Etching solution and method for manufacturing semiconductor device
The use of a periodic acid and fluoride-based etching solution for SiGe compounds addresses the instability issue in conventional etching solutions, ensuring stable etching rates and controlled manufacturing processes.
Patent Information
- Application Number
- JP2023060820
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2038-12-27
AI Technical Summary
Conventional etching solutions for SiGe compounds are chemically unstable, leading to fluctuations in etching rates over time, making it difficult to control the manufacturing process of semiconductor devices.
An etching solution containing periodic acid and fluoride is used to selectively etch SiGe compounds, maintaining a stable etching rate over time.
The etching solution provides improved stability and control over the etching process, ensuring consistent manufacturing of semiconductor devices by maintaining a stable etching rate for SiGe compounds.
Smart Images

Figure 0007573678000001 
Figure 0007573678000002 
Figure 0007573678000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an etching solution and a method for manufacturing a semiconductor device. [Background technology]
[0002] Traditionally, the scaling of features within integrated circuits has allowed for an increased density of functional units on a semiconductor chip: for example, the reduction in transistor size has allowed for more memory elements to be fitted onto a chip, leading to the production of products with increased capacity.
[0003] Ge is used as a semiconducting crystalline material other than silicon in the fabrication of field effect transistors (FETs) for integrated circuit devices. Ge has several advantageous characteristics compared to silicon in some cases, including high charge carrier (hole) mobility, band gap offset, different lattice constant, and ability to alloy with silicon to form the semiconducting binary alloy SiGe.
[0004] However, Ge materials (especially those with the general formula Si 1-x Ge x A compound represented by the formula: where x is greater than 0 and less than 1. Hereinafter, this may simply be referred to as a "SiGe compound." Various etching solutions with high selectivity for SiGe have been proposed. For example, Patent Document 1 describes an etching composition containing at least one diol compound, at least one fluoride species, and at least one oxidizing species. Moreover, Patent Document 2 describes an etching composition containing peracetic acid, fluoric acid and an oxide. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2018-519674 [Patent Document 2] U.S. Patent No. 7,176,041 Summary of the Invention [Problem to be solved by the invention]
[0006] However, conventional etching solutions such as those described in Patent Documents 1 and 2 are chemically unstable, and the etching rate for a SiGe compound may vary over time, making it difficult to control the manufacturing process. The present invention has been made in view of the above circumstances, and relates to a compound represented by the general formula Si 1-x Ge x The present invention aims to provide an etching solution having improved stability over time of the etching rate for a compound represented by the following formula: [Means for solving the problem]
[0007] In order to solve the above problems, the present invention employs the following configuration.
[0008] The first aspect of the present invention is to provide a compound represented by the general formula Si 1-x Ge x The etching solution is for selectively etching a compound represented by the following formula (where x is greater than 0 and less than 1), and contains periodic acid and a fluoride.
[0009] The second aspect of the present invention is to use the etching solution to form a compound having the general formula Si 1-x Ge x The present invention relates to a method for treating an object to be treated, the method comprising the step of etching an object to be treated, the object including a compound represented by the formula:
[0010] The third aspect of the present invention is to use the etching solution to form a compound having the general formula Si 1-x Ge x The present invention relates to a method for manufacturing a semiconductor device, the method comprising the step of etching an object to be treated, the object including a compound represented by the formula: Effect of the Invention
[0011] According to the present invention, the general formula Si 1-x Ge x The present invention provides an etching solution having improved stability over time of the etching rate for a compound represented by the formula (I) and a method for treating an object to be treated and a method for producing a semiconductor device using the etching solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (etchant) The etching solution according to the first aspect of the present invention contains periodic acid and a fluoride. The etching solution according to this aspect has a general formula Si 1-x Ge x The compound represented by the formula (hereinafter, sometimes simply referred to as "SiGe compound") is used for selective etching treatment.
[0013] <Periodic acid> The etching solution according to the present embodiment contains periodic acid. The periodic acid may be orthoperiodic acid (H5IO6) or metaperiodic acid (HIO4), but orthoperiodic acid (H5IO6) is preferred. The SiGe compound can be made soluble by oxidation. Periodic acid is an oxidizing agent that releases oxygen atoms for oxidizing the SiGe compound, and the redox potential of periodic acid is sufficient to oxidize the SiGe compound, so that the SiGe compound can be efficiently oxidized.
[0014] The content of periodic acid in the etching solution of the present embodiment is not particularly limited, but is, for example, 0.02 to 5 mass% relative to the total mass of the etching solution, preferably 0.05 to 4.5 mass%, more preferably 0.1 to 4 mass%, and even more preferably 0.20 to 3 mass%. When the content of periodic acid is within the above range, the stability over time of the etching rate for the SiGe compound is likely to be improved.
[0015] <Fluoride> The etching solution according to this embodiment contains a fluoride. The fluoride is not particularly limited, and examples thereof include hexafluorotitanic acid, hexafluorosilicic acid, hexafluorozirconic acid, tetrafluoroboric acid, tetrabutylammonium trifluoromethanesulfonate, tetraalkylammonium tetrafluoroborate (NR1R2R3R4BF4) such as tetrabutylammonium tetrafluoroborate, tetraalkylammonium hexafluorophosphate (NR1R2R3R4PF6), tetraalkylammonium fluoride (NR1R2R3R4F) such as tetramethylammonium fluoride (anhydride or hydrate thereof), ammonium bifluoride, ammonium fluoride (wherein R1, R2, R3, and R4 may be the same or different from each other and are selected from the group consisting of hydrogen, linear or branched C1-C6 alkyl groups (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl), C1-C6 alkoxy groups (e.g., hydroxyethyl, hydroxypropyl), or substituted or unsubstituted aryl groups (e.g., benzyl).). Among these, the fluoride is preferably hydrofluoric acid (DHF) and / or ammonium fluoride (NH4F).
[0016] In the etching solution of the present embodiment, one type of fluoride may be used alone, or two or more types may be used in combination. The content of the fluoride in the etching solution of the present embodiment is not particularly limited, but is, for example, 0.02 to 5 mass% relative to the total mass of the etching solution, preferably 0.025 to 3.00 mass%, more preferably 0.03 to 2.50 mass%, and even more preferably 0.04 to 2.00 mass%. When the content of the fluoride is within the above range, the etching rate for the SiGe compound is more likely to be improved. In addition, the fluorine ion concentration of the etching solution of the present embodiment is not particularly limited, but is, for example, 0.005 to 2.50 mol / L, preferably 0.007 to 1.50 mol / L, more preferably 0.008 to 1.25 mol / L, and even more preferably 0.010 to 1.00 mol / L. When the fluorine ion concentration is within the above range, the etching rate for the SiGe compound is more likely to be improved.
[0017] <Other ingredients> The etching solution of the present embodiment may contain other components in addition to the above components, as long as the effects of the present invention are not impaired. Examples of other components include water, a water-soluble organic solvent, a pH adjuster, an oxidizing agent, a passivation agent, and a surfactant.
[0018] ·water The etching solution of the present embodiment preferably contains water as a solvent for the above components. The water may contain trace components that are inevitably mixed in. The water used in the etching solution of the present embodiment is preferably water that has been subjected to a purification treatment, such as distilled water, ion-exchanged water, or ultrapure water, and it is more preferable to use ultrapure water that is generally used in semiconductor manufacturing. The content of water in the etching solution of this embodiment is not particularly limited, but is preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 94 mass% or more. The upper limit is not particularly limited, but is preferably less than 99.95 mass%, more preferably 99.9 mass% or less, and even more preferably 99.5 mass% or less. The etching solution of this embodiment is preferably an aqueous solution containing periodic acid and a fluoride.
[0019] Water-soluble organic solvents The etching solution of the present embodiment may contain a water-soluble organic solvent within a range that does not impair the effects of the present invention. Examples of the water-soluble organic solvent include alcohols (e.g., methanol, ethanol, ethylene glycol, propylene glycol, glycerin, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, diethylene glycol, dipropylene glycol, furfuryl alcohol, and 2-methyl-2,4-pentanediol), dimethyl sulfoxide, and ethers (e.g., ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and propylene glycol dimethyl ether).
[0020] In the etching solution of the present embodiment, the water-soluble organic solvent may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a water-soluble organic solvent, the content of the water-soluble organic solvent is preferably 50 mass % or less, more preferably 30 mass % or less, and even more preferably 10 mass % or less, based on the total amount of water and the water-soluble organic solvent.
[0021] pH adjuster The etching solution of the present embodiment may contain a pH adjuster in order to further improve the etching rate for the SiGe compound. The pH adjuster is preferably at least one selected from the group consisting of acids and their salts. Specifically, methanesulfonic acid, trifluoromethanesulfonic acid, oxalic acid dihydrate, citric acid, tartaric acid, picolinic acid, succinic acid, acetic acid, lactic acid, sulfosuccinic acid, benzoic acid, propionic acid, formic acid, pyruvic acid, maleic acid, malonic acid, fumaric acid, malic acid, ascorbic acid, mandelic acid, heptanoic acid, butyric acid, valeric acid, glutaric acid, phthalic acid, hypophosphorous acid, salicylic acid, 5-sulfosalicylic acid, hydrochloric acid, ethanesulfonic acid, butanesulfonic acid, p-toluenesulfonic acid, dichloroacetic acid, difluoroacetic acid, monochloroacetic acid, monofluoroacetic acid, trichloroacetic acid, trifluoroacetic acid, hydrobromic acid (62% by weight), sulfuric acid, ammonium acetate, sodium acetate, potassium acetate, tetramethylammonium acetate, and other tetraacetates. alkylammonium, phosphonium acetate, ammonium butyrate, ammonium trifluoroacetate, ammonium carbonate, ammonium chloride, ammonium sulfate, phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, bis(tetramethylammonium) hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, ditetraalkylammonium hydrogen phosphate, ditetraalkylammonium dihydrogen phosphate, diphosphonium hydrogen phosphate, phosphonium dihydrogen phosphate, ammonium phosphonate, tetraalkylammonium phosphonate, sodium phosphonate, potassium phosphonate, phosphonium phosphonate, etidronic acid, and salts thereof. Among these, methanesulfonic acid or oxalic acid is preferred as the acid pH adjuster.
[0022] The etching solution of the present embodiment may contain a basic compound as a pH adjuster. As such a basic compound, an organic alkaline compound or an inorganic alkaline compound can be used, and suitable examples of the organic alkaline compound include quaternary ammonium salts such as organic quaternary ammonium hydroxides, and salts of alkylamines and their derivatives such as trimethylamine and triethylamine. Examples of inorganic alkaline compounds include inorganic compounds containing alkali metals or alkaline earth metals and their salts, such as lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide.
[0023] In the etching solution of the present embodiment, the pH adjuster may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a pH adjuster, the content is, for example, 0.01 to 10 mass % relative to the total mass of the etching solution, preferably 0.02 to 4.5 mass %, more preferably 0.03 to 4 mass %, and even more preferably 0.05 to 3 mass %. When the content of the pH adjuster is within the above range, the etching rate for the SiGe compound is more likely to be improved.
[0024] Oxidizing agents The etching solution of the present embodiment may contain other oxidizing agents in addition to periodic acid. Examples of the oxidizing agent include hydrogen peroxide, FeCl3, FeF3, Fe(NO3)3, Sr(NO3)2, CoF3, MnF3, oxone (2KHSO5·KHSO4·K2SO4), iodic acid, vanadium(V) oxide, vanadium(IV,V) oxide, ammonium vanadate, ammonium peroxomonosulfate, ammonium chlorite, ammonium chlorate, ammonium iodate, ammonium nitrate, ammonium perborate, ammonium perchlorate, ammonium periodate, ammonium persulfate, ammonium hypochlorite, ammonium hypobromite, ammonium tungstate, sodium persulfate, sodium hypochlorite, sodium perborate, sodium hypobromite, potassium iodate, potassium permanganate, potassium persulfate, nitric acid, and potassium iodate. Examples of the antibacterial agent include potassium sulfate, potassium hypochlorite, tetramethylammonium chlorite, tetramethylammonium chlorate, tetramethylammonium iodate, tetramethylammonium perborate, tetramethylammonium perchlorate, tetramethylammonium periodate, tetramethylammonium persulfate, tetrabutylammonium peroxomonosulfate, peroxomonosulfuric acid, ferric nitrate, urea peroxide, peracetic acid, methyl-1,4-benzoquinone (MBQ), 1,4-benzoquinone (BQ), 1,2-benzoquinone, 2,6-dichloro-1,4-benzoquinone (DCBQ), toluquinone, 2,6-dimethyl-1,4-benzoquinone (DMBQ), chloranil, alloxan, N-methylmorpholine N-oxide, and trimethylamine N-oxide.
[0025] In the etching solution of the present embodiment, the oxidizing agent may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains an oxidizing agent, the content of the oxidizing agent is preferably 0.01 to 10 mass %, and more preferably 0.1 to 7 mass %, relative to the total mass of the etching solution.
[0026] Passivation agent The etching solution of this embodiment may contain a passivation agent for germanium. Passivation agents include ascorbic acid, L(+)-ascorbic acid, isoascorbic acid, ascorbic acid derivatives, boric acid, ammonium diborate, borate salts (e.g., ammonium pentaborate, sodium tetraborate, and ammonium diborate), alanine, arginine, asparagine, aspartic acid, cysteine, glutamic acid, glutamine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, valine, sodium bromide, potassium bromide, rubidium bromide, magnesium bromide, calcium bromide, and amines of the formula NR 1 R 2 R 3 R 4 Br (wherein, R 1 , R 2 , R 3 and R 4 can be the same or different from each other and are selected from the group consisting of hydrogen and branched or straight chain C1-C6 alkyl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl).
[0027] In the etching solution of the present embodiment, the passivation agent may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a passivation agent, the content of the passivation agent is preferably 0.01 to 5 mass %, and more preferably 0.1 to 1 mass %, relative to the total mass of the etching solution.
[0028] Surfactants The etching solution of the present embodiment may contain a surfactant for the purpose of adjusting the wettability of the etching solution to the object to be treated, etc. As the surfactant, a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant may be used, and these may be used in combination.
[0029] Examples of nonionic surfactants include polyalkylene oxide alkyl phenyl ether surfactants, polyalkylene oxide alkyl ether surfactants, block polymer surfactants consisting of polyethylene oxide and polypropylene oxide, polyoxyalkylene distyrene-type phenyl ether surfactants, polyalkylene tribenzyl phenyl ether surfactants, and acetylene polyalkylene oxide surfactants.
[0030] Examples of anionic surfactants include alkylsulfonic acids, alkylbenzenesulfonic acids, alkylnaphthalenesulfonic acids, alkyldiphenylethersulfonic acids, fatty acid amidesulfonic acids, polyoxyethylene alkylether carboxylic acids, polyoxyethylene alkylether acetic acids, polyoxyethylene alkylether propionic acids, alkylphosphonic acids, and salts of fatty acids. Examples of "salts" include ammonium salts, sodium salts, potassium salts, and tetramethylammonium salts.
[0031] Examples of cationic surfactants include quaternary ammonium salt surfactants and alkylpyridinium surfactants.
[0032] Examples of amphoteric surfactants include betaine type surfactants, amino acid type surfactants, imidazoline type surfactants, and amine oxide type surfactants.
[0033] These surfactants are generally commercially available. The surfactants may be used alone or in combination of two or more.
[0034] <Object to be treated> The etching solution of the present embodiment is used for etching a SiGe compound, and an object to be treated containing a SiGe compound is the subject of etching treatment. The object to be treated is not particularly limited as long as it contains a SiGe compound, and examples thereof include a substrate having a SiGe compound-containing layer (SiGe compound-containing film). The substrate is not particularly limited, and examples thereof include various substrates such as a semiconductor wafer, a glass substrate for a photomask, a glass substrate for a liquid crystal display, a glass substrate for a plasma display, a substrate for an FED (Field Emission Display), a substrate for an optical disk, a substrate for a magnetic disk, and a substrate for a magneto-optical disk. The substrate is preferably a substrate used for manufacturing a semiconductor device. In addition to the SiGe compound-containing layer and the substrate base material, the substrate may have various layers and structures, such as metal wiring, a gate structure, a source structure, a drain structure, an insulating layer, a ferromagnetic layer, and a nonmagnetic layer, as appropriate. In addition, the top layer of the device surface of the substrate does not need to be a SiGe compound-containing layer, and for example, an intermediate layer of a multilayer structure may be a SiGe compound-containing layer. The size, thickness, shape, layer structure, etc. of the substrate are not particularly limited and can be appropriately selected depending on the purpose.
[0035] The SiGe compound-containing layer is preferably a layer containing a SiGe compound, more preferably a SiGe compound film. The thickness of the SiGe compound-containing layer on the substrate is not particularly limited and can be appropriately selected according to the purpose. The thickness of the SiGe compound-containing layer can be, for example, in the range of 1 to 500 nm or 1 to 300 nm.
[0036] The etching solution of the present embodiment may be used for microfabrication of a SiGe compound-containing layer in a substrate, may be used for removing a SiGe compound-containing deposit attached to a substrate, or may be used for removing impurities such as particles from a processing object having a SiGe compound-containing layer on the surface thereof.
[0037] According to the etching solution of the present embodiment described above, since it contains periodic acid as an oxidizing agent, the stability of the etching rate for the SiGe compound over time can be improved. Although the reason is not clear, it is presumed that the etching rate for the SiGe compound of the etching solution of the present embodiment does not deteriorate over time because periodic acid is very stable as an oxidizing agent. For example, even after storing the etching solution of the present embodiment at room temperature for 3 days or more or 7 days or more, the etching rate for the SiGe compound hardly changes. Therefore, it is presumed that the manufacturing process including the etching step of the SiGe compound can be stably controlled by the etching solution of the present embodiment.
[0038] (Method for treating object to be treated) A method for processing an object according to a second aspect of the present invention is characterized by comprising the step of etching an object containing a SiGe compound with the etching solution according to the first aspect.
[0039] Examples of the object to be processed containing a SiGe compound include the same as those described in "<Object to be processed>" in the above "(Etching solution)", and a preferred example is a substrate having a SiGe compound-containing layer. The method for forming the SiGe compound-containing layer on the substrate is not particularly limited, and a known method can be used. Examples of such methods include sputtering, chemical vapor deposition (CVD), molecular beam epitaxy (MBE), and atomic layer deposition (ALD). The raw material of the SiGe compound-containing layer used when forming the SiGe compound-containing layer on the substrate is also not particularly limited, and can be appropriately selected depending on the film formation method.
[0040] <Step of Etching Object> This step is a step of etching a workpiece containing a SiGe compound using the etching solution according to the first embodiment, and includes an operation of contacting the workpiece with the etching solution. The etching method is not particularly limited, and a known etching method can be used. Examples of such methods include, but are not limited to, a spray method, a dipping method, a liquid puddle method, and the like. In the spray method, for example, the object to be treated is conveyed or rotated in a predetermined direction, and the etching solution according to the first aspect is sprayed into the space between the object to be treated and the etching solution is brought into contact with the object to be treated. If necessary, the etching solution may be sprayed onto the substrate while rotating the substrate using a spin coater. In the immersion method, the object to be treated is immersed in the etching solution according to the first aspect to bring the etching solution into contact with the object to be treated. In the puddle method, the etching liquid according to the first aspect is puddled on the object to be treated, and the object to be treated is brought into contact with the etching liquid. These etching methods can be appropriately selected depending on the structure, material, etc. of the object to be treated. In the case of the spray method or the puddle method, the amount of the etching liquid supplied to the object to be treated may be an amount that allows the surface of the object to be treated to be sufficiently wetted with the etching liquid.
[0041] The purpose of the etching process is not particularly limited, and may be fine processing of a surface of a workpiece containing a SiGe compound (e.g., a SiGe compound-containing layer on a substrate), removal of a SiGe compound-containing deposit adhering to a workpiece (e.g., a substrate having a SiGe compound-containing layer), or cleaning of a surface of a workpiece containing a SiGe compound (e.g., a SiGe compound-containing layer on a substrate). When the purpose of the etching process is to microfabricate the surface of the workpiece containing a SiGe compound, the workpiece is usually brought into contact with the etching solution after covering the areas that should not be etched with an etching mask. When the purpose of the etching process is to remove SiGe compound-containing deposits adhering to a workpiece, the etching solution according to the first aspect is brought into contact with the workpiece, whereby the SiGe compound-containing deposits are dissolved and the SiGe compound deposits can be removed from the workpiece. When the purpose of the etching process is to clean a surface of a processing object containing a SiGe compound, the processing object is quickly dissolved by contacting the etching solution according to the first aspect with the processing object, and impurities such as particles adhering to the surface of the processing object are removed from the surface of the processing object in a short time.
[0042] The temperature at which the etching process is carried out is not particularly limited, and may be any temperature at which the SiGe compound dissolves in the etching solution. The etching temperature may be, for example, 15 to 60°C. In any of the spray method, the immersion method, and the puddle method, the etching rate increases by increasing the temperature of the etching solution, but the processing temperature can be appropriately selected while keeping the composition change of the etching solution small, and taking into consideration workability, safety, cost, etc.
[0043] The time for performing the etching process may be appropriately selected depending on the purpose of the etching process, the amount of the SiGe compound to be removed by etching (e.g., the thickness of the SiGe compound-containing layer, the amount of SiGe compound deposits, etc.), and the etching process conditions.
[0044] According to the method for treating a workpiece of the present embodiment described above, the etching solution according to the first aspect containing periodic acid as an oxidizing agent is used to etch the workpiece. The etching solution has a high stability over time in the etching rate for a SiGe compound, so that the manufacturing process including the etching step for the SiGe compound can be stably controlled.
[0045] (Method of manufacturing semiconductor device) A method for producing a semiconductor device according to a third aspect of the present invention is characterized by comprising the step of etching an object to be processed containing a SiGe compound with the etching solution according to the first aspect.
[0046] The step of etching the object containing the SiGe compound can be carried out in the same manner as described in the above "(Method of processing object)". The object containing the SiGe compound is preferably a substrate having a SiGe compound-containing layer. The substrate may be a substrate that is generally used for manufacturing semiconductor devices.
[0047] <Other processes> The method for manufacturing a semiconductor device according to the present embodiment may include other steps in addition to the etching process. The other steps are not particularly limited, and include known steps carried out when manufacturing a semiconductor device. Examples of such steps include, but are not limited to, steps for forming each structure such as metal wiring, gate structure, source structure, drain structure, insulating layer, ferromagnetic layer, and non-magnetic layer (layer formation, etching other than the above etching process, chemical mechanical polishing, modification, etc.), resist film formation, exposure step, development step, heat treatment step, cleaning step, inspection step, etc. These other steps can be appropriately carried out before or after the above etching process step, as necessary.
[0048] According to the method for manufacturing a semiconductor device of the present embodiment described above, an etching process for an object to be processed is performed using the etching solution according to the first aspect, which contains periodic acid as an oxidizing agent. The etching solution has a high stability over time in the etching rate for a SiGe compound, so that the manufacturing process, including the etching step for the SiGe compound, can be stably controlled. EXAMPLES
[0049] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0050] <Preparation of etching solution> (Examples 1 to 4, Comparative Examples 1 to 3) The components shown in Table 1 were mixed to prepare the etching solutions of the respective examples.
[0051] [Table 1]
[0052] In Table 1, the abbreviations have the following meanings: The numbers in brackets [ ] are the blend amounts (% by mass). DHF: Hydrofluoric acid NH4F: Ammonium fluoride PAA: Peracetic acid PIA: Periodic acid (H5IO6) AA: Acetic acid MSA: Methanesulfonic acid
[0053] <Etching of object to be treated (1)> A SiGe film was epitaxially grown on a silicon substrate to obtain a processed object (1) on which a SiGe film was formed. A test piece was cut from the obtained processed object (1) and the thickness of the SiGe film was measured by fluorescent X-ray analysis, and the thickness was found to be 50 nm. The etching solution of each example was placed in a beaker, and the test piece was immersed in the etching solution of each example for 5 minutes at room temperature (23°C) to perform an etching treatment. After the etching treatment, the test piece was dried by nitrogen blowing, and the thickness of the SiGe film was measured by fluorescent X-ray analysis. The etching rate (Å / min) for SiGe was calculated from the thickness of the SiGe film before and after the etching treatment. The results are shown in Table 2.
[0054] <Etching of object to be treated (2)> A test piece was cut from the SOI (100) substrate to obtain the treated object (2). The thickness of the Si film of the treated object (2) was measured by spectroscopic ellipsometry, and the thickness was 100 nm. The etching solution of each example was placed in a beaker, and the test piece was immersed in the etching solution of each example for 5 minutes at room temperature (23°C) to perform an etching treatment. After the etching treatment, the test piece was dried by nitrogen blowing, and the thickness of the Si film was measured by spectroscopic ellipsometry. The etching rate (Å / min) for Si was calculated from the thickness of the Si film before and after the etching treatment. The results are shown in Table 2.
[0055] <Etching process of the object to be processed (3)> A silicon oxide film was formed on a silicon substrate by chemical vapor deposition (CVD) to obtain an object to be processed (3). When a test piece was cut out from the obtained object to be processed (3) and the film thickness of the silicon oxide film was measured by spectroscopic ellipsometry, the film thickness was 100 nm. The etching solution of each example was put into a beaker, and the test piece was immersed in the etching solution of each example at room temperature (23 ° C) for 5 minutes to perform an etching process. After the etching process, the test piece was dried by nitrogen blowing, and the film thickness of the silicon oxide film was measured by spectroscopic ellipsometry. From the film thickness of the silicon oxide film before and after the etching process, the etching rate (Å / min) for Si was calculated. The results are shown in Table 2.
[0056] <Evaluation of etching selectivity> Based on the etching rate results obtained in the above "etching process of the object to be processed (1)", "etching process of the object to be processed (2)", and "etching process of the object to be processed (3)", the etching selectivity of the object to be processed (1) / the object to be processed (2) and the etching selectivity of the object to be processed (1) / the object to be processed (3) were calculated. The results are shown in Table 2.
[0057]
Table 2
[0058] From the results shown in Table 2, it was confirmed that the etching solutions of Examples 1 to 4 can obtain an SiGe etching selectivity equal to or higher than that of the etching solutions of Comparative Examples 1 to 3. In particular, it was confirmed that the etching solutions of Examples 3 and 4 containing a pH adjuster have an improved SiGe etching selectivity compared to the etching solutions of Comparative Examples 1 to 3.
[0059] <Evaluation of the temporal stability of the SiGe etching rate> The etching solution of Example 2 and the etching solution of Comparative Example 3 were stored in a bottle, and for each etching solution after 3 days of storage, the etching rate ER3 (Å / min) for SiGe was calculated by the same operation as in the above "Etching treatment of treated object (1)". In addition, for each etching solution 7 days after the start of storage, the etching rate ER7 (Å / min) for SiGe was calculated by the same procedure as in the above "Etching treatment of treated object (1)". The etching rate obtained in the above "etching treatment of treated object (1)" was defined as the etching rate ER0 for SiGe 0 days after the start of storage. The variation rate (%) from the etching rate ER0 was calculated for each of the etching rates ER3 and ER7. The results are shown in Table 3.
[0060] [Table 3]
[0061] From the results shown in Table 3, it was confirmed that the etching rate of the etching solution of Example 2 for SiGe hardly changed even after 7 days of storage.
Claims
1. For Si and its oxides, the general formula Si 1-x Ge x An etching solution for selectively etching a compound represented by the formula: comprising periodic acid, fluoride, and water; The etching solution has a water content of 80 mass% or more based on the total mass of the etching solution.
2. The etching solution according to claim 1 , further comprising a pH adjuster.
3. The etching solution according to claim 1 or 2 is used to form a compound having the general formula Si 1-x Ge x A method for manufacturing a semiconductor device, comprising the step of etching a processing object containing a compound represented by the formula:
Citation Information
Patent Citations
Etching agent
JP2003183652A
PAA system etching liquid, etching method utilizing it, and structure of resultant material
JP2005303305A
Formulations that selectively etch silicon germanium relative to germanium
JP2018519674A
Etchant for selective removal of silicon relative to silicon-germanium alloy from silicon-germanium / silicon stack during manufacturing of semiconductor device
JP2019050364A
Etchant for selective removal of silicon-germanium alloy from silicon-germanium / silicon stack during semiconductor device fabrication
JP2019050365A