Encapsulating resin composition and semiconductor device
The sealing resin composition with epoxy resin, silicone resin, and phosphoric acid polyester addresses filling challenges in large semiconductor chips, ensuring low viscosity, low CTE, and high fracture toughness for improved reliability.
Patent Information
- Application Number
- JP2021563894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-12
- Filing Date
- 2020-12-02
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-12-02
AI Technical Summary
Existing sealing materials face challenges in filling gaps between large semiconductor chips and base materials, leading to issues such as cracking, peeling, and reduced thermal shock resistance due to increased stress and viscosity, especially with high filler content.
A sealing resin composition containing epoxy resin with silicone resin having multiple epoxy groups, phosphoric acid, and phosphoric acid polyester, which maintains low viscosity and fluidity, reduces coefficient of thermal expansion (CTE), and enhances fracture toughness, ensuring easy filling and crack resistance.
The composition achieves low CTE, low elastic modulus, and high fracture toughness, preventing cracks and improving reliability in semiconductor devices, even with larger chip sizes.
Smart Images

Figure 0007573244000007 
Figure 0007573244000001 
Figure 0007573244000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an encapsulating resin composition and a semiconductor device, and more particularly to an encapsulating resin composition for encapsulating electronic components such as semiconductor elements, and a semiconductor device including an encapsulant made from the encapsulating resin composition. [Background technology]
[0002] Patent Document 1 discloses a liquid epoxy resin composition for sealing, which contains a liquid bisphenol epoxy resin, silicone rubber particles, a silicone-modified epoxy resin, an aromatic amine curing agent, a coupling agent, an inorganic filler, and an organic solvent. It is disclosed that this liquid epoxy resin composition for sealing can suppress warpage to a minimum even when applied to electronic component devices that require low warpage, and has excellent reliability such as strength, thermal shock resistance, and moisture resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-23272 A Summary of the Invention
[0004] An object of the present disclosure is to provide an encapsulating resin composition that is easily filled between a substrate and a chip and is less likely to cause cracks in the encapsulating material, even when preparing an encapsulating material that seals between the substrate and a large chip, and a semiconductor device that includes an encapsulating material made of a cured product of this encapsulating resin composition.
[0005] The encapsulating resin composition according to one embodiment of the present disclosure contains an epoxy resin (A), a phosphoric acid (B), and a phosphate polyester (C). The epoxy resin (A) contains a silicone resin (A1) having two or more epoxy groups in one molecule.
[0006] A semiconductor device according to an embodiment of the present disclosure includes a substrate, a mounting component mounted on the substrate, and a sealant that seals a gap between the substrate and the mounting component, the sealant being made of a cured product of the encapsulating resin composition. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a semiconductor device according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1. Overview The encapsulating resin composition according to the present embodiment contains an epoxy resin (A), a phosphoric acid (B), and a phosphate polyester (C). The epoxy resin (A) contains a silicone resin (A1) having two or more epoxy groups in one molecule.
[0009] Conventionally, in a resin composition for sealing, an inorganic filler such as silica has been blended to improve the heat resistance and reduce the coefficient of thermal expansion (CTE) of the sealing material made from the resin composition. However, if the ratio of the filler in the resin composition is too high, the filler tends to aggregate, and the viscosity of the resin composition increases excessively, which reduces the flowability, and as a result, there is a risk of reducing the moldability. If the moldability of the resin composition is reduced when molding the resin composition, there is a problem that the resin composition cannot be sufficiently filled deep into the gap between the substrate and the semiconductor chip in the semiconductor device when sealing the gap with the resin composition.
[0010] In addition, in recent years, chips have been enlarged. As the chips become larger, the size of the encapsulant also becomes larger, which tends to increase the stress applied to the encapsulant, and therefore the performance such as thermal shock resistance may not be sufficiently obtained. Therefore, the encapsulant is likely to crack, peel off, etc. In addition, when the encapsulant is produced from the composition, there is a problem that it becomes difficult to sufficiently fill the gap between the chip and the base material such as a substrate when the chip becomes larger.
[0011] In contrast, the encapsulating resin composition of the present embodiment can impart thermosetting properties to the encapsulating resin composition and can reduce the storage modulus of the encapsulating resin composition and the cured product of the encapsulating resin composition by containing the silicone resin (A1) in the epoxy resin (A). In addition, the CTE of the cured product produced from the encapsulating resin composition can be reduced. In addition, the encapsulating resin composition of the present embodiment can maintain a low viscosity and can have a thixotropic index close to 1, so that it can have good fluidity.
[0012] Furthermore, the encapsulating resin composition contains phosphoric acid (B) and phosphoric acid polyester (C), which improves the dispersibility of the components in the encapsulating resin composition. Therefore, even if the silicone resin (A1) makes the viscosity of the composition increase, the encapsulating resin composition has high dispersibility and can maintain good flowability. This makes it easy for the encapsulating resin composition to flow in the gap between the substrate and the mounting board, and therefore makes it easy to fill the gap with the encapsulant.
[0013] As described above, the encapsulating resin composition of this embodiment can achieve good fluidity, and can achieve a low CTE and low elastic modulus of the cured product produced from the encapsulating resin composition. In particular, the cured product produced from the encapsulating resin composition of this embodiment can achieve not only a low CTE and low elastic modulus, but also an improvement in fracture toughness K1c, by containing the silicone resin (A1), phosphoric acid (B), and phosphate polyester (C). In this disclosure, fracture toughness K1c is resistance to fracture when a force is applied to a material having a defect. The fracture toughness is measured by the method described in the examples below. In addition, the encapsulating resin composition of this embodiment has high fracture toughness, making it possible to produce an encapsulating material that is less likely to crack. In particular, in this embodiment, it is possible to make it less likely to crack when the chip size of a semiconductor chip is increased due to the high functionality of the semiconductor device, and to improve the reliability of the semiconductor device.
[0014] In this disclosure, the term "larger chips" refers to, for example, a chip size of a semiconductor chip or the like in a mounting component that is rectangular in plan view with a side length of 25 mm or more, or an area of 625 mm or more in plan view. 2 However, in this embodiment, the size of the chip is not limited to the above, and the composition according to this embodiment can be applied regardless of the size of the chip.
[0015] More specifically, such preferable properties of the encapsulating resin composition can be realized by appropriately adjusting the components of the composition described below.
[0016] As shown in Fig. 1, the encapsulating resin composition according to this embodiment can be suitably used as an encapsulating material 4 that encapsulates between a substrate 2 and a mounting component 3 such as a semiconductor chip in a semiconductor device 1. In particular, the encapsulating resin composition can be suitably used as an underfill material. When the encapsulating resin composition is used as an underfill material and the encapsulating material 4 is produced from the encapsulating resin composition, the encapsulating material 4 is less likely to crack.
[0017] 2.Details Components that may be contained in the encapsulating resin composition will be described in detail.
[0018] [Epoxy resin (A)] The encapsulating resin composition of this embodiment contains an epoxy resin (A). The epoxy resin (A) is a thermosetting component. The epoxy resin (A) has at least one epoxy group in one molecule. In this embodiment, the epoxy resin (A) contains a silicone resin (A1) having two or more epoxy groups in one molecule.
[0019] The epoxy resin (A) preferably has a viscosity of 100 mPa·s or more and 20 Pa·s or less at 25° C. The viscosity of the epoxy resin (A) can be measured, for example, using a B-type rotational viscometer at a rotation speed of 50 rpm.
[0020] [Silicone resin (A1)] As described above, the encapsulating resin composition contains the silicone resin (A1), which has two or more epoxy groups in one molecule.
[0021] A silicone resin is a compound having a siloxane bond in a molecule. In this embodiment, the silicone resin (A1) has at least one siloxane bond and two or more epoxy groups in one molecule. The silicone resin (A1) in the encapsulating resin composition of this embodiment has a siloxane skeleton, which can contribute to a decrease in CTE. In addition, since it has an epoxy group, it can impart thermosetting properties to the encapsulating resin composition.
[0022] The silicone resin (A1) preferably has at least one epoxy group at the end of one molecule. In this case, the silicone resin (A1) is unlikely to cause aggregation, and therefore is unlikely to excessively increase the viscosity of the encapsulating resin composition, and therefore good fluidity can be ensured. Here, the end of one molecule refers to the position of the end of the linking chain that is bonded to the silicon atom in the siloxane bond in the molecule, which is the farthest from the silicon atom. For example, even if the silicone resin (A1) is branched, the end may be any of the ends of each branch. In the silicone resin (A1), when an epoxy group is present at the end of the molecule, the reactivity of the encapsulating resin composition is unlikely to increase excessively, and the storage stability of the encapsulating resin composition can be maintained. Therefore, when the encapsulating resin composition is molded, moldability (processability) can be maintained, it is unlikely to harden during molding, and it is easy to fill the gap between the substrate and the semiconductor chip.
[0023] The silicone resin (A1) is preferably liquid at 25°C. In this case, the viscosity of the encapsulating resin composition is particularly easy to adjust to a suitable viscosity for molding. In addition, even if the encapsulating resin composition does not contain a solvent, it is easy to prepare the composition to have a suitable viscosity. The viscosity of the silicone resin (A1) at 25°C is preferably, for example, 1000 mPa·s or less.
[0024] The content of the silicone resin (A1) relative to the total amount of the epoxy resin (A) is preferably 0.1% by mass or more and 15.0% by mass or less. In this case, it can contribute to lowering the viscosity of the encapsulating resin composition and improving the fracture toughness K1c. The content of the silicone resin (A1) is more preferably 0.5% by mass or more and 12.0% by mass or less, and even more preferably 1.0% by mass or more and 10.0% by mass or less.
[0025] [Bisphenol type epoxy resin (A2)] The epoxy resin (A) preferably further contains a bisphenol-type epoxy resin (A2). That is, the encapsulating resin composition preferably further contains a bisphenol-type epoxy resin (A2). In this case, the encapsulating resin composition can be provided with thermosetting properties.
[0026] The bisphenol type epoxy resin (A2) contains at least one selected from the group consisting of, for example, bisphenol A type epoxy resin, bisphenol type epoxy resin, bisphenol S type epoxy resin, and derivatives of these resins. The bisphenol type epoxy resin (A2) particularly preferably contains bisphenol F type epoxy resin. In this case, better thermosetting properties can be imparted to the encapsulating resin composition. The bisphenol F type epoxy resin is a compound in which two phenol skeletons are bonded via one ethylene chain. The bisphenol F type epoxy resin may have a substituent in the phenol skeleton.
[0027] The viscosity of the bisphenol type epoxy resin (A2) at 25° C. is preferably, for example, 1000 mPa·s or more and 4000 mPa·s or less.
[0028] [Aromatic amino epoxy resin (A3)] The epoxy resin (A) preferably further contains an aromatic aminoepoxy resin (A3). That is, the encapsulating resin composition preferably further contains an aromatic aminoepoxy resin (A3). In this case, the encapsulating resin composition can be imparted with better thermosetting properties while maintaining the storage stability of the encapsulating resin composition.
[0029] The aromatic aminoepoxy resin (A3) preferably has an aromatic ring, an amino group bonded to the aromatic ring, and three or more epoxy groups in one molecule, i.e., the aromatic aminoepoxy resin (A3) is preferably trifunctional or higher.
[0030] The aromatic aminoepoxy resin (A3) preferably has an aromatic ring, an amino group bonded to the aromatic ring, an epoxy group bonded to the amino group, and an epoxy group bonded to a position other than that of the amino group bonded to the aromatic ring. That is, when the aromatic aminoepoxy resin (A3) has three or more epoxy groups, it is preferred that at least one of them is bonded to the amino group bonded to the aromatic ring.
[0031] Specific examples of the aromatic aminoepoxy resin (A3) include N,N-diglycidyl-p-glycidyloxyaniline, etc. The aromatic aminoepoxy resin (A3) is not limited to the above-mentioned compounds.
[0032] The viscosity of the aromatic aminoepoxy resin (A3) at 25° C. is preferably 400 mPa·s or more and 800 mPa·s or less.
[0033] The epoxy resin (A) preferably further contains at least one of a bisphenol type epoxy resin (A2) and an aromatic amino epoxy resin (A3). The encapsulating resin composition more preferably contains both the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3). In this case, it is easy to proceed with a moderate curing reaction of the components in the encapsulating resin composition, and therefore it is easy to seal the gap between the substrate and the semiconductor chip with the encapsulant made from the encapsulating resin composition. When the encapsulating resin composition contains the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3), it is preferable that the mass ratio of the total amount of the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3) to the epoxy resin (A) is 85 mass% or more and 95 mass% or less.
[0034] When the encapsulating resin composition contains the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3), the total content of the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3) relative to the total amount of the encapsulating resin composition is preferably 30% by mass or more and 50% by mass or less, more preferably 35% by mass or more and 45% by mass or less, and even more preferably 30% by mass or more and 40% by mass or less. Within this range, the fluidity of the encapsulating resin composition is more easily maintained and the gap between the substrate and the semiconductor chip can be filled well, so that the gap between the substrate and the semiconductor chip can be sufficiently sealed.
[0035] In addition, the components that can be contained in the epoxy resin (A) in the encapsulating resin composition are not limited to those described above, and the composition may contain a resin having an epoxy group other than those described above.
[0036] [Phosphoric acid (B)] The encapsulating resin composition contains phosphoric acid (B). The phosphoric acid (B) has a structure represented by the following formula (1).
[0037] [ka]
[0038] When the encapsulating resin composition contains phosphoric acid (B), it can promote the effect of improving the dispersibility in the encapsulating resin composition by the phosphoric acid polyester (C) described later. It is preferable that the phosphoric acid (B) is mixed with the phosphoric acid polyester (C) to prepare a mixture, and the mixture is blended in the encapsulating resin composition.
[0039] [Phosphate polyester (C)] The encapsulating resin composition contains a phosphate polyester (C). When the encapsulating resin composition contains the phosphate polyester (C), the dispersibility of the components in the encapsulating resin composition is easily increased. Therefore, even if the encapsulating resin composition contains a silicone resin (A1) that is a compound containing silicon, the viscosity of the encapsulating resin composition is unlikely to increase excessively, and good fluidity can be ensured. Furthermore, the effect of reducing the CTE of the cured product produced from the encapsulating resin composition is unlikely to be hindered. In addition, since the encapsulating resin composition contains phosphoric acid (B) and the phosphate polyester (C), the dispersibility is unlikely to decrease even if the proportion of the inorganic filler (filler) is increased. Therefore, the proportion of the filler in the encapsulating resin composition can be easily increased, and it is easier to achieve a reduction in the CTE of the cured product produced from the encapsulating resin composition.
[0040] The phosphate polyester (C) may have a structure represented by the following formula (2).
[0041] [ka]
[0042] In formula (2), R1, R2, and R3 are, for example, each independently a substituent selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group. R1, R2, and R3 may each independently be a long chain or a branched chain. At least one of R1, R2, and R3 may be a hydrogen atom. That is, the phosphoric acid polyester (C) is a compound in which at least two hydrogen atoms in the formula (1) of the phosphoric acid (B) are each independently substituted with R1, R2, and R3.
[0043] The substituents R1, R2, and R3 may each contain a phosphorus atom, and the phosphate polyester (C) may be, for example, a compound derived from polyphosphoric acid represented by the following formula (3). That is, the phosphate polyester (C) may have two or more phosphorus atoms in one molecule.
[0044] [ka]
[0045] In formula (3), n is 2 or more. When the phosphoric acid polyester (C) is derived from formula (3), at least two of the hydrogen atoms in formula (3) may be substituted with a group selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group. The phosphoric acid polyester (C) may have a hydroxyl group at the terminal. When n=1, it corresponds to phosphoric acid (B) represented by formula (1).
[0046] The phosphate polyester (C) is not limited to the above, and may include, for example, a reaction product obtained by reacting an appropriate alkyl ether, polyalkylene glycol monoalkyl ether, or the like with a phosphate esterifying agent.
[0047] Specific examples of the phosphate polyester (C) include phosphate polyesters that may be included in the BYK-W series (e.g., BYK-W9010, etc.) and DISPERBYK series (e.g., DISPERBYK-111, etc.) manufactured by BYK-Chemie Japan Co., Ltd.
[0048] In the encapsulating resin composition, the mass proportion of the phosphate polyester (C) is preferably more than 0 mass% and less than 100 mass%, more preferably 0.01 mass% or more and 90 mass% or less, even more preferably 0.02 mass% or more and 50 mass% or less, and particularly preferably 0.05 mass% or more and less than 10 mass%.
[0049] When the encapsulating resin composition contains silica (E1), the total mass ratio of phosphoric acid (B) and phosphate polyester (C) to silica (E1) is preferably 0.05 mass% or more and 1.0 mass% or less. In this case, the CTE of the cured product of the encapsulating resin composition can be further reduced. The mass ratio of the phosphate polyester (C) is more preferably 0.1 mass% or more and 0.5 mass% or less, and even more preferably 0.2 mass% or more and 0.4 mass% or less. In this case, the encapsulating resin composition can be given better fluidity, which makes it easier to fill the encapsulating resin composition into gaps.
[0050] In the encapsulating resin composition, the total mass ratio of the phosphoric acid (B) and the phosphate polyester (C) to the silicone resin (A1) is more preferably 30 mass% or more and 70 mass% or less, and even more preferably 40 mass% or more and 60 mass% or less.
[0051] [Curing agent (D)] The encapsulating resin composition preferably contains a curing aid (D). In this case, it can contribute to the storage stability of the encapsulating resin composition. In addition, in this case, when the encapsulating resin composition is cured, the speed of the curing reaction can be controlled. The curing aid (D) includes a curing accelerator. The curing aid (D) has a function of promoting the progress of the reaction of the curable components in the encapsulating resin composition. In this embodiment, it can gently promote the progress of the curing reaction of the silicone resin (A1) in the encapsulating resin composition. In addition, when the encapsulating resin composition contains curable components such as the bisphenol type epoxy resin (A2) and the aromatic amino epoxy resin (A3), it can also promote the curing of these components. Particularly in this embodiment, when the epoxy resin (A) in the encapsulating resin composition is cured, the curing aid (D) can suppress the curing reaction from proceeding excessively. That is, the curing aid (D) is unlikely to excessively increase the reactivity of the curing of the encapsulating resin composition, and can proceed with the curing at a good curing speed. Therefore, even if the encapsulating resin composition begins to harden due to a rise in temperature during molding, etc., the hardening is unlikely to progress rapidly, so that the fluidity is unlikely to be lost during molding, and therefore the encapsulating resin composition can be hardened after being sufficiently filled.
[0052] The curing aid (D) preferably contains a chelate compound (D1). In this case, the metal atom in the chelate compound (D1) can coordinate with the oxygen atom in the epoxy resin (A), and therefore, excessive thermosetting reaction of the epoxy resin (A) in the encapsulating resin composition can be suppressed. This can further improve the storage stability of the encapsulating resin composition. In addition, in this case, an excessive increase in the viscosity of the encapsulating resin composition can also be suppressed. Therefore, the fluidity of the encapsulating resin composition can be better maintained.
[0053] The chelate compound (D1) contains at least one compound selected from the group consisting of aluminum acetylacetonate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium acetoacetate, zirconium ethylacetoacetate, and zirconium tetraacetylacetonate. The chelate compound (D1) preferably contains aluminum acetylacetonate.
[0054] When the curing aid (D) is contained, the mass ratio of the curing aid (D) to the epoxy resin (A) is preferably 0.01 mass% or more and 2.0 mass% or less, more preferably 0.03 mass% or more and 1.5 mass% or less, and even more preferably 0.1 mass% or more and 1.0 mass% or less. Within this range, the curability of the epoxy resin (A) in the encapsulating resin composition can be improved, and even if the chip size is increased, the gap between the substrate and the semiconductor chip can be sufficiently sealed with the cured product of the encapsulating resin composition.
[0055] The content of the chelate compound (D1) relative to the curing auxiliary (D) is preferably from 20% by mass to 100% by mass, more preferably from 30% by mass to 90% by mass, and even more preferably from 50% by mass to 70% by mass.
[0056] [Inorganic filler (E)] The encapsulating resin composition preferably contains an inorganic filler (E). The inorganic filler (E) can contribute to a decrease in the linear expansion coefficient of the cured product produced from the encapsulating resin composition. In addition, in this embodiment, since the encapsulating resin composition contains phosphoric acid (B) and phosphoric acid polyester (C), even if the encapsulating resin composition contains the inorganic filler (E), the dispersibility of the encapsulating resin composition is unlikely to decrease. Therefore, the viscosity of the encapsulating resin composition is unlikely to increase excessively, the fluidity can be maintained, and the thixotropy is unlikely to deteriorate. As a result, even if the content of the inorganic filler (E) is increased, the fluidity of the encapsulating resin composition is unlikely to deteriorate, and the linear expansion coefficient of the encapsulating resin composition can be reduced.
[0057] The inorganic filler (E) preferably contains silica (E1), and it is also preferable that at least a part of the silica (E1) is surface-treated with a coupling agent. In this case, the silica (E1) can be easily compatible with the silicone resin (A1), which can further contribute to improving the dispersibility of the encapsulating resin composition. The coupling agent is, for example, a silane coupling agent. Examples of the silane coupling agent include compounds having at least one functional group selected from the group consisting of an epoxy group, an amino group, a (meth)acryloyl group, and a phenyl group. The silane coupling agent is preferably a silane coupling agent having a phenyl group. That is, it is preferable that at least a part of the silica (E1) is surface-treated with a silane coupling agent having a phenyl group. In this case, the silica (E1) can be particularly easily compatible with the silicone resin (A1) in the encapsulating resin composition, which can further improve the dispersibility of the encapsulating resin composition.
[0058] When the inorganic filler (E) contains silica (E1), the silica (E1) preferably contains a first silica filler (E11) and a second silica filler (E12) having an average particle size different from that of the first silica filler (E11). In the present disclosure, the "average particle size" is a volume average diameter. The volume average diameter is calculated from a particle size distribution obtained by measuring by a laser diffraction / scattering method. The particle size distribution can be measured, for example, by a laser diffraction particle size distribution measuring device, and an example of the laser diffraction particle size distribution measuring device can be the LA-960 series manufactured by Horiba, Ltd.
[0059] The average particle size of the first silica filler (E11) is preferably 0.1 μm or more and 1.5 μm or less, and in this case, the standard deviation in the particle size distribution of the first silica filler (E11) is preferably 0.01 or more and less than 1.0. The average particle size of the second silica filler (E12) is preferably 10% or more and 50% or less of the average particle size of the first silica filler (E11), and the standard deviation in the particle size distribution of the second silica filler (E12) is preferably 0.01 or more and less than 1.0. Here, the "standard deviation in the particle size distribution" in the present disclosure is an index showing the width or narrowness of the particle size distribution. The standard deviation in the particle size distribution can be used to determine whether the particle size of the particles is uniform or not. The standard deviation in the particle size distribution can be calculated as follows. As with the above average particle size (volume average diameter), the standard deviation can be calculated from the particle size data of each particle and the average particle size in the particle size distribution obtained by measuring using a laser diffraction / scattering method. When the silica particles in each of the first silica filler (E11) and the second silica filler (E12) of the silica (E1) in the encapsulating resin composition have a standard deviation in particle size distribution of 0.01 or more and less than 1.0, the viscosity of the encapsulating resin composition can be further reduced. This ensures the flowability of the encapsulating resin composition. Therefore, when the encapsulating resin composition is used to seal the gap between the substrate and the semiconductor element, it is possible to achieve better moldability.
[0060] The average particle size of the first silica filler (E11) is preferably 0.1 μm or more and 1.0 μm or less. The standard deviation in the particle size distribution of the first silica filler (E11) is preferably 0.01 or more and 0.6 or less, more preferably 0.02 or more and 0.40 or less, even more preferably 0.02 or more and 0.36 or less, and particularly preferably 0.05 or more and 0.36 or less. The average particle size of the second silica filler (E12) is not particularly limited as long as it satisfies the above, but the average particle size of the second silica filler (E12) can be, for example, 0.01 μm or more and 0.75 μm or less. The standard deviation in the particle size distribution of the second silica filler (E12) is preferably 0.01 or more and less than 0.10, more preferably 0.02 or more and 0.08 or less, even more preferably 0.03 or more and 0.08 or less, and particularly preferably 0.04 or more and 0.06 or less.
[0061] It is preferable that the first silica filler (E11) and the second silica filler (E12) are both wet silica. Wet silica is amorphous silica synthesized in a liquid, and for example, wet silica can be prepared by at least one method selected from the group consisting of a precipitation method and a sol-gel method. It is particularly preferable that the wet silica is prepared by a sol-gel method. In this case, the average particle size of the wet silica particles can be kept relatively small, such as 0.1 μm or more and 1.5 μm or less, and the particle size distribution can be made less likely to vary. That is, in this case, the particle size of the first silica filler (E11) and the second silica filler (E12) can be easily made uniform. The sol-gel method is a synthesis method in which a solid substance is obtained from a sol state in which fine particles such as colloids are dispersed in a solution, via a gel state in which fluidity is lost, and an appropriate synthesis method may be adopted. The fact that the first silica filler (E11) of the present disclosure is produced by the sol-gel method can be confirmed by cutting an appropriate particle of the first silica filler (E11) and observing the cross section. Specifically, for example, the cured product of the encapsulating resin composition is cut, the cut surface is observed with an electron microscope, etc., and the particle size of silica on the cut surface is measured, so that it can be determined that it is produced by the sol-gel method. It can also be confirmed that the second silica filler (E12) and the third silica filler (E13) described later are produced by the sol-gel method in the same manner as the first silica filler (E11).
[0062] It is also preferred that the silica (E1) further contains a third silica filler (E13) whose average particle size is different from both the first silica filler (E11) and the second silica filler (E12). That is, it is also preferred that the encapsulating resin composition contains the first silica filler (E11), the second silica filler (E12), and the third silica filler (E13). When the silica (E1) contains the third silica filler (E13), the average particle size of the third silica filler (E13) is not particularly limited as long as it is smaller than the average particle size of the second silica filler (E12). The standard deviation in the particle size distribution of the third silica filler (E13) is preferably 0.01 or more and less than 0.10, more preferably 0.02 or more and 0.09 or less, even more preferably 0.03 or more and 0.08 or less, and particularly preferably 0.04 or more and 0.06 or less. When the encapsulating resin composition contains the third silica filler (E13), the encapsulating resin composition can have a lower fluidity, and can have good thixotropy even if the fluidity of the encapsulating resin composition is lowered. The mass ratio of the third silica filler (E13) is preferably 5% by mass or more and 40% by mass or less based on the total amount of silica (E1). If the mass ratio of the third silica filler (E13) to the total amount of silica (E1) is 5% by mass or more, the thixotropy can be made better, and if it is 40% by mass or less, good fluidity can be maintained.
[0063] When the silica (E1) contains a third silica filler (E13), the third silica (E13) is also preferably a wet silica. In this case, the third silica filler (E13) is also preferably a wet silica produced by a sol-gel method. In this case, it is easy to adjust each of the first silica filler (E11), the second silica filler (E12), and the third silica filler (E13) to be silica particles with a uniform particle size.
[0064] The first silica filler (E11) may be surface-treated with a coupling agent. The surface treatment of the silica filler can be performed, for example, by reacting wet silica produced by a sol-gel method with a coupling agent (e.g., a silane coupling agent). The second silica filler (E12) and the third silica filler (E13) may also be surface-treated with a coupling agent.
[0065] The mass ratio of the first silica filler (E11) to the second silica filler (E12) in the silica (E1) is preferably within a range of 60:40 to 98:2. When the silica (E1) further contains a third silica filler (E13), the mass ratio of the first silica filler (E11), the second silica filler (E12) and the third silica filler (E13) is preferably within a range of 60:30:10 to 90:8:2.
[0066] When the inorganic filler (E) is contained, the content of the inorganic filler (E) relative to the total amount of the encapsulating resin composition is preferably 50% by mass or more and 75% by mass or less. In this case, it is possible to further reduce the CTE of the encapsulating resin composition. In this embodiment, even if the proportion of the inorganic filler is relatively high, the fluidity of the encapsulating resin composition can be particularly well maintained. Therefore, it is possible to prevent the encapsulating resin composition from being left unfilled in gaps. The content of the inorganic filler (E) is more preferably 50% by mass or more and 70% by mass or less, and even more preferably 55% by mass or more and 65% by mass or less.
[0067] The inorganic filler (E) may contain a filler other than silica as long as the effects of the present disclosure are not impaired.
[0068] [Other ingredients] The encapsulating resin composition may contain components other than those described above, as long as the effects of the present disclosure are not impaired. For example, the encapsulating resin composition may contain a resin component other than those described above.
[0069] The encapsulating resin composition may contain appropriate additives, such as a curing agent, a flux, a viscosity modifier, a surface modifier, a silane coupling agent, a defoaming agent, a leveling agent, a stress reducing agent, and a pigment.
[0070] For example, it is preferable that the encapsulating resin composition contains a silane coupling agent. In this case, the compatibility between the silicone resin (A1) and the silane coupling agent in the encapsulating resin composition is improved, and the dispersibility of the encapsulating resin composition is easily improved. In addition, even when the encapsulating resin composition contains silica (E1), the dispersibility of the encapsulating resin composition is easily improved. As the silane coupling agent, an appropriate coupling agent can be adopted, and it may be, for example, an epoxy silane coupling agent such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0071] It is preferable that the encapsulating resin composition does not contain an organic solvent, or the content of the organic solvent is 0.5 mass % or less.
[0072] The encapsulating resin composition can be obtained, for example, by blending the above-mentioned components and adding appropriate additives as necessary. Specifically, the encapsulating resin composition can be prepared, for example, by the following method.
[0073] First, the components that can be contained in the encapsulating resin composition described above are mixed together or sequentially to obtain a mixture. The mixture is stirred and mixed while being heated or cooled as necessary.
[0074] Next, additives are added to the mixture as necessary, and the mixture is stirred again while being heated or cooled as necessary until it is uniformly dispersed. This allows the encapsulating resin composition to be obtained. For stirring the mixture, for example, a disperser, a planetary mixer, a ball mill, a three-roll mill, a bead mill, and the like can be used in appropriate combination as necessary.
[0075] The viscosity of the encapsulating resin composition at 25°C is preferably less than 35 Pa·s. In this case, when molding the encapsulating resin composition, the coating workability by jet dispensing and the discharge stability can be improved. In addition, in this case, good filling properties can be achieved under mounting components such as semiconductor chips. The viscosity of the encapsulating resin composition at 25°C is more preferably 25 Pa·s or less, and even more preferably 20 Pa·s or less. The lower limit of the viscosity of the encapsulating resin composition at 25°C is not particularly limited, but is, for example, 2 Pa·s or more.
[0076] The encapsulating resin composition can be cured, for example, by heating. Heating conditions, such as heating temperature, heating time, and maximum heating temperature, may be appropriately adjusted depending on the type of the curable component (A) and the type of the curing agent.
[0077] The glass transition temperature Tg of the cured product of the encapsulating resin composition is preferably 80° C. or higher. The glass transition temperature Tg is also preferably lower than 180° C. If the glass transition temperature Tg is 80° C. or higher, the cured product of the encapsulating resin composition can have heat resistance. The glass transition temperature Tg is more preferably 90° C. or higher and 170° C. or lower. The glass transition temperature can be measured, for example, by TMA (Thermomechanical Analysis).
[0078] The linear expansion coefficient (CTE) of the cured product of the encapsulating resin composition at a glass transition temperature Tg or lower is preferably 20 ppm / °C or higher and 40 ppm / °C or lower, more preferably 30 ppm / °C or lower, and even more preferably 25 ppm / °C or lower. In this case, the encapsulating resin composition and the cured product of the encapsulating resin composition are less likely to warp due to heating. Therefore, the cured product of the encapsulating resin composition is less likely to crack. The linear expansion coefficient of the cured product of the encapsulating resin composition is obtained by calculating the slope of the tangent based on the dimensional change at a temperature below Tg and the dimensional change at any temperature above Tg from the Tg obtained by the measurement using TMA.
[0079] The storage modulus of the cured product of the encapsulating resin composition at 25°C is preferably 6.0 GPa or more and 12.0 GPa or less, more preferably 6.5 GPa or more and 10 GPa or less. In this case, the dimensional change of the cured product of the encapsulating resin composition due to heating is unlikely to occur. This makes it possible to make the cured product of the encapsulating resin composition less susceptible to cracks. The storage modulus of the cured product of the encapsulating resin composition is obtained by measuring with a DMA device in accordance with JIS K6911.
[0080] The fracture toughness K1c of the cured encapsulating resin composition at 25°C is 2.0 MPa m 1 / 2 It is preferable that the cured product of the encapsulating resin composition has a fracture toughness K1c of 2.5 MPa m or more. In this case, it is possible to further reduce the occurrence of cracks in the cured product of the encapsulating resin composition. This can improve the reliability of a semiconductor device provided with an encapsulant made of a cured product of the encapsulating resin composition. The fracture toughness K1c of the cured product is 2.5 MPa m 1 / 2 More preferably, it is 3.0 MPa m 1 / 2 The fracture toughness K1c can be measured in accordance with JIS R1607. Specifically, it can be measured by the method described in the examples below.
[0081] As described above, the encapsulating resin composition of the present embodiment can be suitably used as an underfill material. The encapsulating resin composition can be particularly suitably used as a post-supply type underfill material in flip chip mounting.
[0082] An example of a semiconductor device 1 according to this embodiment is shown in Fig. 1. The semiconductor device 1 includes a base material 2 supporting a mounting component 3 such as a semiconductor chip, the mounting component 3 mounted face-down on the base material 2, and an encapsulant 4 sealing a gap between the base material 2 and the mounting component 3. The encapsulant 4 is made of a cured product of the liquid encapsulating resin composition described above.
[0083] The semiconductor device 1 and the manufacturing method thereof will now be described in detail.
[0084] The semiconductor device 1 includes a base material 2 having conductor wiring 21, a mounting component 3 such as a semiconductor chip having bump electrodes 33 and mounted on the base material 2 by bonding the bump electrodes 33 to the conductor wiring, and an encapsulant 4 that covers the bump electrodes 33. The encapsulant 4 is a cured product of the encapsulating resin composition described above.
[0085] The substrate 2 is, for example, a mother substrate, a package substrate, or an interposer substrate. For example, the substrate 2 includes an insulating substrate made of glass epoxy, polyimide, polyester, ceramic, or the like, and conductor wiring 21 made of a conductor such as copper formed on the surface of the insulating substrate. The conductor wiring 21 includes, for example, an electrode pad.
[0086] The mounting component 3 is, for example, a semiconductor chip. The semiconductor chip is, for example, a flip-chip type chip such as a BGA (ball grid array), an LGA (land grid array), or a CSP (chip size package). The semiconductor chip may be a PoP (package on package) type chip.
[0087] The mounting component 3 may include a plurality of bump electrodes 33. The bump electrodes 33 include solder. For example, as shown in Fig. 1, the bump electrodes 33 include a pillar 31 and a solder bump 32 provided at the tip of the pillar 31. The solder bump 32 is made of solder, and therefore the bump electrodes 33 include solder. The pillars 31 are made of copper, for example.
[0088] The melting point of the solder (for example, the solder in the solder bump 32) of the bump electrode 33 is not particularly limited, but may be a temperature at which it can melt at or below the mounting temperature (for example, 220 to 260°C) when mounting a mounting component 3 such as a semiconductor chip. The composition of the solder is not particularly limited and may be an appropriate composition, for example, Sn-Ag solder and Sn-Ag-Cu solder. The structure of the bump electrode 33 with solder is not limited to the above, and for example, the bump electrode 33 may have only a spherical solder bump 32 (solder ball). In other words, the bump electrode 33 does not need to have a pillar.
[0089] 1, the sealing material 4 fills the entire gap between the base material 2 and the mounted component 3. As a result, the sealing material 4 covers the entire bump electrode 33, and also covers the joint between the bump electrode 33 and the conductor wiring 21. In other words, this sealing material 4 is a so-called underfill.
[0090] An example of a manufacturing method for the semiconductor device 1 will be described below, but the manufacturing method for the semiconductor device 1 is not limited to the method described below, and it is sufficient that the semiconductor device 1 can cover and seal the gap between the base material 2 and the mounting component 3 with the sealing resin composition described above.
[0091] First, the base material 2 having the conductor wiring 21 and the mounting component 3 having the bump electrodes 33 are prepared. The mounting component 3 is placed on the base material 2, and the bump electrodes 33 are placed on the conductor wiring 21.
[0092] Next, the encapsulating resin composition is disposed so as to cover the bump electrode 33, and the encapsulating resin composition and the bump electrode 33 are subjected to a heat treatment, thereby hardening the encapsulating resin composition to produce the encapsulant 4, and electrically connecting the bump electrode 33 and the conductor wiring 21. Here, disposing the encapsulating resin composition is not limited to disposing a solid encapsulating resin composition on the object to be encapsulated (such as the bump electrode 33), but also includes applying a liquid encapsulating resin composition to the object to be encapsulated, and injecting the liquid encapsulating resin composition into the gap between the objects to be encapsulated so as to cover the objects to be encapsulated.
[0093] The above order does not have to be as described above. For example, the mounting component 3 may be disposed on the base material 2, the bump electrode 33 may be disposed on the conductor wiring 21, and then the encapsulating resin composition may be disposed so as to cover the bump electrode 33. Conversely, the encapsulating resin composition may be disposed so as to cover the bump electrode 33, and then the mounting component 3 may be disposed on the base material 2, and the bump electrode 33 may be disposed on the conductor wiring 21. Furthermore, as long as the encapsulating resin composition can be disposed so as to cover the bump electrode 33 as a result during the manufacturing process, the encapsulating resin composition may be disposed at any time and at any position on the mounting component 3 and the base material 2.
[0094] Specifically, when preparing the encapsulant 4 shown in FIG. 1, for example, first, an encapsulating resin composition is placed on the substrate 2, and then the mounting component 3 is placed on the substrate 2 such that the encapsulating resin composition is interposed between the substrate 2 and the mounting component 3 and the bump electrode 33 is placed on the conductor wiring 21. In this way, the encapsulating resin composition is placed so as to cover the bump electrode 33. Alternatively, first, the mounting component 3 is placed on the substrate 2 such that the bump electrode 33 is placed on the conductor wiring 21, and then the encapsulating resin composition is supplied between the substrate 2 and the mounting component 3, so that the encapsulating resin composition is interposed between the substrate 2 and the mounting component 3 and the encapsulating resin composition is placed so as to cover the bump electrode 33.
[0095] 1, for example, first, an encapsulating resin composition is placed on a mounting component 3 so as to cover the bump electrodes 33. Then, the mounting component 3 is placed on a substrate 2 so that the encapsulating resin composition is interposed between the substrate 2 and the mounting component 3 and the bump electrodes 33 are placed on the conductor wiring 21. In this way, the encapsulating resin composition is placed so as to cover the bump electrodes 33.
[0096] When the encapsulating resin composition is disposed on the substrate 2 or on the mounted component 3, the encapsulating resin composition is disposed by, for example, a method using a dispenser, a screen printing method, an inkjet method, a dipping method, or the like.
[0097] The heat treatment of the encapsulating resin composition and the bump electrode 33 is performed using a heating furnace such as a reflow furnace. The heat treatment may be performed by an appropriate method using equipment other than a reflow furnace. When the encapsulating resin composition and the bump electrode 33 are subjected to the heat treatment, the solder in the bump electrode 33 melts, electrically connecting the bump electrode 33 and the conductor wiring 21, and the encapsulating resin composition hardens to produce the encapsulant 4. This results in the semiconductor device 1. The conditions of the heat treatment may be appropriately set according to the composition of the encapsulating resin composition. In the heat treatment, the maximum heating temperature is preferably, for example, 220°C or higher and 260°C or lower. Although an example of the heat treatment has been described above, the present invention is not limited to the above, and the maximum heating temperature may also be appropriately set according to the composition of the encapsulating resin composition. EXAMPLES
[0098] Specific examples of the present disclosure will be presented below, but the present disclosure is not limited to the examples.
[0099] 1. Preparation of resin composition [Examples 1 to 5 and Comparative Examples 1 to 5] The components shown in Table 1 below were charged into a mixer in the mixing ratios (parts by mass) shown in Table 1, stirred and mixed, and uniformly dispersed using a three-roll mill to obtain a resin composition. Details of the components shown in Table 1 are as follows. (Epoxy resin) · Epoxy modified silicone resin 1: Momentive Performance Materials Japan, LLC, product name TSL9906, silicone resin with epoxy modification at both ends. · Epoxy modified silicone resin 2: ADEKA Corporation, product name EP-3400L, silicone resin with epoxy modification at both ends. Bisphenol type epoxy resin: Bisphenol F type epoxy resin (manufactured by Tohto Kasei Co., Ltd., product name YDF8170. Epoxy equivalent 175 eq. / g). Aromatic amino epoxy resin: Product name 636 manufactured by JRR Corporation. (Mixture of phosphoric acid and polyester phosphate) Mixture of phosphoric acid and phosphate polyester: BYK Japan Co., Ltd. Product name BYK-W 9010 (composition: phosphate polyester content 90% by weight or more and less than 100% by weight, phosphoric acid content 1% by weight or more and less than 10% by weight). (hardening agent) Amine hardener: Product name: Kayabard AA, manufactured by Nippon Kayaku Co., Ltd. Amine equivalent: 65eq. / g. (Curing agent) Chelate compound 1: Manufactured by Kawaken Fine Chemicals Co., Ltd. Product name: Aluminum Chelate A (W). Metal chelate hardening assistant. Aluminum tris(acetylacetonate). Chelate compound 2: Matsumoto Fine Chemicals Co., Ltd. Product name: TC-100. Titanium tris(acetylacetonate). (Inorganic filler) Silica 1: Silica prepared by the sol-gel method and surface-treated with a silane coupling agent having a phenyl group (average particle size 1.0 μm. Standard deviation in particle size distribution is 0.04 to 0.5). Silica 2: Silica prepared by the sol-gel method and surface-treated with a silane coupling agent having a phenyl group (average particle size: 0.3 μm. Standard deviation in particle size distribution is 0.04 to 0.5). Silica 3: Silica prepared by the sol-gel method and surface-treated with a silane coupling agent having a phenyl group (average particle size: 0.1 μm. Standard deviation in particle size distribution is 0.04 to 0.5). Silica 4: Silica prepared by the sol-gel method and surface-treated with phenylsilane (average particle size: 50 nm, standard deviation in particle size distribution: 0.04 to 0.5). · Silica 5: Silica prepared by the sol-gel method and surface-treated with phenylsilane (average particle size 10 nm, standard deviation in particle size distribution is 0.04 to 0.5). (Additives) Coupling agent: Epoxy silane (silane coupling agent. Product name KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.). Colorant: Carbon black (product name MA100, manufactured by jER Co., Ltd.).
[0100] 2. Evaluation 2.1.Viscosity The viscosity of the resin composition prepared in 1 above was measured using a BM type viscometer (Model No. TVB-10, manufactured by Toki Sangyo Co., Ltd.) at a temperature of 25°C and a rotation speed of 5 rpm using rotor No. 6. The measurement results were evaluated according to the following criteria. A: Viscosity is less than 25 Pa·s. B: Viscosity is 25 Pa·s or more and 35 Pa·s or less. C: Viscosity is 35 Pa· or more.
[0101] 2.2. Thixotropy Index The viscosity at 25°C was measured in the same manner as in 2.1 above. Next, the rotation speed of 5 rpm was changed to about one-tenth the original speed of 5 rpm, and the viscosity was measured. The viscosity change rate (viscosity at low speed / viscosity at high speed) was calculated from the viscosity before the rotation speed was changed (at low speed) and the viscosity after the rotation speed was changed (at high speed), and this was taken as the thixotropic index (TI). Based on the obtained thixotropic index, the following criteria were used for evaluation. A: TI is greater than or equal to 0.7 and less than 1.5. B: TI is greater than or equal to 1.5 and less than 2.5. C:TI is 2.5 or more.
[0102] 2.3.Liquidity Two flat glass plates were placed on a heatable stage with a gap of 10 μm between them, and the temperature of the stage was set to 90° C. to heat the two glass plates. After the temperature of the glass plates reached 90° C., the resin composition prepared in 1 above was injected into the 10 μm gap and allowed to flow through the gap by utilizing capillary action. The time it took for the resin composition to travel a distance of 30 mm from the start of injection was measured. Based on the results obtained by the measurement, evaluation was performed according to the following criteria. A: It takes less than 300 seconds to move 30 mm. B: The time required to advance 30 mm is greater than or equal to 300 seconds and less than 500 seconds. C: The time required to advance 30 mm is 500 seconds or more.
[0103] 2.4. Glass transition temperature (DMA test) The resin composition prepared in 1 above was applied onto a substrate and heated at 100°C for 2 hours, and then heated further to 150°C for 2 hours to cure the resin composition, thereby obtaining a cured product of the resin composition.
[0104] The cured product was then measured at a temperature rise rate of 5°C / min from room temperature -60°C to 280°C using a dynamic viscoelasticity measurement (DMA) device (Hitachi High-Tech Science Corporation, Model No. DMA7100), and the glass transition temperature of the cured product was obtained from the results. The obtained glass transition temperature values (°C) are shown in Table 1.
[0105] 2.5. Linear expansion coefficient (TMA test) A cured product of the resin composition prepared under the same conditions as in 2.4. above was heated from -60°C to 280°C using a thermomechanical analyzer (TMA) (Hitachi High-Tech Science Corporation, Model No. TMA7000) under conditions of a load of 1g and a heating rate of 5°C / min, and the dimensional change was measured. From the results obtained, the linear expansion coefficient was calculated and evaluated according to the following criteria. A: Less than 35 ppm / ℃. C: 35 ppm / ℃ or more.
[0106] 2.6. Elastic modulus (storage modulus) The elastic modulus of the cured resin composition prepared under the same conditions as in 2.4 above was measured at each temperature using a DMA device under the same conditions as in 2.4. From the results obtained, the storage modulus was calculated and evaluated according to the following criteria. A: 6.5 GPa or more but less than 12.0 GPa. C: 12.0 GPa or more.
[0107] 2.7. Fracture toughness (K1c test) Test pieces (length L: 50 mm, width W: 10 mm, thickness B: 5 mm) for test measurements were prepared from the cured product of the resin composition prepared under the same conditions as in 2.4. above, and a pre-crack with a crack length a: 4 mm was made in the test piece. In accordance with JIS R1607 (room temperature fracture toughness test method for fine ceramics), pressure was applied to the test piece at a rate of 10 mm / min, and the test force until fracture was measured. From the measurement results obtained, the K1c value was calculated based on the following formulas (1) and (2), and the obtained values are shown in Table 1. It can be evaluated that the higher the fracture toughness K1c value, the higher the resistance to cracking.
[0108]
number
[0109]
number
[0110] In the above formulas (1) and (2), Pα is the maximum load [kgf] until the test piece breaks, S is the distance between the three-point bending supports [mm], B is the thickness of the test piece [mm], W is the width of the test piece [mm], and a is the length of the pre-crack [mm].
[0111] [Table 1] [Explanation of symbols]
[0112] 1 Semiconductor device 2 Base material 3. Mounting parts 4. Encapsulating material
Claims
1. An epoxy resin (A), Phosphoric acid (B) and A phosphate polyester (C), The epoxy resin (A) contains a silicone resin (A1) having two or more epoxy groups in one molecule, The epoxy resin (A) further contains one or both of a bisphenol F type epoxy resin (A2) and an aromatic amino epoxy resin (A3). Sealing resin composition.
2. An epoxy resin (A), Phosphoric acid (B) and A phosphate polyester (C), The epoxy resin (A) contains a silicone resin (A1) having two or more epoxy groups in one molecule, Further containing a curing aid (D), The curing aid (D) contains a chelate compound (D1). Sealing resin composition.
3. Further containing a curing aid (D), The curing aid (D) contains a chelate compound (D1). The encapsulating resin composition according to claim 1 .
4. Further containing a mechanical filler (E), The encapsulating resin composition according to claim 1 .
5. The inorganic filler (E) contains silica (E1), At least a part of the silica (E1) is surface-treated with a coupling agent. The encapsulating resin composition according to claim 4 .
6. It is an underfill material. The encapsulating resin composition according to claim 1 .
7. A substrate; A mounting component to be mounted on the base material; a sealant that seals a gap between the base material and the mounted component, The encapsulant is made of a cured product of the encapsulating resin composition according to any one of claims 1 to 6. Semiconductor device.
Citation Information
Patent Citations
Preparation of epoxidized organopolysiloxane, resin additive, and semiconductor-sealing epoxy resin composition
JP1994287306A
Liquid epoxy resin composition for sealing and electronic part device and wafer level chip size package
JP2007023272A
Liquid epoxy resin composition for sealing and sealed semiconductor device
JP2008291189A
Epoxy resin composition, and curable resin composition
JP2011111584A
Sealant for optical semiconductor device and optical semiconductor device produced by using the same
JP2011127011A