Curable resin composition and its uses

A curable resin composition with alkali-soluble resin and vinyl ether groups addresses solvent resistance and temperature-related issues in color filters by enabling low-temperature curing, ensuring high-quality and efficient production.

JP7572810B2Active Publication Date: 2024-10-24NIPPON SHOKUBAI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020132002
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-03
Publication Date
2024-10-24
Estimated Expiration
2040-08-03

AI Technical Summary

Technical Problem

Conventional curable resin compositions used in color filters experience issues with solvent resistance, particularly when used with coloring materials, leading to elution into washing solvents, and high-temperature curing processes result in discoloration and generation of by-products, affecting the quality and efficiency of color filters.

Method used

A curable resin composition comprising an alkali-soluble resin with acid groups and a polymer containing vinyl ether groups, which allows for curing at low temperatures (200°C or less) while maintaining excellent solvent resistance, achieved by combining an acid group-containing alkali-soluble resin and a polymer with a vinyl ether group in the side chain, optionally with a photopolymerization initiator, polymerizable compound, and photoacid generator.

Benefits of technology

The composition provides a cured product with enhanced solvent resistance and improved production efficiency by allowing curing at lower temperatures, suitable for applications like color filters and other optical and electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572810000001
    Figure 0007572810000001
  • Figure 0007572810000002
    Figure 0007572810000002
  • Figure 0007572810000003
    Figure 0007572810000003
Patent Text Reader

Abstract

To provide a curable resin composition that can give a cured product having excellent solvent resistance even under the condition of low-temperature curing and can be suitably used for color filters or the like.SOLUTION: A curable resin composition contains an acid group-containing alkali-soluble resin and / or a resin having a group to produce an acid radical by heat or acid, and a polymer having a vinyl ether group in a side chain.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition. More specifically, the present invention relates to a curable resin composition capable of giving a cured product having excellent solvent resistance even under low-temperature curing conditions, and uses thereof. [Background technology]

[0002] Curable resin compositions that can be cured by heat or active energy rays have been studied for various applications, such as color filters used in liquid crystal displays and solid-state imaging devices, inks, printing plates, printed wiring boards, semiconductor devices, photoresists, organic insulating films, organic protective films, and other various optical members and electric and electronic devices, and resin compositions excellent in the properties required for each application have been developed.

[0003] In recent years, optical components and electric / electronic devices have become smaller, thinner, and more energy-efficient, and as a result, higher performance is required for the various components used in these devices. In order to meet such demands, research is being conducted on curable resin compositions that can be used as materials for various components.

[0004] Up to now, curable resin compositions have been developed in response to various demands. For example, Patent Document 1 describes a curable composition containing a vinyl ether group-containing polymer and a compound with a specific structure that generates cations or radicals when irradiated with energy rays. The curable composition does not generate bubbles even when cured by irradiation with energy rays, and has extremely high curing performance when irradiated with energy rays, so that it can give a high-quality cured product.

[0005] For example, Patent Document 2 describes a formulation that contains a polymer containing at least one pendant vinyl ether monomer repeat unit having a specific structure, a solvent, and further contains a thermal acid generator. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-298884 [Patent Document 2] Patent No. 6181294 Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, various studies have been conducted on curable resin compositions, but when a conventional curable resin composition is used together with a coloring material as a raw material for a color filter or the like, there is a problem that the coloring material is eluted from the raw material into a cleaning solvent during the production of the color filter. Therefore, there has been a demand for further improvement in the solvent resistance of the curable resin composition.

[0008] In recent years, particularly in color filter applications, there has been a strong demand for higher performance, such as higher brightness and higher contrast, in display panels, due to the improvement in quality and expansion of applications of color liquid crystal displays and the like. However, in the manufacture of color filters, if the baking process (post-curing process) after exposure and development is performed at a high temperature of over 200°C, the obtained cured product will discolor, such as yellowing, and the desired color cannot be sufficiently colored. In addition, if the baking process is performed at a high temperature, unnecessary reactions will proceed, producing by-products, which will deteriorate the properties of the substrate and the cured film. In order to suppress such unnecessary reactions and efficiently obtain a color filter having the desired properties, it is desirable that the curing reaction proceeds sufficiently even under relatively low heating conditions of 200°C or less. In addition, if the curable resin composition can be cured at a relatively low temperature, the manufacturing efficiency of the color filter can also be improved.

[0009] The present invention has been made in consideration of the above-mentioned current situation, and an object of the present invention is to provide a curable resin composition that can give a cured product having excellent solvent resistance even under low-temperature curing conditions and can be suitably used in applications such as color filters. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into curable resin compositions and have found that by containing an acid group-containing alkali-soluble resin and / or a resin having a group that generates an acid group by heat or acid, and a polymer having a vinyl ether group in a side chain, it is possible to give a cured product having excellent solvent resistance even under curing conditions at relatively low temperatures of 200°C or less, thereby completing the present invention.

[0011] That is, the present invention relates to a curable resin composition comprising an acid group-containing alkali-soluble resin and / or a resin having a group that generates an acid group by heat or acid, and a polymer having a vinyl ether group in a side chain.

[0012] The polymer having a vinyl ether group in the side chain preferably has a structural unit represented by the following general formula (1).

[0013] [ka]

[0014] (In the formula, R 1 R represents a hydrogen atom or a methyl group. 2 represents a hydrogen atom or an organic group. W represents a direct bond or a divalent organic group.

[0015] The resin having a group that generates an acid group by heat or acid preferably has a structural unit represented by the following general formula (2).

[0016] [ka]

[0017] (In the formula, R 3 represents a hydrogen atom or a methyl group. X represents a direct bond or a divalent organic group. A represents a group that generates an acid group by the action of heat or an acid.

[0018] The acid group-containing alkali-soluble resin preferably has an acid value of 20 to 230 mgKOH / g.

[0019] The acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid is preferably a polymer having a ring structure in the main chain.

[0020] The curable resin composition preferably further contains a photopolymerization initiator.

[0021] The curable resin composition preferably further contains a polymerizable compound.

[0022] The curable resin composition preferably further contains a photoacid generator.

[0023] In the curable resin composition, it is preferred that the acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid further has an epoxy group, and / or the curable resin composition further contains an epoxy compound.

[0024] The curable resin composition is preferably for use as a resist.

[0025] The curable resin composition is preferably for use in a color filter.

[0026] The present invention also relates to a color filter comprising a substrate and a cured product of the above-mentioned curable resin composition on the substrate.

[0027] The present invention also provides a display device comprising the above-mentioned color filter. Effect of the Invention

[0028] The curable resin composition of the present invention can provide a cured product having excellent solvent resistance even under relatively low curing conditions of 200° C. or less. The curable resin composition of the present invention is suitably used for various applications such as various optical members used in liquid crystal, organic EL, quantum dot, and micro LED liquid crystal displays, solid-state imaging elements, touch panel display devices, etc., and components of electric and electronic devices, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention. In this specification, "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid", and "(meth)acrylate" means "acrylate and / or methacrylate".

[0030] 1. Curable resin composition The present invention relates to a curable resin composition comprising an acid group-containing alkali-soluble resin and / or a resin having a group that generates an acid group by heat or acid, and a polymer having a vinyl ether group in a side chain.

[0031] Since the curable resin composition of the present invention has the above-mentioned constitution, it can give a cured product with extremely excellent solvent resistance even when cured under relatively low temperature conditions of 200° C. or less (for example, about 110° C.) The reason why the curable resin composition of the present invention can give a cured product with excellent solvent resistance even under relatively low temperature curing conditions is considered to be as follows. That is, in the curable resin composition of the present invention, the reactivity between the acid group of the acid group-containing alkali-soluble resin or the acid group of the resin having a group that generates an acid group by heat or acid and the vinyl ether group is high, and the crosslinking reaction can proceed even under relatively low curing conditions of about 100 to 200°C, so that a strong cured film can be formed and a cured product with excellent solvent resistance can be obtained.

[0032] Each component contained in the resin composition of the present invention will be described. (A) Acid group-containing alkali-soluble resin The acid group-containing alkali-soluble resin (hereinafter also referred to as "resin (A)") is a polymer having an acid group. The presence of an acid group makes the resin alkali-soluble. Examples of the acid group include functional groups that undergo a neutralization reaction with alkaline water, such as a carboxyl group, a phenolic hydroxyl group, a carboxylic anhydride group, a phosphoric acid group, and a sulfonic acid group, and the like. Only one of these may be present, or two or more of these may be present. Among these, a carboxyl group or a carboxylic anhydride group is preferred, and a carboxyl group is more preferred.

[0033] (a1) Structural unit having an acid group The resin (A) preferably has the above-mentioned structural unit having an acid group (hereinafter also referred to as "structural unit (a1)"). Examples of methods for obtaining a polymer having the structural unit (a1) include a method (1) in which a monomer component containing an acid group-containing monomer is polymerized, and a method (2) in which a monomer component containing an epoxy group-containing monomer is polymerized to obtain a polymer containing an epoxy group, and then the epoxy group is subjected to an addition reaction with the acid group of the acid group-containing monomer to open the epoxy group, and the hydroxyl group generated during the reaction is reacted with a polybasic acid or a polybasic acid anhydride to generate a carboxyl group. Alternatively, these methods may be combined. In the method (1), the structural unit (a1) is a structural unit derived from an acid group-containing monomer. In the method (2), the structural unit (a1) is a structural unit containing a carboxyl group produced by reacting a structural unit derived from an epoxy group-containing monomer with an acid group-containing monomer and further reacting the structural unit with a polybasic acid or a polybasic acid anhydride. Among these, the structural unit (a1) is preferably a structural unit derived from an acid group-containing monomer.

[0034] The above-mentioned acid group-containing monomer may be a compound having the above-mentioned acid group and a polymerizable double bond (carbon-carbon double bond) in the molecule. The above-mentioned polymerizable double bond may be, for example, a (meth)acryloyl group, a vinyl group, an allyl group, a methallyl group, etc. Among them, a (meth)acryloyl group is preferred.

[0035] Specific examples of the acid group-containing monomer include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, cinnamic acid, and vinylbenzoic acid; unsaturated polyvalent carboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid; long-chain unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, such as β-carboxyethyl (meth)acrylate, mono(2-acryloyloxyethyl) succinate, and mono(2-methacryloyloxyethyl) succinate; unsaturated acid anhydrides such as maleic anhydride and itaconic anhydride; and phosphoric acid group-containing unsaturated compounds such as Light Ester P-1M (manufactured by Kyoeisha Chemical Co., Ltd.). Among these, from the viewpoints of versatility, availability, and the like, carboxylic acid-based monomers (unsaturated monocarboxylic acids, unsaturated polyvalent carboxylic acids, long-chain unsaturated monocarboxylic acids, and unsaturated acid anhydrides) are preferred. From the standpoint of reactivity, alkali solubility, etc., the acid group-containing monomer is more preferably an unsaturated monocarboxylic acid, and even more preferably (meth)acrylic acid.

[0036] The epoxy group-containing monomer includes a compound having an epoxy group and the above-mentioned polymerizable double bond in the molecule, and preferably includes an epoxy group-containing (meth)acrylate. Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, vinylbenzyl glycidyl ether, allyl glycidyl ether, (3,4-epoxycyclohexyl)methyl (meth)acrylate, vinylcyclohexene oxide, etc. Among these, glycidyl (meth)acrylate and (3,4-epoxycyclohexyl)methyl (meth)acrylate are preferred, and glycidyl (meth)acrylate is more preferred.

[0037] Examples of the polybasic acid or polybasic acid anhydride include polybasic acids such as succinic acid, maleic acid, phthalic acid, and tetrahydrophthalic acid; dibasic acid anhydrides such as succinic anhydride (also known as succinic anhydride), maleic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, and itaconic anhydride; and polybasic acid anhydrides such as trimellitic anhydride. Among these, polybasic acid anhydrides are preferred.

[0038] The resin (A) may have only one type of the structural unit (a1), or may have two or more types.

[0039] In order to maintain appropriate developability, the content of the structural unit (a1) is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more, relative to 100% by mass of all structural units in the resin (A), and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0040] (a2) Structural unit having a ring structure in the main chain The resin (A) is preferably a polymer having a ring structure in the main chain. By having a ring structure in the main chain, the heat resistance of the resin (A) can be improved. Examples of the ring structure include an imide ring, a tetrahydrofuran ring, and a lactone ring. In order to have these ring structures, the resin (A) preferably further has a structural unit (a2) having a ring structure in the main chain.

[0041] Examples of the monomer that can introduce the structural unit (a2) include a monomer having a double bond-containing ring structure in the molecule, a monomer that forms a polymer having a ring structure in the main chain by cyclic polymerization, and a monomer that forms a ring structure after polymerization. Among them, from the viewpoint of good heat resistance, solvent resistance, hardness, colorant dispersibility, etc., at least one monomer selected from the group consisting of N-substituted maleimide monomers, dialkyl-2,2'-(oxydimethylene) diacrylate monomers, and α-(unsaturated alkoxyalkyl) acrylate monomers is preferred, and from the viewpoint of further excellent heat coloring resistance, at least one monomer selected from the group consisting of N-substituted maleimide monomers and dialkyl-2,2'-(oxydimethylene) diacrylate monomers is more preferred.

[0042] Examples of the N-substituted maleimide monomer include N-cyclohexylmaleimide, N-phenylmaleimide, N-methylmaleimide, N-ethylmaleimide, N-isopropylmaleimide, Nt-butylmaleimide, N-dodecylmaleimide, N-benzylmaleimide, and N-naphthylmaleimide, and one or more of these can be used. Among them, from the viewpoint of transparency, N-phenylmaleimide, N-benzylmaleimide, and N-cyclohexylmaleimide are preferred, and N-cyclohexylmaleimide is particularly preferred. In addition, from the viewpoint of improving heat coloration resistance and water unevenness suppression effect, N-phenylmaleimide and / or N-cyclohexylmaleimide are preferred, and N-phenylmaleimide is more preferred.

[0043] Examples of the N-benzylmaleimide include benzylmaleimide; alkyl-substituted benzylmaleimides such as p-methylbenzylmaleimide and p-butylbenzylmaleimide; phenolic hydroxyl group-substituted benzylmaleimides such as p-hydroxybenzylmaleimide; and halogen-substituted benzylmaleimides such as o-chlorobenzylmaleimide, o-dichlorobenzylmaleimide and p-dichlorobenzylmaleimide.

[0044] Examples of the dialkyl-2,2'-(oxydimethylene) diacrylate monomer include dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, diethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, di(n-propyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(isopropyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(n-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, and di(isobutyl)-2,2'-[oxybis(methylene)]bis-2-propenoate. Examples of the di(t-butyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(t-amyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(stearyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(lauryl)-2,2'-[oxybis(methylene)]bis-2-propenoate, di(2-ethylhexyl)-2,2'-[oxybis(methylene)]bis-2-propenoate, etc. Among these, dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate is more preferred from the viewpoints of transparency, dispersibility, ease of industrial availability, etc.

[0045] The α-(unsaturated alkoxyalkyl)acrylate monomer may, for example, be an α-(allyloxymethyl)acrylate monomer. Specific examples of the α-(allyloxymethyl)acrylate monomer include, for example, α-allyloxymethylacrylic acid; methyl α-allyloxymethylacrylate, ethyl α-allyloxymethylacrylate, n-propyl α-allyloxymethylacrylate, i-propyl α-allyloxymethylacrylate, n-butyl α-allyloxymethylacrylate, s-butyl α-allyloxymethylacrylate, t-butyl α-allyloxymethylacrylate, n-amyl α-allyloxymethylacrylate, s-amyl α-allyloxymethylacrylate, t-amyl α-allyloxymethylacrylate, n-hexyl α-allyloxymethylacrylate, s-hexyl α-allyloxymethylacrylate, n-heptyl α-allyloxymethylacrylate, n-octyl α-allyloxymethylacrylate, s-octyl α-allyloxymethylacrylate, α-allyloxymethylacrylate, alkyl-(α-allyloxymethyl)acrylate monomers such as t-octyl α-allyloxymethylacrylate, 2-ethylhexyl α-allyloxymethylacrylate, capryl α-allyloxymethylacrylate, nonyl α-allyloxymethylacrylate, decyl α-allyloxymethylacrylate, undecyl α-allyloxymethylacrylate, lauryl α-allyloxymethylacrylate, tridecyl α-allyloxymethylacrylate, myristyl α-allyloxymethylacrylate, pentadecyl α-allyloxymethylacrylate, cetyl α-allyloxymethylacrylate, heptadecyl α-allyloxymethylacrylate, stearyl α-allyloxymethylacrylate, nonadecyl α-allyloxymethylacrylate, eicosyl α-allyloxymethylacrylate, ceryl α-allyloxymethylacrylate, and melissyl α-allyloxymethylacrylate;Alkoxyalkyl-(α-allyloxymethyl)acrylate monomers such as methoxyethyl α-allyloxymethylacrylate, methoxyethoxyethyl α-allyloxymethylacrylate, methoxyethoxyethoxyethyl α-allyloxymethylacrylate, 3-methoxybutyl α-allyloxymethylacrylate, ethoxyethyl α-allyloxymethylacrylate, ethoxyethoxyethyl α-allyloxymethylacrylate, phenoxyethyl α-allyloxymethylacrylate, and phenoxyethoxyethyl α-allyloxymethylacrylate;Hydroxyethyl α-allyloxymethylacrylate, Hydroxypropyl α-allyloxymethylacrylate, Hydroxybutyl α-allyloxymethylacrylate, Fluoroethyl α-allyloxymethylacrylate, Difluoroethyl α-allyloxymethylacrylate, Chloroethyl α-allyloxymethylacrylate, Dichloroethyl α-allyloxymethylacrylate, Bromoethyl α-allyloxymethylacrylate, Dibromoethyl α-allyloxymethylacrylate, Vinyl α-allyloxymethylacrylate, Allyl α-allyloxymethylacrylate, Methallyl α-allyloxymethylacrylate, Crotyl α-allyloxymethylacrylate, Propargyl α-allyloxymethylacrylate, Cyclopentyl α-allyloxymethylacrylate, Cyclohexyl α-allyloxymethylacrylate, 4-Methylcyclohexyl α-allyloxymethylacrylate, α-Allyloxymethylacrylate Examples of the acrylate monomer include 4-t-butylcyclohexyl acrylate, tricyclodecanyl α-allyloxymethylacrylate, isobornyl α-allyloxymethylacrylate, adamantyl α-allyloxymethylacrylate, dicyclopentadienyl α-allyloxymethylacrylate, phenyl α-allyloxymethylacrylate, methylphenyl α-allyloxymethylacrylate, dimethylphenyl α-allyloxymethylacrylate, trimethylphenyl α-allyloxymethylacrylate, 4-t-butylphenyl α-allyloxymethylacrylate, benzyl α-allyloxymethylacrylate, diphenylmethyl α-allyloxymethylacrylate, diphenylethyl α-allyloxymethylacrylate, triphenylmethyl α-allyloxymethylacrylate, cinnamyl α-allyloxymethylacrylate, naphthyl α-allyloxymethylacrylate, and anthranyl α-allyloxymethylacrylate. Among these, alkyl-(α-allyloxymethyl)acrylate monomers are preferred. As the alkyl-(α-allyloxymethyl)acrylate monomer, methyl α-allyloxymethylacrylate (also called methyl-(α-allyloxymethyl)acrylate) is particularly preferred from the viewpoints of transparency, dispersibility, ease of industrial availability, etc.;

[0046] The above-mentioned α-(unsaturated alkoxyalkyl) acrylate monomer can be produced, for example, by the production method disclosed in WO 2010 / 114077.

[0047] Preferred examples of the monomer that provides the structural unit (a2) include 2-(hydroxyalkyl)acrylic acid alkyl esters, which can react with (meth)acrylic acid to form a lactone ring structure in the main chain.

[0048] The 2-(hydroxyalkyl)acrylic acid alkyl esters include 2-(1-hydroxyalkyl)acrylic acid alkyl esters, 2-(2-hydroxyalkyl)acrylic acid alkyl esters, etc., and specifically include, for example, 2-(1-hydroxymethyl)methyl acrylate, 2-(1-hydroxymethyl)ethyl acrylate, 2-(1-hydroxymethyl)isopropyl acrylate, 2-(1-hydroxymethyl)n-butyl acrylate, 2-(1-hydroxymethyl)t-butyl acrylate, 2-(1-hydroxymethyl)2-ethylhexyl acrylate, etc. Among them, 2-(1-hydroxymethyl)methyl acrylate and 2-(1-hydroxymethyl)ethyl acrylate are preferred.

[0049] The resin (A) may have only one type of the structural unit (a2), or may have two or more types.

[0050] The content of the structural unit (a2) is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to 100% by mass of all structural units in the resin (A), in terms of good heat resistance and solvent resistance, and is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less.

[0051] (a3) Other structural units The resin (A) may have a structural unit (a3) ​​other than the structural units (a1) and (a2) described above. Examples of the other structural unit (a3) ​​include structural units derived from the following monomers. hydroxyl group-containing monomers such as hydroxyalkyl (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2,3-hydroxypropyl (meth)acrylate; Methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, n-amyl (meth)acrylate, s-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, cyclohexyl (meth)acrylate, (Meth)acrylic acid ester monomers such as dicyclopentanyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, 1,4-dioxaspiro[4,5]dec-2-yl methacrylic acid, (meth)acryloylmorpholine, 4-(meth)acryloyloxymethyl-2-methyl-2-ethyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-isobutyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-cyclohexyl-1,3-dioxolane, and 4-(meth)acryloyloxymethyl-2,2-dimethyl-1,3-dioxolane; Aromatic vinyl monomers such as styrene, vinyltoluene, α-methylstyrene, and methoxystyrene; Epoxy group-containing monomers such as glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, vinylbenzyl glycidyl ether, allyl glycidyl ether, (3,4-epoxycyclohexyl)methyl (meth)acrylate, and vinylcyclohexene oxide; (Meth)acrylamides such as N,N-dimethyl(meth)acrylamide and N-methylol(meth)acrylamide; Macromonomers having a (meth)acryloyl group at one end of the polymer molecular chain, such as polystyrene, polymethyl (meth)acrylate, polyethylene oxide, polypropylene oxide, polysiloxane, polycaprolactone, and polycaprolactam; Conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; Vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, lauryl vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, 2-hydroxyethyl vinyl ether, and 4-hydroxybutyl vinyl ether; N-vinyl compounds such as N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylimidazole, N-vinylmorpholine, and N-vinylacetamide; Unsaturated isocyanates such as isocyanatoethyl (meth)acrylate and allyl isocyanate; and the like.

[0052] In particular, the structural unit (a3) ​​is preferably a structural unit derived from at least one monomer selected from the group consisting of a hydroxyl group-containing monomer, a (meth)acrylic acid ester monomer, an aromatic vinyl monomer, and an epoxy group-containing monomer.

[0053] The resin (A) may have only one type of the structural unit (a3), or may have two or more types.

[0054] The content of the structural unit (a3) ​​is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, relative to 100% by mass of all structural units in the resin (A), in terms of good developability, and is preferably 92% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. When the resin (A) contains two or more types of the structural unit (a3), the content of each structural unit can be appropriately set depending on the application and purpose of the curable resin composition of the present invention.

[0055] The resin (A) preferably further has an epoxy group. When the resin (A) further has an epoxy group, the curability of the curable resin composition of the present invention can be improved, and a cured product having even better solvent resistance can be obtained. The resin (A) having an epoxy group can be obtained by polymerizing a monomer component containing the above-mentioned epoxy group-containing monomer.

[0056] When the resin (A) has an epoxy group, the epoxy equivalent of the resin (A) is preferably from 100 to 20,000 in terms of good solvent resistance, more preferably from 200 to 8,000, and even more preferably from 500 to 5,000. The epoxy equivalent can be determined by dividing the amount of resin by the number of moles of epoxy groups contained in the resin.

[0057] The acid value of the resin (A) is preferably 20 to 230 mgKOH / g. When the acid value is within the above range, the developability is good and a cured film having excellent solvent resistance can be obtained. The acid value is more preferably 30 to 200 mgKOH / g, and further preferably 40 to 180 mgKOH / g. The acid value is a value obtained by measurement by neutralization titration using a KOH solution.

[0058] The weight average molecular weight of the resin (A) is not particularly limited and may be appropriately set depending on the purpose and use of the curable resin composition, but is preferably 1,000 to 100,000, more preferably 2,000 to 50,000, and even more preferably 4,000 to 30,000. The dispersity (weight average molecular weight / number average molecular weight) of the resin (A) is preferably from 1.0 to 4.0, more preferably from 1.1 to 3.5, and even more preferably from 1.5 to 3.0. The weight average molecular weight and dispersity are values ​​obtained by measuring by gel permeation chromatography (GPC) in the manner described in the Examples.

[0059] The resin (A) may have a polymerizable double bond in a side chain. By having a polymerizable double bond in a side chain, the curability of the resin (A) can be improved. The polymerizable double bond can be the above-mentioned polymerizable double bond. Among them, a (meth)acryloyl group is preferable in terms of reactivity.

[0060] When the resin (A) has a polymerizable double bond in a side chain, the double bond equivalent is preferably from 200 to 8000 g / equivalent, more preferably from 250 to 5000 g / equivalent, and further preferably from 300 to 1500 g / equivalent.

[0061] The double bond equivalent is the mass of the solid content of the resin solution per 1 mol of double bonds in the resin (A). The mass of the solid content of the resin solution is the sum of the mass of the monomer components constituting the resin (A) and the mass of the polymerization inhibitor. The double bond equivalent can be obtained by dividing the mass (g) of the resin solid content of the resin solution by the amount of double bonds (mol) of the resin. The amount of double bonds in the resin can be obtained from the amount of the acid group-containing monomer used in the polymerization and the amount of the compound having a functional group and a polymerizable double bond that can be bonded to the acid group. Examples of the functional group that can be bonded to the acid group include a hydroxyl group and an epoxy group. It can also be measured by various analyses such as titration, elemental analysis, NMR, and IR, or a differential scanning calorimeter method.

[0062] (Method for producing acid group-containing alkali-soluble resin) The method for producing the acid group-containing alkali-soluble resin (A) is not particularly limited as long as it can produce a polymer having at least the structural unit (a1) and, if necessary, the structural units (a2) and (a3), and includes a method of polymerizing a monomer component including a monomer capable of introducing each of the structural units (a1) to (a3) ​​by a known method. The amount of each monomer can be appropriately adjusted so that the content of each structural unit in the polymer is within a desired range.

[0063] The method for polymerizing the monomer components is not particularly limited, and commonly used methods such as bulk polymerization, solution polymerization, and emulsion polymerization can be used. Among them, solution polymerization is preferred because it is industrially advantageous and allows easy structural adjustment such as molecular weight. As the polymerization mechanism of the monomer components, a polymerization method based on a mechanism such as radical polymerization, anionic polymerization, cationic polymerization, and coordination polymerization can be used, but a polymerization method based on a radical polymerization mechanism is preferred because of its industrial advantages. The molecular weight of the polymer obtained by polymerizing the above-mentioned monomer components can be controlled by adjusting the amount and type of the polymerization initiator, the polymerization temperature, the type and amount of the chain transfer agent, and the like.

[0064] The polymerization initiator may be a peroxide or an azo compound that is usually used as a polymerization initiator. The chain transfer agent may be a compound having a mercapto group, such as alkyl mercaptans, mercapto carboxylic acids, and mercapto carboxylic acid esters, that are usually used as a chain transfer agent. These may be used alone or in combination of two or more. The amount of these to be added may be appropriately determined by a known method.

[0065] Regarding the polymerization conditions, the polymerization temperature may be appropriately set depending on the type and amount of the monomer used, the type and amount of the polymerization initiator, etc., and is, for example, preferably 50 to 130° C., more preferably 60 to 120° C. Similarly, the polymerization time can also be appropriately set, and is, for example, preferably 1 to 5 hours, more preferably 2 to 4 hours.

[0066] Alternatively, a method may be used in which an acid group is introduced by addition reaction of an acid group-containing compound with a polymer (base polymer) obtained by polymerizing a monomer component containing a hydroxyl group-containing monomer to obtain an acid group-containing alkali-soluble resin. The method for obtaining the base polymer is not particularly limited, and may be the same as the polymerization method described above.

[0067] Examples of the acid group-containing compound include carboxylic acids such as succinic acid, maleic acid, phthalic acid, tetrahydrophthalic acid, and trimellitic acid; and carboxylic acid anhydrides such as succinic anhydride, maleic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, itaconic anhydride, and trimellitic anhydride.

[0068] The above-mentioned addition reaction is not particularly limited and can be carried out by a known method, for example, under conditions of 70 to 100° C. for 1 to 10 hours, preferably 60 to 30° C. for 1 to 7 hours. In the above-mentioned addition reaction, a catalyst, a solvent, etc. that are usually used may be used.

[0069] An example of a method for producing an acid group-containing alkali-soluble resin having a polymerizable double bond in a side chain is a method in which a base polymer having an acid group is prepared, and then a compound having an epoxy group and a polymerizable double bond, such as glycidyl (meth)acrylate, is reacted with the acid group to introduce a polymerizable double bond into the side chain of the resin through an addition reaction caused by cleavage of the epoxy group. Another method is to prepare a base polymer having a hydroxyl group, and then add a compound having an acid group or an isocyanate group and a polymerizable double bond, such as (meth)acrylic acid or 2-isocyanatoethyl (meth)acrylate, to the hydroxyl group, thereby introducing a polymerizable double bond into the side chain of the resin. It is also suitable to introduce a polymerizable double bond into the side chain of a resin by addition reaction of a compound having an acid group, such as (meth)acrylic acid, and a polymerizable double bond with a resin having an epoxy group in the side chain.

[0070] The above-mentioned addition reaction is not particularly limited and can be carried out by a known method. In addition, in the above-mentioned addition reaction, a catalyst, a solvent, etc. that are usually used may be used.

[0071] The method for producing the resin (A) may include other steps in addition to the polymerization reaction step. For example, there may be mentioned an aging step, a neutralization step, a deactivation step of the polymerization initiator or the chain transfer agent, a dilution step, a drying step, a concentration step, a purification step, etc. These steps can be carried out by known methods.

[0072] The content of the resin (A) in the curable resin composition of the present invention is preferably 10 to 60 mass%, more preferably 20 to 50 mass%, and even more preferably 30 to 45 mass%, based on 100 mass% of the total solid content of the curable resin composition. In this specification, the term "total solid content" refers to the total amount of components that form the cured product (components excluding the solvent and the curing catalyst that volatilize during the formation of the cured product).

[0073] (B) Resin having a group that generates an acid group by heat or acid The resin (B) having a group that generates an acid group by heat or acid (hereinafter also referred to as "resin (B)") includes a resin having a structure or group that generates an acid group by the action of heat or acid.

[0074] Examples of structures or groups that generate an acid group by the action of heat or acid include a tertiary carbon-containing group, a group in which an acid group is blocked with a vinyl ether compound, and a group in which a phenolic hydroxyl group is protected with a protecting group such as a t-butyl group or an acetyl group.

[0075] The tertiary carbon-containing group is preferably -COO * R 4 (R 4 represents a monovalent organic group, O * The carbon atom bonded to is a tertiary carbon atom.

[0076] Above - COO * R 4 R 4 represents a monovalent organic group, O * A carbon atom bonded to is a tertiary carbon atom. By tertiary carbon atom, we mean a carbon atom that has three other carbon atoms bonded to it.

[0077] The monovalent organic group is preferably a monovalent linear, branched or cyclic saturated or unsaturated hydrocarbon group having a carbon number of 1 to 91. The organic group may have a substituent. R 4 The number of carbon atoms is more preferably 1 to 50, even more preferably 1 to 35, still more preferably 1 to 20, particularly preferably 1 to 12, and most preferably 1 to 9.

[0078] R 4 is preferably -C(R 5 )(R 6 )(R 7 ) In this case, R 5 , R 6 , and R7 are preferably the same or different and each is a hydrocarbon group having 1 to 30 carbon atoms. The hydrocarbon group may be a saturated or unsaturated hydrocarbon group, may have a cyclic structure, or may have a substituent. 5 , R 6 , and R 7 may be linked to each other at their terminal sites to form a cyclic structure.

[0079] In the above tertiary carbon-containing group, it is preferable that at least one of the adjacent carbon atoms of the tertiary carbon atom is bonded to a hydrogen atom. 4 But -C(R 5 )(R 6 )(R 7 ), R 5 , R 6 and R 7 It is preferable that at least one of the groups contains a carbon atom having one or more hydrogen atoms, and that the carbon atom is bonded to a tertiary carbon atom. Above R 5 , R 6 and R 7 are the same or different and are preferably saturated hydrocarbon groups having 1 to 15 carbon atoms, more preferably saturated hydrocarbon groups having 1 to 10 carbon atoms, even more preferably saturated hydrocarbon groups having 1 to 5 carbon atoms, and particularly preferably saturated hydrocarbon groups having 1 to 3 carbon atoms. Above R 4 is preferably a t-butyl group or a t-amyl group.

[0080] To obtain a polymer having the tertiary carbon-containing group, a tertiary carbon-containing monomer may be used as a monomer component. Preferred examples of the tertiary carbon-containing monomer include t-butyl (meth)acrylate and t-amyl (meth)acrylate.

[0081] Examples of the above-mentioned group in which an acid group is blocked with a vinyl ether compound include groups in which a vinyl ether compound is bonded to the above-mentioned acid group such as a carboxyl group. Examples of the vinyl ether compound include aliphatic vinyl ether compounds such as methyl vinyl ether, ethyl vinyl ether, i-propyl vinyl ether, n-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, 2-ethylhexyl vinyl ether, and cyclohexyl vinyl ether; and cyclic ether compounds such as dihydropyran that can generate vinyl ethers by ring-opening. Among the above vinyl ether compounds, dihydropyran is preferred since the protecting group is easily removed at a lower temperature.

[0082] The above-mentioned group in which an acid group is blocked with dihydropyran is preferably a group represented by the following formula:

[0083] [ka]

[0084] Preferred examples of the group in which a phenolic hydroxyl group is protected by a protecting group such as a t-butyl group or an acetyl group include groups represented by the following formula.

[0085] [ka] (In the formula, n represents the number of substituents and is an integer of 1 to 5.)

[0086] The group represented by the above formula is reacted, for example, in a solvent in the presence of an acid catalyst such as hydrochloric acid or sulfuric acid at a temperature of 50 to 150° C. for 1 to 30 hours, whereby the protecting group is eliminated and an acid group is generated.

[0087] Among these, the above-mentioned groups in which the acid group is blocked with dihydropyran are preferred, since the acid group can be generated at a lower temperature.

[0088] (b1) Structural unit represented by general formula (2) The resin (B) is preferably a resin having a structural unit (b1) represented by the following general formula (2).

[0089] [ka]

[0090] (In the formula, R 3 represents a hydrogen atom or a methyl group. X represents a direct bond or a divalent organic group. A represents a group that generates an acid group by the action of heat or an acid. In the above general formula (2), R 3 represents a hydrogen atom or a methyl group. Among these, R 3 is preferably a methyl group. X represents a direct bond or a divalent organic group.

[0091] The divalent organic group includes a divalent hydrocarbon group which may have a substituent.

[0092] Examples of the divalent hydrocarbon group include an alkylene group, a cycloalkylene group, and an arylene group. In the divalent hydrocarbon group, at least one of the atoms constituting the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, or a sulfur atom. Examples of the substituent include a hydroxyl group, an alkoxy group, and a halogen atom. X is preferably a direct bond.

[0093] In the above general formula (2), A represents a group that generates an acid group by the action of heat or acid. Examples of the group that generates an acid group by the action of heat or acid include the same structures or groups that generate an acid group by the action of heat or acid described above.

[0094] The resin (B) may have only one type of the structural unit (b1), or may have two or more types.

[0095] The content of the structural unit (b1) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of all structural units in the resin (B), in terms of good solvent resistance, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0096] (b2) Structural unit having a ring structure in the main chain The resin (B) is preferably a polymer having a ring structure in the main chain. By having a ring structure in the main chain, the heat resistance of the resin (B) can be improved. Examples of the ring structure include the same ring structure as described in (a2) above. The resin (B) preferably further has a structural unit (b2) having a ring structure in the main chain. Examples of the monomer capable of introducing the structural unit (b2) include the same monomers as those capable of introducing the structural unit (a2) described above. The resin (B) may have only one type of the structural unit (b2), or may have two or more types.

[0097] The content of the structural unit (b2) is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to 100% by mass of all structural units in the resin (B), in terms of good heat resistance and solvent resistance, and is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less.

[0098] (b3) Other structural units The resin (B) may further include a structural unit (b3) other than the structural units (b1) and (b2) described above. Examples of the other structural unit include the same structural units as the other structural unit (a3) ​​described above. In particular, the structural unit (b3) is preferably a structural unit derived from at least one monomer selected from the group consisting of a hydroxyl group-containing monomer, a (meth)acrylic acid ester monomer, an aromatic vinyl monomer, and an epoxy group-containing monomer.

[0099] The resin (B) may have only one type of the structural unit (b3), or may have two or more types.

[0100] The content of the structural unit (b3) is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, relative to 100% by mass of all structural units in the resin (B), in terms of good developability, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. When the resin (B) contains two or more types of the structural unit (b3), the content ratio of each structural unit can be appropriately designed depending on the application and purpose of the curable resin composition of the present invention.

[0101] The resin (B) preferably further has an epoxy group. When the resin (B) further has an epoxy group, the curability of the curable resin composition can be improved, and a cured product having even better solvent resistance can be obtained. The resin (B) having an epoxy group can be obtained by polymerizing a monomer component containing the above-mentioned epoxy group-containing monomer.

[0102] The acid value of the resin (B) is preferably 20 to 230 mgKOH / g. When the acid value is within the above range, the developability is good and a cured film having excellent solvent resistance can be obtained. The acid value is more preferably 30 to 200 mgKOH / g, and further preferably 40 to 180 mgKOH / g. The acid value is a value obtained by measurement by neutralization titration using a KOH solution.

[0103] The weight average molecular weight of the resin (B) is not particularly limited and may be appropriately set depending on the purpose and use of the curable resin composition of the present invention, but is preferably 1,000 to 100,000, more preferably 2,000 to 50,000, and even more preferably 4,000 to 30,000. The dispersity (weight average molecular weight / number average molecular weight) of the resin (B) is not particularly limited, but is preferably from 1.0 to 4.0, more preferably from 1.1 to 3.5, and even more preferably from 1.5 to 3.0. The weight average molecular weight and dispersity of the polymer are values ​​obtained by measuring by gel permeation chromatography (GPC) in the manner described in the Examples.

[0104] The resin (B) may have a polymerizable double bond in a side chain. By having a polymerizable double bond in a side chain, the curability of the resin (B) can be improved. The polymerizable double bond is preferably the same as that in the acid group-containing alkali-soluble resin (A) described above. When the resin (B) has a polymerizable double bond in a side chain, the double bond equivalent is preferably in the same range as that in the acid group-containing alkali-soluble resin (A) described above.

[0105] (Method of producing a resin having a group that generates an acid group by heat or acid) The method for producing the resin (B) having a group that generates an acid group by heat or acid is not particularly limited as long as it is a method that can obtain a polymer having at least the structural unit (b1) and, if necessary, the structural units (b2) and (b3), and includes a method of polymerizing a monomer component containing a monomer that can introduce each of the structural units (b1) to (b3) by a known method. In addition, a protecting group may be added to the acid group after polymerizing the monomer component containing an acid group-containing monomer. The amount of each monomer can be appropriately adjusted so that the content of each structural unit in the polymer falls within a desired range. The polymerization method is not particularly limited, and may be the same as the method for producing the resin (A) described above.

[0106] The content of the resin (B) is preferably 10 to 60 mass%, more preferably 20 to 50 mass%, and further preferably 30 to 45 mass%, relative to 100 mass% of the total solid content of the curable resin composition. When the resin (A) and the resin (B) are used in combination, the total content of the resin (A) and the resin (B) is preferably 1 to 50 mass%, more preferably 3 to 40 mass%, and further preferably 5 to 35 mass%, based on 100 mass% of the total solid content of the curable resin composition.

[0107] In the present invention, the resin (B) may have the above-mentioned acid group. In the present invention, the resin (B) may have the above-mentioned group that generates an acid group by heat or acid and the above-mentioned acid group.

[0108] (C) Polymer having vinyl ether group in the side chain The polymer (C) having a vinyl ether group in a side chain (hereinafter also referred to as "polymer (C)") is not particularly limited as long as it is a polymer having at least one vinyl ether group represented by -O-CH=CH2 in a side chain, but preferably has a structural unit (c1) represented by the following general formula (1).

[0109] [ka] (In the formula, R 1 R represents a hydrogen atom or methyl. 2 represents a hydrogen atom or an organic group. W represents a direct bond or a divalent organic group.

[0110] In the above general formula (1), R 1 represents a hydrogen atom or a methyl group. R 2 represents a hydrogen atom or an organic group. 2Examples of the organic group represented by the formula (I) include linear or cyclic monovalent hydrocarbon groups having 1 to 20 carbon atoms, and such hydrocarbon groups in which at least a portion of the atoms constituting the hydrocarbon groups has been substituted with a halogen atom, an oxygen atom, a nitrogen atom, or a sulfur atom.

[0111] The chain hydrocarbon group may be a linear or branched aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated hydrocarbon group such as an alkyl group, or an unsaturated hydrocarbon group such as an alkenyl group, preferably a saturated hydrocarbon group. Specific examples of the aliphatic hydrocarbon group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a hexyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a heptyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 2,2-dimethylpentyl group, a 2,3-dimethylpentyl group, a 2,4-dimethylpentyl group, a 3-ethylpentyl group, a 2,2,3-trimethylbutyl group, an octyl group, a methylheptyl group, a dimethylhexyl group, a 2-ethylhexyl group, a 3-ethylhexyl group, a trimethylpentyl group, a 3-ethyl-2-methylpentyl group, a 2-ethyl-3-methylpentyl group, a 2,2,3,3-trimethylbutyl group, a Tetramethylbutyl group, nonyl group, methyloctyl group, 3,7-dimethyloctyl group, dimethylheptyl group, 3-ethylheptyl group, 4-ethylheptyl group, trimethylhexyl group, 3,3-diethylpentyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group, eicosyl group, etc. alkyl groups such as those mentioned above; and alkenyl groups such as a vinyl group, an n-propenyl group, an isopropenyl group, a 1-butenyl group, a 2-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 2-methyl-1-butenyl group, a 2-methyl-2-butenyl group, a 3-methyl-1-butenyl group, a 1-hexenyl group, a 2-hexenyl group, a 1-heptenyl group, a 2-heptenyl group, a 1-octenyl group, or a 2-octenyl group.

[0112] Examples of the cyclic hydrocarbon group include alicyclic hydrocarbon groups and aromatic hydrocarbon groups. Examples of the alicyclic hydrocarbon group include cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, and a cyclododecyl group. Examples of the aromatic hydrocarbon group include a phenyl group, a naphthyl group, a biphenyl group, a methoxyphenyl group, a trichlorophenyl group, an ethylphenyl group, a tolyl group, a xylyl group, and a benzyl group. The halogen atom is preferably chlorine, bromine or fluorine, and more preferably fluorine.

[0113] Among them, the above R 2 The organic group represented by the formula (I) is preferably a linear or cyclic hydrocarbon group having 1 to 11 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or an aromatic hydrocarbon group having 6 to 11 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms.

[0114] W represents a direct bond or a divalent organic group. The divalent organic group may be any of the divalent organic groups described above, and preferably includes a divalent hydrocarbon group and a group containing a bond such as -O-, -COO-, -CO-, -S-, -SO-, or -SO2- together with a divalent hydrocarbon group. The divalent hydrocarbon group includes a divalent group obtained by removing one hydrogen atom from the above-mentioned monovalent hydrocarbon group, such as an alkylene group, a cycloalkylene group, and an arylene group. In the divalent hydrocarbon group, at least one of the atoms constituting the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, a sulfur atom or a halogen atom. The divalent hydrocarbon group may have a substituent, and examples of the substituent include a hydroxyl group, a carboxyl group, an alkoxy group, and a halogen atom.

[0115] Examples of the group containing a bond such as -O-, -COO-, -CO-, -S-, -SO-, -SO2-, etc. together with the divalent hydrocarbon group include -(OR) a -(a is an integer from 1 to 5), -(RO) a -(a is an integer of 1 to 5), -R-COO-, -COO-R-, -CO-R-, -R-CO-R'-, -O-CO-R-, -RO-CO-R'-, -RS-, -RS-R'-, -R-SO-, -R-SO2-R'- (in each case, R and R' are the same or different and represent the above-mentioned divalent hydrocarbon group), and the like. Among these, a group containing the above divalent hydrocarbon group and an -O- bond is preferred, a group represented by -(OR)a- (wherein R represents the above divalent hydrocarbon group, and a is an integer of 1 to 5) is more preferred, and -(OR) a - (R represents an alkylene group having 1 to 2 carbon atoms, and a is an integer of 1 or 2) is more preferable.

[0116] The divalent organic group preferably has 1 to 10 carbon atoms, more preferably 2 to 6 carbon atoms, and even more preferably 3 or 4 carbon atoms.

[0117] Among them, the structural unit (c1) represented by the above general formula (1) is preferably one represented by the following general formula (1-1).

[0118] [ka] (In the formula, R 1 R represents a hydrogen atom or a methyl group. 2 represents a hydrogen atom or an organic group. 8 and R 9 are the same or different and represent a hydrogen atom or an organic group; and m represents an integer of 1 or more.

[0119] In the above general formula (1-1), R 1 and R 2 is R in the above general formula (1). 1 and R 2 is the same as: In the above general formula (1-1), R8 and R 9 are the same or different and represent a hydrogen atom or an organic group. R 8 and R 9 The organic group represented by the above-mentioned R 2 Among them, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogenated alkyl group having 1 to 5 carbon atoms, and an aromatic hydrocarbon group having 6 to 12 carbon atoms are preferred, an alkyl group having 1 to 6 carbon atoms, a halogenated alkyl group having 1 to 5 carbon atoms, and an aromatic hydrocarbon group having 6 to 11 carbon atoms are more preferred, and an alkyl group having 1 to 2 carbon atoms, a halogenated alkyl group having 1 to 2 carbon atoms, and an aromatic hydrocarbon group having 6 to 8 carbon atoms are even more preferred.

[0120] The polymer having the structural unit (c1) can be obtained, for example, by polymerizing a monomer component containing a vinyl ether group-containing (meth)acrylic acid ester represented by the following general formula (1-2).

[0121] [ka] In the above general formula (1-2), R 1 , R 2 and W is R in the above general formula (1). 1 , R 2 and W, respectively.

[0122] Specific preferred examples of the vinyl ether group-containing (meth)acrylic acid esters represented by the above general formula (1-2) include 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, 2-vinyloxyethyl (meth)acrylate, and the like.

[0123] The polymer (C) may have only one type of the structural unit (c1), or may have two or more types.

[0124] The content of the structural unit (c1) in the polymer (C) is preferably 1 to 100 mol % relative to 100 mol % of all structural units. The content of the structural unit (c1) is more preferably 4 mol % or more, and even more preferably 8 mol % or more, in terms of increasing the crosslinking density and imparting solvent resistance, hardness, etc. to the cured product. The content of the structural unit (c1) is preferably 95 mol % or less, and more preferably 90 mol % or less. When two or more types of the structural unit (c1) are contained, the above content is the total content of the two or more types.

[0125] The polymer (C) may further have another structural unit (c2). Examples of the other structural unit (c2) include structural units derived from polymerizable monomers other than the vinyl ether group-containing (meth)acrylic acid esters. Examples of the other polymerizable monomer include polymerizable monomers having an electron-deficient double bond, and these can be appropriately selected depending on the purpose and application of the polymer to be produced.

[0126] Specific examples of the polymerizable monomer having an electron-deficient double bond include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-amyl (meth)acrylate, s-amyl (meth)acrylate, t-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, tridecyl (meth)acrylate, (Meth)acrylic acid esters such as octyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, cyclohexylmethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, 2-(acetoacetoxy)ethyl (meth)acrylate, and allyl (meth)acrylate; cyclic ether group-containing (meth)acrylic acid esters, such as glycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and (3-ethyloxetan-3-yl)methyl (meth)acrylate; Halogen-containing (meth)acrylic acid esters such as trifluoroethyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; nitrogen atom-containing polymerizable monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N,N'-dimethylaminoethyl(meth)acrylate, N-phenylmaleimide, N-cyclohexylmaleimide, and 2-isopropenyl-2-oxazoline; Isocyanate group-containing polymerizable monomers such as 2-(meth)acryloyloxyethyl isocyanate and (meth)acryloyl isocyanate; UV-stable polymerizable monomers such as 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine and 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine; Polymerizable cyclic lactone monomers such as methylene butyrolactone and methyl methylene butyrolactone; (meth)acrylonitrile; maleic anhydride; 1,4-dioxaspiro[4,5]dec-2-yl methacrylic acid, (meth)acryloylmorpholine, tetrahydrofurfuryl acrylate, 4-(meth)acryloyloxymethyl-2-methyl-2-ethyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-isobutyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2-methyl-2-cyclohexyl-1,3-dioxolane, 4-(meth)acryloyloxymethyl-2,2-dimethyl-1,3-dioxolane; and the like.

[0127] Among them, the other structural unit (c2) preferably contains a (meth)acrylic acid ester. Since the vinyl ether group contained in the structural unit (c1) is highly hydrophilic, the compatibility of the curable resin composition can be adjusted by copolymerizing the polymer (C) with a highly hydrophobic (meth)acrylic acid ester, and the content of the polymer (C) can be increased. Among the above (meth)acrylic acid esters, cyclohexyl (meth)acrylate is more preferred.

[0128] The other polymerizable monomer preferably has 1 to 22 carbon atoms, more preferably 1 to 18 carbon atoms, and further preferably 3 to 15 carbon atoms.

[0129] The polymer (C) may have only one type of the other structural unit (c2), or may have two or more types.

[0130] The content of the structural unit (c2) in the polymer (C) is preferably 0 to 99 mol% relative to 100 mol% of all structural units. The content of the structural unit (c2) is more preferably 5 mol% or more, even more preferably 10 mol% or more, more preferably 96 mol% or less, and even more preferably 92 mol% or less, in that the cured product can be provided with various physical properties derived from the structural unit (c2), such as flexibility, adhesion, stability, and heat resistance. When two or more types of structural units (c2) are contained, the above content is the total content of the two or more types.

[0131] The content ratio of the structural units (c1) and (c2) can be determined by gas chromatography, liquid chromatography, 1 Using H-HMR, etc., the reaction ratio of vinyl ether group-containing (meth)acrylic acid esters and other monomers and 1 It can be determined by a method of comparing the corresponding integral values ​​of H-NMR.

[0132] The polymer (C) preferably has a terminal group derived from a silane compound having a carbon-carbon double bond at the end of the main chain. When the polymer (C) is produced by group transfer polymerization using a silane compound having a carbon-carbon double bond as a polymerization initiator as described below, a group derived from the silane compound having a carbon-carbon double bond is formed at the end of the main chain of the polymer on the polymerization initiation side.

[0133] Preferred examples of the terminal group derived from the silane compound having a carbon-carbon double bond include structures represented by the following general formula (3), (4) or (5).

[0134] [ka] (In the formula, R 10 and R 11 R may be the same or different and represents a hydrogen atom or an organic group. 12 represents an organic group.

[0135] [ka] (In the formula, R 10 , R 11 and R 13 are the same or different and represent a hydrogen atom or an organic group.

[0136] [ka] (In the formula, R 10 , R 11 , R 14 , R 15 and R 16 are the same or different and represent a hydrogen atom or an organic group.

[0137] In the above general formulas (3), (4) and (5), R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 Examples of the organic group represented by the formula (I) include the same organic groups as those described above, and among them, a hydrocarbon group having 1 to 12 carbon atoms is preferable.

[0138] Examples of the hydrocarbon group include an alkyl group, an alkenyl group, a cycloalkyl group, a cycloalkenyl group, an aromatic hydrocarbon group, etc. In the hydrocarbon group, at least a part of the atoms constituting the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, or a sulfur atom, and one or more of the hydrogen atoms constituting the hydrocarbon group may be substituted with a substituent such as a halogen atom such as a fluorine atom, a chlorine atom, or a bromine atom; a hydroxyl group; or an alkoxy group.

[0139] Among them, R 10 and R 11The hydrocarbon group represented by the formula (I) is more preferably an alkyl group, a cycloalkyl group, a haloalkyl group, or an aromatic hydrocarbon group having 1 to 6 carbon atoms, even more preferably an alkyl group or a cycloalkyl group having 1 to 6 carbon atoms, even more preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably a methyl group or an ethyl group.

[0140] R 12 , R 13 , R 14 , R 15 and R 16 Examples of the organic group represented by the formula (I) include the same organic groups as those described above. Among them, a hydrocarbon group having 1 to 22 carbon atoms is preferable, an alkyl group, a cycloalkyl group, or an aromatic hydrocarbon group having 1 to 12 carbon atoms is more preferable, a methyl group, an ethyl group, a propyl group, a butyl group, a tert-butyl group, an adamantyl group, a cyclohexyl group, a 2-ethylhexyl group, or a phenyl group is even more preferable, and a methyl group, an ethyl group, or a tert-butyl group is particularly preferable. R 12 , R 13 , R 14 , R 15 and R 16 In the hydrocarbon group represented by the formula (I), at least a portion of the atoms constituting the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom or a sulfur atom, and one or more of the hydrogen atoms constituting the hydrocarbon group may be substituted with a substituent such as a halogen atom such as a fluorine atom, a chlorine atom or a bromine atom; a hydroxyl group; or an alkoxy group.

[0141] Also, R 10 and R 11 , or R 10 Or R 11 and R 12 ~R 16 may be bonded to form a ring structure. Examples of the ring structure include alicyclic hydrocarbon structures such as cycloalkyls (e.g., cyclohexyl, cyclopentyl, etc.), oxygen-containing heterocyclic structures (e.g., dihydrofuran ring, tetrahydrofuran ring, dihydropyran ring, tetrahydropyran ring, etc.), and the like.

[0142] In producing the polymer (C) by the group transfer polymerization, when a silyl ketene acetal represented by the general formula (7), a vinyl silane compound represented by the general formula (8), or an allyl silane compound represented by the general formula (9) described below is used as a polymerization initiator, the resulting polymer has main chain terminals having structures represented by the general formulas (3), (4), and (5), respectively. In particular, the polymer (C) preferably has a terminal group derived from the silyl ketene acetal represented by the above general formula (3) in the main chain, since the molecular weight distribution is easily controlled when the polymer (C) is obtained by group transfer polymerization.

[0143] The polymer (C) may further have a terminal structure represented by the following general formula (6). When one end of the main chain has the terminal structure represented by the following general formula (6), the polymer can be given a desired function. The polymer (C) preferably has an end group derived from the silane compound having a carbon-carbon double bond at one end of the main chain, and has a terminal structure represented by the following general formula (6) at the other end.

[0144] [ka]

[0145] (In the formula, R 1 R represents a hydrogen atom or a methyl group. 2 represents a hydrogen atom or an organic group; W represents a direct bond or a divalent organic group; and Y represents a hydrogen atom, a halogen atom, an alkyl group, a hydroxymethyl group, an allyl group, or a propargyl group.

[0146] In the above general formula (6), R 1 , R 2 and W is R in the above general formula (1). 1 , R 2 and W, respectively.

[0147] In the above general formula (6), Y represents a hydrogen atom, a halogen atom, an alkyl group, a hydroxymethyl group, an allyl group, or a propargyl group. The above alkyl group is preferably an alkyl group having 1 to 8 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Among these, the above-mentioned Y is preferably a hydrogen atom in terms of enabling the terminal groups of the polymer to be unified, is preferably a propargyl group in terms of facilitating the imparting of functionality to the polymer, and is preferably an alkyl group in terms of increasing the stability of the polymer.

[0148] The weight average molecular weight of the polymer (C) has a range suitable for various applications, but is preferably in the range of 1000 to 1,000,000. The weight average molecular weight of the polymer (C) is more preferably in the range of 1000 to 500,000, further preferably in the range of 5,000 to 200,000, and particularly preferably in the range of 10,000 to 200,000.

[0149] The number average molecular weight of the polymer (C) is preferably in the range of 1,000 to 1,000,000. The number average molecular weight of the polymer (C) is more preferably in the range of 1,000 to 500,000, and further preferably in the range of 5,000 to 200,000.

[0150] The polymer (C) preferably has a dispersity (weight average molecular weight / number average molecular weight) of 5.0 or less. When the dispersity is 5.0 or less, the variation in various physical properties of the polymer can be suppressed. The dispersity is more preferably 3.5 or less, and even more preferably 2.5 or less. The lower limit is usually 1.0 or more.

[0151] The weight average molecular weight and number average molecular weight of the polymer (C) can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below. The dispersity can be determined by dividing the weight average molecular weight by the number average molecular weight.

[0152] The amount of insoluble matter in the above polymer (C) is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less, relative to 100% by mass of the above polymer. If the amount of insoluble matter is large, there is a risk that the shape of the cured product of the curable composition may be deteriorated, such as that a flat coating film cannot be obtained, or that the strength of the cured product may be reduced.

[0153] The insoluble matter is a gel component contained in the polymer (C), and is preferably a component insoluble in ethyl acetate, toluene or tetrahydrofuran, and has a solubility at 25°C of 0.5 g or less, preferably 0.1 g or less, per 100 g of ethyl acetate, toluene or tetrahydrofuran.

[0154] The amount of the insoluble matter can be calculated by adding ethyl acetate, toluene or tetrahydrofuran to the mixture so that the concentration of the polymer becomes about 33% by mass, thoroughly stirring the mixture at room temperature, and then passing the mixture through a filter having a pore size of 4 μm. The amount of the insoluble matter remaining on the filter after drying is defined as (b) and the amount of the initial polymer is defined as (a), and the amount of the insoluble matter can be calculated by (b) / (a)×100.

[0155] The content of the polymer (C) is preferably 1 to 50 mass%, more preferably 2 to 40 mass%, and even more preferably 5 to 30 mass%, relative to 100 mass% of the total solid content of the curable resin composition, in terms of good solvent resistance.

[0156] (Method for producing polymer (C)) The method for producing the polymer (C) is not particularly limited as long as it can produce the polymer (C) having the structural unit (c1) described above, but the method of producing the polymer (C) by group transfer polymerization of the monomer component containing the vinyl ether group-containing (meth)acrylic acid esters described above is preferred in terms of efficient production of the polymer (C). By carrying out group transfer polymerization, a polymer obtained by polymerizing only the (meth)acryloyl group of the vinyl ether group-containing (meth)acrylic acid esters can be efficiently produced. In addition, according to this method, the amount of gel components (insolubles) contained in the obtained polymer (C) can be kept low.

[0157] As a preferred method for producing the polymer (C), the method using the group transfer polymerization will be described below. The method for producing the polymer (C) preferably includes a step of subjecting a monomer component containing the vinyl ether group-containing (meth)acrylic acid ester described above to group transfer polymerization in the presence of a silane compound having a carbon-carbon double bond and a catalyst.

[0158] Specifically, in the above polymerization reaction, any two of the above monomer components, catalyst, and silane compound having a carbon-carbon double bond are charged into a reaction vessel before the reaction, and the remaining one is added to start the polymerization. The order in which these are added is not particularly limited, and the polymerization can be started by adding them in any manner. In addition, the silane compound having a carbon-carbon double bond, the catalyst, and the monomer component may each be added in a total amount at once, or may be added continuously in small amounts, or may be added in several portions.

[0159] The molecular weight of the polymer obtained by polymerizing the above-mentioned monomer components can be appropriately controlled by the type and amount of the above-mentioned monomer components, the type and amount of the above-mentioned silane compound having a carbon-carbon double bond, the type and amount of the above-mentioned catalyst, and the type and amount of the solvent used.

[0160] The amount of the silane compound having a carbon-carbon double bond used is not particularly limited as long as the desired polymer can be obtained. However, in order to produce the polymer more efficiently, it is preferable to use a silane compound having a carbon-carbon double bond in an amount of 1×10 to the monomer component used. -4 Preferably, the content is 1×10 -3 More preferably, up to 5 mol%, 1×10 -2 It is more preferably up to 1 mol %.

[0161] The amount of the catalyst used is not particularly limited as long as the desired polymer can be obtained. However, in order to produce the polymer more efficiently, it is preferable to use an amount of the catalyst of 1×10 to the monomer component used. -4 Preferably, the content is 1×10 -3 More preferably, up to 5 mol%, 1×10 -2 It is more preferably up to 1 mol %.

[0162] The polymerization reaction can be carried out without using a solvent, but it is preferable to use a solvent. The solvent to be used is not limited as long as it can dissolve the raw material, catalyst, polymerization initiator, and polymer, but an aprotic solvent is preferable in that the polymerization reaction can proceed efficiently.

[0163] Specific examples of the solvent used in the polymerization include aromatic hydrocarbon solvents such as toluene, xylene, and benzene; aliphatic hydrocarbon solvents such as hexane, pentane, heptane, and cyclohexane; ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; halogenated hydrocarbon solvents such as chlorobenzene, dichloromethane, chloroform, and 1,2-dichloroethane; nitrile solvents such as acetonitrile, propionitrile, and valeronitrile; ester solvents such as methyl acetate, ethyl acetate, isopropyl acetate, and butyl acetate; dimethylformamide (DMF), dimethyla Examples of suitable solvents include amide-based solvents such as cetoamide and N-methylpyrrolidone; ether-based solvents such as diethyl ether, diisopropyl ether, 1,2-dimethoxyethane (DME), 1,4-dioxane, tetrahydrofuran (THF), tetrahydropyran (THP), anisole, diethylene glycol dimethyl ether (diglyme), diethylene glycol ethyl ether (carbitol), and cyclopentyl methyl ether (CPME); fluorine-based solvents such as perfluorohexane, perfluorocyclohexane, pentafluorobenzene, and octafluorotoluene; and DMSO and nitromethane. Among them, in terms of allowing the polymerization reaction to proceed more efficiently, the solvent is preferably at least one selected from the group consisting of aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, ketone solvents, halogenated hydrocarbon solvents, ether solvents, ester solvents, and nitrile solvents, and more preferably an aromatic hydrocarbon solvent, an ether solvent, or an ester solvent. The above solvents may be used alone or in combination of two or more.

[0164] The amount of the solvent used is preferably 10 to 10,000% by mass, more preferably 50 to 5,000% by mass, and even more preferably 100 to 1,000% by mass, based on 100% by mass of the total amount of the monomer components used.

[0165] In addition, in the above polymerization, the oxygen concentration in the solvent at the start of polymerization is preferably 1000 ppm or less. When the oxygen concentration in the solvent at the start of polymerization is within the above range, the activity of the silane compound having the carbon-carbon double bond and the catalyst is less likely to decrease, so that the polymerization reaction proceeds more smoothly and the desired polymer can be produced more efficiently. The oxygen concentration is more preferably 800 ppm or less, and even more preferably 0 to 500 ppm. The oxygen concentration can be measured by a polarographic dissolved oxygen meter.

[0166] In addition, in the above polymerization, the water content in the solvent at the start of polymerization is preferably 1000 ppm or less. When the water content in the solvent at the start of polymerization is within the above range, the silane compound having the carbon-carbon double bond is less likely to decompose and the activity of the catalyst is less likely to decrease, so that the polymerization reaction proceeds better and the desired polymer can be produced more efficiently. The water content is more preferably 500 ppm or less, and even more preferably 300 ppm or less. The water content can be measured by the Karl Fischer water content measurement method.

[0167] The reaction temperature in the polymerization is not particularly limited, but from the viewpoint of controlling the molecular weight and molecular weight distribution and maintaining the catalytic activity, it is preferably −20 to 100° C., more preferably −10 to 50° C., and even more preferably 0 to 30° C. In addition, from the viewpoint of reducing the production cost, a preferable embodiment of the production method of the present invention includes a step of polymerization at room temperature ±20° C. The reaction time is not particularly limited, but is preferably 10 minutes to 48 hours, more preferably 30 minutes to 36 hours, and further preferably 1 to 24 hours.

[0168] The reaction atmosphere in the polymerization may be air, but is preferably an inert gas atmosphere such as nitrogen or argon. The oxygen concentration in the atmosphere during the polymerization is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 100 ppm or less.

[0169] The polymer obtained by the above polymerization reaction has a silyl ketene acetal structure or an enolate anion structure containing the silyl group of the polymerization initiator at the main chain terminal, and the polymerization reaction can be terminated by adding water, alcohol, or acid to the reaction system to convert the silyl ketene acetal or enolate anion at one terminal of the polymer to a carboxylic acid or ester. Examples of the alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol. Examples of the acid include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, and organic acids such as acetic acid and benzoic acid. The amount of water, alcohol or acid used is not particularly limited, but is preferably 1 to 1000 mol, more preferably 1 to 100 mol, and even more preferably 1 to 10 mol per mol of the silane compound having a carbon-carbon double bond used.

[0170] Alternatively, an electrophilic agent may be added instead of the water, alcohol, or acid. By adding the electrophilic agent, a desired functional group can be introduced to terminate the polymerization reaction. Examples of the electrophilic agent include halogens such as iodine and bromine, halogenated succinimide compounds, alkyl halides, allyl halides, propargyl halides, aldehydes, and acid chlorides. The amount of the electrophilic agent used is not particularly limited, but is preferably 0.5 to 1.5 mol, more preferably 0.6 to 1.3 mol, and even more preferably 0.8 to 1.2 mol, per mol of the silyl ketene acetal used.

[0171] The monomer component, the silane compound having a carbon-carbon double bond, and the catalyst used in the above production method will be described below.

[0172] The monomer components include a monomer capable of introducing the structural unit (c1) and a monomer capable of introducing the structural unit (c2). The monomer capable of introducing the structural unit (c1) includes the vinyl ether group-containing (meth)acrylic acid esters described above. The monomer capable of introducing the structural unit (c2) includes the other polymerizable monomers described above. The content of each of the above monomers may be appropriately set so as to obtain a polymer having structural units within a desired content range.

[0173] Examples of the silane compound having a carbon-carbon double bond include a silane compound represented by the following general formula (7):

[0174] [ka]

[0175] (In the formula, R 10 and R 11 R may be the same or different and represents a hydrogen atom or an organic group. 12 , R 17 , R 18 and R 19 R may be the same or different and represents an organic group. 10 and R 11 or R 11 and R 12 may be bonded to form a ring structure. 17 , R 18 and R 19 Two or more of these may be bonded to form a ring structure.) Silyl ketene acetal represented by the following general formula (8):

[0176] [ka]

[0177] (In the formula, R 10 , R 11 and R 13 R may be the same or different and represents a hydrogen atom or an organic group. 17 , R 18and R 19 R may be the same or different and represents an organic group. 10 and R 11 or R 11 and R 13 may be bonded to form a ring structure. 17 , R 18 and R 19 Two or more of these may be bonded to form a ring structure.) and a vinylsilane compound represented by the following general formula (9):

[0178] [ka]

[0179] (In the formula, R 10 , R 11 , R 14 , R 15 and R 16 R may be the same or different and represents a hydrogen atom or an organic group. 17 , R 18 and R 19 R may be the same or different and represents an organic group. 10 and R 11 or R 11 and R 14 may be bonded to form a ring structure. 17 , R 18 and R 19 Two or more of these may be bonded to form a ring structure.) Preferred examples of the allylsilane compounds include one or more of the following: Among these, silyl ketene acetal is more preferred since the polymerization proceeds efficiently.

[0180] In the above general formulas (7), (8) and (9), R 10 and R 11 are the same or different and represent a hydrogen atom or an organic group. Above R 10 and R 11 As the R 10 and R 11The same thing is mentioned in each case. Above R 12 ~R 16 As the R 12 ~R 16 The same thing is mentioned in each case.

[0181] In the above general formulas (7), (8) and (9), R 17 , R 18 , and R 19 may be the same or different and represent an organic group. R 17 , R 18 and R 19 Examples of the organic group represented by the formula (I) include the same organic groups as those described above. Among them, a hydrocarbon group or an alkoxy group having 1 to 12 carbon atoms is preferable, a hydrocarbon group or an alkoxy group having 1 to 6 carbon atoms is more preferable, and a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, a phenyl group, a methoxy group, or an ethoxy group is even more preferable.

[0182] In addition, the above R 17 , R 18 and R 19 In the hydrocarbon group represented by the formula (I), at least a portion of the atoms constituting the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom or a sulfur atom, and one or more of the hydrogen atoms constituting the hydrocarbon group may be substituted with a substituent such as a halogen atom such as a fluorine atom, a chlorine atom or a bromine atom; a hydroxyl group; or an alkoxy group.

[0183] -SiR in the above general formulas (7), (8) and (9) 17 R 18 R 19Specific examples of the group represented by the formula (1) include a trimethylsilyl group, a triethylsilyl group, a triisopropylsilyl group, a triisobutylsilyl group, a tert-butyldimethylsilyl group, a triphenylsilyl group, a methyldiphenylsilyl group, a dimethylphenylsilyl group, a trimethoxysilyl group, a triethoxysilyl group, etc. Among these, a trimethylsilyl group, a triethylsilyl group, a triisopropylsilyl group, a tert-butyldimethylsilyl group, a triethoxysilyl group, and a triphenylsilyl group are preferred in terms of ease of availability and ease of synthesis.

[0184] Specific examples of the silyl ketene acetal represented by the above general formula (7) include methyl(trimethylsilyl)dimethyl ketene acetal, methyl(trimethylsilyl)diisopropyl ketene acetal, methyl(triethylsilyl)dimethyl ketene acetal, methyl(triisopropylsilyl)dimethyl ketene acetal, methyl(tert-butyldimethylsilyl)dimethyl ketene acetal, methyl(trimethylsilyl)diethyl ketene acetal, and methyl(triphenylsilyl)dimethyl ketene acetal. acetal, methyl(methyldiphenylsilyl)dimethylketene acetal, methyl(dimethylphenylsilyl)dimethylketene acetal, methyl(triethoxysilyl)dimethylketene acetal, ethyl(trimethylsilyl)dimethylketene acetal, 2-ethylhexyl(trimethylsilyl)dimethylketene acetal, tert-butyl(trimethylsilyl)dimethylketene acetal, 1-[(1-methoxy-2-methyl-1-propenyl)oxy]-1-methylsilacyclobutane, and the like. Among these, methyl(trimethylsilyl)dimethylketene acetal, methyl(triisopropylsilyl)dimethylketene acetal, and ethyl(trimethylsilyl)dimethylketene acetal are preferred from the standpoints of easy availability, ease of synthesis, and stability. The above silyl ketene acetals may be used alone or in combination of two or more.

[0185] Specific examples of the vinylsilane compound represented by the general formula (8) include vinyltrimethylsilane, 1-trimethylsilylhexene, 1-trimethylsilyloctene, 1-trimethylsilyl-1-phenylethylene, 1-trimethylsilyl-2-phenylethylene, vinyl-tert-butyldimethylsilane, 1-tert-butyldimethylsilylhexene, 1-tert-butyldimethylsilyloctene, 1-tert-butyldimethylsilyl-2-phenylethylene, vinyltris(trimethylsilyl)silane, 1-tris(trimethylsilyl)silylhexene, 1-tris(trimethylsilyl)silyloctene, and 1-tris(trimethylsilyl)silyl-2-phenylethylene.

[0186] Specific examples of the allylsilane compound represented by the general formula (9) include 3-(trimethylsilyl)-1-propene, 3-(triethylsilyl)-1-propene, 3-(dimethylethylsilyl)-1-propene, 3-(triisopropylsilyl)-1-propene, 3-(dimethylisopropylsilyl)-1-propene, 3-(trinormalpropylsilyl)-1-propene, 3-(dimethylnormalpropylsilyl)-1-propene, 3-(trinormalbutylsilyl)-1-propene, 3-(dimethylnormalbutylsilyl)-1-propene, 3-(triphenylsilyl)-1-propene, 3-(dimethylphenylsilyl)-1-propene, 2-methyl-3-(trimethylsilyl)-1-propene, 3-(trimethylsilyl)-2-methyl-1-propene, and 3-(triphenylsilyl)-2-methyl-1-propene.

[0187] Preferred examples of the catalyst include those that act as basic catalysts, such as Bronsted bases and Lewis bases, and examples of the catalyst include inorganic bases, such as alkali metal hydroxides and alkaline earth metal hydroxides; and organic bases, such as trialkylamines and pyridines. Among them, the catalyst is preferably at least one selected from the group consisting of organic phosphorus compounds, N-heterocyclic carbene, fluorine ion-containing compounds, cyclic amine compounds, and ammonium salt compounds, in that the polymerization of the vinyl ether group-containing (meth)acrylic acid esters can be carried out more efficiently. When these specific catalysts are used, cationic polymerization of the vinyl ether group and decomposition of the vinyl ether are unlikely to occur in the vinyl ether group-containing (meth)acrylic acid esters, and only the (meth)acryloyl group can be polymerized more efficiently.

[0188] The organic phosphorus compound is, for example, 1-tert-butyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ 5 ,4λ 5 -Catenazi(phosphazene) (phosphazene base P4-t-BuP4), 1-tert-octyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ 5 ,4λ 5 -Catenazi(phosphazene) (phosphazene base P4-tOct), 1-tert-butyl-2,2,4,4,4-pentakis(dimethylamino)-2λ 5 ,-4λ 5 -Catenazi(phosphazene)(phosphazene base P2-t-Bu), 1-ethyl-2,2,4,4,4-pentakis(dimethylamino)-2λ 5 ,4λ 5- Phosphazene bases such as catenadi(phosphazene) (phosphazene base P2-t-Et), tert-butylimino-tris(dimethylamino)phosphorane (phosphazene base P1-t-Bu), tert-butylimino-tri(pyrrolidino)phosphorane (BTPP), 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorine; tris(2,4,6-trimethoxyphenyl) Phosphine, tributylphosphine, tris(dimethylaminophosphine), 2,8,9-triisobutyl-2,5,8,9-tetraaza-1-phosphabicyclo[3,3,3]undecane, 2,8,9-trimethyl-2,5,8,9-tetraaza-1-phosphabicyclo[3,3,3]undecane, 2,8,9-triisopropyl-2,5,8,9-tetraaza-1-phosphabicyclo[3,3,3]undecane, etc. Among them, the phosphazene base P4-t-BuP4 and 2,8,9-triisobutyl-2,5,8,9-tetraaza-1-phosphabicyclo[3,3,3]undecane are preferred because of their strong basicity and their ability to effectively activate silyl ketene acetal.

[0189] Examples of the N-heterocyclic carbene include 1,3-dimethylimidazol-2-ylidene, 1,3-diethylimidazol-2-ylidene, 1,3-di-tert-butylimidazol-2-ylidene, 1,3-di-cyclohexylimidazol-2-ylidene, 1,3-di-isopropylimidazol-2-ylidene, 1,3-di(1-adamantyl)imidazol-2-ylidene, 1,3-di-mesitylimidazol-2-ylidene, etc. Among these, 1,3-di-tert-butylimidazol-2-ylidene and 1,3-di-isopropylimidazol-2-ylidene are preferred because they can effectively activate silyl ketene acetals.

[0190] Examples of the fluorine ion-containing compound include tetra-n-butylammonium fluoride (TBAF), tris(dimethylamino)sulfonium bifluoride (TASHF2), hydrogen fluoride-pyridine, tetrabutylammonium bifluoride, potassium hydrogen fluoride, etc. Among these, tetra-n-butylammonium fluoride (TBAF), tetrabutylammonium bifluoride, and tris(dimethylamino)sulfonium bifluoride (TASHF2) are preferred because they are easily available and can effectively activate silyl ketene acetal.

[0191] Examples of the cyclic amine compound include 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0192] Examples of the ammonium salt compound include tetrabutylammonium bisacetate, tetrabutylammonium acetate, tetrabutylammonium benzoate, tetrabutylammonium bisbenzoate, tetrabutylammonium metachlorobenzoate, tetrabutylammonium cyanate, tetrabutylammonium methoxide, tetrabutylammonium thiolate, tetrabutylammonium bibromide, and ammonium salt compounds in which the ammonium cation is replaced with a tetramethylammonium, triethylammonium, benzyltributylammonium, N-methyl-N-butylpiperidinium, N-methyl-N-butylpyrrolidinium cation, or a pyridinium cation.

[0193] In addition to the above, strongly basic nitrogen-containing heterocyclic compounds such as 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene can also be used.

[0194] The above catalysts may be used alone or in combination of two or more.

[0195] In the polymerization, other components may be used in addition to the above-mentioned components, as long as they do not affect the effects of the present invention. Examples of the other components include known additives such as polymerization initiators, chain transfer agents, polymerization accelerators, and polymerization inhibitors that are commonly used in polymerization reactions. These can be appropriately selected as needed.

[0196] The above-mentioned production method may include other steps other than the above-mentioned polymerization reaction step. Examples of the other steps include an aging step, a neutralization step, a step of deactivating a polymerization initiator or a chain transfer agent, a dilution step, a drying step, a concentration step, a purification step, etc. These steps can be carried out by known methods.

[0197] The polymer (C) is preferably produced by the above-mentioned production method, that is, the polymer (C) is preferably a group transfer polymer of a monomer component containing a vinyl ether group-containing (meth)acrylic acid ester represented by the above general formula (1-2).

[0198] When the polymer (C) is produced by the above-mentioned production method, the conversion rate of the monomer components used in the polymerization is very high, and the amount of residual monomers can be made very small. On the other hand, when the above polymer (C) is produced by radical polymerization, even if a polymer having a molecular weight distribution controlled within the above-mentioned specified range can be obtained without gelation, the monomer remains and the amount thereof is difficult to control, so that there is a risk of reduced reproducibility of the physical properties of the obtained cured product. The content of the residual monomer in the polymer (C) is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 0 to 3% by mass, based on 100% by mass of the polymer. The residual monomer content is 1It can be measured by H-NMR, gas chromatography, liquid chromatography, or gel permeation chromatography.

[0199] (D) Photopolymerization initiator The curable resin composition of the present invention preferably further contains a photopolymerization initiator. The photopolymerization initiator used in the present invention is preferably a radically polymerizable photopolymerization initiator, which generates polymerization initiating radicals when irradiated with active energy rays such as electromagnetic waves or electron beams.

[0200] Specific examples of the photopolymerization initiator include aminoketone compounds such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one ("IRGACURE907", manufactured by BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 ("IRGACURE369", manufactured by BASF), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one ("IRGACURE379", manufactured by BASF); 2,2-dimethoxy-1,2-diphenylethan-1-one ("IRGACURE651", manufactured by BASF), phenylglyoxylic acid methyl ester ("DAROCURE benzyl ketal compounds such as 1-hydroxy-cyclohexyl-phenyl-ketone ("IRGACURE184", BASF), 2-hydroxy-2-methyl-1-phenyl-propan-1-one ("DAROCUR1173", BASF), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one ("IRGACURE2959", BASF), 2-hydroxy -Hydroketone compounds such as 1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one ("IRGACURE 127", manufactured by BASF), [1-hydroxy-cyclohexyl-phenyl-ketone + benzophenone] ("IRGACURE 500", manufactured by BASF), etc., as well as other alkylphenone compounds exemplified in paragraphs

[0084] to

[0086] of JP 2013-227485 A;1,2-Octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime)] ("OXE01", manufactured by BASF), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) ("OXE02", manufactured by BASF), 1,2-Octanedione, 1-[4-(phenylthio)-, 2-, (O-benzoyloxime)], ethanone ("OXE03", manufactured by BASF), 1-[9-ethyl Examples of suitable oxime ester compounds include oxime ester compounds such as [-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-,1-(O-acetyloxime) ("OXE04", manufactured by BASF); benzophenone compounds; benzoin compounds; thioxanthone compounds; halomethylated triazine compounds; halomethylated oxadiazole compounds; biimidazole compounds; titanocene compounds; benzoic acid ester compounds; acridine compounds; and phosphine oxide compounds. Of these, aminoketone compounds and oxime ester compounds are preferred. The photopolymerization initiators may be used alone or in combination of two or more.

[0201] The content of the photopolymerization initiator is not particularly limited as long as it is within a range in which the effects of the present invention are exhibited, and may be appropriately set. For example, the content is preferably 0.3 to 20 mass%, more preferably 0.5 to 10 mass%, and even more preferably 1 to 8 mass%, relative to 100 mass% of the total solid content of the curable resin composition of the present invention.

[0202] (E) Polymerizable compound The curable resin composition of the present invention preferably further contains a polymerizable compound. By further containing a polymerizable compound, a cured product having excellent physical properties such as curability of the resin composition, mechanical strength, heat resistance, etc. in addition to solvent resistance can be obtained.

[0203] The polymerizable compound is a low molecular weight compound having a polymerizable unsaturated bond (also referred to as a polymerizable unsaturated group) that can be polymerized by irradiation with active energy rays such as free radicals, electromagnetic waves (e.g., infrared rays, ultraviolet rays, X-rays, etc.), and electron beams. Examples of the polymerizable compound include monofunctional compounds having one polymerizable unsaturated group in the molecule and polyfunctional compounds having two or more polymerizable unsaturated groups.

[0204] Examples of the monofunctional compound include N-substituted maleimide monomers, (meth)acrylic acid esters, (meth)acrylamides, unsaturated monocarboxylic acids, unsaturated polycarboxylic acids, unsaturated monocarboxylic acids in which the unsaturated group and the carboxyl group are chain-extended, unsaturated acid anhydrides, aromatic vinyls, conjugated dienes, vinyl esters, vinyl ethers, N-vinyl compounds, unsaturated isocyanates, etc. Examples of the monofunctional compound include the same compounds as those listed as monomer components of the acid group-containing alkali-soluble resin, etc. Also, monomers having an active methylene group or an active methine group can be used.

[0205] Examples of the polyfunctional compound include the following compounds. bifunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, bisphenol A alkylene oxide di(meth)acrylate, and bisphenol F alkylene oxide di(meth)acrylate;

[0206] Trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, ethylene oxide-added ditrimethylolpropane tetra(meth)acrylate, ethylene oxide-added pentaerythritol tetra(meth)acrylate, ethylene oxide-added dipentaerythritol hexa(meth)acrylate, propylene oxide-added trimethylolpropane tri(meth)acrylate, propylene oxide-added ditrimethylolpropane tetra(meth)acrylate, propylene oxide-added pentaerythritol tetra(meth)acrylate, propylene oxide-added dipentaerythritol hexa(meth)acrylate, ε-caprolactone-added trimethylolpropane tri(meth)acrylate, ε-caprolactone-added ditrimethylolpropane tetra(meth)acrylate, ε-caprolactone-added pentaerythritol tetra(meth)acrylate, ε-caprolactone-added dipentaerythritol hexa(meth)acrylate, dipentaerythritol pentaacrylate succinic acid modified product, pentaerythritol triacrylate succinic acid modified product, dipentaerythritol pentaacrylate phthalic acid modified product, pentaerythritol triacrylate phthalic acid modified product,

[0207] [ka]

[0208] a polyfunctional (meth)acrylate compound having three or more functional groups, such as a modified product of dipentaerythritol hexaacrylate represented by the formula:

[0209] Polyfunctional vinyl ethers such as ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerin trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide-added trimethylolpropane trivinyl ether, ethylene oxide-added ditrimethylolpropane tetravinyl ether, ethylene oxide-added pentaerythritol tetravinyl ether, and ethylene oxide-added dipentaerythritol hexavinyl ether;

[0210] vinyl ether group-containing (meth)acrylic acid esters such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate;

[0211] polyfunctional allyl ethers such as ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butylene glycol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, glycerin triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, dipentaerythritol hexaallyl ether, ethylene oxide-added trimethylolpropane triallyl ether, ethylene oxide-added ditrimethylolpropane tetraallyl ether, ethylene oxide-added pentaerythritol tetraallyl ether, and ethylene oxide-added dipentaerythritol hexaallyl ether;

[0212] Allyl group-containing (meth)acrylic acid esters such as allyl (meth)acrylate; polyfunctional (meth)acryloyl group-containing isocyanurates such as tri(acryloyloxyethyl)isocyanurate, tri(methacryloyloxyethyl)isocyanurate, alkylene oxide-added tri(acryloyloxyethyl)isocyanurate, and alkylene oxide-added tri(methacryloyloxyethyl)isocyanurate; polyfunctional allyl group-containing isocyanurates such as triallyl isocyanurate; polyfunctional urethane (meth)acrylates obtained by reacting polyfunctional isocyanates such as tolylene diisocyanate, isophorone diisocyanate, and xylylene diisocyanate with hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; polyfunctional aromatic vinyls such as divinylbenzene; etc. These polymerizable compounds may be used alone or in combination of two or more.

[0213] Among the above polymerizable compounds, it is preferable to use a polyfunctional polymerizable compound from the viewpoint of further increasing the curability of the curable resin composition. The number of functionalities of the above polyfunctional polymerizable compound is preferably 3 or more, more preferably 4 or more. In addition, the number of functionalities is preferably 10 or less, more preferably 8 or less. The molecular weight of the polymerizable compound is not particularly limited, but is preferably, for example, 2000 or less from the viewpoint of handling.

[0214] As the polyfunctional polymerizable compound, from the viewpoints of reactivity, economic efficiency, availability, etc., preferably, a compound having a (meth)acryloyl group, such as a polyfunctional (meth)acrylate compound, a polyfunctional urethane (meth)acrylate compound, or a (meth)acryloyl group-containing isocyanurate compound, is more preferably, a polyfunctional (meth)acrylate compound. By including a compound having a (meth)acryloyl group, the curable resin composition has better photosensitivity and curability, and a cured product having higher hardness and transparency can be obtained. As the polyfunctional polymerizable compound, it is more preferable to use a polyfunctional (meth)acrylate compound having three or more functional groups.

[0215] In the curable resin composition of the present invention, the content of the polymerizable compound is not particularly limited and may be appropriately set as long as the effects of the present invention are exhibited. However, in order to give the curable resin composition an appropriate viscosity, the content is preferably 5 to 60 mass%, and more preferably 10 to 50 mass%, relative to 100 mass% of the total solid content of the curable resin composition.

[0216] (F) Photoacid generator The curable resin composition of the present invention preferably further contains a photoacid generator. By containing the photoacid generator, cationic polymerization proceeds, and a cured product having superior solvent resistance can be obtained. The photoacid generator used in the present invention is a compound that generates radicals and acid simultaneously when irradiated with light.The photoacid generator is, for example, a compound that generates acid when exposed to radiation such as visible light, ultraviolet light, far ultraviolet light, electron beam, X-ray, etc., and specifically includes known compounds such as onium salt compounds, sulfone compounds, sulfonic acid ester compounds, quinone diazide compounds, sulfonimide compounds, diazomethane compounds, etc. Among them, the photoacid generator is preferably at least one selected from the group consisting of an onium salt compound, a sulfonimide compound, and a diazomethane compound, more preferably an onium salt compound, and even more preferably a triarylsulfonium salt.

[0217] Examples of the onium salt compound include diaryliodonium salts, triarylsulfonium salts, and triarylphosphonium salts.

[0218] Specific examples of the diaryliodonium salt include diphenyliodonium salts such as Bluesil PI2074 (manufactured by Elkem), diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluorophosphonate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluoroarsenate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium trifluoroacetate, and diphenyliodonium-p-toluenesulfonate; 4-methoxyphenylphenyliodonium tetrafluoroborate, 4-methoxyphenylphenyliodonium hexafluorophosphonate, 4-methoxyphenylphenyliodonium hexafluoroantimonate, 4-methoxyphenylphenyliodonium hexafluoroarsenate, 4-methoxyphenylphenyliodonium trifluoromethanesulfonate, ... Examples of the iodonium salt include 4-methoxyphenylphenyliodonium salts such as phenylphenyliodonium trifluoroacetate and 4-methoxyphenylphenyliodonium-p-toluenesulfonate; and bis(4-tert-butylphenyl)iodonium salts such as bis(4-tert-butylphenyl)iodonium tetrafluoroborate, bis(4-tert-butylphenyl)iodonium hexafluorophosphonate, bis(4-tert-butylphenyl)iodonium hexafluoroantimonate, bis(4-tert-butylphenyl)iodonium hexafluoroarsenate, bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, bis(4-tert-butylphenyl)iodonium trifluoroacetate, and bis(4-tert-butylphenyl)iodonium-p-toluenesulfonate.

[0219] Examples of the triarylsulfonium salts include triphenylsulfonium salts such as triphenylsulfonium tetrafluoroborate, triphenylsulfonium hexafluorophosphonate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium hexafluoroarsenate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium trifluoroacetate, and triphenylsulfonium-p-toluenesulfonate; 4-methoxyphenyldiphenylsulfonium tetrafluoroborate, 4-methoxyphenyldiphenylsulfonium hexafluorophosphonate, 4-methoxyphenyldiphenylsulfonium hexafluoroantimonate, 4-methoxyphenyldiphenylsulfonium hexafluoroarsenate, and 4-methoxyphenyldiphenylsulfonium trifluoromethanesulfonate. sulfonate, 4-methoxyphenyldiphenylsulfonium salts such as 4-methoxyphenyldiphenylsulfonium trifluoroacetate, 4-methoxyphenyldiphenylsulfonium-p-toluenesulfonate; and 4-phenylthiophenyldiphenylsulfonium salts such as 4-phenylthiophenyldiphenylsulfonium tetrafluoroborate, 4-phenylthiophenyldiphenylsulfonium hexafluorophosphonate, 4-phenylthiophenyldiphenylsulfonium hexafluoroantimonate, 4-phenylthiophenyldiphenylsulfonium hexafluoroarsenate, 4-phenylthiophenyldiphenylsulfonium trifluoromethanesulfonate, 4-phenylthiophenyldiphenylsulfonium trifluoroacetate, 4-phenylthiophenyldiphenylsulfonium-p-toluenesulfonate.

[0220] Examples of the triarylphosphonium salt include triphenylphosphonium salts such as triphenylphosphonium tetrafluoroborate, triphenylphosphonium hexafluorophosphonate, triphenylphosphonium hexafluoroantimonate, triphenylphosphonium hexafluoroarsenate, triphenylphosphonium trifluoromethanesulfonate, triphenylphosphonium trifluoroacetate, and triphenylphosphonium-p-toluenesulfonate; 4-methoxyphenyldiphenylphosphonium tetrafluoroborate, 4-methoxyphenyldiphenylphosphonium hexafluorophosphonate, 4-methoxyphenyldiphenylphosphonium hexafluoroantimonate, 4-methoxyphenyldiphenylphosphonium hexafluoroarsenate, and 4-methoxyphenyldiphenylphosphonium trifluoromethanesulfonate. tris(4-methoxyphenyl)phosphonium salts such as tris(4-methoxyphenyl)phosphonium tetrafluoroborate, tris(4-methoxyphenyl)phosphonium hexafluorophosphonate, tris(4-methoxyphenyl)phosphonium hexafluoroantimonate, tris(4-methoxyphenyl)phosphonium hexafluoroarsenate, tris(4-methoxyphenyl)phosphonium trifluoromethanesulfonate, tris(4-methoxyphenyl)phosphonium trifluoroacetate, and tris(4-methoxyphenyl)phosphonium-p-toluenesulfonate.

[0221] Examples of the sulfonimide compound include N-(trifluoromethylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(trifluoromethylsulfonyloxy)bicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(trifluoromethylsulfonyloxy)-7-oxabicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, and N-(trifluoromethylsulfonyloxy) Sulfonimide compounds having an N-(trifluoromethylsulfonyloxy) group, such as bicyclo-[2,2,1]-heptane-5,6-oxy-2,3-dicarboximide and N-(trifluoromethylsulfonyloxy)naphthylimide; N-(camphanylsulfonyloxy)succinimide, N-(camphanylsulfonyloxy)phthalimide, N-(camphanylsulfonyloxy)diphenylmaleimide, N-(camphanylsulfonyloxy)bicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(camphanylsulfonyloxy)bicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(camphanylsulfonyloxy) Sulfonimide compounds having an N-(camphanylsulfonyloxy) group, such as N-(camphanylsulfonyloxy)-7-oxabicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(camphanylsulfonyloxy)bicyclo-[2,2,1]-heptane-5,6-oxy-2,3-dicarboximide, and N-(camphanylsulfonyloxy)naphthylimide; N-(4-methylphenylsulfonyloxy)succinimide, N-(4-methylphenylsulfonyloxy)phthalimide, and N-(4-methylphenylsulfonyloxy)diphenylmaphthalimide; sulfonimide compounds having an N-(4-methylphenylsulfonyloxy) group, such as N-(4-methylphenylsulfonyloxy)bicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(4-methylphenylsulfonyloxy)-7-oxabicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(4-methylphenylsulfonyloxy)bicyclo-[2,2,1]-heptane-5,6-oxy-2,3-dicarboximide, and N-(4-methylphenylsulfonyloxy)naphthylimide;Examples of the sulfonimide compounds having an N-(2-trifluoromethylphenylsulfonyloxy) group include N-(2-trifluoromethylphenylsulfonyloxy) succinimide, N-(2-trifluoromethylphenylsulfonyloxy) phthalimide, N-(2-trifluoromethylphenylsulfonyloxy) diphenylmaleimide, N-(2-trifluoromethylphenylsulfonyloxy) bicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(2-trifluoromethylphenylsulfonyloxy)-7-oxabicyclo-[2,2,1]-hept-5-ene-2,3-dicarboximide, N-(2-trifluoromethylphenylsulfonyloxy) bicyclo-[2,2,1]-heptane-5,6-oxy-2,3-dicarboximide, and N-(2-trifluoromethylphenylsulfonyloxy) naphthylimide.

[0222] Examples of the diazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, methylsulfonyl-p-toluenesulfonyldiazomethane, 1-cyclohexylsulfonyl-1-1,1-dimethylethylsulfonyl)diazomethane, bis(1,1-dimethylethylsulfonyl)diazomethane, and the like.

[0223] The content of the photoacid generator is not particularly limited as long as it is within a range in which the effects of the present invention are exhibited, and may be set as appropriate. For example, the content is preferably 0.3 to 20 mass%, more preferably 0.5 to 10 mass%, and even more preferably 1 to 8 mass%, relative to 100 mass% of the total solid content of the curable resin composition of the present invention.

[0224] (G) Epoxy compounds The curable resin composition of the present invention preferably further contains an epoxy compound. When the composition contains an epoxy compound, cationic polymerization proceeds, the crosslinking reaction proceeds more easily, and a cured product having excellent solvent resistance can be obtained. The epoxy compound includes a compound having an epoxy group and a polymerizable double bond, such as the above-mentioned epoxy group-containing monomer. When the epoxy compound is contained, the content thereof is preferably 1 to 50 mass%, more preferably 2 to 40 mass%, and further preferably 5 to 30 mass%, relative to 100 mass% of the total solid content of the curable resin composition.

[0225] <Other ingredients> The curable resin composition of the present invention may contain other components as necessary in addition to the above-mentioned components. Examples of the other components include solvents, coloring materials (pigments, dyes), dispersants, heat resistance improvers, leveling agents, development aids, inorganic fine particles such as silica fine particles, coupling agents such as silanes, aluminum, and titanium, thermosetting resins such as fillers, epoxy resins, phenolic resins, and polyvinylphenols, curing aids such as polyfunctional thiol compounds, plasticizers, polymerization inhibitors, ultraviolet absorbers, antioxidants, matting agents, defoamers, antistatic agents, slip agents, surface modifiers, thixotropic agents, thixotropic aids, quinone diazide compounds, polyhydric phenol compounds, cationic polymerizable compounds, and thermal acid generators. These may be used alone or in combination of two or more. These other components may be appropriately selected from known ones and used, and the amount used may be appropriately set. For example, when the curable resin composition is used for a color filter, the curable resin composition preferably contains a color material.

[0226] <Preparation of Curable Resin Composition> The method for preparing the curable resin composition of the present invention is not particularly limited and may be a known method, for example, a method in which the above-mentioned components are mixed and dispersed using various mixers and dispersers. The mixing and dispersion step is not particularly limited and may be performed by a known method. In addition, other steps that are usually performed may be further included. When the curable resin composition contains a colorant, it is preferable to prepare the composition through a known colorant dispersion treatment step.

[0227] <Method of manufacturing the cured product> The method for obtaining a cured product using the cured resin composition of the present invention is not particularly limited, and any known method may be used. For example, the cured product may be obtained by applying the above-mentioned cured resin composition to a substrate, and curing the applied composition by drying, heating, irradiating with energy rays such as ultraviolet rays, or a combination of these.

[0228] When the cured resin composition of the present invention is used, a cured product having excellent solvent resistance can be obtained even under curing conditions at relatively low temperatures. For example, the following method is preferable. That is, the method for producing a cured product includes the steps of applying the above-mentioned curable resin composition onto a substrate to form a coating film, irradiating the formed coating film with light, and heating the light-irradiated coating film at 200°C or less.

[0229] The substrate (base material) is not particularly limited and may be appropriately selected depending on the purpose and application. Examples of the substrate include substrates made of various materials such as glass plates and plastic plates.

[0230] The method for forming a coating film by applying the curable resin composition is not particularly limited, and can be a known method such as spin coating, slit coating, roll coating, or cast coating. In the above-mentioned manufacturing method, it is preferable to coat the curable resin composition on a substrate, and then dry the coating to form a coating film. The drying can be performed by a known method, and specifically, it can be performed by the same method as the drying method described in the "Arrangement step" in "<Manufacturing method for color filter>" described later.

[0231] The above-mentioned manufacturing method includes a step of forming a coating film and then irradiating the coating film with light. The method for irradiating the formed coating film with light is not particularly limited and may be a known method. Specifically, it may be performed by a method similar to the method described in the "Light irradiation step" in "<Color filter manufacturing method>" described later.

[0232] When the coating film is irradiated with light, the light irradiation may be performed through a photomask. As the photomask, a mask in which a light-shielding portion is formed according to a desired pattern may be used. When the light irradiation is performed through a photomask, it is preferable to perform a development process thereafter. By performing the development process, a desired pattern can be formed in the coating film. The development method is not particularly limited and can be performed by a known method, and specifically, it can be performed by the same method as the method described in the "development process" of "<Color filter manufacturing method>" described later.

[0233] The above-mentioned production method also includes a step of heating the light-irradiated coating film at 200° C. or less. Since the production method of the present invention uses the above-mentioned curable resin composition, the heating step (post-curing step) after light irradiation can be carried out under low-temperature conditions of 200° C. or less. The heating temperature is preferably 190° C. or lower, and more preferably 180° C. or lower. The lower limit of the heating temperature is preferably 70° C. or higher, and more preferably 90° C. or higher, in terms of maintaining the curability. The heating method other than the temperature is not particularly limited and can be performed by a known method. For example, it can be performed by a method similar to the method described in the "Heating step" in "<Color filter manufacturing method>" described later.

[0234] <Application> The curable resin composition of the present invention can provide a cured product having excellent solvent resistance even under low temperature curing conditions. Therefore, it can be suitably used in applications requiring excellent solvent resistance or applications requiring a cured product having excellent solvent resistance to be obtained under low temperature conditions. The curable resin composition of the present invention is suitably used for optical materials, and is preferably used for resists. The curable resin composition of the present invention can be suitably used for both negative and positive types.

[0235] Specifically, the curable resin composition of the present invention can be suitably used for, for example, color filters, black matrices, photospacers, black column spacers, inks, printing plates, printed wiring boards, semiconductor elements, photoresists, insulating films, films, organic protective films, and other optical members and components of electric and electronic devices, etc., used in liquid crystal, organic EL, quantum dot, and micro LED liquid crystal displays, solid-state imaging elements, touch panel display devices, etc. Among these, it is preferably used for color filters.

[0236] 2. Color Filters A color filter having a cured product of the above-mentioned curable resin composition on a substrate is also one of the preferred embodiments of the present invention. In the color filter, the cured product formed from the curable resin composition is particularly suitable as a segment that requires coloring, such as a black matrix or each pixel of red, green, blue, yellow, etc., but is also suitable as a segment that does not necessarily require coloring, such as a photospacer, a protective layer, and an alignment control rib.

[0237] Examples of the substrate used in the color filter include glass substrates such as white plate glass, blue plate glass, alkali-reinforced glass, and silica-coated blue plate glass; sheets, films, or substrates made of thermoplastic resins such as polyester, polycarbonate, polyolefin, polysulfone, ring-opening polymers of cyclic olefins, and hydrogenated products thereof; sheets, films, or substrates made of thermosetting resins such as epoxy resins and unsaturated polyester resins; metal substrates such as aluminum plates, copper plates, nickel plates, and stainless steel plates; ceramic substrates; semiconductor substrates having photoelectric conversion elements; glass substrates having a coloring material layer on the surface (e.g., color filters for LCDs); and other members made of various materials. Among these, from the viewpoint of heat resistance, glass substrates and sheets, films, or substrates made of heat-resistant resins are preferred. In addition, it is preferable that the substrate is a transparent substrate. If necessary, the substrate may be subjected to a corona discharge treatment, an ozone treatment, or a chemical treatment using a silane coupling agent or the like.

[0238] <Color filter manufacturing method> To obtain the color filter, for example, it is preferable to adopt a manufacturing method that includes a step of arranging the curable resin composition on a substrate for each pixel color (i.e., for each pixel color), a step of irradiating the curable resin composition arranged on the substrate with light (also referred to as a light irradiation step), a step of developing with a developer (also referred to as a development step), and a step of heating (also referred to as a heating step), and repeat the same method for each color. Note that the order of forming the pixels of each color is not particularly limited.

[0239] (1) Arrangement step (preferably application step) The above-mentioned disposing step is preferably performed by coating. Examples of a method for coating the above-mentioned curable resin composition on a substrate include spin coating, slit coating, roll coating, and casting coating, and any of these methods can be preferably used. In the above-mentioned disposing step, it is also preferable to dry the coating film after applying the above-mentioned curable resin composition on the substrate. The coating film can be dried, for example, using a hot plate, an IR oven, a convection oven, etc. The drying conditions are appropriately selected depending on the boiling point of the solvent component contained, the type of curable component, the film thickness, the performance of the dryer, etc., but it is usually preferable to perform drying at a temperature of 50 to 160°C for 10 to 300 seconds.

[0240] (2) Light irradiation process In the above-mentioned light irradiation step, examples of the light source of the actinic ray used include lamp light sources such as a xenon lamp, a halogen lamp, a tungsten lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp, a carbon arc, and a fluorescent lamp, and laser light sources such as an argon ion laser, a YAG laser, an excimer laser, a nitrogen laser, a helium cadmium laser, and a semiconductor laser. Examples of the exposure method include a proximity method, a mirror projection method, and a stepper method, with the proximity method being preferably used. In addition, in the step of irradiating the active energy ray, depending on the application, the active energy ray may be irradiated through a predetermined mask pattern. In this case, the exposed portion is cured, and the cured portion is made insoluble or hardly soluble in a developer.

[0241] (3)Developing process The developing step is a step of forming a pattern by developing with a developer after the above-mentioned light irradiation step, and removing the unexposed portion. This allows a patterned cured film to be obtained. The developing step can be usually performed at a developing temperature of 10 to 50°C by a method such as immersion development, spray development, brush development, or ultrasonic development.

[0242] The developer used in the developing step is not particularly limited as long as it dissolves the curable resin composition, but usually, an organic solvent or an alkaline aqueous solution is used, and a mixture of these may be used. When an alkaline aqueous solution is used as the developer, it is preferable to wash with water after development. Examples of the organic solvent and the alkaline aqueous solution include those described in JP 2015-157909 A.

[0243] (4)Heating process The heating step is a step (also referred to as a "post-curing step") in which the exposed area (cured area) is further cured by baking after the above-mentioned development step. For example, a light source such as a high-pressure mercury lamp is used, and the cured area is cured by baking at 0.5 to 5 J / cm. 2 and a step of post-exposing the film to a light amount of 1000 to 200° C. for 10 seconds to 120 minutes. By carrying out such a post-curing step, it is possible to further increase the hardness and adhesion of the patterned cured film. The heating step is generally carried out at a temperature of about 200 to 260° C., but by using the curable resin composition, sufficient curing can be achieved under relatively low temperature conditions of 200° C. or lower. Therefore, it is possible to obtain a substrate or a cured product having excellent solvent resistance without impairing the properties retained by the substrate or the cured product.

[0244] In the heating step, the heating temperature is preferably 200° C. or lower, more preferably 190° C. or lower, and even more preferably 180° C. or lower. The heating temperature is preferably 70° C. or higher, more preferably 90° C. or higher, and even more preferably 95° C. or higher.

[0245] The heating time in the heating step is not particularly limited, but is preferably, for example, 5 to 60 minutes. The heating method is also not particularly limited, but can be performed using a heating device such as a hot plate, a convection oven, or a high-frequency heater.

[0246] The thickness of the cured film obtained by the heating step (i.e., the cured coating film obtained by thermally curing the curable resin composition) is preferably 0.1 to 20 μm, more preferably 0.5 to 15 μm, and further preferably 1 to 10 μm.

[0247] 3.Display device A display device including the above-mentioned color filter is also one of the preferred embodiments of the present invention. A display device member and a display device having the cured product of the curable resin composition are also included in the preferred embodiments of the present invention. The cured product (cured film) formed by the curable resin composition has excellent solvent resistance, is stable, has excellent adhesion to a substrate, and has high hardness, and exhibits high smoothness and high transmittance, so that it is particularly suitable as a transparent member and is also useful as a protective film or insulating film in various display devices.

[0248] As the display device, for example, a liquid crystal display device, a solid-state imaging device, a touch panel display device, etc. are suitable. When the cured product (cured film) is used as a member for a display device, the member may be a film-like single-layer or multi-layer member constituted by the cured film, or a member in which another layer is further combined with the single-layer or multi-layer member, or a member containing the cured film in its configuration.

[0249] As described above, the curable resin composition of the present invention can provide a cured product having excellent solvent resistance even under low-temperature curing conditions. In addition, the cured product of the curable resin composition of the present invention is also excellent in adhesion to the substrate, transparency, heat resistance, etc. Such a curable resin composition of the present invention can be suitably used for various applications such as electric and electronic devices as various optical members and components used in liquid crystal, organic EL, quantum dot, and micro LED liquid crystal display devices, solid-state imaging devices, touch panel display devices, etc. EXAMPLES

[0250] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0251] In the examples, various physical properties were measured by the following methods. (1) Weight average molecular weight (Mw) and dispersity (Mw / Mn) The weight average molecular weight (Mw) and the polydispersity (Mw / Mn) were measured by GPC (gel permeation chromatography) using polystyrene as a standard substance and tetrahydrofuran as an eluent, with an HLC-8220GPC (manufactured by Tosoh Corporation) and a column: TSKgel SuperHZM-M (manufactured by Tosoh Corporation).

[0252] (2) Solids Approximately 1 g of the polymer solution was weighed out in an aluminum cup, and about 3 g of acetone was added to dissolve it, and then it was naturally dried at room temperature. Then, it was dried at 170°C under vacuum for 1.5 hours using a hot air dryer (product name: PHH-101, manufactured by Espec Corporation), and then it was cooled in a desiccator and the mass was measured. The solid content (mass%) of the polymer solution was calculated from the mass loss.

[0253] (3) Acid value 3 g of the polymer solution was precisely weighed out and dissolved in a mixed solvent of 90 g of acetone and 10 g of water, and titrated using a 0.1 N KOH aqueous solution as a titrant. The titration was performed using an automatic titrator (product name: COM-555, manufactured by Hiranuma Sangyo Co., Ltd.), and the acid value per 1 g of solid content (mgKOH / g) was calculated from the acid value of the solution and the solid content of the solution.

[0254] (4)NMR A few mg to several tens of mg of the polymer was dissolved in deuterated chloroform and measured using an Agilent Technologies nuclear magnetic resonance spectrometer (600 MHz).

[0255] (5) Solvent resistance The curable resin composition was spin-coated on a 5 cm square glass substrate, dried at 100°C for 3 minutes, exposed to 60 mJ using a high-pressure mercury lamp, and heat-treated (post-cured) at 110°C for 40 minutes to obtain a cured film with a thickness of 5 μm. The cured film was then immersed in 20 g of 1-methyl-2-pyrrolidone (NMP) at 40°C for 10 minutes, removed, and the absorbance of the immersion liquid (NMP) after removing the cured film was measured using a spectrophotometer UV3100 (manufactured by Shimadzu Corporation). The higher the absorbance value, the more the colorant was dissolved in the immersion liquid, and the curable resin composition was evaluated to have low solvent resistance.

[0256] (Production Example 1) Preparation of copolymer solution A-1 (GMA adduct solution of MMA-MAA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 116.2 parts of propylene glycol monomethyl ether acetate and 55.1 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as the dropping vessel (A), 60.0 parts of methyl methacrylate, 40.0 parts of methacrylic acid, 3.4 parts of propylene glycol monomethyl ether acetate, 1.5 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, "Perbutyl (registered trademark) O") were prepared in a beaker by stirring and mixing, and in the dropping vessel (B), 2.0 parts of n-dodecyl mercaptan and 12.3 parts of propylene glycol monomethyl ether acetate were prepared by stirring and mixing. After the temperature of the reaction vessel reached 90°C, the dropping tank was started to drop the solution over 3 hours while maintaining the temperature, and polymerization was carried out. After the dropping was completed, the temperature was kept at 90°C for 30 minutes, and then the temperature was raised to 115°C and aged for 90 minutes. After that, it was cooled to room temperature, and 24.8 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were charged, and the reaction was carried out at 110°C for 7 hours to obtain copolymer solution A-1. Various physical properties are shown in Table 1.

[0257] (Production Example 2) Preparation of copolymer solution A-2 (GMA adduct solution of BzMI-CHMA-MAA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 81.9 parts of propylene glycol monomethyl ether acetate and 37.7 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as the dropping vessel (A), 10.0 parts of N-benzylmaleimide, 70.0 parts of cyclohexyl methacrylate, 20.0 parts of methacrylic acid, 34.2 parts of propylene glycol monomethyl ether acetate, 14.7 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were stirred and mixed in a beaker, and 1.0 parts of n-dodecyl mercaptan and 6.1 parts of propylene glycol monomethyl ether acetate were stirred and mixed in the dropping vessel (B). After the temperature of the reaction vessel reached 90°C, the dropping from the dropping vessel was started over 3 hours while maintaining the same temperature, and polymerization was carried out. After the dropping was completed, the temperature was kept at 90°C for 30 minutes, and then the temperature was raised to 115°C and aged for 90 minutes. After that, it was cooled to room temperature, and 16.5 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were charged, and the reaction was carried out at 110°C for 7 hours to obtain copolymer solution A-2. Various physical properties are shown in Table 1.

[0258] (Production Example 3) Preparation of copolymer solution A-3 (GMA adduct solution of MD-CHMA-MAA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 116.7 parts of propylene glycol monomethyl ether acetate and 52.7 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as the dropping vessel (A), a beaker was prepared by stirring and mixing 10.0 parts of dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, 55.0 parts of cyclohexyl methacrylate, 35.0 parts of methacrylic acid, 34.2 parts of propylene glycol monomethyl ether acetate, 14.7 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate, and a dropping vessel (B) was prepared by stirring and mixing 1.0 parts of n-dodecyl mercaptan and 6.1 parts of propylene glycol monomethyl ether acetate. After the temperature of the reaction vessel reached 90°C, the dropping tank was started over a period of 3 hours while maintaining the same temperature, and polymerization was carried out. After the dropping was completed, the temperature was kept at 90°C for 30 minutes, and then the temperature was raised to 115°C and aged for 90 minutes. After that, it was cooled to room temperature, and 49.5 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were charged, and the reaction was carried out at 110°C for 7 hours to obtain copolymer solution A-3. Various physical properties are shown in Table 1.

[0259] (Production Example 4) Preparation of copolymer solution A-4 (GMA adduct solution of AMA-CHMA-MAA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 57.9 parts of propylene glycol monomethyl ether acetate and 35.3 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as the dropping vessel (A), a beaker was prepared by stirring and mixing 10.0 parts of α- (allyloxymethyl) methyl acrylate, 50.0 parts of cyclohexyl methacrylate, 40.0 parts of methacrylic acid, 34.2 parts of propylene glycol monomethyl ether acetate, 14.7 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate, and a dropping vessel (B) was prepared by stirring and mixing 4.0 parts of n-dodecyl mercaptan and 24.6 parts of propylene glycol monomethyl ether acetate. After the temperature of the reaction vessel reached 90°C, the dropping from the dropping vessel was started over a period of 3 hours while maintaining the same temperature, and polymerization was carried out. After the dropping was completed, the temperature was kept at 90°C for 30 minutes, and then the temperature was raised to 115°C and aged for 90 minutes. After that, it was cooled to room temperature, and 8.3 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were charged, and the reaction was carried out at 110°C for 7 hours, to obtain copolymer solution A-4. Various physical properties are shown in Table 1.

[0260] (Production Example 5) Preparation of copolymer solution A-5 (SAH adduct solution of BzMI-CHMA-GMA-HEMA copolymer) A reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube, and a dropping vessel inlet was charged with 201.0 parts of propylene glycol monomethyl ether acetate, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as a dropping vessel (A), a beaker was prepared in which 10.0 parts of N-benzylmaleimide, 43.6 parts of cyclohexyl methacrylate, 30.0 parts of 2-hydroxyethyl methacrylate, 16.4 parts of glycidyl methacrylate, 30.0 parts of propylene glycol monomethyl ether acetate, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were stirred and mixed, and a dropping vessel (B) was prepared in which 2.0 parts of n-dodecyl mercaptan and 31.3 parts of propylene glycol monomethyl ether acetate were stirred and mixed. After the temperature of the reaction vessel reached 90 ° C., while maintaining the same temperature, dropping was started from the dropping vessel over 3 hours, and polymerization was carried out. After the dropwise addition, the mixture was kept at 90°C for 30 minutes, then heated to 115°C and aged for 90 minutes. After cooling to room temperature, 11.5 parts of succinic anhydride and 0.3 parts of dimethylbenzylamine as a catalyst were added and reacted at 60°C for 3 hours to obtain copolymer solution A-5. Various physical properties are shown in Table 1.

[0261] (Production Example 6) Preparation of copolymer solution A-6 (GMA adduct solution of BzMI-CHMA-2EHA-AA copolymer) A reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet was charged with 185.9 parts of propylene glycol monomethyl ether acetate, and after nitrogen replacement, it was heated to 90 ° C. On the other hand, as a dropping vessel (A), 5.0 parts of N-benzylmaleimide, 25.5 parts of cyclohexyl methacrylate, 42.5 parts of 2-ethylhexyl acrylate, 27.0 parts of acrylic acid, 24.4 parts of propylene glycol monomethyl ether acetate, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were prepared in a beaker by stirring, and 1.8 parts of n-dodecyl mercaptan were prepared in a dropping vessel (B). After the temperature of the reaction vessel reached 90 ° C, the dropping vessel was started to drop from the dropping vessel over 3 hours while maintaining the same temperature, and polymerization was performed. After the dropwise addition, the mixture was kept at 90°C for 30 minutes, then heated to 115°C and aged for 90 minutes. After cooling to room temperature, 39.4 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were added and reacted at 110°C for 7 hours to obtain copolymer solution A-6. Various physical properties are shown in Table 1.

[0262] (Production Example 7) Preparation of copolymer solution A-7 (GMA adduct solution of BzMI-VT-AA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 49.3 parts of propylene glycol monomethyl ether acetate and 24.1 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as a dropping vessel (A), a beaker was prepared by stirring and mixing 30.0 parts of N-benzylmaleimide, 30.0 parts of vinyl toluene, 40.0 parts of acrylic acid, 102.5 parts of propylene glycol monomethyl ether acetate, 43.9 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate, and a dropping vessel (B) was prepared by stirring and mixing 3.0 parts of n-dodecyl mercaptan and 7.0 parts of propylene glycol monomethyl ether acetate. After the temperature of the reaction vessel reached 90 ° C., while maintaining the same temperature, dropping was started from the dropping vessel over 3 hours, and polymerization was carried out. After the dropwise addition, the mixture was kept at 90°C for 30 minutes, then heated to 115°C and aged for 90 minutes. After cooling to room temperature, 49.3 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were added and reacted at 110°C for 7 hours to obtain copolymer solution A-7. Various physical properties are shown in Table 1.

[0263] (Production Example 8) Preparation of copolymer solution A-8 (GMA adduct solution of BzMI-TBMA-HEMA-AA copolymer) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 115.3 parts of propylene glycol monomethyl ether acetate and 49.4 parts of propylene glycol monomethyl ether were charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as a dropping vessel (A), 10.0 parts of N-benzylmaleimide, 35.0 parts of t-butyl methacrylate, 10.0 parts of 2-hydroxyethyl methacrylate, 45.0 parts of acrylic acid, 34.1 parts of propylene glycol monomethyl ether acetate, 14.6 parts of propylene glycol monomethyl ether, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were prepared in a beaker by stirring, and 4.0 parts of n-dodecyl mercaptan were prepared in a dropping vessel (B). After the temperature of the reaction vessel reached 90 ° C., while maintaining the same temperature, dropping was started from the dropping vessel over 3 hours, and polymerization was carried out. After the dropwise addition, the mixture was kept at 90°C for 30 minutes, then heated to 115°C and aged for 90 minutes. After cooling to room temperature, 39.4 parts of glycidyl methacrylate, 0.4 parts of dimethylbenzylamine as a catalyst, and 0.2 parts of topanol as a polymerization inhibitor were added and reacted at 110°C for 7 hours to obtain copolymer solution A-8. Various physical properties are shown in Table 1.

[0264] (Production Example 9) Preparation of copolymer solution A-9 (BzMI-TBMA-GMA copolymer solution) In a reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet, 124.3 parts of propylene glycol monomethyl ether acetate was charged, and after nitrogen replacement, the temperature was raised to 90 ° C. by heating. On the other hand, as a dropping vessel (A), 10.0 parts of N-benzylmaleimide, 55.0 parts of t-butyl methacrylate, 35.0 parts of glycidyl methacrylate, 10.0 parts of propylene glycol monomethyl ether acetate, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were prepared in a beaker by stirring, and 1.0 parts of n-dodecyl mercaptan and 15.7 parts of propylene glycol monomethyl ether acetate were prepared in a dropping vessel (B). After the temperature of the reaction vessel reached 90 ° C., while maintaining the same temperature, dropping was started from the dropping vessel over 3 hours, and polymerization was carried out. After the dropwise addition, the mixture was kept at 90° C. for 30 minutes, then heated to 115° C. and aged for 90 minutes to obtain copolymer solution A-9. Various physical properties are shown in Table 1.

[0265] (Production Example 10) Preparation of copolymer solution A-10 (MMA-HEMA copolymer solution) A reaction vessel equipped with a thermometer, a stirrer, a gas inlet tube, a cooling tube and a dropping vessel inlet was charged with 198.4 parts of propylene glycol monomethyl ether acetate, and after nitrogen replacement, it was heated to 90 ° C. On the other hand, as a dropping vessel (A), 80.0 parts of methyl methacrylate, 20.0 parts of 2-hydroxyethyl methacrylate, 4.9 parts of propylene glycol monomethyl ether acetate, and 2.0 parts of t-butylperoxy-2-ethylhexanoate were prepared by stirring and mixing, and as a dropping vessel (B), 3.0 parts of n-dodecyl mercaptan and 7.0 parts of propylene glycol monomethyl ether acetate were prepared by stirring and mixing. After the temperature of the reaction vessel reached 90 ° C, while maintaining the same temperature, dropping was started from the dropping vessel over 3 hours, and polymerization was carried out. After the dropwise addition, the mixture was kept at 90° C. for 30 minutes, then heated to 115° C. and aged for 90 minutes to obtain copolymer solution A-10. Various physical properties are shown in Table 1.

[0266] (Production Example 11) Preparation of polymer solution B-1 (VEEM polymer solution) In a 200 mL three-neck flask immersed in an acetone (room temperature) bath, 2-(2-vinyloxyethoxy)ethyl methacrylate (VEEM) (15.9 g, 79.5 mmol) was added dropwise to a mixture of dehydrated cyclopentyl methyl ether (30 g), dimethylketene methyl trimethylsilyl acetal (154 uL, 0.75 mmol), and tetrabutylammonium benzoate (2.73 mg, 0.0075 mmol) under a nitrogen stream over a period of 30 minutes. After the addition was completed, the reaction solution was stirred under the same conditions for 5 hours to obtain a cyclopentyl methyl ether solution of the VEEM polymer (polymer solution B-1). The resulting solution was 1 Measurement by H-NMR revealed that the VEEM used in the polymerization was completely consumed. Various physical properties of the polymer solution B-1 are shown in Table 2.

[0267] (Production Example 12) Preparation of polymer solution B-2 (VEEM-CHMA copolymer solution) In a 30 mL Schlenk tube immersed in a thermostatic bath at 20°C, a mixture of VEEM (2.0 g, 10 mmol) and cyclohexyl methacrylate (CHMA) (2.0 g, 12 mmol) was added dropwise to a mixture of dehydrated tetrahydrofuran (8.0 mL), dimethylketene methyl trimethylsilyl acetal (0.12 g, 0.69 mmol), and tetrabutylammonium benzoate (2.5 mg, 0.0069 mmol) under a nitrogen stream over a period of 10 minutes. After the addition was completed, the reaction solution was stirred under the same conditions for 5 hours. The resulting solution was diluted with ethyl acetate, passed through a silica gel short column, and concentrated under reduced pressure to obtain a copolymer solution of VEEM and CHMA (polymer solution B-2). The resulting solution was 1 Measurement by H-NMR revealed that the VEEM and CHMA used in the polymerization were completely consumed. Various physical properties of the polymer solution B-2 are shown in Table 2.

[0268] [Table 1]

[0269] [Table 2]

[0270] The descriptions in Table 1 are as follows. BzMI: N-benzylmaleimide MD: Dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate AMA: α-(allyloxymethyl)methyl acrylate AA: Acrylic acid MAA: Methacrylic acid MMA: Methyl methacrylate CHMA: Cyclohexyl methacrylate GMA: glycidyl methacrylate TBMA: t-butyl methacrylate HEMA: 2-hydroxyethyl methacrylate 2EHA: 2-ethylhexyl acrylate VT: Vinyl toluene nDM: n-dodecyl mercaptan SAH: Succinic anhydride

[0271] The descriptions in Table 2 are as follows. VEEM: 2-(2-vinyloxyethoxy)ethyl methacrylate

[0272] (Preparation Example 1) Preparation of Pigment Dispersion 1 12.9 parts of propylene glycol monomethyl ether acetate, 0.4 parts of Disparlon DA-7301 as a dispersant, 2.25 parts of CI Pigment Green 58 and 1.5 parts of CI Pigment Yellow 138 as colorants were mixed and dispersed for 3 hours using a paint shaker to obtain Pigment Dispersion 1 (solid content 22% by mass).

[0273] Example 1 35.0 parts of copolymer solution A-1 in terms of solid content, 10.0 parts of polymer solution B-1 in terms of solid content, 20.0 parts of dipentaerythritol hexaacrylate as a radical polymerizable compound, 5.0 parts of Irgacure OXE-02 (manufactured by BASF Japan) as a radical polymerizable photopolymerization initiator, 30.0 parts of pigment dispersion 1 in terms of solid content, and further a dilution solvent (propylene glycol monomethyl ether acetate) were added to a solid content concentration of 20%, and the mixture was stirred to obtain curable resin composition 1.

[0274] (Examples 2 to 13, Comparative Examples 1 to 2) Curable resin compositions 2 to 15 were obtained in the same manner as in Example 1 except that the formulations shown in Table 3 were used.

[0275] The solvent resistance of the obtained curable resin compositions 1 to 15 was evaluated. The results are shown in Table 3. The information in Table 3 is as follows: Photoacid generator: CPI-100P (triarylsulfonium salt type, San-Apro Co., Ltd.) Thermal acid generator: SI-100 (San-Aid SI-100L, manufactured by Sanshin Chemical Industry Co., Ltd.)

[0276] [Table 3]

[0277] From Tables 1 to 3, it was found that a curable resin composition containing at least an acid group-containing alkali-soluble resin, or a resin having a group that generates an acid group by heat or acid, and a polymer having a vinyl ether group in a side chain can give a cured product with excellent solvent resistance even at a temperature condition of 110°C.

Claims

1. The composition comprises an acid group-containing alkali-soluble resin and / or a resin having a group that generates an acid group by heat or acid, and a polymer having a vinyl ether group in a side chain, The acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid has a polymerizable double bond in a side chain. A curable resin composition comprising:

2. The curable resin composition described in claim 1, characterized in that the double bond equivalent of the acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid is 200 to 8000 g / equivalent.

3. 3. The curable resin composition according to claim 1, wherein the polymer having a vinyl ether group in a side chain has a structural unit represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 represents a hydrogen atom or a methyl group. 2 represents a hydrogen atom or an organic group; W represents a direct bond or a divalent organic group.

4. The curable resin composition according to any one of claims 1 to 3, characterized in that the polymer having a vinyl ether group in a side chain excludes a polymer containing a structural unit having a partial structure represented by the following formula and a structural unit having at least one group selected from the group consisting of an epoxy group, a mercapto group, a (meth)acryloyl group, a vinyl group, and an amino group. 【Chemistry 2】 (In the formula, R 1 and R 2 each independently represent an alkyl group having 1 to 4 carbon atoms, and n represents an integer of 0 to 2.)

5. The curable resin composition according to any one of claims 1 to 4, characterized in that the resin having a group that generates an acid group by heat or acid has a structural unit represented by the following general formula (2): 【Chemistry 3】 (In the formula, R 3 represents a hydrogen atom or a methyl group; X represents a direct bond or a divalent organic group; A represents a group that generates an acid group by the action of heat or an acid.

6. 6. The curable resin composition according to claim 1, wherein the acid group-containing alkali-soluble resin has an acid value of 20 to 230 mgKOH / g.

7. The curable resin composition according to any one of claims 1 to 6, characterized in that the acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid is a polymer having a ring structure in its main chain.

8. A curable resin composition described in any one of claims 1 to 7, characterized in that the content of the polymer having a vinyl ether group in the side chain is 5 to 50 mass% relative to 100 mass% total solid content of the curable resin composition.

9. The curable resin composition according to any one of claims 1 to 8, further comprising a photopolymerization initiator.

10. The curable resin composition according to any one of claims 1 to 9, further comprising a polymerizable compound.

11. The curable resin composition according to any one of claims 1 to 10, further comprising a photoacid generator.

12. The curable resin composition according to any one of claims 1 to 11, characterized in that the acid group-containing alkali-soluble resin and / or the resin having a group that generates an acid group by heat or acid further has an epoxy group, and / or the curable resin composition further contains an epoxy compound.

13. The curable resin composition according to any one of claims 1 to 12, which is for use as a resist.

14. The curable resin composition according to any one of claims 1 to 13, which is for use in a color filter.

15. A color filter comprising a substrate and a cured product of the curable resin composition according to any one of claims 1 to 14.

16. A display device comprising the color filter according to claim 15.

Citation Information

Patent Citations

  • Automatic constant speed PTO device

    JP1986081294A

  • Curable composition

    JP1994298884A

  • Ink for color filter, color filter, image display device and electronic device

    JP2009128864A

  • Photosensitive resin composition, method for producing cured film, cured film, liquid crystal display device and organic el display device

    WO2015037695A1