New modified sodium fluoride adsorbent, its manufacture and application

A modified sodium fluoride adsorbent, produced by sintering NiCl2·6H2O and NaF, enhances separation and adsorption efficiency for hydrogen fluoride and reduces chlorine trifluoride adsorption, addressing bonding issues and improving purity.

JP7573033B2Active Publication Date: 2024-10-24FUJIAN DEER TECH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022537445
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-11
Publication Date
2024-10-24
Estimated Expiration
2042-02-11

AI Technical Summary

Technical Problem

Chlorine trifluoride and hydrogen fluoride tend to bond, making separation difficult, and common sodium fluoride exhibits low adsorption efficiency for hydrogen fluoride and high loss of chlorine trifluoride.

Method used

A modified sodium fluoride adsorbent is produced by sintering NiCl2·6H2O and porous NaF at specific temperatures and treating with a high-purity fluorine-nitrogen mixed gas to form NiF2 with a NaF skeleton, enhancing its adsorption properties.

Benefits of technology

The modified adsorbent effectively disperses chlorine trifluoride and hydrogen fluoride, improving hydrogen fluoride adsorption efficiency to over 98% and reducing chlorine trifluoride adsorption to about 3%, maintaining high activity and low production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573033000004
    Figure 0007573033000004
  • Figure 0007573033000005
    Figure 0007573033000005
  • Figure 0007573033000001
    Figure 0007573033000001
Patent Text Reader

Abstract

The present invention provides a new type of modified sodium fluoride adsorbent, its manufacturing method and application. The manufacturing method of the new type of modified sodium fluoride adsorbent includes the steps of: providing NiCl2·6H2O and porous NaF, and preparing spherical particles in a mass ratio of 1:3.0-3.5 in step S1; sintering the spherical particles in a vacuum atmosphere at a vacuum degree of 500 Pa or less at temperatures of 120-130°C and 280-300°C for 10-40 hours, respectively, to form an adsorbent intermediate having NiCl2-NaF skeleton; and treating the adsorbent intermediate with high-purity fluorine-nitrogen mixed gas to finally form a new type of sodium fluoride adsorbent having NiF2-NaF skeleton in step S3. The new modified sodium fluoride adsorbent provided by the present invention can efficiently separate chlorine trifluoride and hydrogen fluoride molecules, improve the optimal adsorption efficiency for hydrogen fluoride to 98% or more, and reduce the optimal adsorption efficiency for chlorine trifluoride to about 3%. Furthermore, the manufacturing process of this new modified sodium fluoride adsorbent is simple, the production cost is low, it is economical, and it can be industrially produced.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a new type of modified sodium fluoride special adsorbent, its preparation and application. [Background technology]

[0002] At present, chlorine trifluoride and hydrogen fluoride are easily combined to form polymers, making it difficult to separate the two. Research has shown that common sodium fluoride has strong stability to chlorine trifluoride and hydrogen fluoride at the same time, and can adsorb hydrogen fluoride, but its adsorption efficiency to hydrogen fluoride is less than 90%, and its adsorption effect to chlorine trifluoride is about 10%, so its adsorption efficiency to hydrogen fluoride is low, and the loss of chlorine trifluoride is large. Summary of the Invention

[0003] The present invention provides a new type of modified sodium fluoride adsorbent, its preparation method and application, which can effectively solve the above problems.

[0004] The present invention is realized in the following manner.

[0005] The manufacturing method of the new modified sodium fluoride adsorbent according to the present invention is as follows: A step S1 of providing NiCl2·6H2O and porous NaF and preparing spherical particles in a mass ratio of 1:3.0-3.5; a step S2 of sintering the spherical particles in a vacuum atmosphere at a degree of vacuum of 500 Pa or less at temperatures of 120 to 130° C. and 280 to 300° C. for 10 to 40 hours, respectively, to form an adsorbent intermediate having a NiCl2-NaF skeleton; and a step S3 of treating the adsorbent intermediate with a high purity fluorine-nitrogen mixed gas.

[0006] In addition, the new modified sodium fluoride adsorbent of the present invention has a NiF2-NaF skeleton and a BET specific surface area of ​​2m 2 ·g -1or more, and the pore volume is 0.00015 cm 3 ·g -1 That's all.

[0007] The present invention also provides a new type of modified adsorbent for sodium fluoride obtained by the above-mentioned manufacturing method.

[0008] In addition, the present invention provides the application of the above-mentioned new modified sodium fluoride special adsorbent, specifically, the above-mentioned new modified sodium fluoride special adsorbent is used for separating chlorine trifluoride and hydrogen fluoride.

[0009] The present invention provides the following beneficial effects:

[0010] The present invention develops a new type of modified sodium fluoride adsorbent with NiF2-NaF structure for the binding action of chlorine trifluoride and hydrogen fluoride, which can separate chlorine trifluoride and hydrogen fluoride, remove impurities in hydrogen fluoride, and increase the purity of chlorine trifluoride, thereby meeting the application demands of chlorine trifluoride. The new modified sodium fluoride adsorbent of the present invention can effectively separate chlorine trifluoride and hydrogen fluoride molecules, improve the optimal adsorption efficiency for hydrogen fluoride to more than 98%, and reduce the optimal adsorption efficiency for chlorine trifluoride to about 3%. In addition, the new modified sodium fluoride adsorbent can maintain high activity and high adsorption in all situations. In addition, the manufacturing process of the new modified sodium fluoride adsorbent is simple, the production cost is low, it has good economic effect, and it can be industrialized. [Brief description of the drawings]

[0011] In order to more clearly describe the technical aspects of the embodiments of the present invention, the following briefly describes the drawings required in the embodiments, but the following drawings only show some embodiments of the present invention, and therefore should not be regarded as limiting the scope of the claims. Those skilled in the art can also obtain other related drawings based on these drawings without creative labor.

[0012] [Figure 1] 1 is a scanning electron microscope photograph of conventional sodium fluoride. [Diagram 2] 1 is a scanning electron microscope photograph of a new type of modified sodium fluoride adsorbent provided by an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In order to make the objectives, technical aspects and advantages of the embodiments of the present invention clearer, the technical aspects of the embodiments of the present invention will be described clearly and completely below in accordance with the drawings in the embodiments of the present invention. It is clear that the described embodiments are only some of the embodiments of the present invention, not all of the embodiments. According to the embodiments of the present invention, all other embodiments obtained by those skilled in the art without performing creative labor are all within the scope of protection of the present invention. Therefore, the detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of protection sought, but only represents selected embodiments of the present invention. According to the embodiments of the present invention, all other embodiments obtained by those skilled in the art without performing creative labor are all within the scope of protection of the present invention.

[0014] In the present description, the terms "first" and "second" are used for descriptive purposes only and should not be understood to indicate or imply relative importance or to implicitly designate the number of elements. Thus, an element qualified as "first" or "second" may explicitly or implicitly include one or more elements. In the present description, "plurality" means two or more, unless otherwise limited.

[0015] The manufacturing method of the new modified sodium fluoride adsorbent according to the embodiment of the present invention includes the following steps:

[0016] In step S1, NiCl2·6H2O and porous NaF are provided to prepare spherical particles in a mass ratio of 1:3.0-3.5.

[0017] In step S2, the spherical particles are sintered in a vacuum atmosphere at temperatures of 120 to 130° C. and 280 to 300° C. for 10 to 40 hours, respectively, to form an adsorbent intermediate having a NiF2-NaF skeleton, where the degree of vacuum is 500 Pa or less.

[0018] In step S3, the adsorbent intermediate is treated with a high purity fluorine-nitrogen mixed gas.

[0019] As a further improvement, in step S1, tests have shown that controlling the ratio of NiCl2·6H2O and porous NaF is favorable for sufficient interaction between NiF2 and NaF formed after NiCl2 is fluorinated, and can reduce the adsorption efficiency to chlorine trifluoride to the maximum. Therefore, it is preferable to prepare NiCl2·6H2O and porous NaF as spherical particles with a mass ratio of 1:3.1-3.3. In one embodiment, NiCl2·6H2O and porous NaF are prepared as spherical particles with a mass ratio of 1:3.2.

[0020] The porous NaF can be prepared by the following steps.

[0021] In step S11, NaHF2 is vacuum-treated to release at least some hydrogen atoms from the NaHF2 molecule, forming a material with loose porosity and sodium fluoride properties. The drying temperature is 200-210°C, the drying time is 20-30h, and the vacuum degree is 500 Pa or less. In one embodiment, the drying temperature is about 205°C, the drying time is about 24h, and the vacuum degree is about 100 Pa.

[0022] As a further improvement, in step S1, the spherical particles have a particle size of 5-8 mm. Particles with this particle size are advantageous for packing an adsorption tower and can form a larger porosity. As a further improvement, the NiCl2 may be further processed to form a polyfluorine material, forming nickel fluoride with a high fluorine content.

[0023] As a further improvement, in step S2, sintering is performed in a stepwise manner to prevent the spherical particles from cracking due to a sudden increase in temperature, thereby improving the sintering yield and increasing the specific surface area and pore volume of the sintered adsorbent particles by several times. Furthermore, by sintering in a stepwise manner, the water molecules of NiCl2·6H2O and the H atoms in some NaHF2 where H atoms still remain can be further liberated, forming a gentle porous particle structure. In one embodiment, the spherical particles are sintered in a vacuum atmosphere at temperatures of 125°C and 290°C for 24 hours each, and the vacuum degree is about 100 Pa, so that the final BET specific surface area is 4.0756 m 2 ·g -1 The pore volume is 0.000301 cm 3 ·g -1 In another embodiment, the spherical particles are sintered in a vacuum atmosphere at temperatures of 130° C. and 280° C. for 24 hours each, and the vacuum degree is about 100 Pa, so that the final BET specific surface area is 4.8995 m 2 ·g -1 The pore volume is 0.000356 cm 3 ·g -1 In another embodiment, the spherical particles are sintered in a vacuum atmosphere at temperatures of 120° C. and 300° C. for 24 hours each, and the vacuum degree is about 100 Pa, so that the final BET specific surface area is 3.9781 m 2 ·g -1 The pore volume is 0.000293 cm 3 ·g -1 It becomes.

[0024] As a further improvement, the function of using high purity fluorine nitrogen mixed gas in step S3 is to fluorinate nickel chloride with fluorine gas to form nickel fluoride. Nickel fluoride with high fluorine content (in each molecule, one nickel atom bonds two fluorine atoms) is introduced into sodium fluoride, and the interaction between sodium fluoride molecules and nickel difluoride molecules forms a "molecule" that is similar in spatial structure to chlorine trifluoride and has a multi-fluorine group, and the bond length and bond angle with chlorine trifluoride molecules are twisted to a certain extent, thereby achieving the purpose of separating sodium fluoride molecules and chlorine trifluoride molecules. When such a "molecule" with a multi-fluorine group interacts with hydrogen fluoride molecules, it is easy to form a weak inter-molecular force, and by controlling the temperature of the mixture system, the formation of high polymers of hydrogen fluoride molecules is reduced, and the bimolecular bond of chlorine trifluoride molecules is reduced, and the repulsive force between these highly active molecules and the "modified" sodium fluoride molecules is also increased synchronously. Thus, the "modified" sodium fluoride achieves the purpose of reducing the adsorption to chlorine trifluoride and improving the adsorption to hydrogen fluoride. Nitrogen plays a role in diluting fluorine gas, preventing danger caused by the strong activity of fluorine gas. Tests have proven that if the fluorine concentration is too low, the activity is insufficient, and if the concentration is too high, danger is likely to occur. Therefore, the high purity fluorine nitrogen mixed gas preferably contains F2 with a volume content of 5-15% and N2 with a volume content of 85-95%. In one embodiment, the high purity fluorine nitrogen mixed gas contains F2 with a volume content of about 10% and N2 with a volume content of 90%.

[0025] As a further improvement, in step S3, treating the adsorbent intermediate with a high-purity fluorine-nitrogen mixed gas includes fluorinating the adsorbent intermediate with a high-purity fluorine-nitrogen mixed gas for 24 to 72 hours. In one embodiment, the adsorbent intermediate is fluorinated with a high-purity fluorine-nitrogen mixed gas for 48 hours, and after the fluorination is completed, the high-purity fluorine-nitrogen mixed gas is removed by purging with nitrogen.

[0026] The present invention further provides a compound having a NiF2-NaF framework and a BET specific surface area of ​​2 m 2 ·g-1 or more, the pore volume is 0.00015 cm 3 ·g -1 In one embodiment, the new modified sodium fluoride adsorbent has a BET specific surface area of ​​4.8995 m 2 ·g -1 The pore volume reaches 0.000356 cm 3 ·g -1 can be reached.

[0027] As shown in Figures 1 and 2, currently common sodium fluoride has a dense crystalline arrangement and a small specific surface area, which is disadvantageous for efficient adsorption of hydrogen fluoride (its BET specific surface area is 0.6591 m). 2 ·g -1 The pore volume reaches 0.000054 cm 3 ·g -1 After modification, the new sodium fluoride adsorbent has a sheet structure, a larger specific surface area, and a larger number of pores than conventional sodium fluoride, effectively improving the adsorption efficiency of hydrogen fluoride.

[0028] The embodiment of the present invention also provides the application of the above-mentioned new modified sodium fluoride special adsorbent, which is used to separate chlorine trifluoride and hydrogen fluoride.

[0029] In the present invention, an orthogonal test was carried out for the separation of chlorine trifluoride and hydrogen fluoride under the following process conditions:

[0030] [Table 1]

[0031] [Table 2] JPEG0007573033000003.jpg110170

[0032] As is clear from Table 2 above, the new modified sodium fluoride adsorbent according to the present invention can efficiently separate chlorine trifluoride and hydrogen fluoride molecules, improve the optimal adsorption efficiency for hydrogen fluoride to more than 98%, and reduce the optimal adsorption efficiency for chlorine trifluoride to about 3%. In addition, this new modified sodium fluoride adsorbent can maintain high activity and high adsorption in different situations. Furthermore, this new modified sodium fluoride adsorbent has a simple manufacturing process, low production cost, is economical, and can be industrially produced. Finally, it has been experimentally proven that this adsorbent has a long usage cycle and can maintain the optimal adsorption efficiency for hydrogen fluoride at about 98% and the optimal adsorption efficiency for chlorine trifluoride at about 3% after repeated use 100 times.

[0033] The above is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Various improvements and modifications are possible for those skilled in the art. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included within the protection scope of the present invention.

Claims

1. NiCl 2 ・6H 2 A step S1 of providing O and porous NaF and preparing spherical particles in a mass ratio of 1:3.0 to 3.5; The spherical particles are sintered in a vacuum atmosphere at a degree of vacuum of 500 Pa or less at temperatures of 120 to 130° C. and 280 to 300° C. for 10 to 40 hours, respectively, to form NiCl 2 Step S2 of forming an adsorbent intermediate having a NaF skeleton; A step S3 of treating the adsorbent intermediate with a fluorine-nitrogen mixed gas; A manufacturing method for a new type of modified sodium fluoride adsorbent, comprising:

2. In step S1, the method for producing the porous NaF includes the steps of: The drying temperature is 200 to 210° C., the drying time is 20 to 30 hours, and the degree of vacuum is 500 Pa or less. 2 2. The method for producing the new modified sodium fluoride adsorbent according to claim 1, further comprising the step S11 of subjecting the obtained material to a vacuum drying treatment to form a porous material having sodium fluoride properties.

3. The method for producing a new type of modified sodium fluoride adsorbent as claimed in claim 1, characterized in that in step S1, the particle size of the spherical particles is 5-8 mm.

4. In step S3, the fluorine-nitrogen mixed gas has a volume content of 5 to 15% F. 2 and N with a volume content of 85-95% 2 The method for producing the new type of modified sodium fluoride adsorbent according to claim 1, further comprising:

5. The method for producing the new type of modified adsorbent for sodium fluoride according to claim 1, characterized in that in step S3, the step of treating the adsorbent intermediate with fluorine-nitrogen mixed gas includes fluorinating the adsorbent intermediate with fluorine-nitrogen mixed gas for 24 to 72 hours.

6. NiF 2 -NaF skeleton and BET specific surface area of ​​2 m 2 ・g -1 or more, and the pore volume is 0.00015 cm 3 ・g -1 A new type of modified sodium fluoride adsorbent characterized by the above.

7. A method for using the new modified sodium fluoride-specific adsorbent described in claim 6 in separating chlorine trifluoride and hydrogen fluoride.

8. The method for using the new modified sodium fluoride adsorbent according to claim 7, characterized in that the conditions for separating the chlorine trifluoride and the hydrogen fluoride are: temperature: 80-100°C, flow rate: 0.2-1L / min, and pressure: 0.6-1MPa.

Citation Information

Patent Citations

  • High-cohesive-energy fluoride adsorbent, and preparation and application thereof

    CN113578285A

  • Fluorine adsorbent and preparation and application thereof

    CN113578287A

  • Production of sodium fluoride pellet

    JP1988270310A

  • Method of preparing pure fluorine gas

    US3989808A

  • Method for purifying fluorine compound gas

    WO2017138366A1