements of industrial applications and is suitable for mass production.

CN118942826APending Publication Date: 2024-11-12HUBEI UNIV OF AUTOMOTIVE TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410938675.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the cerium content in cerium-ferroboron permanent magnet is too high, the intrinsic coercive force and squareness of the magnet are low, and cannot be fully saturated and magnetized, and the high-temperature magnetic retardation and residual magnetism are insufficient, which cannot meet the performance requirements of industrial applications.

Method used

The dual alloy powder mixing method and grain boundary diffusion technology are used to adjust the content of praseodymium-neodymium alloy and metal trace elements to form a rare earth magnet hardened shell layer, improve the magnetic performance of the magnet, and optimize the composition of the magnet blank through sintering and tempering treatment and structure.

Benefits of technology

It significantly improves the room temperature intrinsic coercivity of cerium-ferroboron permanent magnets, meets the requirements of magnet devices, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a cerium-iron-boron permanent magnet material and a preparation method thereof. The cerium-iron-boron permanent magnet material contains praseodymium-neodymium alloy, and the magnetic performance of a magnet is enhanced by adjusting the content of the praseodymium-neodymium alloy; 0.5-2 wt% of metal trace elements are added, and the coercive force of the magnet is enhanced by adjusting the element content; 0.5-1.5 wt% of cobalt element is added to improve the squareness of the magnet; then, the coercive force of the cerium-iron-boron magnet can meet the use requirement of a magnet device through a grain boundary diffusion technology; according to the method, a cerium-iron-boron main-phase alloy and a praseodymium-neodymium main-phase alloy with different components are designed through a multi-main-phase alloy method, a cerium-iron-boron magnet blank is prepared through powder preparation, compression and sintering, then the magnet blank is prepared into a flaky magnet, rare earth elements permeate into the magnet from the surface of the flaky magnet through a grain boundary diffusion technology, and the rare earth elements are prepared into the flaky magnet. The coercive force of the magnet is improved; according to the preparation method, the cost of the rare earth permanent magnet material can be reduced, and the magnetic performance of the magnet can meet the use requirement of a magnet device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth permanent magnet materials, and in particular relates to a cerium iron boron permanent magnet material and a preparation method thereof. Background Art

[0002] Rare earth permanent magnet materials are the most widely used and best magnetic materials at present. They are widely used in new energy vehicles, wind power generation, electronic information, instrumentation and other fields. However, there is an extremely unbalanced phenomenon in the utilization of rare earth resources. The application scope of high-abundance rare earth elements such as lanthanum and cerium is relatively small, while praseodymium-neodymium alloys and dysprosium-terbium have a wide range of applications, resulting in a large backlog of high-abundance rare earth elements such as lanthanum and cerium extracted from associated mining. The emergence of rare earth cerium magnets can reduce costs and optimize the utilization of rare earth resources.

[0003] Cerium has variable valence characteristics and a small ion radius. Therefore, when the cerium content is high, it is difficult for the magnet to obtain a high coercive force, especially for ultra-high cerium content magnets with a cerium content of more than 12%. The intrinsic coercive force and squareness are low, and it will not be possible to fully saturate magnetization and high-temperature demagnetization, and it is also impossible to avoid the phenomenon of insufficient magnetic moment when the remanence is satisfied and insufficient thermal demagnetization when the intrinsic coercive force is satisfied. In order to improve the intrinsic coercive force of Cerium Iron Boron permanent magnets, grain boundary diffusion technology is introduced to form a rare earth magnetic hardening shell layer in the boundary layer of the main phase grains to improve the magnetic properties of the magnet, so as to meet the performance requirements of Cerium Iron Boron permanent magnets in various low-end and medium-end application fields. Summary of the invention

[0004] In order to solve the above problems, the present invention aims to provide a Cerium Iron Boron permanent magnet and a preparation method thereof, so as to improve the magnetic properties of the Cerium Iron Boron permanent magnet to meet the requirements of industrial use and realize low-cost, high-efficiency large-scale production and its application.

[0005] The cerium-iron-boron permanent magnet material described in the present invention is characterized in that the components contained in the cerium-iron-boron permanent magnet material and the mass percentage of each component are as follows: 9-16% of praseodymium-neodymium alloy, 16-25% of cerium, 0.5-1.5% of Co, 0.7-1.1% of B, 0.1-1% of aluminum, 0.2-1% of niobium, 0.1-1% of copper, 0.1-1% of gallium, 0.05-0.5% of zirconium, 0.05-0.5% of titanium, and the balance is iron.

[0006] Furthermore, the magnet blank contains 16-25% cerium, 9-15% praseodymium-neodymium alloy, and the total amount of 6 metal trace elements, namely aluminum, niobium, copper, gallium, zirconium and titanium, is added in an amount of 0.5-2%.

[0007] On the one hand, the preparation method of the cerium iron boron permanent magnet material provided by the present invention is prepared from components including cerium iron boron main phase alloy I and praseodymium neodymium alloy main phase alloy II, wherein: The mass ratio of the main phase alloy I to the main phase alloy II is 9:1 to 8:2; In the main phase alloy I, the mass percentages of the components are as follows: 5-15% praseodymium-neodymium alloy, 20-28% cerium, 0.5-1.5% cobalt, 0.7-1.1% boron, 0.1-1% aluminum, 0.2-1% niobium, 0.1-1% copper, 0.1-1% gallium, 0.05-0.5% zirconium, 0.05-0.5% titanium, and the balance is iron; In the main phase alloy II, the mass percentages of the components are as follows: praseodymium-neodymium alloy 29-35%, cobalt 0.5-1.5%, boron 0.7-1.1%, aluminum 0.1-1%, niobium 0.2-1%, copper 0.1-1%, gallium 0.1-1%, zirconium 0.05-0.5%, titanium 0.05-0.5%, and the balance is iron; The cerium iron boron permanent magnet is prepared by the following steps: (1) Main phase alloy I and main phase alloy II are separately batched, smelted, hydrogen-decomposed and jet-milled to obtain two alloy powders, and then the alloy powders are uniformly mixed according to a certain proportion, oriented pressed and isostatically pressed in a magnetic field to obtain a block body, and the block body after isostatic pressing is sintered in a vacuum furnace at 900-1100° C. for 2-6 hours, tempered at 850-920° C. for 1-4 hours, and tempered at 450-650° C. for 2-6 hours to obtain a magnet blank after tempering; (2) Cutting the magnet blank into sheet magnets, grinding and cleaning, coating and drying the sheet magnets, placing the dried sheet magnets into a vacuum diffusion furnace for grain boundary diffusion treatment, the grain boundary diffusion temperature is 800-950°C, and the diffusion time is 6-20 hours; then tempering at 450-650°C for 2-6 hours, and obtaining cerium iron boron permanent magnets after tempering.

[0008] According to the preparation method of the present invention, preferably, the average particle size of the main phase alloy I and the main phase alloy II powders is 2.8-3.5 μm.

[0009] According to the preparation method of the present invention, the preparation process and process parameters of the magnet blank are optimized, and the intrinsic coercive force of the obtained magnet blank at room temperature is less than 8.5 kOe.

[0010] According to the preparation method of the present invention, preferably, praseodymium, neodymium, dysprosium and their alloy powders are used as diffusion sources, and are uniformly mixed with organic solutions, binders, etc. to obtain diffusion slurry, and the slurry is uniformly coated on the surface of the sheet magnet.

[0011] According to the preparation method of the present invention, preferably, the coating is divided into two modes: single-sided coating and double-sided coating; the single-sided coating amount does not exceed 0.4% of the magnet weight, and the double-sided coating amount does not exceed 0.6% of the magnet weight.

[0012] According to the preparation method of the present invention, preferably, the coating method adopts any one of magnetron sputtering, mechanical spraying, screen printing, immersion plating and manual coating.

[0013] According to the preparation method of the present invention, the intrinsic coercive force of the CeFeB permanent magnet prepared after the grain boundary diffusion process is implemented is greater than 9.5 kOe at room temperature.

[0014] The beneficial effects of the present invention are as follows: the present invention can obtain cerium iron boron permanent magnet materials with different maximum magnetic energy products by adjusting the praseodymium-neodymium alloy content through a dual alloy mixed powder method, and can improve the coercive force of the magnet by adding an appropriate amount of metal trace elements; the above two methods for improving the magnetic properties of the magnet cannot make the coercive force of the cerium iron boron magnet meet the use requirements of the magnet device; the grain boundary diffusion process can make the coercive force of the cerium iron boron magnet meet the use requirements of the magnet device, and is suitable for the mass production of cerium iron boron permanent magnet devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 1 is a microstructure and element distribution diagram of the magnet blank of Example 1 of the present invention; Figure 2 This is a magnetic performance diagram of a single-sided coated magnet after grain boundary diffusion provided by Example 3 of the present invention; Figure 3 This is a magnetic performance diagram of the double-sided coated magnet after grain boundary diffusion provided by Example 4 of the present invention. DETAILED DESCRIPTION

[0016] The following is a more detailed description of the specific implementation of the present invention in conjunction with the accompanying drawings and examples, so that the scheme of the present invention and its advantages in various aspects can be better understood. However, the specific implementation methods and examples described below are only for the purpose of illustration, rather than for limiting the present invention.

[0017] Hereinafter, wt% refers to mass percentage (weight percentage).

[0018] The present invention provides a cerium-iron-boron permanent magnet material, which is prepared from components including a cerium-iron-boron main phase alloy I and a praseodymium-neodymium alloy main phase alloy II; The composition of the main phase alloy I is: cerium 20wt%, praseodymium-neodymium alloy 11wt%, cobalt 0.5wt%, boron 0.94wt%, aluminum 0.5wt%, niobium 0.3wt%, copper 0.5wt%, gallium 0.2wt%, zirconium 0.2wt%, titanium 0.1wt%, and the balance is iron; The composition of the main phase alloy II is: 31% praseodymium-neodymium alloy, 0.5wt% cobalt, 0.94wt% boron, 0.5wt% aluminum, 0.3wt% niobium, 0.5wt% copper, 0.2wt% gallium, 0.2wt% zirconium, 0.1wt% titanium, and the balance is iron; After the main phase alloy I and the main phase alloy II of the present invention are mixed in a ratio of 8:2, the obtained magnet blank has the following components: cerium content is 16wt%, praseodymium-neodymium alloy content is 15wt%, cobalt is 0.5wt%, boron is 0.94wt%, aluminum is 0.5wt%, niobium is 0.3wt%, copper is 0.5wt%, gallium is 0.2wt%, zirconium is 0.2wt%, titanium is 0.1wt%, and the balance is iron.

[0019] Embodiment 1: The present invention provides a method for preparing a cerium iron boron permanent magnet blank, comprising the following steps: The main phase alloy I and the main phase alloy II are smelted, hydrogen-broken and air-flow-milled to obtain two kinds of alloy powders, and the average particle size of the alloy powders is controlled to be 2.8-3.5 μm; The two main phase alloy powders are mixed evenly according to the above proportions, and the alloy composition after mixing is: 16wt% cerium, 15wt% praseodymium-neodymium alloy, 0.5wt% cobalt, 0.94wt% boron, 0.5wt% aluminum, 0.3wt% niobium, 0.5wt% copper, 0.2wt% gallium, 0.2wt% zirconium, 0.1wt% titanium, and the balance is iron; The mixed alloy powder is oriented and pressed to obtain a block body with a density greater than 4.0 g / cm3; after isostatic pressing, it is placed in a vacuum sintering furnace for high-temperature sintering and tempering to obtain a cerium iron boron permanent magnet blank; Figure 1 The figure shows the microstructure and element distribution of the cerium iron boron permanent magnet blank. The figure shows that the granular rare earth-rich phase is seriously aggregated, the praseodymium and neodymium content in the rare earth-rich phase is significantly higher than that in the main phase grains, but the Ce content in the rare earth-rich phase is not always higher than that in the main phase grains, and the Fe element content is significantly lower than that in the main phase grains.

[0020] The specific sintering and tempering process is: sintering temperature is 1040°C, sintering holding time is 4 hours; primary tempering temperature is 900°C, holding time is 2h; secondary tempering temperature is 650°C, holding time is 4h.

[0021] After the prepared magnet blank is ground flat, the magnetic properties of the magnet are tested using the AMT-4A permanent magnet property automatic measuring instrument. The results are as follows: r =10.87kGs, H cb =7.85kOe, H cj =8.12kOe, (BH) max =27.6MGOe,H k / H cj =0.94.

[0022] Example 2: The magnet blank obtained in Example 1 is processed into a sheet magnet, and then the magnet surface is pretreated; the pretreatment process is: using a composite degreasing liquid with a sodium hydroxide concentration of 15g / L and a sodium dodecyl sulfate concentration of 3g / L to degrease the sheet magnet at 60°C for 2 to 3 minutes; then pickling with a 25wt% citric acid aqueous solution for 15 to 20 seconds, and finally placing the sheet magnet in deionized water for ultrasonic cleaning for 2 to 3 minutes; The dried sheet magnet is evenly coated with dysprosium hydride slurry, which is obtained by mixing dysprosium hydride powder, alcohol and silicone binder in a uniform proportion; the coating process is divided into single-sheet coating and double-sided coating, the single-sided coating weight is 0.2% of the sheet magnet weight, and the double-sided coating weight is 0.4% of the sheet magnet weight; The coated sheet magnet is placed in an oven for drying, then loaded into a stainless steel material box, and then placed in a high vacuum diffusion furnace for grain boundary diffusion treatment; the grain boundary diffusion treatment process is: the grain boundary diffusion temperature is 900°C, the diffusion time is 6 to 18 hours, and the sheet magnet after the grain boundary diffusion treatment is tempered, and the tempering treatment process is: tempering at 450 to 650°C for 4 hours to obtain a cerium iron boron permanent magnet that meets the performance requirements.

[0023] Example 3: The magnet blank obtained in Example 1 was wire-cut into a rectangular sheet-shaped magnet substrate of 140×25×7 mm, and then degreased, pickled and ultrasonically cleaned to remove surface impurities; 3 grams of dysprosium hydride powder was mixed in 50 milliliters of alcohol, and 1 wt% of silicone binder was added; the mixed slurry was then coated on one side of the substrate surface, and dried at 150°C for 2 hours. The magnet gained 0.2 wt% on one side after coating; The coated magnet was subjected to grain boundary diffusion treatment, the grain boundary diffusion temperature was 900°C, the diffusion holding time was 6 hours, 9 hours, 12 hours, 15 hours and 18 hours respectively; the tempering temperature was 650°C, and the tempering holding time was 4 hours.

[0024] refer to Figure 2 The magnetic properties obtained in Example 3 are shown in Table 1:

[0025] Example 4: The magnet blank obtained in Example 1 was wire-cut into a rectangular sheet-shaped magnet substrate of 140×25×7 mm, and then degreased, pickled and ultrasonically cleaned to remove surface impurities; 3 grams of dysprosium hydride powder was mixed in 50 milliliters of alcohol, and 1 wt% of silicone binder was added; the mixed slurry was then coated on both sides of the substrate surface, and dried at 150°C for 2 hours. The magnet double-sided coating weight gain was measured to be 0.4 wt%; The coated magnet was subjected to grain boundary diffusion treatment, the grain boundary diffusion temperature was 900°C, the diffusion holding time was 6 hours, 9 hours, 12 hours, 15 hours and 18 hours respectively; the tempering temperature was 650°C, and the tempering holding time was 4 hours.

[0026] refer to Figure 3 The magnetic properties obtained in Example 4 are shown in Table 2:

[0027] Example 5: The magnet blank obtained in Example 1 was wire-cut into a rectangular sheet-shaped magnet substrate of 140×25×7 mm, and then degreased, pickled and ultrasonically cleaned to remove surface impurities; 3 grams of dysprosium hydride powder was mixed in 50 milliliters of alcohol, and 1 wt% of silicone binder was added; the mixed slurry was then coated on one side of the substrate surface, and dried at 150°C for 2 hours. The magnet gained 0.2 wt% on one side after coating; The coated magnets were subjected to grain boundary diffusion treatment, with a grain boundary diffusion temperature of 900°C and a diffusion holding time of 9 hours; the tempering temperatures were 600°C, 550°C, 500°C and 450°C, and the tempering holding time was 4 hours.

[0028] The magnetic properties obtained in Example 5 are shown in Table 3:

[0029] Example 6: The magnet blank obtained in Example 1 was wire-cut into a rectangular sheet-shaped magnet substrate of 140×25×7 mm, and then degreased, pickled and ultrasonically cleaned to remove surface impurities; 3 grams of dysprosium hydride powder was mixed in 50 milliliters of alcohol, and 1 wt% of silicone binder was added; the mixed slurry was then coated on both sides of the substrate surface, and dried at 150°C for 2 hours. The magnet double-sided coating weight gain was measured to be 0.4 wt%; The coated magnets were subjected to grain boundary diffusion treatment, with a grain boundary diffusion temperature of 900°C and a diffusion holding time of 9 hours; the tempering temperatures were 600°C, 550°C, 500°C and 450°C, and the tempering holding time was 4 hours.

[0030] The magnetic properties obtained in Example 6 are shown in Table 4:

[0031] Comparative Example 1: The magnetic properties of the magnet blank were directly compared with those of Example 4 and Example 6. The results are shown in Table 5:

[0032] It can be seen from Table 5 above that the method of this embodiment can improve the intrinsic coercivity of the CeFeB permanent magnet, making its intrinsic coercivity significantly higher than that of the magnet substrate, and has little effect on the remanence and the maximum magnetic energy product.

[0033] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in this specification and the summary of the implementation methods; the invention is fully applicable to various suitable fields, and researchers familiar with the rare earth field can easily implement additional modifications. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A cerium iron boron permanent magnet material, Features The components contained in the cerium-iron-boron permanent magnet material and the mass percentage of each component are as follows: 9-16% of praseodymium-neodymium alloy, 16-25% of cerium, 0.5-1.5% of Co, 0.7-1.1% of B, 0.1-1% of aluminum, 0.2-1% of niobium, 0.1-1% of copper, 0.1-1% of gallium, 0.05-0.5% of zirconium, 0.05-0.5% of titanium, and the balance is iron.

2. The cerium iron boron permanent magnet material according to claim 1, It is characterized in that The magnet blank contains 16-25% cerium, 9-15% praseodymium-neodymium alloy, and the total amount of 6 metal trace elements, namely aluminum, niobium, copper, gallium, zirconium and titanium, is added at 0.5-2%.

3. A method for preparing a cerium-iron-boron permanent magnetic material, It is characterized in that The invention is prepared from the components including the main phase alloy I of cerium iron boron and the main phase alloy II of praseodymium neodymium alloy, wherein: The mass ratio of the main phase alloy I to the main phase alloy II is 9:1 to 8:2; In the main phase alloy I, the mass percentages of the components are as follows: 5-15% praseodymium-neodymium alloy, 20-28% cerium, 0.5-1.5% cobalt, 0.7-1.1% boron, 0.1-1% aluminum, 0.2-1% niobium, 0.1-1% copper, 0.1-1% gallium, 0.05-0.5% zirconium, 0.05-0.5% titanium, and the balance is iron; In the main phase alloy II, the mass percentages of the components are as follows: praseodymium-neodymium alloy 29-35%, cobalt 0.5-1.5%, boron 0.7-1.1%, aluminum 0.1-1%, niobium 0.2-1%, copper 0.1-1%, gallium 0.1-1%, zirconium 0.05-0.5%, titanium 0.05-0.5%, and the balance is iron; The cerium iron boron permanent magnet is prepared by the following steps: (1) Main phase alloy I and main phase alloy II are separately batched, smelted, hydrogen-decomposed and jet-milled to obtain two alloy powders, and then the alloy powders are uniformly mixed according to a certain proportion, oriented pressed and isostatically pressed in a magnetic field to obtain a block body, and the block body after isostatic pressing is sintered in a vacuum furnace at 900-1100° C. for 2-6 hours, tempered at 850-920° C. for 1-4 hours, and tempered at 450-650° C. for 2-6 hours to obtain a magnet blank after tempering; (2) Cutting the magnet blank into sheet magnets, grinding and cleaning, coating and drying the sheet magnets, placing the dried sheet magnets into a vacuum diffusion furnace for grain boundary diffusion treatment, the grain boundary diffusion temperature is 800-950°C, and the diffusion time is 6-20 hours; then tempering at 450-650°C for 2-6 hours, and obtaining cerium iron boron permanent magnets after tempering.

4. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 3, It is characterized in that The average particle size of the main phase alloy I and the main phase alloy II powders is 2.8-3.5 μm.

5. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 3, It is characterized in that The intrinsic coercive force of the magnet blank obtained after sintering and tempering at room temperature is less than 8.5 kOe.

6. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 3, It is characterized in that Praseodymium, neodymium, dysprosium and their alloy powders are used as diffusion sources and are evenly mixed with an organic solution, a binder, etc. to obtain a diffusion slurry, which is then evenly coated on the surface of a sheet magnet.

7. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 6, It is characterized in that The coating is divided into two modes: single-sided coating and double-sided coating; the single-sided coating amount does not exceed 0.4% of the magnet weight, and the double-sided coating amount does not exceed 0.6% of the magnet weight.

8. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 3, It is characterized in that The coating method may be any one of magnetron sputtering, mechanical spraying, screen printing, immersion plating and manual coating.

9. The method for preparing the cerium-iron-boron permanent magnetic material according to claim 3, It is characterized in that The intrinsic coercivity of the magnet after grain boundary diffusion heat treatment at room temperature is greater than 9.5kOe.

Citation Information

Cited By

  • Cerium-containing high-coercivity rare earth permanent magnet and preparation method thereof

    CN119252590A

  • A cerium-containing high-coercivity rare earth permanent magnet and preparation method thereof

    CN119252590B

  • Neodymium-iron-boron sintered magnet and preparation method and application thereof

    CN119560253A