Production method of iron-chromium-aluminum cold rolled coils in a continuous annealing and pickling line

The continuous wire annealing and pickling method addresses weldability and oxide film removal issues in 1Cr13Al4 coils by employing precise welding, annealing, and specialized pickling, achieving high-quality 1Cr13Al4 coils with improved mechanical properties and efficiency.

JP7573734B2Active Publication Date: 2024-10-25SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023516172
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-19
Filing Date
2022-05-11
Publication Date
2024-10-25
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

The production of 1Cr13Al4 iron-chromium-aluminum alloy coils on continuous annealing and pickling lines faces challenges due to poor weldability, large grain growth leading to brittleness, and the difficulty in removing a dense oxide film during annealing, which affects the quality and efficiency of the process.

Method used

A continuous wire annealing and pickling method involving precise welding, degreasing, controlled annealing, cooling, and specialized pickling processes to produce 1Cr13Al4 coils with a 2B surface, including double welding wheel resistance welding, controlled heat treatment, and the use of electrolytic sodium sulfate, nitric acid, and mixed acids for pickling.

Benefits of technology

The method enables stable production of 1Cr13Al4 coils with fine grain size and improved mechanical properties, meeting GB/T1234-2012 standards, while ensuring a 2B surface finish and reducing production costs with enhanced efficiency up to 16 tons/hour.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573734000001
    Figure 0007573734000001
  • Figure 0007573734000002
    Figure 0007573734000002
  • Figure 0007573734000003
    Figure 0007573734000003
Patent Text Reader

Abstract

The present invention includes the steps of: (1) welding two adjacent rolls of iron-chromium-aluminum cold-rolled coils to obtain a steel strip; (2) degreasing the steel strip; (3) annealing the degreasing steel strip; (4) cooling the annealing steel strip; and (5) pickling the cooled steel strip. In step (3), the degreasing steel strip is preheated to 600-800°C in a heating furnace, and then heated to a final heat treatment temperature of 880-960°C, with a holding time of 1.0-3.0 min / mm, and a tensile density in the heating furnace of 0.5-0.8 kg / mm. 2 This paper presents a continuous wire annealing and pickling production method for iron chromium aluminum cold rolled coils, which can produce 1Cr13Al4 cold coils with widths of 900-1300mm, thicknesses of 0.5-1.2mm, and coil weights of over 10 tons, with annealed grain sizes of grade 4-6 and mechanical properties that meet the requirements of GB / T1234-2012 "High Resistance Electric Heating Alloys," and the finished products have a qualified 2B surface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a patent application filed on May 19, 2021, entitled "Production method for continuous wire annealing and pickling of wide-width iron-chromium-aluminum cold-rolled coil" and bearing Chinese patent application number "202110546721.2", the entire contents of which are incorporated herein by reference.

[0002] (Technical field) The present invention relates to the technical field of iron-chromium-aluminum alloy coil processing, in particular, the present invention relates to a method for producing continuous wire annealing and pickling of wide iron-chromium-aluminum cold rolled coil, more particularly, to a method for producing continuous wire annealing and pickling of 1Cr13Al4 iron-chromium-aluminum alloy cold rolled coil. [Background technology]

[0003] 1Cr13Al4 is a common iron-chromium-aluminum alloy, with a Cr content of 12.0%-15.0% and an Al content of 4.0%-6.0%. 1Cr13Al4 has the advantages of a large resistivity coefficient, a small temperature coefficient of resistance, good heat resistance, low specific gravity, good high-temperature oxidation resistance, and low price, and is widely used in the electric heating industry.

[0004] 1Cr13Al4 is a ferritic alloy, and the grains grow rapidly at high temperatures, which makes it difficult to weld, and the temperature and heat retention time of the recrystallization annealing must be precisely controlled. In addition, the addition of Al also greatly reduces the toughness of the material, and a dense oxide film forms on the surface during annealing, which is difficult to remove by ordinary pickling methods.

[0005] Due to the poor weldability, poor toughness, narrow window for recrystallization annealing process, and surface oxide film difficult to pickle, currently, domestic and foreign manufacturers basically use the method of bright annealing on flat-type production line to produce 1Cr13Al4 cold rolled sheet. In this method, the weld bead does not bend after welding the material, so the requirements for the quality of the weld bead are low, and the surface of the steel strip is protected from oxidation by hydrogen gas or nitrogen gas during annealing. However, this method is limited by the length of the annealing furnace, the annealing efficiency is low, and electric heating and hydrogen protection are adopted during annealing, which is costly and has certain risks.

[0006] The continuous annealing and pickling line is used to produce cold-rolled 1Cr13Al4 coils with a width of 900-1300 mm, a thickness of 0.5-1.2 mm, and a winding weight of more than 10 tons, and the finished product has a 2B surface, which has not yet been applied in China. The continuous annealing and pickling production line has a large number of loopers, tension rolls, and bending rolls, and has high quality requirements for the weld beads. After crystallization, 1Cr13Al4 is prone to extremely large crystal grains, which leads to increased brittleness, so the annealing temperature and annealing speed must be accurately controlled. A dense oxide layer is formed on the surface after annealing, which cannot be cleanly pickled using ordinary stainless steel pickling methods, and the annealing speed and pickling speed must be matched. All of the above points are issues that need to be resolved in the production of cold-rolled 1Cr13Al4 in a continuous annealing and pickling line. Summary of the Invention [Means for solving the problem]

[0007] In order to solve the above problems in the prior art, the present invention provides a continuous wire annealing and pickling production method for wide iron chromium aluminum cold rolled coil, which is especially suitable for cold rolled coil of brand 1Cr13Al4. This production method can produce 1Cr13Al4 cold coil with width of 900-1300mm, thickness of 0.5-1.2mm, and winding weight of more than 10 tons, in which the steel strip is directly connected by welding, the grain size after annealing is 4-6 grade, the mechanical properties meet the requirements of GB / T1234-2012 "High resistance electric heating alloy", and the surface is treated by pickling, and the finished product has a qualified 2B surface.

[0008] The technical solution of the present invention is specifically as follows: The production method of iron chromium aluminum cold rolled coil continuous wire annealing pickling is: (1) welding two adjacent rolls of iron-chromium-aluminum cold-rolled coils to obtain a steel strip; (2) degreasing the steel strip; (3) annealing the steel strip after the degreasing treatment; (4) cooling the steel strip after the annealing treatment; and (5) pickling the cooled steel strip, In step (3), the degreased steel strip is preheated to 600-800℃ in a heating furnace, and then heated to a final heat treatment temperature of 880-960℃. The heat retention time is 1.0-3.0min / mm, and the tension density in the heating furnace is 0.5-0.8Kg / mm. 2 It is.

[0009] Optionally, before step (1), the iron-chromium-aluminum cold rolled coil is subjected to a process of neatly cutting off the unrolled portion and the cold-rolled transition portion having a thickness of ≧1.0 mm at the start and end of the winding of the iron-chromium-aluminum cold rolled coil.

[0010] Optionally, in step (1), the welding method is double welding wheel resistance welding; The thickness difference between two adjacent rolls of Fe-Cr-Aluminum cold rolled coil is less than 30%, the lap amount of the weld bead is 1.5-3mm, the welding speed is 6.5-8.5m / min, and the welding current is 3800-4800A. The main weld bead is reinforced with steel strips.

[0011] Optionally, in step (2), the temperature of the degreasing liquid used in the degreasing treatment is 60-100°C.

[0012] Optionally, in step (4), the step of cooling the steel strip after the annealing treatment includes: Cooling the steel strip to 250-400°C by air cooling, the air pressure being 2700-3500 Pa; A step of cooling the steel strip to below 120°C by high pressure mist cooling, with a water flow rate of 3-5m 3 / h, and the compressed air flow rate is 1300-1700Nm 3 / h and the pressure is 2-4 bar.

[0013] Optionally, in step (5), the pickling treatment is carried out using electrolytic sodium sulfate + electrolytic nitric acid + a mixture of nitric acid and hydrofluoric acid; For electrolytic sodium sulfate, the sodium sulfate concentration is 1.12-1.20g / L, the electrolysis current is 2000-5000A, and the temperature is 65-85℃; In electrolytic nitric acid, the nitric acid concentration is 40-90g / L, the electrolytic current is 2000-5000A, and the temperature is 45-65℃. In the mixed acid of nitric acid and hydrofluoric acid, the nitric acid concentration is 40-90g / L, the hydrofluoric acid concentration is 25-50g / L, and the temperature is 35-55°C.

[0014] Optionally, the grade of the iron chromium aluminum cold rolled coil is 1Cr13Al4.

[0015] Alternatively, the specifications of the Fe-Cr-Aluminum cold rolled coil are: width 900-1300mm, thickness 0.5-1.2mm, and coil weight 10 tons or more. Effect of the Invention

[0016] Compared with the prior art, the method for producing continuous wire annealing and pickling of iron chromium aluminum cold coil of the present invention has at least the following beneficial effects: (1) By designing the welding process, annealing process, and pickling process of 1Cr13Al4 cold rolled coil, it is possible to produce 1Cr13Al4 cold rolled coil in a continuous annealing and pickling line. (2) Welding between 1Cr13Al4 cold-rolled coils has been achieved, and the weld bead will not crack even when exposed to harsh conditions on the production line, such as tension, repeated bending, and high temperatures in the heating furnace. (3) After annealing, the cold-rolled 1Cr13Al4 steel coil has a grain size of 4-6 grade, and the mechanical properties and resistivity meet the requirements of GB / T1234-2012 "high resistance electric heating alloy". (4) After annealing, the 1Cr13Al4 surface is treated by pickling, and the finished product is qualified 2B surface. (5) Compared with other production methods, this method can reduce production costs, the production efficiency can reach 16 tons / hour, and the product performance is stable. It can produce 1Cr13Al4 cold rolled coils with a thickness range of 0.5-1.2mm and a width range of 900-1300mm. [Brief description of the drawings]

[0017] Various other benefits and advantages will become apparent to those skilled in the art upon reading the following detailed description of the preferred embodiments. The drawings are used only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the invention.

[0018] [Figure 1] Shown is the spot welding method used when lapping. [Diagram 2] FIG. 2 is a metallographic structure diagram of the material after annealing in Example 1. [Diagram 3] 1 shows the state of the weld bead of the steel strip obtained in Example 1 after annealing and pickling. [Figure 4] FIG. 1 is a metallographic structure diagram of the material after annealing in Example 2. [Diagram 5] FIG. 11 is a metallographic structure diagram of the material after annealing in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In order to fully understand the objectives, features and effects of the present invention, the present invention will be described in detail with reference to the following specific embodiments. Except for the following content, the process method of the present invention adopts all other conventional methods or devices in the art. The following noun terms have the meanings commonly understood by those skilled in the art unless otherwise specified.

[0020] The present inventors have conducted research into problems encountered in the production of cold-rolled 1Cr13Al4 iron-chromium-aluminum alloy coils with a width of 900-1300 mm, a thickness of 0.5-1.2 mm, a coil weight of 10 tons or more, and a 2B surface, using a continuous annealing and pickling line, and have found the following:

[0021] After cold rolling (for example, cold rolling by a twenty-roll Sendzimir rolling mill), the 1Cr13Al4 hot-rolled coil has about 15m of unrolled and transitional sections at the head, which are very brittle due to size effects and work hardening effects, so this section must be cut off cleanly before passing through the continuous annealing and pickling line. 1Cr13Al4 has poor weldability, so in order to prevent the steel strip from cracking due to repeated bending, tensioning, and furnace overburning when passing through the continuous annealing and pickling line, the heat input must be strictly controlled during welding, and 304 steel strips must be wrapped to reinforce the weld bead. 1Cr13Al4 belongs to ferritic steel, and the crystal grains after recrystallization are very easy to become large, but the larger the crystal grains, the greater the brittleness of the material and the greater the risk of strip breakage, so the heat treatment temperature, heat retention time, and tension in the heating furnace must be precisely controlled. During annealing, 1Cr13Al4 forms a dense oxide film on the surface, which is made of complex oxides such as Al2O3, FeO, and Cr2O3. It is necessary to use a special pickling method and pickling time to ensure that the oxide film on the surface is pickled cleanly and does not have defects due to over-pickling or over-corrosion. In addition, in ordinary annealing and pickling lines, the annealing speed and the pickling speed are consistent, so the selection of the annealing and pickling speed is particularly important, which not only ensures the material performance after annealing, but also ensures that the surface passes the pickling test.

[0022] Based on the above considerations, the present inventor proposes a method for producing cold-rolled coil of 1Cr13Al4 iron-chromium-aluminum alloy by continuous wire annealing and pickling, in which the Cr13Al4 iron-chromium-aluminum alloy has an elemental composition commonly known to those skilled in the art, and the brand is based on the national standard GB / T1234-2012 "High-resistance electric heating alloy".

[0023] In a preferred embodiment, the method for producing continuous wire annealing and pickling of cold rolled coil of 1Cr13Al4 iron chromium aluminum alloy of the present invention comprises the following steps:

[0024] (1) Welding For 1Cr13Al4 steel coil in cold rolled state, pretreatment is required before welding. Specifically, when 0.5mm≦steel coil thickness≦1.0mm, after unwinding, first cleanly cut off the unrolled part and cold rolled transition part at the beginning of winding where the actual thickness is ≧1.0mm, and ensure that there is no rolling machine stop coil mark at the part of the steel coil where the actual thickness is ≧1.0mm; when 1.0mm<steel coil thickness≦1.2mm, all unrolled parts and cold rolled transition parts must be cleanly cut off, and the end of the steel coil must also be cleanly cut off. 1Cr13Al4 has high strength, and the unrolled parts and transition parts should not be cut into steel sheets, but can be directly made into small rolls and packed to increase efficiency.

[0025] When welding, the start of the neatly cut steel coil is sent to the welding machine and welded to the end of the previous neatly cut coil. The welding method is double welding wheel resistance welding, and after the front and rear steel strips are wrapped, the welding wheel applies a large current and moves laterally to complete the welding.

[0026] Welding is a critical process, if the heat input is too large, the brittleness of the heat affected zone will increase significantly and the toughness of the weld bead will decrease, and if the heat input is too small, unfused joints will be formed. After deep research by the inventor, the following welding process is determined. That is, the thickness difference between the front and rear steel strips is less than 30%, the lap amount of the weld bead is 1.5-3mm (e.g., 1.5mm, 1.6mm, 1.7mm, 1.8mm, 1.9mm, 2.0mm, 2.1mm, 2.2mm, 2.3mm, 2.4mm, 2.5mm, 2.6mm, 2.7mm, 2.8mm, 2.9mm, 3.0mm, etc.), the welding speed is 6.5-8.5m / min (e.g., 6.5m / min, 7.0m / min, 7.5m / min, 8.0m / min, 8.5m / min, etc.), and the welding current is 3800-4800A (e.g., 3800A, 4000A, 4200A, 4400A, 4600A, 4800A, etc.). The main weld bead is reinforced with lap steel. For example, the main weld bead needs to be reinforced by welding 2-3 pieces of 304 steel strips with a thickness of 1.5-2.5 mm (for example, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, etc.) and a standard of 150 x 250 mm by manual arc welding. Spot welding is used for welding, as shown in Figure 1.

[0027] By adopting a method of double-welded wheel resistance welding + reinforcing with 304 steel strip and welding 1Cr13Al4 steel strip, the difficult problems of 1Cr13Al4's high brittleness and poor weldability are overcome and continuous production is realized.

[0028] (2) Degreasing treatment After welding, the 1Cr13Al4 steel strip is degreased in the degreasing step to clean the rolling oil on the surface of the steel strip after cold rolling. The temperature of the degreasing liquid used in the degreasing process is 60-100°C. The degreasing liquid can be obtained by purchasing it on the market, and all the degreasing liquids commonly used in this field can be applied to the present invention.

[0029] (3) Annealing treatment During annealing, the strip steel is first preheated to 600-800°C (e.g., 600°C, 650°C, 700°C, 750°C, 800°C, etc.) with hot air from the heating stage of the heating furnace, and then the strip steel is heated to the final heat treatment temperature. The temperature in the heating furnace is controlled to 880-960°C (e.g., 880°C, 900°C, 920°C, 940°C, 960°C, etc.), and the heating furnace is kept warm for 1.0-3.0 min / mm (immediately). That is, the thickness of the strip steel is 1.0-3.0 min per 1 mm, i.e., the heating furnace warming time = (1.0 min~3.0 min) x thickness of the strip steel, where the unit of thickness of the strip steel is millimeters (for example, 1.0 min / mm, 1.5 min / mm, 2.0 min / mm, 2.5 min / mm, 3.0 min / mm, etc.), and the tension density in the heating furnace is 0.5-0.8 kg / mm. 2 (For example, 0.5 kg / mm 2 , 0.6Kg / mm2, 0.7Kg / mm 2 , 0.8Kg / mm 2 etc.).

[0030] 1Cr13Al4 is a ferritic steel, if the annealing temperature is too high or the heat retention time is too long, the grains after annealing are easy to become extremely large, but the larger the grains, the more brittle the material will be, and the greater the risk of strip breakage. If the annealing temperature is low or the heat retention time is short, the grains will not fully recover, which will affect the elongation, strength and other mechanical properties of the finished product. Therefore, the annealing temperature must be accurately controlled. On the other hand, the tension in the heating furnace during annealing is also important. If the tension in the heating furnace is too large, the steel strip will be narrowed and easily deformed under the high-temperature heating environment in the heating furnace. If the tension in the heating furnace is too small, the steel strip will be prone to quality accidents such as meandering in the heating furnace or pulling the ends. Therefore, the tension in the heating furnace must be strictly controlled. The tension setting in the heating furnace should refer to the density, high-temperature strength and other data of the steel strip.

[0031] (4) Cooling After the high temperature insulation is finished, first use the blower to rapidly cool the steel strip (for example, cool the steel strip to 250-400℃ within 1 minute), and then set the wind pressure to 2700-3500Pa (for example, 2700Pa, 2800Pa, 2900Pa, 3000Pa, 3100Pa, 3200Pa, 3300Pa, 3400Pa, 3500Pa, etc.), air-cool the steel strip to 250-400℃, and continue high-pressure mist cooling, with a water flow rate of 3-5m 3 / h, for example, 3m 3 / h, 4m 3 / h, 5m 3 / h, etc., and the compressed air flow rate is 1300-1700Nm 3 / h, for example, 1300Nm 3 / h, 1400Nm 3 / h, 1500Nm 3 / h, 1600Nm 3 / h, 1700Nm 3 / h, etc., and the pressure is 2-4 bar, for example, 2 bar, 3 bar, 4 bar, etc. After cooling to 120°C by mist cooling, the steel strip comes out.

[0032] After the high temperature insulation is completed, rapid cooling should be performed to prevent the growth of crystal grains and to prevent the formation of precipitates such as A' during cooling, which could affect the performance of the material.

[0033] (5) Pickling For pickling, electrolytic sodium sulfate + electrolytic nitric acid + a mixture of nitric acid and hydrofluoric acid are used.

[0034] In electrolytic sodium sulfate, the sodium sulfate concentration is 1.12-1.20g / L (e.g., 1.12g / L, 1.13g / L, 1.14g / L, 1.15g / L, 1.16g / L, 1.17g / L, 1.18g / L, 1.19g / L, 1.20g / L, etc.) and the electrolysis current is 2000-5000A (e.g., 2000A, 2500A, 300 0A, 3500A, 4000A, 4500A, 5000A, etc.), temperature is 65-85°C (e.g., 65°C, 70°C, 75°C, 80°C, 85°C, etc.), and pickling time is 1.5-5min (e.g., 1.5min, 2.0min, 2.5min, 3.0min, 3.5min, 4.0min, 4.5min, 5.0min, etc.).

[0035] In electrolytic nitric acid, the nitric acid concentration is 40-90g / L (e.g., 40g / L, 45g / L, 50g / L, 55g / L, 60g / L, 65g / L, 70g / L, 75g / L, 80g / L, 85g / L, 90g / L, etc.), the electrolysis current is 2000-5000A (e.g., 2000A, 2500A, 3000A, 3500A, 4000A, 4500A, 5000A, etc.), the temperature is 45-65°C (e.g., 45°C, 50°C, 55°C, 60°C, 65°C, etc.), and the pickling time is 0.5-1.7min (e.g., 0.5min, 0.7min, 0.9min, 1.1min, 1.3min, 1.5min, 1.7min, etc.).

[0036] In the process of electrolytic pickling, the 1Cr13Al4 steel strip serves as the anode to carry out the electrolytic reaction, mainly dissolving the chromium oxide on the surface, and the reaction generates oxygen, which causes the iron scale to peel off. The electrolytic current, concentration and temperature mainly affect the speed and progress of the reaction.

[0037] In the mixed acid of nitric acid and hydrofluoric acid, the nitric acid concentration is 40-90g / L (e.g., 40g / L, 45g / L, 50g / L, 55g / L, 60g / L, 65g / L, 70g / L, 75g / L, 80g / L, 85g / L, 90g / L, etc.), the hydrofluoric acid concentration is 25-50g / L (e.g., 25g / L, 30g / L, 35g / L, 40g / L, 45g / L, 50g / L, etc.), the temperature is 35-55°C (e.g., 35°C, 40°C, 45°C, 50°C, 55°C, etc.), and the pickling time is 1.3-4min (e.g., 1.3min, 2.0min, 2.5min, 3.0min, 3.5min, 4.0min, etc.).

[0038] Mixed acids are mainly used to dissolve iron and aluminum oxides and obtain the surface required for the final product. The above acid concentration is significantly different from that used when pickling normal stainless steel, mainly because aluminum oxide is dense and difficult to pickle.

[0039] By using a special pickling method, using electrolytic sodium sulfate + electrolytic nitric acid + mixed acid of nitric acid and hydrofluoric acid, the dense oxide layer formed on the surface during annealing of 1Cr13Al4 can be removed by pickling.

[0040] According to the production method of the present invention, the iron chromium aluminum cold rolled steel coil with the grade of 1Cr13Al4, the thickness range of 0.5-1.2mm, the width range of 900-1300mm can be produced, and the production efficiency can reach 16 tons / hour. And, according to the above production method, the grain of the steel coil obtained is relatively fine and uniform, the grain size is 4-6 grade, the corresponding A50 elongation is 30-35%, the yield strength Rp0.2 is 445-465MPa, the tensile strength Rm is 600-620MPa, and the mechanical properties meet the requirements of GB / T1234-2012 "High Resistance Electrical Heat Alloy".

[0041] [Example] The present invention will be further described below with reference to examples, but the present invention is not limited to the scope of the above examples. In the following examples, the experimental methods for which no specific conditions are specified are selected according to the usual methods and conditions or product instructions.

[0042] First, it should be noted that in the following examples, the grain size, A50, yield strength, tensile strength and surface grade are all determined with reference to GB / T1234-2012 "High resistance electric heating alloys."

[0043] [Example 1] The raw material is a cold-rolled 1Cr13Al4 coil with a thickness of 1.0 mm, width of 1240 mm, and wound weight of 14 tons. This coil is rolled from a hot-rolled coil with a thickness of 3.5 mm on a 20-roll Sendzimir rolling mill. Its chemical composition, in mass%, is as follows: C: 0.0143%, Cr: 13.8%, Al: 5.2922%, Si: 0.1787%, Mn: 0.0759%, P: 0.0114%, S: 0.001%, Ti: 0.3174%, N: 0.0024%, and the remainder is Fe and other unavoidable impurities.

[0044] The production method of this embodiment is as follows. (1) After unwinding the cold-rolled 1Cr13Al4 coil, first, the unrolled part and the cold-rolled transition part at the start of winding where the actual thickness is ≧1.0 mm are neatly cut off, and it is ensured that there are no traces of the rolling mill's stopped coil in the part of the coil where the actual thickness is ≧1.0 mm. The unrolled part and the transition part are wound into small coils and then packed.

[0045] The beginning of the cleanly cut coil is sent to the welding machine, and the end of the 1.0 mm thick 1Cr13Al4 cold rolled coil, cleanly cut in the same way as before, is welded by double welding wheel resistance welding, where the lap amount of the weld bead is 2 mm, the welding speed is 7.0 m / min, and the welding current is 4200 A. The main weld bead needs to be reinforced by welding two 2.0 mm thick, 200 mm standard 304 steel strips by manual arc welding, and the welding method is spot welding.

[0046] (2) After welding, the 1Cr13Al4 steel strip was degreased in the degreasing stage, and the rolling oil on the surface of the steel strip after cold rolling was washed off. The temperature of the degreasing liquid was 80°C.

[0047] (3) During annealing, the strip steel is first preheated to 700°C with hot air from the heating stage of the heating furnace, and then the strip steel is heated to the final heat treatment temperature. The temperature in the heating furnace is controlled to 950°C, the heating furnace warming time is 1.5 min / mm, the annealing speed is 30 m / min, and the tension density in the heating furnace is 0.65 kg / mm 2 The metal structure after annealing is shown in Figure 2. As can be seen from Figure 2, the strip steel has been annealed and meets the mechanical performance requirements.

[0048] (4) After the high temperature insulation is completed, the steel strip is first rapidly cooled by a blower, the wind pressure is set to 3000 Pa, the steel strip is air-cooled to 350°C, and high-pressure mist cooling is continued, the water flow rate is 4 m 3 / h, compressed air flow rate is 1500Nm 3 / h, pressure 3 bar. After cooling to 80°C by mist cooling, the steel strip emerged.

[0049] (5) For pickling, electrolytic sodium sulfate + electrolytic nitric acid + mixed acid of nitric acid and hydrofluoric acid are used, where the electrolytic sodium sulfate has a sodium sulfate concentration of 1.13 g / L, the electrolytic current is 2000 A, and the temperature is 75°C, the electrolytic nitric acid has a nitric acid concentration of 55 g / L, the electrolytic current is 5000 A, and the temperature is 55°C, and the mixed acid has a nitric acid concentration of 60 g / L, a hydrofluoric acid concentration of 33 g / L, and the temperature is 50°C.

[0050] The production method of this embodiment can smoothly carry out continuous production of steel coils, the steel strip is connected by direct welding, the grain size after annealing is grade 5, the A50 elongation is 31%, the yield strength Rp0.2 is 455MPa, and the tensile strength Rm is 612MPa, which meets the mechanical performance requirements of GB / T1234-2012 ``High resistance electric heating alloy'', and the surface is treated by pickling treatment, and the finished product has a qualified 2B surface.

[0051] The weld bead of the steel strip produced in this embodiment is annealed, pickled, and wound on the tail. As shown in FIG. 3, the weld bead does not crack even after being subjected to severe conditions such as tension, repeated bending, and high temperatures in a heating furnace.

[0052] [Example 2] The raw material is a cold-rolled 1Cr13Al4 coil with a thickness of 0.8 mm, width of 1255 mm, and wound weight of 15 tons. This coil is rolled from a hot-rolled coil with a thickness of 3.5 mm on a 20-roll Sendzimir rolling mill. Its chemical composition, in mass%, is C: 0.025%, Cr: 13.7749%, Al: 5.0072%, Si: 0.0889%, Mn: 0.0835%, P: 0.0155%, S: 0.0011%, Ti: 0.2519%, N: 0.0043%, and the remainder is Fe and other unavoidable impurities.

[0053] The production method of this embodiment is as follows. (1) After unwinding the cold-rolled 1Cr13Al4 coil, first, the unrolled part and the cold-rolled transition part at the start of winding where the actual thickness is ≧1.0 mm are neatly cut off, and it is ensured that there are no traces of the rolling mill's stopped coil in the part of the coil where the actual thickness is ≧1.0 mm. The unrolled part and the transition part are wound into small coils and then packed.

[0054] The beginning of the cleanly cut coil is sent to the welding machine, and the end of the 1.0 mm thick 1Cr13Al4 cold rolled coil, cleanly cut in the same way as before, is welded by double welding wheel resistance welding, where the lap amount of the weld bead is 2 mm, the welding speed is 7.2 m / min, and the welding current is 4100 A. The main weld bead needs to be reinforced by welding two 2.0 mm thick, 200 mm standard 304 steel strips by manual arc welding, and the welding method is spot welding.

[0055] (2) After welding, the 1Cr13Al4 steel strip was degreased in the degreasing stage, and the rolling oil on the surface of the steel strip after cold rolling was washed off. The temperature of the degreasing liquid was 80°C.

[0056] (3) During annealing, the strip steel is first preheated to 700°C with hot air from the heating stage of the heating furnace, and then the strip steel is heated to the final heat treatment temperature. The temperature in the heating furnace is controlled to 940°C, the heating furnace warming time is 1.75min / mm, the annealing speed is 32m / min, and the tension density in the heating furnace is 0.6Kg / mm 2 The metal structure after annealing is shown in Figure 4. As can be seen from Figure 4, the strip steel has been annealed and meets the mechanical performance requirements.

[0057] (4) After the high temperature insulation is completed, the steel strip is first rapidly cooled by a blower, the wind pressure is set to 2900 Pa, the steel strip is air-cooled to 350°C, and high-pressure mist cooling is continued, the water flow rate is 4 m 3 / h, compressed air flow rate is 1500Nm 3 / h, pressure 3 bar. After cooling to 80°C by mist cooling, the steel strip emerged.

[0058] (5) For pickling, electrolytic sodium sulfate + electrolytic nitric acid + mixed acid of nitric acid and hydrofluoric acid are used, where the electrolytic sodium sulfate has a sodium sulfate concentration of 1.12 g / L, the electrolytic current is 2000 A, and the temperature is 75°C, the electrolytic nitric acid has a nitric acid concentration of 64 g / L, the electrolytic current is 5000 A, and the temperature is 55°C, and the mixed acid has a nitric acid concentration of 55 g / L, a hydrofluoric acid concentration of 32.5 g / L, and the temperature is 51°C.

[0059] The production method of this embodiment can smoothly carry out continuous production of steel coils, the steel strip is connected by direct welding, the grain size after annealing is grade 5, the A50 elongation is 32%, the yield strength Rp0.2 is 466MPa, and the tensile strength Rm is 606MPa, which meets the mechanical performance requirements of GB / T1234-2012 ``High resistance electric heating alloy'', and the surface is treated by pickling treatment, and the finished product has a qualified 2B surface.

[0060] [Example 3] The raw material is a cold-rolled 1Cr13Al4 coil with a thickness of 1.2 mm, width of 1262 mm, and wound weight of 15 tons. This coil is rolled from a hot-rolled coil with a thickness of 3.5 mm on a 20-roll Sendzimir rolling mill. Its chemical composition, in mass%, is C: 0.0191%, Cr: 13.6657%, Al: 5.1831%, Si: 0.103%, Mn: 0.0808%, P: 0.0144%, S: 0.001%, Ti: 0.2373%, N: 0.002%, and the remainder is Fe and other unavoidable impurities.

[0061] The production method of this embodiment is as follows. (1) After the cold-rolled 1Cr13Al4 coil is unwound, first, all the unrolled parts and cold-rolled transition parts are neatly cut off, and the unrolled parts and transition parts are wound into small coils to ensure that there are no traces of the rolling mill's stopped coil on the coil, and then the coil is packed.

[0062] The beginning of the cleanly cut coil is sent to the welding machine, and the end of the 1.0 mm thick 1Cr13Al4 cold rolled coil, cleanly cut in the same way as before, is welded by double welding wheel resistance welding, where the lap amount of the weld bead is 2 mm, the welding speed is 7.0 m / min, and the welding current is 4300 A. The main weld bead needs to be reinforced by welding two 2.0 mm thick, 200 mm standard 304 steel strips by manual arc welding, and the welding method is spot welding.

[0063] (2) After welding, the 1Cr13Al4 steel strip was degreased in the degreasing stage, and the rolling oil on the surface of the steel strip after cold rolling was washed off. The temperature of the degreasing liquid was 80°C.

[0064] (3) During annealing, the strip steel is first preheated to 700°C with hot air from the heating stage of the heating furnace, and then the strip steel is heated to the final heat treatment temperature. The temperature in the heating furnace is controlled to 950°C, the heating furnace warming time is 1.5 min / mm, the annealing speed is 25 m / min, and the tension density in the heating furnace is 0.68 kg / mm 2 The metal structure after annealing is shown in Figure 5. As can be seen from Figure 5, the strip steel has been annealed and meets the mechanical performance requirements.

[0065] (4) After the high temperature insulation is completed, the steel strip is first rapidly cooled by a blower, the wind pressure is set to 3100 Pa, the steel strip is air-cooled to 350°C, and then high-pressure mist cooling is continued, with the water flow rate set to 4 m 3 / h, compressed air flow rate is 1500Nm 3 / h, pressure 3 bar. After cooling to 80°C by mist cooling, the steel strip emerged.

[0066] (5) For pickling, electrolytic sodium sulfate + electrolytic nitric acid + mixed acid of nitric acid and hydrofluoric acid are used, where the electrolytic sodium sulfate has a sodium sulfate concentration of 1.12 g / L, the electrolytic current is 2000 A, and the temperature is 75°C, the electrolytic nitric acid has a nitric acid concentration of 60 g / L, the electrolytic current is 5000 A, and the temperature is 55°C, and the mixed acid has a nitric acid concentration of 62 g / L, a hydrofluoric acid concentration of 34.7 g / L, and the temperature is 52°C.

[0067] The production method of this embodiment can smoothly carry out continuous production of steel coils, the steel strip is connected by direct welding, the grain size after annealing is grade 5, the A50 elongation is 32%, the yield strength Rp0.2 is 446MPa, and the tensile strength Rm is 597MPa, which meets the mechanical performance requirements of GB / T1234-2012 ``High resistance electric heating alloy'', and the surface is treated by pickling treatment, and the finished product has a qualified 2B surface.

[0068] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above examples. Any substitutions, modifications, combinations, changes, simplifications, etc. made without departing from the spirit and principles of the present invention are equivalent replacement forms and should be included in the protection scope of the present invention.

[0069] (Additional Note) (Appendix 1) (1) welding two adjacent rolls of iron-chromium-aluminum cold-rolled coils to obtain a steel strip; (2) degreasing the steel strip; (3) annealing the steel strip after the degreasing treatment; (4) cooling the steel strip after the annealing treatment; and (5) pickling the cooled steel strip, In step (3), the degreased steel strip is preheated to 600-800℃ in a heating furnace, and then heated to a final heat treatment temperature of 880-960℃. The heat retention time is 1.0-3.0min / mm, and the tension density in the heating furnace is 0.5-0.8Kg / mm. 2 That is, The present invention relates to a method for producing continuous wire annealed and pickled iron chromium aluminum cold rolled coil.

[0070] (Appendix 2) Before step (1), the iron-chromium-aluminum cold-rolled coil is subjected to a process of neatly cutting off the unrolled parts and cold-rolled transition parts having a thickness of ≧1.0 mm at the start and end of the winding of the iron-chromium-aluminum cold-rolled coil; 2. The production method according to claim 1.

[0071] (Appendix 3) In step (1), the welding method is double welding wheel resistance welding; The thickness difference between two adjacent rolls of Fe-Cr-Aluminum cold rolled coil is less than 30%, the lap amount of the weld bead is 1.5-3mm, the welding speed is 6.5-8.5m / min, and the welding current is 3800-4800A. The main weld bead is reinforced with steel strips. 2. The production method according to claim 1.

[0072] (Appendix 4) In step (2), the temperature of the degreasing solution used in the degreasing process is 60-100°C; 2. The production method according to claim 1.

[0073] (Appendix 5) In step (4), the step of cooling the steel strip after the annealing treatment includes: Cooling the steel strip to 250-400°C by air cooling, the air pressure being 2700-3500 Pa; A step of cooling the steel strip to below 120°C by high pressure mist cooling, with a water flow rate of 3-5m 3 / h, and the compressed air flow rate is 1300-1700Nm 3 / h and the pressure is 2-4 bar, 2. The production method according to claim 1.

[0074] (Appendix 6) In step (5), the pickling treatment is carried out using electrolytic sodium sulfate + electrolytic nitric acid + a mixture of nitric acid and hydrofluoric acid; For electrolytic sodium sulfate, the sodium sulfate concentration is 1.12-1.20g / L, the electrolysis current is 2000-5000A, and the temperature is 65-85℃; In electrolytic nitric acid, the nitric acid concentration is 40-90g / L, the electrolytic current is 2000-5000A, and the temperature is 45-65℃. For the mixed acid of nitric acid and hydrofluoric acid, the nitric acid concentration is 40-90g / L, the hydrofluoric acid concentration is 25-50g / L, and the temperature is 35-55℃. 2. The production method according to claim 1.

[0075] (Appendix 7) The grade of iron chrome aluminum cold rolled coil is 1Cr13Al4. 2. The production method according to claim 1.

[0076] (Appendix 8) The specifications of the cold rolled FeCrAl coil are: width 900-1300mm, thickness 0.5-1.2mm, and winding weight more than 10 tons. 2. The production method according to claim 1.

Claims

1. (1) welding two adjacent iron-chromium-aluminum cold-rolled coils to obtain a steel strip; (2) a step of degreasing the steel strip; (3) annealing the steel strip after the degreasing treatment; (4) cooling the steel strip after the annealing treatment; (5) pickling the cooled steel strip; In step (3), the degreased steel strip is preheated to 600-800°C in a heating furnace, and then heated to a final heat treatment temperature of 880-960°C. The holding time at the final heat treatment temperature is 1.0-3.0 min / mm, and the tension density in the heating furnace is 0.5-0.8 kg / mm. 2 That is, A method for producing iron-chromium-aluminum cold rolled coils in a continuous annealing and pickling line, comprising:

2. Before step (1), the iron-chromium-aluminum cold-rolled coil is subjected to a process of neatly cutting off the unrolled portion and the cold-rolled transition portion having a thickness of ≧1.0 mm at the start and end of the winding of the iron-chromium-aluminum cold-rolled coil; 2. The method of claim 1.

3. In step (1), the welding method is double welding wheel resistance welding; The thickness difference between two adjacent turns of the iron-chromium-aluminum cold rolled coil is not more than 30%, the lap amount of the weld bead is 1.5-3 mm, the welding speed is 6.5-8.5 m / min, and the welding current is 3800-4800 A. The main weld bead is reinforced with steel strips.

2. The method of claim 1.

4. In step (2), the temperature of the degreasing solution used in the degreasing process is 60-100°C; 2. The method of claim 1.

5. In step (4), the step of cooling the steel strip after the annealing treatment includes: Cooling the steel strip to 250-400°C by air cooling, the air pressure being 2700-3500 Pa; A step of cooling the steel strip to below 120°C by high pressure mist cooling, with a water flow rate of 3-5m 3 / h, and the compressed air flow rate is 1300-1700 Nm 3 / h, and the pressure of the compressed air is 2-4 bar; 2. The method of claim 1.

6. In step (5), the pickling treatment is performed using electrolytic sodium sulfate + electrolytic nitric acid + a mixture of nitric acid and hydrofluoric acid; For electrolytic sodium sulfate, the sodium sulfate concentration is 1.12-1.20 g / L, the electrolysis current is 2000-5000 A, and the temperature is 65-85° C. In the electrolytic nitric acid, the nitric acid concentration is 40-90 g / L, the electrolytic current is 2000-5000 A, and the temperature is 45-65° C. For the mixed acid of nitric acid and hydrofluoric acid, the nitric acid concentration is 40-90 g / L, the hydrofluoric acid concentration is 25-50 g / L, and the temperature is 35-55°C.

2. The method of claim 1.

7. The grade of iron chrome aluminum cold rolled coil is 1Cr13Al4.

2. The method of claim 1.

8. The specifications of the iron-chromium-aluminum cold rolled coil are: width 900-1300mm, thickness 0.5-1.2mm, and winding weight 10 tons or more.

2. The method of claim 1.

Citation Information

Patent Citations

  • Method for continuous pickling of double-phase stainless steel coil

    CN101709477A

  • Method for processing ferrochrome aluminum cold-rolled strip

    CN107287407A

  • Manufacturing method for continuous annealing and pickling of wide steel strip iron-chromium-aluminum alloy hot coil

    CN112267008A

  • Continuous annealing unit for hoop