Raw material for forming thin film, thin film manufacturing method, and novel scandium compound

A low-melting-point scandium compound with specific structures addresses the inefficiencies of conventional compounds, enabling high-quality thin film production with enhanced productivity in CVD and ALD methods.

JP7573514B2Active Publication Date: 2024-10-25ADEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021512008
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-04
Filing Date
2020-03-27
Publication Date
2024-10-25
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Conventional scandium compounds used in thin film formation for CVD methods have high melting points, making them unsuitable for efficient vaporization and production of high-quality thin films with high productivity.

Method used

A scandium compound with a specific structure, represented by general formulas (1) and (2), is developed to have a low melting point, allowing for easy vaporization and high thermal stability, suitable for CVD and ALD methods.

Benefits of technology

The new scandium compound enables the production of high-quality thin films with higher productivity and suitability for CVD and ALD methods, achieving lower residual carbon content and improved film thickness per cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573514000010
    Figure 0007573514000010
  • Figure 0007573514000011
    Figure 0007573514000011
  • Figure 0007573514000012
    Figure 0007573514000012
Patent Text Reader

Abstract

The present invention provides: a raw material which is for forming a thin film and contains a scandium compound represented by general formula (1) below; a method for producing a thin film using the raw material for forming a thin film; and a novel scandium compound. (In the formula, R1 represents a C1-C4 alkyl group, R2 represents C2-C3 alkyl group, and R3 represents a hydrogen atom or C1-C4 alkyl group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thin film-forming material, a method for producing a thin film using the thin film-forming material, and a novel compound. [Background technology]

[0002] Thin film materials containing scandium exhibit unique electrical properties and are used in a variety of technologies, such as electrode materials for memory elements such as DRAM elements, piezoelectric thin films, doping materials, and fuel cell materials.

[0003] Examples of methods for manufacturing the above-mentioned thin films include sputtering, ion plating, MOD methods such as coating pyrolysis and sol-gel methods, chemical vapor deposition, etc. Among these, chemical vapor deposition (hereinafter sometimes simply referred to as "CVD") methods including ALD (Atomic Layer Deposition) are the most suitable manufacturing processes because they have many advantages such as excellent composition controllability and step coverage, suitability for mass production, and the possibility of hybrid integration.

[0004] As a scandium compound used as a raw material for forming a thin film, various scandium compounds have been conventionally known. For example, Patent Documents 1 and 2 disclose scandium compounds to which a diketone group having a specific structure is bonded. However, the scandium compounds disclosed in Patent Documents 1 and 2 have melting points of 140° C. or higher, and therefore are not fully satisfactory compounds as raw materials for chemical vapor deposition. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] US Publication No. 2009 / 0253270 [Patent Document 2] US Publication No. 2014 / 0084355 Summary of the Invention [Problem to be solved by the invention]

[0006] In a method for forming a thin film by vaporizing a compound, such as a CVD method, the compound (precursor) used as a raw material is required to have a low melting point and be transportable in a liquid state, a low liquid viscosity, a high vapor pressure and easy vaporization, high thermal stability, and high productivity for high-quality thin films. In particular, there has been a strong demand for a compound with a low melting point and be transportable in a liquid state, and for high productivity for high-quality thin films, but there has been no conventional scandium compound that is fully satisfactory in these respects.

[0007] Therefore, an object of the present invention is to provide a thin film forming raw material containing a scandium compound which is capable of producing a high quality thin film with high productivity as compared to conventional scandium compounds and has a low melting point, and a thin film manufacturing method for forming a thin film containing scandium using the raw material. [Means for solving the problem]

[0008] As a result of extensive investigations, the inventors have discovered that the above-mentioned problems can be solved by a thin-film-forming raw material containing a scandium compound having a specific structure, and a method for producing a scandium-atom-containing thin film using the thin-film-forming raw material, and have arrived at the present invention.

[0009] That is, the present invention provides a thin film forming material containing a compound represented by the following general formula (1) and a method for producing a thin film using the material.

[0010] [ka]

[0011] (In the formula, R 1 and R 2 teeth, ethyl represents a group, R 3 is a hydrogen atom Childrepresent.)

[0012] The present invention also provides a compound represented by the following general formula (2):

[0013] [ka]

[0014] (In the formula, R 4 and R 5 teeth, ethyl represents a group, R 6 is a hydrogen atom Child represent.) Effect of the Invention

[0015] According to the present invention, a scandium compound having a low melting point can be obtained, and the compound is suitable as a raw material for forming a thin film in a CVD method. In particular, the scandium compound used in the present invention has an ALD window, and therefore can be suitably used as a raw material for forming a thin film in an ALD method. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic diagram showing an example of a chemical vapor deposition apparatus used in a thin film manufacturing method according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing yet another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. [Figure 4] FIG. 2 is a schematic diagram showing yet another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The thin film forming material of the present invention is a thin film forming material containing the compound represented by the above general formula (1), and is suitable as a precursor for a thin film production method having a vaporization step such as a CVD method, and can also form a thin film using an ALD method.

[0018] In the above general formula (1), R 1 represents an alkyl group having 1 to 4 carbon atoms, R 2 represents an alkyl group having 2 to 3 carbon atoms, R 3 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0019] In the above general formula (1), R 1 and R 3 Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and an isobutyl group. 2 Examples of the alkyl group having 2 to 3 carbon atoms represented by the formula (1) include an ethyl group, an n-propyl group, and an isopropyl group.

[0020] In the above general formula (1), R 1 , R 2 and R 3 is appropriately selected depending on the manufacturing method of the thin film to be applied. When used in a manufacturing method of a thin film having a step of vaporizing a compound, R 1 , R 2 and R 3 It is preferable that the combination of the above is in a liquid state at normal temperature and pressure and has a high vapor pressure. Specifically, the melting point of the compound is lowered, so that R 1 or R 2 is preferably an alkyl group having 2 to 3 carbon atoms, and R 1 or R 2 More preferred is a compound in which R is an ethyl group. 1 and R 2 Compounds in which both are ethyl groups are particularly preferred. 3 is a hydrogen atom. 1and R 2 are both ethyl groups, and R 3 On the other hand, in the case of a thin film manufacturing method using the MOD method that does not involve a vaporization step, the R 1 , R 2 and R 3 can be arbitrarily selected depending on the solubility in the solvent used, the thin film forming reaction, and the like.

[0021] Preferable specific examples of the scandium compound represented by the above general formula (1) include the following compounds No. 1 to No. 30. In the following chemical formulas, "Me" represents a methyl group, "Et" represents an ethyl group, "nPr" represents an n-propyl group, "iPr" represents an isopropyl group, "nBu" represents an n-butyl group, and "tBu" represents a tert-butyl group.

[0022] [ka]

[0023] [ka]

[0024] The compound represented by the above general formula (1) is not particularly limited by its manufacturing method, and is manufactured by applying a well-known reaction. For example, the compound can be obtained by reacting an alkanedione compound having a corresponding structure with an alkane lithium such as butyl lithium, reacting this with scandium chloride, and distilling and purifying the resulting reaction product.

[0025] Examples of the alkanedione compound include 3,5-heptanedione, 3,5-octanedione, 4,6-nonanedione, 2,6-dimethyl-3,5-heptanedione, and 6-methyl-3,5-heptanedione, and it is preferable to use 3,5-heptanedione.

[0026] Next, the thin film forming raw material of the present invention contains the above-mentioned scandium compound as a precursor of the thin film. The form differs depending on the manufacturing process to which the thin film forming raw material is applied. For example, when manufacturing a thin film containing only scandium as a metal, the thin film forming raw material of the present invention does not contain metal compounds and metalloid compounds other than the above-mentioned scandium compound. On the other hand, when manufacturing a thin film containing two or more kinds of metals and / or metalloids, the thin film forming raw material of the present invention can also contain a compound containing a desired metal and / or a compound containing a metalloid (hereinafter, sometimes referred to as "other precursors") in addition to the above-mentioned scandium compound. The thin film forming raw material of the present invention may further contain an organic solvent and / or a nucleophilic reagent, as described below. As described above, the thin film forming raw material of the present invention is particularly useful as a raw material for chemical vapor deposition (hereinafter, sometimes referred to as "raw material for CVD"), since the physical properties of the scandium compound, which is a precursor, are suitable for the CVD method and the ALD method.

[0027] When the thin film forming material of the present invention is a material for chemical vapor deposition, its form is appropriately selected depending on the method of transportation and supply in the CVD method to be used.

[0028] The above-mentioned transport supply method includes a gas transport method in which the CVD raw material is heated and / or depressurized in a container (hereinafter sometimes referred to as a "raw material container") in which the raw material is stored, thereby vaporizing the raw material into a vapor, and the vapor is introduced into a film formation chamber (hereinafter sometimes referred to as a "deposition reaction section") in which a substrate is placed together with a carrier gas such as argon, nitrogen, or helium used as necessary; and a liquid transport method in which the CVD raw material is transported in a liquid or solution state to a vaporization chamber, vaporized in the vaporization chamber by heating and / or depressurizing the vapor, and the vapor is introduced into a film formation chamber. In the case of the gas transport method, the scandium compound represented by the above general formula (1) itself can be used as the CVD raw material. In the case of the liquid transport method, the scandium compound represented by the above general formula (1) itself or a solution in which the compound is dissolved in an organic solvent can be used as the CVD raw material. These CVD raw materials may further contain other precursors, nucleophilic reagents, etc.

[0029] In addition, in the multi-component CVD method, there is a method in which each component of the CVD raw material is vaporized and supplied independently (hereinafter, sometimes referred to as the "single source method"), and a method in which a mixed raw material in which multi-component raw materials are mixed in advance with a desired composition is vaporized and supplied (hereinafter, sometimes referred to as the "cocktail source method"). In the case of the cocktail source method, a mixture of the scandium compound represented by the general formula (1) and other precursors, or a mixed solution in which the mixture is dissolved in an organic solvent, can be used as the CVD raw material. This mixture or mixed solution may further contain a nucleophilic reagent, etc.

[0030] The organic solvent is not particularly limited, and any well-known organic solvent can be used. Examples of the organic solvent include acetates such as ethyl acetate, butyl acetate, and methoxyethyl acetate; ethers such as tetrahydrofuran, tetrahydropyran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, dibutyl ether, and dioxane; ketones such as methyl butyl ketone, methyl isobutyl ketone, ethyl butyl ketone, dipropyl ketone, diisobutyl ketone, methyl amyl ketone, cyclohexanone, and methylcyclohexanone; hexane, cyclohexane, methylcyclohexanone, and methylcyclohexanone; and methylcyclohexanone. Examples of suitable solvents include hydrocarbons such as hexane, dimethylcyclohexane, ethylcyclohexane, heptane, octane, toluene, and xylene; hydrocarbons having a cyano group such as 1-cyanopropane, 1-cyanobutane, 1-cyanohexane, cyanocyclohexane, cyanobenzene, 1,3-dicyanopropane, 1,4-dicyanobutane, 1,6-dicyanohexane, 1,4-dicyanocyclohexane, and 1,4-dicyanobenzene; and pyridine and lutidine. These are used alone or as a mixture of two or more solvents depending on the solubility of the solute, the relationship between the use temperature and the boiling point and the flash point, etc. The CVD raw material (solution state) obtained by dissolving the precursor in the above organic solvent usually contains the entire precursor in an amount of 0.01 to 2.0 mol / L, and preferably contains the entire precursor in an amount of 0.05 to 1.0 mol / L. When the thin-film forming raw material of the present invention does not contain any metal compound or metalloid compound other than the scandium compound represented by general formula (1), the total amount of the precursors means the amount of the scandium compound represented by general formula (1). When the thin-film forming raw material of the present invention contains, in addition to the scandium compound, a compound containing another metal and / or a compound containing a metalloid, the total amount of the precursors means the combined amount of the scandium compound represented by general formula (1) and the other precursors.

[0031] In the case of a multi-component CVD method, other precursors used together with the scandium compound represented by general formula (1) are not particularly limited, and any well-known precursor used as a CVD material can be used.

[0032] Examples of the other precursors include compounds of silicon or metal with one or more selected from the group consisting of compounds used as organic ligands such as alcohol compounds, glycol compounds, β-diketone compounds, cyclopentadiene compounds, and organic amine compounds. Examples of the metal species of the precursor include lithium, sodium, potassium, magnesium, calcium, strontium, barium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, zinc, aluminum, gallium, indium, germanium, tin, lead, antimony, bismuth, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0033] Examples of the alcohol compounds that can be used as organic ligands for the other precursors include alkyl alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, sec-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, pentyl alcohol, isopentyl alcohol, and tert-pentyl alcohol; 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-methoxy-1-methylethanol, 2-methoxy-1,1-dimethylethanol, 2-ethoxy-1,1-dimethylethanol, 2-isopropoxy-1,1-dimethylethanol, 2-butoxyethanol, and 2-isopropoxy-1,1-dimethylethanol. ether alcohols such as 2-(2-methoxyethoxy)-1,1-dimethylethanol, 2-propoxy-1,1-diethylethanol, 2-s-butoxy-1,1-diethylethanol, and 3-methoxy-1,1-dimethylpropanol; and dialkylamino alcohols such as dimethylaminoethanol, ethylmethylaminoethanol, diethylaminoethanol, dimethylamino-2-pentanol, ethylmethylamino-2-pentanol, dimethylamino-2-methyl-2-pentanol, ethylmethylamino-2-methyl-2-pentanol, and diethylamino-2-methyl-2-pentanol.

[0034] Examples of glycol compounds that can be used as organic ligands for the other precursors include 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 2,4-hexanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,3-butanediol, 2,4-butanediol, 2,2-diethyl-1,3-butanediol, 2-ethyl-2-butyl-1,3-propanediol, 2,4-pentanediol, 2-methyl-1,3-propanediol, 2-methyl-2,4-pentanediol, 2,4-hexanediol, and 2,4-dimethyl-2,4-pentanediol.

[0035] In addition, examples of β-diketone compounds include acetylacetone, hexane-2,4-dione, 5-methylhexane-2,4-dione, heptane-2,4-dione, 2-methylheptane-3,5-dione, 5-methylheptane-2,4-dione, 6-methylheptane-2,4-dione, 2,2-dimethylheptane-3,5-dione, 2,6-dimethylheptane-3,5-dione, 2,2,6-trimethylheptane-3,5-dione, 2,2,6,6-tetramethylheptane-3,5-dione, octane-2,4-dione, 2,2,6-trimethyloctane-3,5-dione, 2,6-dimethyloctane-3,5-dione, 2,9-dimethylnonane-4,6-dione, and 2-methyl-6-ethyldecane-3,5-dione. 1,1,1-trifluoropentane-2,4-dione, 1,1,1-trifluoro-5,5-dimethylhexane-2,4-dione, 1,1,1,5,5,5-hexafluoropentane-2,4-dione, 1,3-diperfluorohexylpropane-1,3-dione, and other fluorine-substituted alkyl β-diketones; 1,1,5,5-tetramethyl-1-methoxyhexane-2,4-dione, 2,2,6,6-tetramethyl-1-methoxyheptane-3,5-dione, 2,2,6,6-tetramethyl-1-(2-methoxyethoxy)heptane-3,5-dione, and other ether-substituted β-diketones.

[0036] Examples of the cyclopentadiene compound include cyclopentadiene, methylcyclopentadiene, ethylcyclopentadiene, propylcyclopentadiene, isopropylcyclopentadiene, butylcyclopentadiene, sec-butylcyclopentadiene, isobutylcyclopentadiene, tert-butylcyclopentadiene, dimethylcyclopentadiene, and tetramethylcyclopentadiene. Examples of the organic amine compound used as the organic ligand include methylamine, ethylamine, propylamine, isopropylamine, butylamine, sec-butylamine, tert-butylamine, isobutylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, ethylmethylamine, propylmethylamine, and isopropylmethylamine.

[0037] The above other precursors are known in the art, and their manufacturing methods are also known. As an example of the manufacturing method, when an alcohol compound is used as the organic ligand, the precursor can be manufactured by reacting the inorganic salt of the metal or its hydrate described above with an alkali metal alkoxide of the alcohol compound. Here, examples of the inorganic salt of the metal or its hydrate include metal halides and nitrates, and examples of the alkali metal alkoxide include sodium alkoxide, lithium alkoxide, potassium alkoxide, and the like.

[0038] In the case of a single source method, it is preferable to use a compound that exhibits similar thermal decomposition and / or oxidative decomposition behavior to the scandium compound represented by general formula (1) as the other precursor. In the case of a cocktail source method, it is preferable to use a compound that exhibits similar thermal decomposition and / or oxidative decomposition behavior to the scandium compound represented by general formula (1) as the other precursor, and that does not undergo changes that impair the desired properties of the precursor due to chemical reactions during mixing, etc.

[0039] Furthermore, the thin film-forming raw material of the present invention may contain a nucleophilic reagent, if necessary, in order to provide stability to the scandium compound represented by general formula (1) and other precursors. Examples of the nucleophilic reagent include ethylene glycol ethers such as glyme, diglyme, triglyme, and tetraglyme, crown ethers such as 18-crown-6, dicyclohexyl-18-crown-6, 24-crown-8, dicyclohexyl-24-crown-8, and dibenzo-24-crown-8, ethylenediamine, N,N'-tetramethylethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 1,1,4,7,7-pentamethyldiethylenetriamine, 1,1,4,7,10,10-hexamethyltriethylenetetramine ... Examples of the nucleophilic reagent include polyamines such as ethoxytriethyleneamine, cyclic polyamines such as cyclam and cyclen, heterocyclic compounds such as pyridine, pyrrolidine, piperidine, morpholine, N-methylpyrrolidine, N-methylpiperidine, N-methylmorpholine, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, oxazole, thiazole, and oxathiolane, β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, and 2-methoxyethyl acetoacetate, and β-diketones such as acetylacetone, 2,4-hexanedione, 2,4-heptanedione, 3,5-heptanedione, and dipivaloylmethane. The amount of these nucleophilic reagents used is preferably in the range of 0.1 mol to 10 mol, and more preferably 1 to 4 mol, relative to 1 mol of the total amount of the precursor.

[0040] The thin film forming material of the present invention is made to contain as little impurity metal elements, impurity halogens such as impurity chlorine, and impurity organic matter as possible, other than the components constituting the thin film. The impurity metal elements are preferably 100 ppb or less, more preferably 10 ppb or less, and the total amount is preferably 1 ppm or less, more preferably 100 ppb or less. In particular, when used as a gate insulating film, gate film, or barrier layer of an LSI, it is necessary to reduce the content of alkali metal elements and alkaline earth metal elements that affect the electrical properties of the resulting thin film. The impurity halogens are preferably 100 ppm or less, more preferably 10 ppm or less, and most preferably 1 ppm or less. The impurity organic matter is preferably 500 ppm or less, more preferably 50 ppm or less, and most preferably 10 ppm or less, in total. In addition, moisture causes particle generation in the chemical vapor deposition material and particle generation during thin film formation. Therefore, it is preferable to remove moisture as much as possible from the precursor, organic solvent, and nucleophilic reagent before use. The moisture content of each of the precursor, the organic solvent and the nucleophilic reagent is preferably 10 ppm or less, and more preferably 1 ppm or less.

[0041] In addition, the thin film forming material of the present invention is preferably free of particles as much as possible in order to reduce or prevent particle contamination of the thin film to be formed. Specifically, in particle measurement in the liquid phase using a light scattering type liquid-borne particle detector, the number of particles larger than 0.3 μm is preferably 100 or less per 1 mL of liquid phase, more preferably the number of particles larger than 0.2 μm is 1000 or less per 1 mL of liquid phase, and most preferably the number of particles larger than 0.2 μm is 100 or less per 1 mL of liquid phase.

[0042] The method for producing a thin film of the present invention using the thin film-forming raw material of the present invention is a CVD method in which the vapor obtained by vaporizing the thin film-forming raw material of the present invention and a reactive gas used as necessary are introduced into a film-forming chamber (treatment atmosphere) in which a substrate is placed, and then the precursor is decomposed and / or chemically reacted on the substrate to grow and deposit a thin film containing a metal on the substrate surface. There are no particular limitations on the method for transporting and supplying the raw material, the deposition method, the production conditions, the production equipment, etc., and well-known general conditions and methods can be used.

[0043] Examples of the reactive gases used as necessary as above include oxygen, ozone, nitrogen dioxide, nitrogen monoxide, water vapor, hydrogen peroxide, formic acid, acetic acid, acetic anhydride, etc. as oxidizing gases, hydrogen as reducing gases, and organic amine compounds such as monoalkylamines, dialkylamines, trialkylamines, alkylenediamines, etc., hydrazine, ammonia, etc. as gases for producing nitrides, and these can be used alone or in combination. Among these, since the thin film forming material of the present invention has good reactivity with ozone, it is preferable to use ozone when using one type as the reactive gas, and it is preferable to use at least ozone when using a mixed gas of two or more types as the reactive gas.

[0044] The above-mentioned transport supply method may include the gas transport method, liquid transport method, single source method, cocktail source method, etc.

[0045] In addition, examples of the above deposition method include thermal CVD, which deposits a thin film by reacting a source gas or a source gas and a reactive gas using only heat, plasma CVD, which uses heat and plasma, photo-CVD, which uses heat and light, photo-plasma CVD, which uses heat, light, and plasma, and ALD, which divides the CVD deposition reaction into elementary processes and deposits in stages at the molecular level.

[0046] Examples of the material of the substrate include silicon, ceramics such as silicon nitride, titanium nitride, tantalum nitride, titanium oxide, titanium nitride, scandium oxide, zirconium oxide, hafnium oxide, and lanthanum oxide, glass, and metals such as metal cobalt. Examples of the shape of the substrate include plate-like, spherical, fibrous, and scaly shapes. The surface of the substrate may be flat or may have a three-dimensional structure such as a trench structure.

[0047] The above-mentioned production conditions include reaction temperature (substrate temperature), reaction pressure, deposition rate, etc. The reaction temperature is preferably 100° C. or higher, at which the compound of the present invention reacts sufficiently, more preferably 150° C. to 400° C., and particularly preferably 200° C. to 350° C. The reaction pressure is preferably 10 Pa to atmospheric pressure in the case of thermal CVD or photo-CVD, and is preferably 10 Pa to 2000 Pa in the case of using plasma. The deposition rate can be controlled by the supply conditions of the raw material (vaporization temperature, vaporization pressure), the reaction temperature, and the reaction pressure. If the deposition rate is high, the properties of the obtained thin film may deteriorate, and if it is low, problems may occur in productivity, so that the deposition rate is preferably 0.01 nm / min to 100 nm / min, and more preferably 1 nm / min to 50 nm / min. In the case of the ALD method, the deposition rate is controlled by the number of cycles so as to obtain a desired film thickness.

[0048] Further examples of the above manufacturing conditions include the temperature and pressure when the thin film forming raw material is vaporized to form vapor. The step of vaporizing the thin film forming raw material to form vapor may be performed in a raw material container or in a vaporization chamber. In either case, the thin film forming raw material of the present invention is preferably evaporated at 0°C to 150°C. In addition, when the thin film forming raw material is vaporized to form vapor in a raw material container or in a vaporization chamber, the pressure in the raw material container and the pressure in the vaporization chamber are both preferably 1 Pa to 10,000 Pa.

[0049] The method for producing a thin film of the present invention employs an ALD method, and may include a raw material introduction step of vaporizing a thin film-forming raw material to form vapor by the above-mentioned transport and supply method and introducing the vapor into a film formation chamber, as well as a precursor thin film formation step of forming a precursor thin film on the surface of the substrate using the above-mentioned compound in the vapor, an exhaust step of exhausting unreacted compound gas, and a metal-containing thin film formation step of chemically reacting the precursor thin film with a reactive gas to form a thin film containing a metal on the surface of the substrate.

[0050] Each step of the ALD method will be described in detail below, taking the case of forming a metal oxide thin film as an example. First, the above-mentioned raw material introduction step is performed. The preferable temperature and pressure when the raw material for forming the thin film is vaporized are the same as those conditions described in the thin film manufacturing method by the CVD method. Next, the vapor introduced into the film formation chamber comes into contact with the surface of the substrate to form a precursor thin film on the substrate surface (precursor thin film formation step). At this time, heat may be applied by heating the substrate or the film formation chamber. The precursor thin film formed in this step is a thin film formed from a compound represented by general formula (1), or a thin film formed by decomposition and / or reaction of a part of the compound represented by general formula (1), and has a different composition from the target metal oxide thin film. The substrate temperature when this step is performed is preferably room temperature to 500°C, more preferably 150°C to 350°C. The pressure of the system (inside the film formation chamber) when this step is performed is preferably 1 Pa to 10,000 Pa, more preferably 10 Pa to 1000 Pa.

[0051] Next, unreacted compound gases and by-produced gases are exhausted from the deposition chamber (exhaust process). Ideally, unreacted compound gases and by-produced gases are completely exhausted from the deposition chamber, but it is not necessary to exhaust them completely. Exhaust methods include a method of purging the system with an inert gas such as nitrogen, helium, or argon, a method of exhausting by reducing the pressure in the system, and a combination of these methods. When reducing the pressure, the pressure in the system is preferably set to 0.01 Pa to 300 Pa, and more preferably to 0.01 Pa to 100 Pa.

[0052] Next, an oxidizing gas is introduced into the deposition chamber as a reactive gas, and a metal oxide thin film is formed from the precursor thin film obtained in the previous precursor thin film forming step by the action of the oxidizing gas or the action of the oxidizing gas and heat (metal oxide-containing thin film forming step). The temperature when applying heat in this step is preferably room temperature to 500°C, more preferably 150 to 350°C. The pressure of the system (inside the deposition chamber) when this step is performed is preferably 1 Pa to 10,000 Pa, more preferably 10 Pa to 1,000 Pa. The compound of the present invention has good reactivity with the oxidizing gas, and therefore a high-quality metal oxide thin film with a low residual carbon content can be obtained.

[0053] In the thin film manufacturing method of the present invention, when the ALD method is adopted as described above, thin film deposition by a series of operations consisting of the raw material introduction step, precursor thin film formation step, exhaust step, and metal oxide-containing thin film formation step is regarded as one cycle, and this cycle may be repeated several times until a thin film of a required thickness is obtained. In this case, after one cycle, it is preferable to exhaust unreacted compound gas and reactive gas (oxidizing gas in the case of forming a metal oxide thin film) from the deposition reaction section, as well as by-product gas, in the same manner as in the exhaust step, and then perform the next cycle.

[0054] In addition, in forming a metal oxide thin film by the ALD method, energy such as plasma, light, voltage, etc. may be applied, and a catalyst may be used. The timing of applying the energy and the timing of using the catalyst are not particularly limited, and may be, for example, when introducing a compound gas in the raw material introduction step, when heating in the precursor thin film formation step or the metal oxide-containing thin film formation step, when exhausting the system in the exhaust step, when introducing an oxidizing gas in the metal oxide-containing thin film formation step, or between the above steps.

[0055] In the method for producing a thin film of the present invention, after deposition of the thin film, an annealing treatment may be performed in an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere in order to obtain better electrical properties, and a reflow step may be performed if step filling is required. The temperature in this case is usually 200°C to 1000°C, and preferably 250°C to 500°C.

[0056] The apparatus for manufacturing a thin film using the thin film forming material of the present invention may be a well-known chemical vapor deposition apparatus. Specific examples of the apparatus include an apparatus capable of bubbling and supplying a precursor as shown in Fig. 1, and an apparatus having a vaporization chamber as shown in Fig. 2. In addition, an apparatus capable of performing plasma treatment on a reactive gas as shown in Figs. 3 and 4 may be used. Note that the apparatus is not limited to the single-wafer type apparatus as shown in Figs. 1 to 4, and an apparatus capable of simultaneously processing multiple wafers using a batch furnace may also be used.

[0057] The thin film produced by using the thin film forming material of the present invention can be a desired type of thin film such as metal, oxide ceramics, nitride ceramics, glass, etc., by appropriately selecting other precursors, reactive gases, and production conditions. It is known that the thin film exhibits electrical properties and optical properties. For example, metal scandium thin film, scandium oxide thin film, scandium alloy, and scandium-containing complex oxide thin film can be mentioned. Scandium alloy can be Al-Sc alloy. These thin films are applied to various products, and are widely used for example in the production of electrode materials for memory elements such as DRAM elements, resistive films, diamagnetic films used in the recording layers of hard disks, and catalyst materials for solid polymer fuel cells.

[0058] Among the above-mentioned thin film forming materials, the compound represented by the general formula (2) is also a novel compound. The novel compound of the present invention has a low melting point, is applicable to the ALD method, and is particularly suitable as a precursor for a thin film manufacturing method having a vaporization step such as the CVD method.

[0059] In the above general formula (2), R 4 and R 5 each independently represents an alkyl group having 2 to 3 carbon atoms; R 6 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 2 to 3 carbon atoms include an ethyl group, an n-propyl group, and an isopropyl group.

[0060] In the above general formula (2), R 4 or R 5 is preferably an ethyl group since it has a low melting point, and R 4 and R 5 It is particularly preferred that both R are ethyl groups. 6 is preferably a hydrogen atom. An example of the compound is 4 and R 5 are both ethyl groups, and R 6 is a hydrogen atom (the above compound No. 7).

[0061] The compound represented by the above general formula (2) is not particularly limited by its manufacturing method, and is manufactured by applying a well-known reaction. As a manufacturing method, it can be obtained by reacting scandium chloride with an alkanedione compound having a corresponding structure, and purifying it by distillation, in the same manner as the manufacturing method of the compound represented by the above general formula (1).

[0062] Specific examples of the novel compound represented by the above general formula (2) include the compounds represented by the above compound Nos. 7 to 18. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples, production examples, comparative examples and evaluation examples, but the present invention is not limited to the following examples.

[0064] [Example 1] Synthesis of Compound No. 7 Add 2.1 g (1.6 x 10 -2 mol) of 3,5-heptanedione and 16 g (0.22 mol) of dehydrated tetrahydrofuran were added, and the mixture was cooled to -40°C, after which 9.9 ml (1.6 mol / l) of n-butyllithium / hexane solution was added dropwise. The mixture was warmed to room temperature and stirred for 6 hours. -3The reaction mixture was added dropwise to a mixture of 10 g (0.11 mol) of anhydrous ScCl3 and 20 g (0.22 mol) of toluene. 10 g (0.11 mol) of toluene was added to this reaction mixture and refluxed and stirred in an oil bath at 110°C for 12 hours. The solvent was removed under reduced pressure in an oil bath at 80°C, and 20 g (0.23 mol) of hexane was added and filtered. The filtrate was removed from the solvent under reduced pressure in an oil bath at 70°C. The resulting orange liquid was purified by distillation at a heating temperature of 160°C and a pressure of 30 Pa, yielding 1.1 g of a colorless, transparent liquid.

[0065] (Analysis value) (1) Ambient Pressure TG-DTA 50% mass reduction Temperature: 253℃ (Ar flow rate: 100ml / min, temperature increase 10℃ / min) (2) Low-pressure TG-DTA Mass reduction by 50% Temperature: 174℃ (Ar flow rate: 50ml / min, temperature increase 10℃ / min) (3) 1H-NMR (heavy benzene) 1.01ppm (6H, triplet), 2.05 (4H, qualtet), 5.43ppm (1H, singlet) (4) Elemental analysis (theoretical value) Sc:10.7%(10.56%), C:59.3%(59.15%), H:7.6%(7.75%), O:22.4%(22.54%)

[0066] [Evaluation Example 1 and Comparative Evaluation Examples 1-2] Evaluation of the physical properties of scandium compounds The state of the compound No. 7 of the present invention obtained in Example 1 and the comparative compounds 1 and 2 below at 25°C was visually observed. The melting points of those that were solid at 25°C were measured. The results are shown in Table 1. In addition, in the chemical formulae of the comparative compounds 1 and 2 below, "Me" represents a methyl group, and "tBu" represents a tertiary butyl group.

[0067] [ka]

[0068] [Table 1]

[0069] The results in Table 1 show that compound No. 7 has a melting point significantly lower than those of comparative compound 1 and comparative compound 2.

[0070] [Example 2] Preparation of scandium oxide thin film Using compound No. 7 as a raw material for atomic layer deposition, a scandium oxide thin film was produced on a silicon wafer by the ALD method under the following conditions using the apparatus shown in Figure 1. The composition of the thin film was confirmed by X-ray photoelectron spectroscopy, which showed that the thin film was scandium oxide with a residual carbon content of less than 1.0 atom%. The film thickness was also measured by X-ray reflectivity and the average value was calculated to be 25.7 nm, and the film thickness obtained per cycle was 0.05 nm on average.

[0071] (conditions) Substrate: Silicon wafer Reaction temperature (silicon wafer temperature): 300°C Reactive gas: Ozone A series of steps (1) to (4) below constitutes one cycle, and 500 cycles were repeated: (1) A source material for atomic layer deposition vaporized under the conditions of source material container temperature: 120°C, source material container internal pressure: 100 Pa is introduced into a film formation chamber, and deposition is performed for 30 seconds at a system pressure of 100 Pa; (2) 15 seconds of argon purge to remove undeposited material; (3) Introduce reactive gas into the deposition chamber and react for 5 seconds at a system pressure of 100 Pa; (4) Unreacted reactive gases and by-product gases are removed by argon purging for 15 seconds.

[0072] [Example 3] Preparation of scandium oxide thin film A scandium oxide thin film was produced under the same conditions as in Example 2, except that Compound No. 1 was used as the atomic layer deposition raw material. The composition of the resulting thin film was confirmed by X-ray photoelectron spectroscopy, and it was found to be scandium oxide with a residual carbon content of less than 1.0 atom%. In addition, the film thickness was measured by X-ray reflectivity and the average value was calculated to be 15.5 nm on average, and the film thickness obtained per cycle was 0.03 nm on average.

[0073] [Comparative Example 1] Preparation of scandium oxide thin film A scandium oxide thin film was produced under the same conditions as in Example 2, except that Comparative Compound 1 was used as the raw material for atomic layer deposition. The composition of the obtained thin film was confirmed by X-ray photoelectron spectroscopy, and it was found to be scandium oxide with a residual carbon content of 5.0 atom%. In addition, the film thickness was measured by X-ray reflectivity and the average value was calculated, which gave an average film thickness of 5.1 nm, and the film thickness obtained per cycle was an average of 0.01 nm.

[0074] From the results of Examples 2 and 3, it was found that a scandium oxide thin film of high quality with a low residual carbon content was produced in both cases. On the other hand, it was found that the thin film obtained in Comparative Example 1 had a very high residual carbon content, resulting in a low-quality scandium oxide thin film. Furthermore, when the film thickness obtained per cycle in Examples 2 and 3 and Comparative Example 1 were compared, it was found that Examples 2 and 3 were able to produce a scandium oxide thin film with productivity three times higher than that of Comparative Example 1. In particular, it was found that Example 2 was able to produce a scandium oxide thin film with extremely high productivity. From the above results, it is evident that according to the present invention, a high-quality scandium oxide thin film can be produced with high productivity by the ALD method.

Claims

1. A thin film-forming material containing a scandium compound represented by the following general formula (1): [Formula 1] (In the formula, R 1 and R 2 represents an ethyl group, R 3 represents a hydrogen atom.)

2. A method for producing a thin film containing scandium atoms on a surface of a substrate, comprising the steps of: A step of vaporizing the thin film forming material according to claim 1; Introducing vapor containing the vaporized scandium compound represented by general formula (1) into a treatment atmosphere; and Decomposing and / or chemically reacting the compound to deposit it on the surface of the substrate. A method for producing a thin film, comprising:

3. Use of a scandium compound represented by the following general formula (1) for producing a thin film containing scandium atoms on the surface of a substrate. [chemical 2] (In the formula, R 1 and R 2 represents an ethyl group, R 3 represents a hydrogen atom.)

4. A scandium compound represented by the following general formula (2): [C3] (In the formula, R 4 and R 5 represents an ethyl group, R 6 represents a hydrogen atom.)

Citation Information

Patent Citations

  • COMPOSITION FOR FORMING METALLIC OXIDE THIN FILM, AND METHOD FOR STABILIZING beta-DIKETONE METALLIC COMPLEX SOLUTION

    JP2005179777A

  • Diamond semiconductor and method for producing the same

    JP2010189208A

  • Deposition method for high-k dielectric materials

    US20090253270A1

  • Apparatus having a dielectric containing scandium and gadolinium

    US20140084355A1