Film-forming salt-reducing agent

A film-forming salt reducing agent using a resin-based solution forms a removable film on steel structures, solving the inefficiencies and environmental issues of conventional salt removal methods by manually peeling off residual salts, ensuring effective and sustainable salt reduction.

JP7572940B2Active Publication Date: 2024-10-24DAISHIN CHEM
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021199870
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-16
Filing Date
2021-12-09
Publication Date
2024-10-24
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

Conventional methods for removing salt from steel structures, such as high-pressure water washing and power tool methods, are environmentally harmful, costly, and inefficient, particularly in removing residual salts that cannot be visually confirmed, leading to potential damage and reduced coating effectiveness.

Method used

A film-forming salt reducing agent containing a viscous aqueous solution with a film-forming resin is applied to the steel surface, forming a film that can be manually peeled off without power tools, effectively capturing and removing residual salts.

Benefits of technology

The method is simple, environmentally friendly, and cost-effective, reducing salt content without generating waste or damaging the steel structure, and can be performed regardless of location or season, addressing the limitations of existing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572940000001
    Figure 0007572940000001
  • Figure 0007572940000002
    Figure 0007572940000002
  • Figure 0007572940000003
    Figure 0007572940000003
Patent Text Reader

Abstract

To provide a film-forming type salt content reducer for reducing an amount of a salt content attached to a surface of a steel structure, and a salt content reduction method using the film-forming type salt content reducer which is simple and has no environmental load.SOLUTION: Viscous aqueous solution containing at least one kind of a resin as a film-forming component can be used as a film-forming type salt content reducer for reducing an amount of a salt content attached to a surface of a steel structure, and an amount of a salt content attached to the surface of the steel structure can be simply reduced by a method for coating the film-forming type salt content reducer to the surface of the steel structure to form a film, and then peeling the film without giving environmental load.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film-forming salt-reducing agent containing at least one resin as a film-forming component. The present invention also relates to a method for reducing the amount of salt adhering to the surface of a steel structure using the film-forming salt-reducing agent. This method can be used particularly when the steel structure has undergone surface preparation in a repainting work for the steel structure. [Background technology]

[0002] Steel structures such as steel bridges are part of the infrastructure of the nation and society. Steel structures have a coating to protect the base from the environment, but the coating deteriorates over time in outdoor environments that are subject to the weather, so they generally require periodic repainting, about once every 5 to 50 years. When repainting steel structures, the old coating is removed by surface preparation, and any substances adhering to the steel structure surface (rust, salt, etc.) are removed, and then a new coating is formed.

[0003] Surface preparation is generally called "cleaning". There are several types of cleaning (Type 1 to Type 4 cleaning), of which Type 1 cleaning is the most thorough surface preparation (i.e. the highest level of surface preparation) (for definitions of the various types of cleaning, see the Japan Road Association's "Handbook for Steel Highway Bridge Corrosion Prevention, March 2014"). Type 1 cleaning is usually done by blasting. When surface preparation is done using Type 1 cleaning, all of the old paint film and all of the rust adhering to the surface of the steel structure are removed. However, since the presence of adhering salt is often not visible to the naked eye, there may still be a large amount of salt remaining on the surface of the steel structure even after surface preparation using Type 1 cleaning. For example, when a steel structure is located along the ocean coast or in a cold region, salt (mainly sodium chloride) that drifts in from the ocean and salt (sodium chloride, calcium chloride, magnesium chloride, etc.) that comes from snow-melting agents sprayed in cold regions adhere to the steel structure, and even after surface preparation using a type 1 scraper, a large amount of salt often still adheres to the surface of the steel structure. If large amounts of salt are left unremoved, it will have a detrimental effect not only on the steel structure but also on the newly formed paint film. For this reason, it is necessary to remove the salt that has adhered to the surface of the steel structure and reduce the amount of salt to below a certain value before applying a new coat of paint. The above-mentioned "Handbook for Corrosion Prevention of Steel Highway Bridges" and other sources recommend that the amount of sodium chloride be reduced to 50 mg / m before applying a new coat of paint. 2 It is recommended to reduce the salt content to below 10%. In this specification, "salt" refers to a compound containing chloride ions. Examples of salt include sodium chloride, potassium chloride, calcium chloride, and magnesium chloride.

[0004] Removal of residual salt from the surfaces of steel structures is conventionally accomplished by high pressure water washing or power tool methods.

[0005] The high-pressure water washing method is a method for removing salt by spraying a large amount of high-pressure water on the surface of a steel structure. This method has the problem that a large amount of water is required, and also has cost and environmental problems because a large amount of wastewater is generated and the wastewater needs to be treated. Another problem with this method is that it can only be carried out in seasons when the water is not frozen.

[0006] The power tool method is a method of removing salt using power tools. This method has the problem of requiring specialized tools and is labor-intensive. This method also has the problem of noise and dust generated by the use of power tools, and the environmental impact of dealing with industrial waste such as used power tools. In addition, this method has the risk of damaging the surface of the steel structure due to the use of power tools, and the risk of salt on the surface of the steel structure penetrating into the interior of the steel structure due to such damage.

[0007] Furthermore, particularly when the steel structure is a bridge, the parts other than the supporting parts are often located in high spaces, and it is often difficult to carry out salt removal work, whether by high-pressure water washing or power tools.

[0008] Under these circumstances, there is a demand for simple, environmentally friendly alternatives to conventional technologies.

[0009] Japanese Patent Publication No. 2002-045811 (Patent Document 1) discloses a method for removing contaminants attached to the surface of a building or furniture. In this document, an aqueous solution of polyvinyl alcohol resin is applied to the surface of the building or furniture, dried, and the formed film is peeled off and removed together with the contaminants, thereby removing the contaminants attached to the surface of the building or furniture. In this document, a house is assumed as the building, and contaminants in the house are assumed as the contaminants to be removed, but removal of salt remaining on the surface of a steel structure such as a bridge is not assumed. Note that in this document, a preferred embodiment is to make the formed film function as a protective film on the surface of the building or furniture until it is peeled off and removed.

[0010] Japanese Patent Publication No. 2007-283237 (Patent Document 2) discloses a method for removing salt remaining on the surface of a steel structure after the exposed surface area of ​​the steel structure is adjusted to 60% or more by surface preparation in repainting work for the steel structure. In this method, an aqueous solution of sodium carbonate is applied to the surface of the steel structure, chloride ions are ion-exchanged with carbonate ions to remove salt from the surface of the steel structure, sodium carbonate powder is crystallized by drying, and this powder is removed with a nylon cup wire brush attached to an electric rotary tool, after which a new coating film is formed. In this document, a power tool is used to remove the powder, and the above-mentioned problems associated with the use of power tools inevitably occur.

[0011] Japanese Patent Publication No. 2017-213557 (Patent Document 3) discloses a method for removing salt remaining on the surface of a steel structure after the exposed surface area of ​​the steel structure is adjusted to 30% or more by adjusting the surface in a repainting work of the steel structure. In this method, a corrosion inhibitor containing hydrocalumite and / or hydrotalcite, which are ion scavengers, is applied to the surface of the steel structure and dried to form a film that captures chloride ions. This document assumes that the formed film is strongly fixed to the surface of the steel structure and that the film will remain unpeeled for a long period of time, and that a power tool method must be used to remove the film. Therefore, the method of this document inevitably causes the problems associated with the use of power tools as described above.

[0012] Thus, Patent Document 1 is a technology unrelated to removing salt remaining on the surface of a steel structure such as a bridge. In addition, Patent Documents 2 and 3 form a crystal powder or film to remove salt remaining on the surface of a steel structure after surface preparation, but since a power tool is required to remove the powder or film, the problems associated with the power tool method are not resolved. Therefore, there is still a demand for a simple method that is environmentally friendly and can replace the high-pressure water washing method and the power tool method. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Japanese Patent Application Publication No. 2002-045811 [Patent Document 2] Japanese Patent Publication No. 2007-283237 [Patent Document 3] Japanese Patent Application Publication No. 2017-213557 Summary of the Invention [Problem to be solved by the invention]

[0014] The object of the present invention is to provide a method for reducing the amount of salt adhering to the surface of a steel structure, which is a simple and environmentally friendly method that can replace the conventional high-pressure water washing method and power tool method. [Means for solving the problem]

[0015] In the course of research to develop the above method, the inventors discovered that when a viscous aqueous solution containing a film-forming resin is applied to the surface of a steel structure and dried to form a film, the film incorporates chloride ions, and further discovered that some such films can be peeled off by hand without using power tools (i.e., without the need for power tools) from the surface of the steel structure. In other words, they discovered that a viscous aqueous solution containing a specific resin as a film-forming component functions as a salt content reducer for reducing the amount of salt adhering to the surface of a steel structure, that the aqueous solution, which is a film-forming salt content reducer, is applied to the surface of a steel structure and dried to obtain a film that can be peeled off by hand without using power tools from the surface of the steel structure, and therefore that the problems of the present invention can be solved by the method of applying the aqueous solution to the surface of a steel structure to form a film and peeling off the film from the surface, and thus completed the present invention. Effect of the Invention

[0016] The method for reducing salt content of the present invention using a film-forming salt content reducing agent can be easily performed from film formation to peeling, and in particular, the peeling of the film can be performed manually without using power tools (i.e., without the need for power tools). Therefore, the method of the present invention is a simple method that does not put a burden on the environment, and can solve all the problems of the conventional high-pressure water washing method and power tool method. Specific examples of the effects of the present invention include that it can be easily performed, that it puts no burden on the environment, that it is inexpensive, that it does not require a large amount of water, that it does not generate a large amount of wastewater, that it does not require equipment for treating the wastewater, that it can be performed regardless of the location of the steel structure, that it can be performed regardless of the season, that it does not require power tools, and that there is no risk of damage to the surface of the steel structure caused by the use of power tools, or that the salt on the surface of the steel structure will penetrate into the interior of the steel structure due to the damage. Furthermore, by combining the method of the present invention with a conventional method, the problems of the conventional method can be alleviated. For example, the number of times and the time required for high-pressure water washing, which are required when reducing salt content using the conventional high-pressure water washing method, can be reduced by combining the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention relates to A chloride reducer that is applied to the surface of a steel structure that has been subjected to surface preparation using a type 1 or type 2 scraper, and then dried to form a film that captures the chlorides remaining on the surface of the steel structure, and then peels off the film together with the chlorides to remove the chlorides remaining on the surface, comprises a mixture of polyvinyl alcohol and an ethylene-vinyl acetate copolymer; water and From a viscous aqueous solution The mixture is mixed with 24 to 26% of the total mass of the salt-reducing agent. mass% Characterized in that it contains It is a film-forming chloride reducer for the surface of steel structures.

[0018] The present invention relates to The surface was prepared using a type 1 or type 2 scraper. On the surface of steel structures By applying and drying, a film is formed that incorporates the chlorides remaining on the surface of the steel structure, and the film is peeled off together with the chlorides, and the surface of the steel structure is 1. A method for reducing chloride comprising the steps of: (1)Claims 1 to The chloride reducing agent for the surface of a steel structure of the film-forming type described above is The above By applying it to the surface of the steel structure and letting it dry, The above steel structures of surface The remaining chloride was taken up A film is formed. (2) Removing the membrane from the surface of the steel structure Per chloride Peel off.

[0019] In order to facilitate understanding of the present invention, the basic features and preferred aspects of the present invention will be listed below.

[0020] 1. A film-forming salt reducing agent which is a viscous aqueous solution containing at least one resin as a film-forming component.

[0021] 2. A film-forming salt-reducing agent according to the preceding paragraph 1, which does not contain an ion scavenger.

[0022] 3. The film-forming salt-reducing agent according to item 1 or 2 above, wherein the resin is a vinyl resin.

[0023] 4. A film-forming salt-reducing agent according to any one of items 1 to 3 above, which is used to reduce the amount of salt adhering to the surface of a steel structure.

[0024] 5. A method for reducing the amount of salt adhering to the surface of a steel structure, comprising the steps of: (1) The film-forming salt-reducing agent according to any one of the preceding paragraphs 1 to 4 is applied to the surface of a steel structure having salt attached thereto, and then dried to form a film on the surface of the steel structure. (2) Peel the membrane off from the surface of the steel structure.

[0025] 6. The method according to item 5 above, wherein the salt comprises at least one selected from the group consisting of sodium chloride, potassium chloride, calcium chloride and magnesium chloride.

[0026] 7. The method according to the preceding paragraph 5 or 6, characterized in that the steel structure has undergone surface preparation in a repainting work.

[0027] 8. The salt contains sodium chloride, the surface preparation is by type 1 scraping, and the amount of sodium chloride adhering to the surface of the steel structure after the surface preparation is 50 mg / m 2 8. The method according to claim 7, wherein the number of times ... of the

[0028] The present invention will be described in detail below.

[0029] As will be explained in detail later, the film-forming salt content reducing agent of the present invention can be used to reduce the amount of salt adhering to the surface of a steel structure, and the amount of salt is reduced by applying the film-forming salt content reducing agent to the surface of a steel structure to which salt has adhered and drying the agent to form a film on the surface of the steel structure, and then peeling off the film. As mentioned above, in this specification, "salt" means a compound containing chloride ions, and examples of salt include sodium chloride, calcium chloride, and magnesium chloride.

[0030] The film-forming salt content reducing agent of the present invention is a viscous aqueous solution containing at least one resin as a film-forming component (hereinafter, the resin as a film-forming component is often abbreviated as "film-forming resin"). From the viewpoint of rust prevention, the pH of the film-forming salt content reducing agent is preferably in the alkaline range. There is no particular limitation on the viscosity of the film-forming salt content reducing agent, so long as it is capable of forming a film and can be peeled off by hand without using a power tool after film formation.

[0031] The components of the film-forming salt-reducing agent of the present invention are as follows.

[0032] (A) Film-forming resin The film-forming resin is an essential component. The film-forming resin may be used alone or in combination. The amount of the film-forming resin is not particularly limited as long as the object of the present invention can be achieved, but is preferably 5 to 39 mass % of the total mass of the film-forming salt-reducing agent, more preferably 11 to 33 mass %, and particularly preferably 22 to 30 mass %.

[0033] The resin used is not particularly limited as long as it is capable of forming a film and can be peeled off by hand without using a power tool. The film-forming resin may be a homopolymer or a copolymer. Examples of film-forming resins include vinyl resins. Examples of vinyl resins include polyvinyl alcohol and vinyl acetate resins (such as ethylene-vinyl acetate copolymers). Further examples of film-forming resins include polyvinyl butyral resins, acrylic resins, and urethane resins.

[0034] From the viewpoint of film-forming properties and ease of peeling after film formation, the film-forming resin is preferably a vinyl resin, and more preferably polyvinyl alcohol or a vinyl acetate resin (such as an ethylene-vinyl acetate copolymer).

[0035] There is no particular restriction on the degree of polymerization of polyvinyl alcohol, and the degree of polymerization can be appropriately selected depending on the manner in which the salt content reducing agent is applied to the steel structure.

[0036] When applying by spraying, the degree of polymerization of polyvinyl alcohol is preferably 300 to 4000, more preferably 400 to 2500, and particularly preferably 500 to 1000. Moreover, polyvinyl alcohol having a higher degree of polymerization may be used in combination with polyvinyl alcohol in the particularly preferred range (500 to 1000) as the main component.

[0037] When applying by a method other than a spray method (for example, a method using a brush or roller), the degree of polymerization is preferably 500 to 4000, more preferably 2000 to 3000, and particularly preferably 2400 to 2600. Furthermore, polyvinyl alcohol in the particularly preferred range (2400 to 2600) may be used as the main component, and polyvinyl alcohol having a lower degree of polymerization than this may be used in combination.

[0038] There is no particular limitation on the saponification degree of polyvinyl alcohol, so long as it is capable of forming a film and can be peeled off by hand without using a power tool after film formation. Generally, the higher the saponification degree, the lower the fluidity of the film-forming salt-reducing agent, which is a viscous aqueous solution. However, when the amount of polyvinyl alcohol blended is relatively small, the use of a fully saponified type does not impair the fluidity, and the fully saponified type has superior film strength. Those skilled in the art can appropriately determine the maximum saponification degree of polyvinyl alcohol that can be used, taking into account the amount of polyvinyl alcohol blended.

[0039] There is no particular limitation on the degree of polymerization of the ethylene-vinyl acetate copolymer, so long as it is capable of forming a film and the film can be peeled off by hand without the use of power tools.

[0040] There is no particular limitation on the ratio of ethylene to vinyl acetate in the ethylene-vinyl acetate copolymer, so long as a film can be formed and the film can be peeled off by hand without using a power tool.

[0041] Two or more types of film-forming resins may be used in combination. The ratio of the amounts of the resins when two or more types of resins are used in combination is not particularly limited as long as the resins can be used to form a film and can be peeled off by hand without using a power tool. Those skilled in the art can determine the ratio of the amounts while taking into consideration the degree of polymerization of each resin. For example, when polyvinyl alcohol and ethylene-vinyl acetate copolymer are used in combination, if the degree of polymerization of polyvinyl alcohol is high, the strength of the film will be high even if the amount of polyvinyl alcohol is relatively small, so the ratio of polyvinyl alcohol may be small. Note that if the amount of polyvinyl alcohol is large, it may not be possible to apply the resin by spraying it with an airless spray, but in such a case, it is sufficient to apply the resin using a brush or roller.

[0042] (B)Water Water is an essential component. There is no particular limitation on the amount of water as long as the object of the present invention can be achieved. In general, the greater the amount of water, the greater the contact between the salt on the steel structure surface and moisture, and therefore the greater the salt reduction effect, but if the amount of water is too large, drying will be slow. From this viewpoint, the amount of water is preferably 10 to 70 mass %, more preferably 20 to 60 mass %, and particularly preferably 35 to 50 mass % of the total mass of the film-forming salt-reducing agent.

[0043] In addition, the water is preferably one having a low ion content, such as distilled water, ion-exchanged water, or pure water.

[0044] (C) Peelability improver The peelability improver is an optional component. It can be used to improve peelability after film formation. When using a peelability improver, the amount depends on the type of peelability improver, but is preferably 0.5 to 5 mass %, more preferably 1 to 4 mass %, and particularly preferably 2 to 3 mass % of the total mass of the film-forming salt-reducing agent.

[0045] Examples of the release enhancer include fatty acid esters (sorbitan fatty acid esters, etc.), fatty acid salts (sodium oleate, potassium oleate, etc.), alkylamine ethylene oxide adducts, and fluorine-based surfactants.

[0046] (D) Thickener The thickener is an optional component. It can be used to improve film-forming properties. The thickener may be an inorganic thickener or an organic thickener. The thickener may be used alone or in combination of multiple types. When used in combination, any multiple types may be selected from the group consisting of a single or multiple inorganic thickeners and a single or multiple organic thickeners and used in combination. When a thickener is used, the amount thereof is preferably 0.5 to 20 mass%, more preferably 1.0 to 10 mass%, and particularly preferably 1.5 to 5.0 mass% of the total mass of the film-forming salt-reducing agent.

[0047] The inorganic thickener may be a natural or synthetic product. Examples of inorganic thickeners include silica, kaolin minerals, serpentine, talc, mica, vermiculite, smectite (including montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite), bentonite, sepiolite, organoclay, and organobentonite.

[0048] Examples of organic thickeners include anionic thickeners such as polyacrylic acid or a salt thereof, an acrylic acid-acrylic acid ester copolymer or a salt thereof, an acrylic acid-acrylamide copolymer or a salt thereof, an olefin-maleic acid copolymer or a salt thereof, a styrene-maleic acid copolymer or a salt thereof, methylcellulose, carboxymethylcellulose, hydroxyethylmethylcellulose, hydroxypropylmethylcellulose or a salt thereof, and nonionic thickeners such as polyacrylamide, alkylcellulose, polyethylene oxide, and polyethylene oxide.

[0049] (E) Rust inhibitor The rust inhibitor is an optional component. When the rust inhibitor is used, the amount thereof is preferably 0.1 to 3 mass %, more preferably 0.5 to 1.0 mass %, of the total mass of the film-forming salt-reducing agent.

[0050] Examples of the rust inhibitor include organic acid salts, fatty acid salts, organic acid amine salts, alkanolamines, alkylamine ethylene oxide adducts, alkyl phosphate ester salts, and 3-(2-benzothiazylthio)propionic acid·alkanolamine salts.

[0051] (F) pH adjuster The pH adjuster is an optional component. It is preferable to add the pH adjuster from the viewpoint of rust prevention. When an alkaline pH adjuster is used, if the amount of the adjuster is large, it tends to be reflected in the measured value when the surface salt content is measured by a surface salinity meter. Therefore, from the viewpoint of the accuracy of the measurement by the surface salinity meter, when an alkaline pH adjuster is used, it is desirable to add the pH adjuster in a range in which the pH of the film-forming salt content reducer containing the pH adjuster is in a weak alkaline region. When a pH adjuster is used, the amount is preferably 0.1 to 5 mass % of the total mass of the film-forming salt content reducer, more preferably 0.5 to 3 mass %, and particularly preferably 0.8 to 1.5 mass %.

[0052] Examples of pH adjusters include ammonia, 2-methylaminoethanol, monoisopropanolamine, diisopropanolamine, 2-dimethylaminoethanol, triethanolamine, triethylamine, sodium hydroxide, potassium hydroxide, lactic acid, succinic acid, gluconic acid, citric acid, malic acid, oxalic acid, and phosphoric acid.

[0053] (G) Ion scavenger The ion scavenger is an optional component. Basically, it is preferable not to use an ion scavenger for the reasons described below, but use of the ion scavenger is not excluded.

[0054] Examples of ion scavengers include the IXE series manufactured by Toagosei Co., Ltd. of Japan, and hydrotalcite (such as Kyoward 500 manufactured by Kyowa Chemical Industry Co., Ltd. of Japan). The IXE series has a higher ion-scavenging ability than hydrotalcite. Among the IXE series, IXE-600, IXE-6107, IXE-100 and IXE-700F are preferred.

[0055] Since it takes time for the ion trapping agent to exert its ion trapping ability, when it is intended to peel off the film about 24 hours after applying the film-forming salt content reducing agent, the use of the ion trapping agent is not very effective. In addition, since the ion trapping agent is preferably used in a neutral or acidic region, it is not preferable to include it in the film-forming salt content reducing agent of the present invention, which is preferably used in an alkaline region from the viewpoint of rust prevention. Furthermore, when the film-forming salt content reducing agent of the present invention contains an ion trapping agent, the peelability of the obtained film tends to decrease. However, if the obtained film is to be maintained for a certain period of time and sufficient measures are taken to address the above problems associated with the use of the ion trapping agent, the ion trapping agent may be used.

[0056] The film-forming salt-reducing agent of the present invention may contain additives other than those mentioned above in order to improve film-forming properties, peelability, drying properties, thixotropy, etc. Examples of additives (some of which overlap with the above additives) include organic solvents, thickeners, film-forming assistants, plasticizers, thixotropy-imparting agents, pigments, dyes, emulsifiers, solubilizers, surfactants, dispersants, release agents, anti-settling agents, leveling agents, rust inhibitors, preservatives, antioxidants, defoamers, ultraviolet absorbers, chelating agents, and ion scavengers.

[0057] The film-forming salt-reducing agent of the present invention can be used to reduce the amount of salt adhering to the surface of a steel structure. A method of using the agent includes the following steps. (1) The film-forming salt reducing agent of the present invention is applied to the surface of a steel structure having salt attached thereto, and then dried to form a film on the surface of the steel structure. (2) Peel the membrane off from the surface of the steel structure.

[0058] There are no particular limitations on the steel structure. Examples of the steel structure include steel bridges, steel plants, steel buildings, steel pipes, steel materials, steel plates, and other steel structures.

[0059] There is no particular limitation on the method of application, and application can be performed using a spray, brush, roller, or the like, as appropriate, taking into consideration the characteristics of the film-forming salt-reducing agent, which is the coating liquid, the size, shape, installation location, and the like of the steel structure. If the film thickness is not uniform, it may cause the film to tear when peeled off, so it is preferable to apply it as uniformly as possible. When using a spray, a wide area can be coated in a short time compared to manual work using a brush or roller. The spray may be an air spray or an airless spray. The air spray may be a handy air spray or a non-handy air spray. The airless spray may also be a handy airless spray or a non-handy airless spray. In addition, since the coating liquid can be filled more easily with a non-handy airless spray than with a handy airless spray, from this viewpoint, a non-handy airless spray is more suitable for coating a wide area than a handy airless spray.

[0060] The coating amount is such that the resulting film has a desired thickness. There is no particular limitation on the thickness of the film. From the viewpoint of easy peeling of the film after drying, the wet film thickness is preferably 500 to 1500 μm, more preferably 800 to 1200 μm, and the dry film thickness is preferably 10 to 300 μm, more preferably 50 to 200 μm, and particularly preferably 75 to 150 μm. If the film thickness is not uniform, it may cause the film to tear when peeled off, so the film thickness is preferably uniform. In addition, the coating weight is preferably 0.5 to 1.5 kg / m 2 , and more preferably 0.8 to 1.2 kg / m 2 The coating amount is easily controlled by the wet film thickness and coating weight. If the time from coating to peeling is relatively short, such as 24 hours, the film does not require a particularly high strength.

[0061] There is no particular limitation on the method of drying, and it may be simply left to dry, or a fan may be used to speed up the drying. In the case of leaving to dry, the time may be set so that the film is sufficiently dried and easy to peel off, and the specific time of leaving to dry varies depending on the season and weather. For example, in winter, a longer time of leaving to dry is required. In addition, from the viewpoint of the number of days of the process, it is not preferable to leave to dry for too long. Considering these, the time of leaving to dry is generally preferably 10 to 48 hours, more preferably 15 to 35 hours, and particularly preferably 20 to 30 hours. In addition, it is preferable to leave to dry at a temperature of 5°C or higher and a humidity of 85% or lower. In addition, "humidity" here means "relative humidity", and the same applies below.

[0062] We verified whether the film could be peeled off within 24 hours after application in several test environments. Specifically, a salt content reducing agent having the same composition as Sample 5 used in the examples described later was applied to a blasted steel test piece (size: 200 x 100 x 6 mm, material: SM400A) with a brush at 1.0 kg / m. 2 The coating was applied at a coating amount of 100g, dried using an explosion-proof thermostatic and humidity chamber PR-4KPH (manufactured by Espec Corporation, Japan), and verification was conducted under several temperature and humidity conditions to see whether peeling was possible within 24 hours after coating. The verification results are as follows. When the temperature was 10°C and the humidity was 85%, peeling was not possible within 24 hours after coating. On the other hand, when the temperature was 10°C and the humidity was 50%, when the temperature was 20°C and the humidity was 85%, when the temperature was 20°C and the humidity was 50%, when the temperature was 30°C and the humidity was 85%, and when the temperature was 30°C and the humidity was 50%, peeling was possible within 24 hours after coating.

[0063] There are no particular limitations on the method of peeling. The film can be peeled off by hand without using a power tool. When peeling off by hand without using a power tool, peel off the film from the edge and pull the film with a certain force to remove it. If it is difficult to peel off the edge of the film, insert a simple tool (for example, a tool with a thin blade such as a cutter or scraper) into the interface between the steel base material and the film, lift it up, and then peel it off.

[0064] The method of the present invention can be preferably used when the steel structure has undergone surface preparation in a repainting work.

[0065] There are no particular limitations on the surface preparation in repainting work. Scraping may be any of type 1 scraping, type 2 scraping, type 3 scraping, and type 4 scraping, and type 3 scraping may be any of type 3A, type 3B, and type 3C. In the present invention, surface preparation is preferably by type 1 scraping (the highest degree of surface preparation), but it is acceptable for there to be many areas of the old coating film that are not removed, as with type 3 scraping and type 4 scraping.

[0066] There is no limitation on the method of surface preparation, and conventional surface preparation methods, such as blasting, or treatment using tools such as a grinder having a rotating grindstone or grinding disk attached to an electric rotary drive, a disk grinder, etc. Furthermore, there is no particular limitation on the amount of salt remaining on the surface of the steel structure after surface preparation.

[0067] When surface preparation is performed by type 1 scraping, all of the old paint film and all of the rust on the steel structure surface are removed. The amount of sodium chloride remaining on the steel structure surface after surface preparation by type 1 scraping is 50 mg / m2. 2 may exceed 50 mg / m 2 The amount of sodium chloride adhering to the surface of a steel structure is 50 mg / m2 or less after surface preparation using a type 1 cleaning method. 2 When the amount of sodium chloride adhering to the surface of a steel structure exceeds 50 mg / m2, the present invention is applied. 2 The above-mentioned "Handbook for Corrosion Prevention of Steel Highway Bridges" and other publications recommend that the amount of sodium chloride adhering to the surface of a steel structure before the application of new paint should be 50 mg / m 2 It is recommended that the amount of sodium chloride remaining on the surface of a steel structure after surface preparation using a type 1 scraper be reduced to 50 mg / m2 or less. 2Even if this is the case, the present invention can be applied to further reduce the amount of sodium chloride.

[0068] After reducing the amount of salt remaining on the surface of the steel structure, a new coating film is applied to the steel structure. There are no particular limitations on the coating composition used for the new coating, the type of coating film obtained, or the coating method, and these may be determined appropriately taking into account factors such as the period for which the coating film will be maintained. EXAMPLES

[0069] The following are examples 1 to 3, Comparative Examples 1 and 2, and Reference example 1~ 3 The present invention will be described more specifically with reference to the following examples (hereinafter, these are often collectively referred to as "Examples, etc."). As described below, Example 1 , Comparative Examples 1 and 2 and Reference Example 1 were carried out in parallel over a period of three days, and 2 and 3, and Reference example 2 and 3 The same test was carried out separately over two days in parallel. 3. Comparative Examples 1 and 2 and Reference Example 3 In the example, the salt content was reduced by a salt-reducing agent, and in Reference Examples 1 and 2, the salt content was reduced by washing with water. The examples do not limit the scope of the present invention.

[0070] The test steel materials and sample film-forming salt-reducing agents used in the examples are as follows.

[0071] Example 1 , Comparative Examples 1 and 2, and Test steels used in Reference Example 1 (Test steels 1 to 4) Test steels 1 to 4 are waste materials of corroded lower cross struts that were removed from a bridge (under the jurisdiction of the Tosa National Highway Office of the Ministry of Land, Infrastructure, Transport and Tourism) along the coast of Kochi Prefecture due to replacement work of components caused by corrosion. This bridge was erected in 1970 and repainted (with polyurethane paint) in 1999. The corroded lower cross struts were removed in 2013 (43 years after erection) and transported to the Kamogawa Exposure Test Site of the Civil Engineering Research Center (Kamogawa City, Chiba Prefecture) on October 29, 2013, where they were exposed, and were provided to the applicant this time. The dimensions of the horizontal surface that corresponds to the underside of the flanges of test steels 1 to 4 are 0.17m x 1.2m. An overview of the Civil Engineering Research Center's Kamogawa Exposure Test Site and the test steel material, which is waste material from the corroded lower cross structure, are explained in the technical journal "Civil Engineering Technical Materials" 57-1 (2015) pp.60-63.

[0072] Test steel materials 1 to 4 are the same as those in Example 1. , Comparative Examples 1 and 2, and Used in Reference Example 1.

[0073] Working Example 2 and 3, and Test steel used in Reference Example 2 (Test steel 5) Test steel material 5 is a component that was used as the main girder of a bridge erected in an area free from salt damage, and is a waste material that was removed for replacement work and stored at the Inagawa Warehouse (Inagawa-cho, Kawabe-gun, Hyogo Prefecture) of Japan Far East Metallicon Industries Co., Ltd. The Inagawa Warehouse is located in an area free from salt damage. Test steel material 5 was provided to the applicant this time. The dimensions of the vertical surface of test steel material 5, which corresponds to the main girder web surface, are 1.17m long and 0.92m wide. Hereinafter, this vertical surface will be referred to simply as "the vertical surface of test steel material 5", or even more simply as "the vertical surface".

[0074] First, a high-concentration calcium chloride aqueous solution was applied evenly to both vertical surfaces (i.e., the front and rear surfaces) of the test steel 5 on weekdays (every day except Saturdays, Sundays, and other holidays) for one month, twice each on weekdays, using a roller, to fix calcium chloride on both vertical surfaces. Furthermore, from the stage of the salt content reduction process described later, a partition with a width of 0.02 m was provided vertically in the center of both surfaces, and each surface was divided into two parts, a left part and a right part, for a total of four sections (the dimensions of each section were 1.17 m vertical x 0.45 m horizontal). Hereinafter, the front and rear vertical surfaces of the test steel 5 are often simply referred to as the "front" and "rear", respectively, and the left section of the front, the right section of the front, the left section of the rear, and the right section of the rear are often referred to as the "front A", "front B", "rear A" and "rear B", respectively.

[0075] The front surface A, the front surface B, the rear surface A and the rear surface B are respectively 2 , Working Example 3 , Reference Example 2 and Reference example 3 Used in.

[0076] Example 1 , Comparative Examples 1 and 2 Samples of the film-forming salt-reducing agent used in (Samples 1 to 3) The components and amounts of Samples 1 to 3 are shown in Table 1.

[0077] [Table 1]

[0078] Sumikaflex 455HQ and Sumikaflex 456HQ in Table 1 contain moisture, as described below. Therefore, the total amount of "film-forming resin" listed in item (A) does not represent the total amount of resin in Sample 1 or Sample 2, and the amount of "moisture" listed in item (B) does not represent the total amount of moisture in Sample 1 or Sample 2. The resin amount and moisture amount of Sample 1 are about 26% by mass and about 64% by mass, respectively. The resin amount and moisture amount of Sample 2 are about 28% by mass and about 53% by mass, respectively.

[0079] Details of the components shown in Table 1 are as follows:

[0080] JC-25 (manufactured by Japan Vinyl Acetate & Poval Co., Ltd.) Polyvinyl alcohol resin Degree of polymerization: 2500 Saponification degree: 99 mol%

[0081] Sumikaflex 455HQ (manufactured by Sumika Chemtex Co., Ltd., Japan) Ethylene-vinyl acetate copolymer emulsion Non-volatile content: 54-57% by mass (moisture: 46-43% by mass) Glass transition temperature (Tg): 0℃

[0082] Sumikaflex 456HQ (manufactured by Sumika Chemtex Co., Ltd., Japan) Ethylene-vinyl acetate copolymer emulsion Non-volatile content: 54-56% by mass (moisture: 46-44% by mass) Glass transition temperature (Tg): 0℃

[0083] IONET T-80V (manufactured by Sanyo Chemical Industries, Ltd., Japan) A surfactant whose main component is polyoxyethylene sorbitan fatty acid ester

[0084] hi-Metolose 90SH-15000 (manufactured by Shin-Etsu Chemical Co., Ltd., Japan) Hydroxypropyl methylcellulose (glyoxal treated)

[0085] Aron B-500 (manufactured by Toagosei Co., Ltd., Japan) Carboxylic Acid Copolymer Emulsion Solid content: 36±1% by mass

[0086] Kiresuto Light W-510 (manufactured by Kiresuto Co., Ltd., Japan) Organic acid amine salts

[0087] Sunhibitor No. 50 (manufactured by Sanyo Chemical Industries, Ltd., Japan) Amine-based nonionic surfactants

[0088] DIPA(85%) Diisopropanolamine: 85% by mass Moisture: 15% by mass

[0089] Working Example 2 and 3, and Reference Example 3 Samples used in (Samples 4-5) The components and amounts thereof of Samples 4 and 5 are shown in Table 2.

[0090] [Table 2]

[0091] Sumikaflex 400HQ and Sumikaflex 408HQE in Table 2 contain moisture, as described below. Therefore, the total amount of "film-forming resin" listed in item (A) does not represent the total amount of resin in Sample 4 or Sample 5, and the amount of "moisture" listed in item (B) does not represent the total amount of moisture in Sample 4 or Sample 5. The resin amount and moisture amount of Sample 4 are about 24% by mass and about 71% by mass, respectively. The resin amount and moisture amount of Sample 5 are also about 24% by mass and about 71% by mass, respectively.

[0092] Details of the components shown in Table 2 are as follows:

[0093] JF-05 (manufactured by Japan Vinyl Acetate & Poval Co., Ltd.) Polyvinyl alcohol resin Degree of polymerization: 500 Saponification degree: 98 to 99 mol%

[0094] Sumikaflex 400HQ (manufactured by Sumika Chemtex Co., Ltd., Japan) Ethylene-vinyl acetate copolymer emulsion Non-volatile content: 54-56% by mass (moisture: 46-44% by mass) Glass transition temperature (Tg): 0℃

[0095] Sumikaflex 408HQE (manufactured by Sumika Chemtex Co., Ltd., Japan) Ethylene-vinyl acetate copolymer emulsion Non-volatile content: 49-51% by mass (moisture: 51-49% by mass) Glass transition temperature (Tg): -30℃

[0096] IONET T-80V (manufactured by Sanyo Chemical Industries, Ltd., Japan) A surfactant whose main component is polyoxyethylene sorbitan fatty acid ester

[0097] Laponite EP (BYK-Chemie, Germany) Synthetic Hectorite

[0098] Kiresuto Light W-510 (manufactured by Kiresuto Co., Ltd., Japan) Organic acid amine salts

[0099] MMEA amine 2-Methylaminoethanol

[0100] BYK-014 (BYK-Chemie, Germany) Antifoaming agent that is a mixture of foam-busting polymer and hydrophobic particles

[0101] The method of applying the sample to the test steel material and the method of washing the test steel material with water used in the examples are as follows.

[0102] Example 1 , Comparative Examples 1 and 2 How to apply the sample The sample was applied using a brush to the horizontal surface that corresponds to the underside of the flange of test steels 1 to 3. However, as mentioned above, the dimensions of the horizontal surface are 0.17m x 1.2m, but because there were holes on both sides of the test steel, the sample was applied to the area excluding both sides (0.17m x 1.0m), so the application area was 0.17m 2 The coating amount was 1.0 kg / m 2 It was.

[0103] Working Example 1 and 3, and Reference Example 3 How to apply the sample Sample application was performed using a spray on the entire surface (1.17m long x 0.45m wide) of each of the front surface A, front surface B, and rear surface B, with the vertical surface of the test steel material 5 (a steel plate measuring 1.17m long x 0.92m wide) in an upright position. The spray used for the front surface A and rear surface B was a handy airless sprayer (Ultramax Cordless) (manufactured by GRACO, USA), and for the front surface B was a high-pressure airless sprayer (Ecopon series) (manufactured by Asahi Sunac Corporation, Japan). The nozzle tip used for the high-pressure airless sprayer was LP525 (manufactured by GRACO, USA). The application amount was 1.0 kg / m for each. 2 It was.

[0104] Method of washing with water in Reference Example 1 The water washing treatment was performed using a handy airless sprayer (Ultramax Cordless) (manufactured by GRACO, USA) on the horizontal surface corresponding to the underside of the flange of the test steel 4. However, as in the case of painting, the water washing area was limited to the parts excluding both sides of the test steel, so the water washing area was 0.17 m 2 The washing area was 1m 2 The amount of water used per unit was set at 7L, so the total amount of water used was approximately 1.2L.

[0105] Washing area 1m 2 The reason for setting the amount of water used per unit at 7 liters is as follows. In the lecture "Experiment for removing salt adhering to bridges" (56th Annual Academic Lecture Meeting of the Japan Society of Civil Engineers, October 2001, pp. 340-341), an experiment was carried out to remove salt adhering to the surface of a steel bridge, and it was found that "in order to satisfy the allowable amount of salt adhering during repair, the minimum amount of water required is sufficient, and the amount of washing water is 6 to 8 liters / m. 2 Therefore, the water washing area is 1m 2 The amount of water used per unit was determined to be 7L, taking the midpoint between the lower limit (6L) and the upper limit (8L) of the range of 6 to 8L.

[0106] Method of washing treatment in Reference Example 2 The water washing treatment was carried out on the rear surface A of the vertical surface of the test steel material 5 (a steel plate measuring 1.17 m in length and 0.92 m in width) in an upright position using the above-mentioned handy airless spray. The amount of water used per square meter of the washed area was reduced compared to Reference Example 1, and 2 and 3, and Reference Example 3 The amount of sample applied was 1 L (i.e., 1.0 kg / m 2 ) was decided.

[0107] The measurements carried out in the examples are as follows.

[0108] Example 1 , Comparative Examples 1 and 2, and Measurement using a surface salinity meter in Reference Example 1 The surface salinity meter used was a portable surface salinity meter (SSM-21P) manufactured by DKK Toa Corporation of Japan.

[0109] The amount of salt remaining on the surface of test steel materials 1 to 4 after the blast treatment described below and the amount of salt remaining on the surface of test steel materials 1 to 4 after the salt reduction treatment process described below were measured using a surface salinity meter. Since the main component of the salt contained on the surface of test steel materials 1 to 4 is sodium chloride, the measured salt concentration value, which converts the measured electrical conductivity value into the concentration of sodium chloride, was used as the amount of salt.

[0110] Measurements were performed at five locations for all test steels (test steels 1 to 4). Specifically, when looking at the test steels from left to right in the longitudinal direction, measurements were performed at five locations: left, left center, center, right center, and right (one end of the test steel is considered to be the left end, and the other end is considered to be the right end, and from the left end to the right end, the locations were left, left center, center, right center, and right). However, due to the nature of the surface salinity meter, the measurement water may leak from the surface salinity meter, and if leakage occurs, this will have a significant effect on the measurement values, so if leakage occurs, the measurement value at that location was not counted.

[0111] Additionally, the average of the counted measurements was calculated.

[0112] Working Example 2 and 3, and Reference example 2 and 3 Measurements using a surface salinity meter As the surface salinity meter, the above-mentioned surface salinity meter was used.

[0113] The amount of salt remaining on the surface of the test steel 5 after the blast treatment described below and the amount of salt remaining on the surface of the test steel 5 after the salt reduction treatment process described below were measured using a surface salinity meter. Since the salt contained on the surface of the test steel 5 was essentially calcium chloride only, the measured salt concentration, which was obtained by converting the measured electrical conductivity value into the concentration of water-soluble salt based on the IMO PSPC, was used as the amount of salt.

[0114] Measurements were taken at multiple locations as follows: For measurements after blasting (at this point, the front and rear of test steel 5 had not yet been divided into two), nine locations on each of the front and rear were selected as measurement locations. For measurements after the salt reduction treatment process (at this point, the front was divided into front A and front B, and the rear was divided into rear A and rear), five locations each on front A, front B, and rear A were selected as measurement locations, and six locations on rear B were selected as measurement locations. However, due to the nature of the surface salinity meter, there is a possibility that the measurement water will leak from the surface salinity meter, and since leakage will have a significant effect on the measurement values, if leakage occurred, the measurement value at that location was not counted.

[0115] Additionally, the average of the counted measurements was calculated.

[0116] Examples 1 to 3 , Comparative Examples 1 and 2, and Reference example 1~3 Measurement by ion chromatography in The ion chromatograph used was a Dionex ICS-1100 manufactured by Thermo Fisher Scientific, USA.

[0117] The liquid used in the measurement using the surface salinity meter (only those that have been counted) is collected, and the collected liquid is used as a sample for ion chromatography to extract chloride ions (Cl - ), nitrite ion (NO2 - ), nitrate ion (NO3 - ), and sulfate ions (SO42- ) were measured, and the total amount of these four types of anions was calculated. Note that the measurement principles of ion chromatography and surface salinity meters are different, and there may be measurement errors, so the chloride ion (Cl - ) does not necessarily correlate with the amount of salt (sodium chloride or calcium chloride) measured using a surface salinity meter.

[0118] In addition, the average values ​​of the measurements were calculated.

[0119] Example 1 , Comparative Examples 1 and 2, and Reference example 1 From the first to third days, salt reduction experiments using test steels 1 to 4 were carried out in parallel as described below. As described later, the experiments using test steels 1 to 3 were carried out in the same manner as in Example 1. , Comparative Examples 1 and 2 The experiment using the test steel 4 is Reference Example 1. Reference Example 1 is an experimental example of salt content reduction using a conventional high-pressure water washing method, and was carried out to serve as a reference for evaluating the salt content reduction effect of the present invention.

[0120] In the afternoon of the first day, test steels 1 to 4 were blasted (equivalent to Class 1 scraping). In the morning of the second day, the amount of salt on the surface of test steels 1 to 4 after blasting was measured using a surface salt meter. The liquid used for the measurement using the surface salt meter was also collected and measured by ion chromatography at a later date.

[0121] For test steels 1 to 3, the above-mentioned surface salinity measurements were carried out using a surface salinity meter, and then in the morning of the second day, samples 1 to 3 were applied, left to dry for 24 hours to form a film, and in the morning of the third day, the film was peeled off by hand. In the afternoon of the third day, the amount of salt on the surface of test steels 1 to 3 after the film was peeled off was measured using a surface salinity meter. The liquid used for the measurements using the surface salinity meter was also collected, and measurements were carried out using an ion chromatograph at a later date.

[0122] For test steel 4, the above-mentioned surface salinity measurement was carried out using a surface salinity meter, and then a water rinsing treatment was carried out in the afternoon of the second day. In the afternoon of the third day, the amount of salt on the surface of test steel 4 after the water rinsing treatment was measured using a surface salinity meter. The liquid used for the measurement using the surface salinity meter was also collected, and was later measured using an ion chromatograph.

[0123] On the second day, the temperature was 27.2°C and the humidity was 50%, and on the third day, the temperature was 28.1°C and the humidity was 45%.

[0124] Experiments using test steels 1 to 3 (respectively, salt content reduction was performed using samples 1 to 3) were performed as Example 1. , Comparative Examples 1 and 2 The experiment using test steel 4 (wherein the salt content was reduced by washing with water) was set as Reference Example 1. , Comparative Examples 1 and 2 In this example, the process from sample application to peeling and removal of the film is referred to as the salt reduction treatment process, and in Reference Example 1 (water washing experiment example), the water washing process is referred to as the salt reduction treatment process.

[0125] Table 3 shows the results of measurements using a surface salinity meter after blasting (only those whose measured values ​​were counted), and the results of measurements using an ion chromatograph conducted at a later date on the measurement solutions used in the measurements (only those whose measured values ​​were counted using the surface salinity meter). Table 4 also shows the average values ​​of the measurements.

[0126] Table 5 shows the results of measurements using a surface salinity meter after the salt reduction treatment process (only those whose measured values ​​were counted), and the results of measurements using an ion chromatograph taken at a later date after recovering the measurement solution used in the measurements (only those whose measured values ​​were counted using the surface salinity meter). Table 6 also shows the average values ​​of the measurements.

[0127] Table 7 shows the salt removal rate calculated based on the surface salt content meter measurements. Table 7 also shows the salt removal rate of four types of anions (i.e., chloride ion (Cl)) calculated based on the ion chromatograph measurements. - ), nitrite ion (NO2- ), nitrate ion (NO3 - ), and sulfate ions (SO4 2- The removal rate of each of the four anions is shown in Table 1, as well as the total removal rate of these four anions. The removal rate indicates how much the amount of salt or anion has been reduced by carrying out the salt reduction treatment process, and was calculated using the following formula.

[0128] Removal rate (%) = (Measurement value after blasting process - Measurement value after salt reduction process) ÷ Measurement value after blasting process ×100

[0129] Table 8 shows Example 1 , Comparative Examples 1 and 2 An overall evaluation is shown for each of the cases of Example 1 and Reference Example 1. This overall evaluation includes evaluation of film formation, evaluation of peelability by hand, and evaluation of salt reduction effect. However, in the case of Reference Example 1, since no film is formed, there is no evaluation of peelability by hand.

[0130] As can be seen from Table 8, Example 1 , Comparative Examples 1 and 2 In the case of the present invention, the evaluation of film formation, the evaluation of manual peelability, and the salt content reducing effect all reach a practical level. Therefore, the film formed from the film-forming salt content reducing agent of the present invention reduces the salt content adhering to the surface of the steel sheet, and the film can be peeled off and removed by hand without using a power tool.

[0131] [Table 3]

[0132] [Table 4]

[0133] [Table 5]

[0134] [Table 6]

[0135] [Table 7]

[0136] [Table 8]

[0137] The evaluation criteria shown in Table 8 are as follows:

[0138] Assessment of membrane formation The test steel was , Comparative Examples 1 and 2 In the case of the sample, the film-forming salt-reducing agent was used, and in the case of the reference example, water was used) and the film was evaluated as to whether it could be formed, together with the degree of dripping. The specific evaluation criteria are as follows:

[0139] ◎: No dripping and film can be formed. ○: There is a small amount of dripping (some of the liquid causes an avalanche), but a film can be formed. △: There is a lot of dripping (some of the liquid drips from the steel material onto the floor), but a film can be formed. ×: Dripping was severe and no film could be formed.

[0140] Manual peelability evaluation The film after drying was evaluated as to whether it could be peeled off by hand from the surface of the test steel material, together with the ease of peeling. The specific evaluation criteria were as follows:

[0141] : Very easy to peel off. ◯: Easy to peel off, but since there are weak parts of the film, it cannot be said that it is very easy to peel off. Δ: Peeling is possible, but it does not peel off as a unit, so it cannot be said to be easy to peel off. ×: Cannot be peeled off.

[0142] Evaluation of salt reduction effect The salt reduction effect was evaluated based on the salt removal rate (A) measured by a surface salt meter and the chloride ion removal rate (B) measured by an ion chromatograph. The specific evaluation criteria are as follows:

[0143] ◎: Particularly effective (over 70% for both A and B). ○: Significant effect (either A or B exceeds 70%) △: Somewhat effective (both A and B are below 70%).

[0144] Working Example 2 and 3, and Reference example 2 and 3 From the first to the second day, salt reduction experiments were carried out in parallel on the front surface (divided into front surface A and front surface B after blasting) and rear surface (divided into rear surface A and rear surface B after blasting) of the test steel material 5 as follows. As described later, the experiments using front surface A, front surface B, rear surface A, and rear surface B are respectively referred to as Examples. 2 , Working Example 3 , Reference Example 2 and 3 Reference Example 2 is an experimental example of salt content reduction using a conventional high-pressure water washing method, and was carried out to serve as a reference for evaluating the salt content reduction effect of the present invention.

[0145] At 11:00 am on the first day, the front and rear surfaces were blasted (equivalent to type 1 scraping). After blasting, the front surface was divided into front A and front B, and the rear surface was divided into rear A and rear B. At 1:00 pm on the first day, the surface salt content of front A, front B, rear A, and rear B after blasting was measured using a surface salt meter. The liquid used for the measurements with the surface salt meter was also collected and measured by ion chromatography at a later date.

[0146] For the front surface A, the front surface B and the rear surface B, the above-mentioned surface salt content measurement was carried out using a surface salt content meter, and then at 4:00 p.m. on the first day, Sample 4, Sample 5 and Sample 5 were applied, respectively (thus, Sample 5 was applied to the front surface B and the rear surface B), and the surface was left to dry to form a film. For the front surface A and the front surface B, the formed film was peeled off and removed by hand at 11:00 a.m. on the second day (thus, for the front surface A and the front surface B, the drying time was 19 hours), and the amount of salt on the surface after the film was peeled off and removed was measured using a surface salt content meter at 11:30 a.m. on the second day. For the rear surface B, the formed film was peeled off and removed by blasting (equivalent to a type of scraping) at 1:00 p.m. on the second day (thus, for the rear surface B, the drying time was 21 hours), and the amount of salt on the surface after the film was peeled off and removed was measured using a surface salt content meter at 3:00 p.m. on the second day. In addition, the liquids used for the measurements using the surface salinity meter were collected for each of the front surface A, front surface B, and rear surface B, and measurements were performed using an ion chromatograph at a later date. Reference example 3 ), the film was peeled off and removed by blasting, so two blasting treatments were performed, including the first blasting treatment. In order to distinguish between these two blasting treatments, the first blasting treatment will simply be referred to as the "blasting treatment" and the second blasting treatment (i.e., the blasting treatment to peel off and remove the film) will be referred to as the "further blasting treatment."

[0147] The wet and dry film thicknesses were measured for the films formed on the front surface A, front surface B, and rear surface B. The wet film thickness was measured using a wet gauge, and the dry film thickness was measured using a film thickness gauge, at three locations each. Since accurate measurements could not be obtained for the wet film thickness, measurements were taken at three locations to obtain approximate values. The dry film thickness was the average of the measurements at three locations. For the film formed on the front surface A, the wet film thickness was 1000 μm and the dry film thickness was 169 μm. For the film formed on the front surface B, the wet film thickness was 800 to 1300 μm and the dry film thickness was 215 μm. For the film formed on the rear surface B, the wet film thickness was 800 to 900 μm and the dry film thickness was 183 μm.

[0148] For rear surface A, the above-mentioned surface salinity measurement was carried out using a surface salinity meter, and then the surface was washed with water at 2:00 PM on the first day. At 11:30 AM on the second day, the amount of salt on the surface after the washing with water treatment was measured using the surface salinity meter. The liquid used for the measurement with the surface salinity meter was also collected, and was later measured using an ion chromatograph.

[0149] On the first day, the temperature was 29°C and the humidity was 50%, while on the second day, the temperature was 26°C and the humidity was 43%.

[0150] Experiments using front surface A, front surface B, and rear surface B (respectively, salt reduction is performed using sample 4, sample 5, and sample 5) are respectively examples. 2 and 3 and Reference Example 3 The experiment using the rear surface A (reducing salt content by washing with water) was set as Reference Example 2. 2 and 3 and Reference Example 3 In Example 2 (water washing experiment), the water washing step is referred to as the salt reduction treatment step.

[0151] Table 9 shows the average values ​​of the measurements taken with a surface salinity meter after the blast treatment, and the average values ​​of the measurements taken with an ion chromatograph at a later date after recovering the measurement solution used in the measurements.

[0152] Table 10 shows the average values ​​of the measurements taken using a surface salinity meter after the salt reduction treatment process, and the average values ​​of the measurements taken using an ion chromatograph at a later date after recovering the measurement liquid used in the measurements.

[0153] Table 11 shows the salt removal rate calculated based on the surface salt content meter measurements. Table 11 also shows the salt removal rate of four types of anions (i.e., chloride ion (Cl)) calculated based on the ion chromatograph measurements. - ), nitrite ion (NO2 - ), nitrate ion (NO3 - ), and sulfate ions (SO4 2-The removal rate of each of the four anions is shown in Table 1, as well as the total removal rate of these four anions. The removal rate indicates how much the amount of salt or the amount of anions is reduced by carrying out the salt reduction treatment step. , Comparative Examples 1 and 2, and Reference example 1 and 2 This was calculated using the same formula as in the case of

[0154] Table 12 shows the examples. 2 and 3, and Reference example 2 and 3 A comprehensive evaluation is shown for each of the above cases. This comprehensive evaluation includes evaluation of film formation, evaluation of manual peelability, and evaluation of salt reduction effect, and the criteria for these evaluations are the same as those for the above Examples 1 to 3 and Reference Example 1. However, in the case of Example 6, peeling and removal by hand is not performed, and in the case of Reference Example 2, no film is formed, so there is no evaluation of manual peelability.

[0155] As can be seen from Table 12, Example 2 and 3 In the case of the present invention, the evaluation of film formation, the evaluation of manual peelability, and the salt content reducing effect all reach a practical level. Therefore, the film formed from the film-forming salt content reducing agent of the present invention reduces the salt content adhering to the surface of the steel sheet, and the film can be peeled off and removed by hand without using a power tool.

[0156] [Table 9]

[0157] [Table 10]

[0158] [Table 11]

[0159] [Table 12] [Industrial Applicability]

[0160] By using the film-forming salt-reducing agent of the present invention, all of the problems associated with the conventional high-pressure water washing method and power tool method can be eliminated, and this excellent salt-reducing method is simple, does not place a burden on the environment, and is highly economical, making it possible to reduce the amount of salt adhering to the surface of steel structures such as steel bridges, steel plants, steel buildings, steel pipes, steel materials, steel plates, and other steel structures.

Claims

1. A chloride reducer for the surface of a steel structure which has been subjected to surface preparation using a type 1 or type 2 scraper, which is then dried to form a film which absorbs the chlorides remaining on the surface of the steel structure, and which then peels off the film together with the chlorides, thereby removing the chlorides remaining on the surface, said chloride reducer being a film-forming type for the surface of a steel structure, characterized in that the chloride reducer comprises a viscous aqueous solution consisting of a mixture of polyvinyl alcohol and ethylene-vinyl acetate copolymer and water, and that the mixture comprises 24 to 26 mass % of the total mass of the chloride reducer.

2. A method for reducing the chlorides on the surface of a steel structure by applying a coating to the surface of a steel structure that has been prepared by a type 1 or type 2 scraping and drying it to form a film that absorbs the chlorides remaining on the surface of the steel structure, and then peeling off the film together with the chlorides, the method comprising the following steps. (1) The film-forming chloride reducer for the surface of a steel structure as described in claim 1 is applied to the surface of the steel structure and dried to form a film that absorbs the chlorides remaining on the surface of the steel structure. (2) The film is peeled off from the surface of the steel structure together with the chlorides.

3. 3. The method according to claim 2, wherein the chloride is at least one selected from the group consisting of sodium chloride, potassium chloride, calcium chloride and magnesium chloride.

Citation Information

Patent Citations

  • Method for cleaning surface

    JP2002045811A

  • High-durability repair coating method

    JP2007283237A

  • Material for two-part aqueous Anti-corrosive coating and method for Anti-corrosive coating

    JP2009149791A

  • Method of removing contaminants from structural surfaces

    JP2014190829A

  • Aqueous anticorrosive coating and aqueous anticorrosive coating method

    JP2017013474A