Method for producing a second dehydrated superabsorbent polymer for a superabsorbent recycled polymer, and method for producing a superabsorbent recycled polymer

The method addresses the challenges of recycling superabsorbent polymers by employing primary and secondary dehydration steps with acids and metal ions, resulting in a highly absorbent recycled polymer with reduced excrement and improved water absorption.

JP7573817B2Active Publication Date: 2024-10-28UNI CHARM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021126208
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-30
Publication Date
2024-10-28
Estimated Expiration
2041-07-30

AI Technical Summary

Technical Problem

Existing methods for recycling superabsorbent polymers from used sanitary products face challenges such as low dehydration efficiency, residual excrement, and separation issues between pulp fibers and superabsorbent polymers, leading to high energy consumption and incomplete recycling.

Method used

A method involving primary and secondary dehydration steps, where superabsorbent polymers are first dehydrated using an acid and then further dehydrated with a polyvalent metal ion source, followed by treatment with an alkali metal ion source to form a superabsorbent recycled polymer.

Benefits of technology

This method effectively reduces residual excrement and improves dehydration efficiency, enabling the production of a highly absorbent recycled polymer with minimal ash content and enhanced water absorption capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573817000001
    Figure 0007573817000001
Patent Text Reader

Abstract

To provide a method for producing secondarily dehydrated highly water-adsorbent polymer for highly water-adsorbent recycled polymer, which can easily form a highly adsorbent recycled polymer with little amount of residual excrement.SOLUTION: Provided is a method for producing secondarily dehydrated highly water-adsorbent polymer for a highly water-adsorbent recycled polymer, comprising: a preparation step where a primarily dehydrated highly water-absorbent polymer is prepared by forming the primarily dehydrated highly water-adsorbent polymer by immersing constituent materials of a sanitary article in an aqueous acid-containing solution and separating the primarily dehydrated highly water-adsorbent polymer from the constituent materials of the sanitary article; and a secondary dehydration step of forming a secondarily dehydrated highly water-adsorbent polymer by contacting the primarily dehydrated highly water-adsorbing polymer with a polyvalent metal ion supply source which can supply multivalent metal ions to further dehydrate the primarily dehydrated highly water-adsorbent polymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a second dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer, a method for producing a superabsorbent recycled polymer, and a method for producing a superabsorbent recycled polymer from used sanitary products that contain pulp fibers and a superabsorbent polymer having acid groups. [Background technology]

[0002] Recycling of materials that make up used sanitary products is being considered. For example, Patent Document 1 discloses a method for regenerating a superabsorbent polymer inactivated by acid into a superabsorbent recycled polymer having a predetermined water absorption, the method including a preparation step of preparing a superabsorbent polymer having acid groups and inactivated by acid, a superabsorbent recycled polymer formation step of adding an alkali metal ion source capable of supplying alkali metal ions to an aqueous regeneration solution containing the superabsorbent polymer inactivated by acid, and forming the superabsorbent recycled polymer in a wet state from the superabsorbent polymer inactivated by acid, and a drying step of drying the superabsorbent recycled polymer in a wet state to form the superabsorbent recycled polymer having the predetermined water absorption (Claim 1).

[0003] Furthermore, Patent Document 2 discloses a method for treating a water absorbent resin, characterized in that an alkali metal salt of a weak acid is added to and mixed with an agglomerate of a water absorbent resin powder formed by agglomeration of the water absorbent resin powder through absorption of water (Claim 1), and that the agglomerate of the water absorbent resin powder has been subjected to a dehydration treatment with a divalent metal salt (Claim 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-135046 A [Patent Document 2] JP 2015-4034 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the method described in Patent Document 1, the superabsorbent polymer is inactivated (dehydrated) with acid, so ash is less likely to remain in the recycled pulp fibers. However, the degree of dehydration of the superabsorbent polymer tends to be low, which may lead to residual excrement, and the drying energy required to form the superabsorbent recycled polymer tends to be large. In addition, in the method described in Patent Document 2, although the degree of dehydration of the superabsorbent polymer is high, the separation of the pulp fibers and the superabsorbent polymer is likely to be insufficient, and the pulp fibers tend to remain in the superabsorbent polymer. In addition, when forming recycled pulp fibers, ash tends to remain in the recycled pulp fibers.

[0006] Therefore, an object of the present disclosure is to provide a method for producing a secondarily dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer, which can easily form a superabsorbent recycled polymer with a low residual amount of excrement. [Means for solving the problem]

[0007] The present inventors have discovered a method for producing a secondarily dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer, the method comprising the steps of: immersing a sanitary product component material constituting a sanitary product, the sanitary product component material including pulp fibers and a superabsorbent polymer having acid groups, in an acid-containing aqueous solution containing an acid to form a first-dehydrated superabsorbent polymer; and separating the first-dehydrated superabsorbent polymer from the sanitary product component material, to prepare the first-dehydrated superabsorbent polymer; and a second-dehydration step of contacting the first-dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the first-dehydrated superabsorbent polymer and form the second-dehydrated superabsorbent polymer. Effect of the Invention

[0008] The method of producing a secondarily dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer according to the present disclosure can easily form a superabsorbent recycled polymer with a small amount of residual excrement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Specifically, the present disclosure relates to the following aspects: [Aspect 1] A method for producing a second dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer, comprising: a preparation step of preparing a primarily dehydrated superabsorbent polymer by immersing a sanitary product component material constituting a sanitary product, the sanitary product component material including pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution containing an acid to form a primarily dehydrated superabsorbent polymer, and separating the primarily dehydrated superabsorbent polymer from the sanitary product component material; a secondary dehydration step of contacting the first dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the first dehydrated superabsorbent polymer to form the second dehydrated superabsorbent polymer; The above method, comprising:

[0010] In the above-mentioned manufacturing method, in order to produce a superabsorbent recycled polymer, a superabsorbent polymer that has been primarily dehydrated with an acid is prepared, and then the primarily dehydrated superabsorbent polymer is further dehydrated using a polyvalent metal ion source to form a secondarily dehydrated superabsorbent polymer. The secondarily dehydrated superabsorbent polymer has a lower water content (higher dehydration rate) than when dehydrated using only an acid (same type and amount of acid) or when dehydrated using a polyvalent metal ion source (same type and amount of polyvalent metal ion source), i.e., the amount of remaining excrement is smaller, and thus the amount of remaining excrement in the superabsorbent recycled polymer can be reduced. Moreover, the secondarily dehydrated superabsorbent polymer formed by the above-mentioned method can be easily converted into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like. In this specification, the "primarily dehydrated superabsorbent polymer" and the "secondarily dehydrated superabsorbent polymer" may be referred to as the "primarily dehydrated superabsorbent polymer" and the "secondarily dehydrated superabsorbent polymer", respectively.

[0011] [Aspect 2] The method according to aspect 1, wherein in the secondary dehydration step, the primarily dehydrated superabsorbent polymer is further dehydrated to a moisture content of 50.0 to 80.0 mass % to form the secondarily dehydrated superabsorbent polymer.

[0012] In the above-mentioned manufacturing method, the first dehydrated superabsorbent polymer is further dehydrated to a predetermined moisture content to form a second dehydrated superabsorbent polymer, so that the amount of remaining excrement in the second dehydrated superabsorbent polymer and, in turn, in the superabsorbent recycled polymer can be reduced. In addition, the second dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method can be easily formed into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like.

[0013] [Aspect 3] 3. The method of claim 1 or 2, wherein the polyvalent metal ion source is an alkaline earth metal salt or a hydroxide of a transition metal, a salt of an alkaline earth metal salt or a hydroxide of a transition metal and an acid, or an alkaline earth metal salt or an oxide of a transition metal.

[0014] In the above-mentioned manufacturing method, since the polyvalent metal ion source is selected from a predetermined source, the amount of remaining excrement in the secondarily dehydrated superabsorbent polymer and, in turn, in the superabsorbent recycled polymer can be reduced. In addition, the secondarily dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method can be easily formed into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like.

[0015] [Aspect 4] The method according to any one of aspects 1 to 3, wherein in the second dehydration step, the first dehydrated superabsorbent polymer is contacted with the polyvalent metal ion source or an aqueous solution of the polyvalent metal ion source to form the second dehydrated superabsorbent polymer.

[0016] In the above-mentioned manufacturing method, the first dehydrated superabsorbent polymer is contacted with a polyvalent metal ion source itself or an aqueous solution thereof, so that the amount of excrement remaining in the second dehydrated superabsorbent polymer and, in turn, in the superabsorbent recycled polymer can be reduced. In addition, the second dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method can be easily formed into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like.

[0017] [Aspect 5] The method of embodiment 4, wherein the second dehydration step further comprises a drying step of drying the second dehydrated superabsorbent polymer. In the above-mentioned manufacturing method, since the secondary dehydration step further includes a predetermined drying step, the moisture content of the secondary dehydrated superabsorbent polymer can be further reduced, and the amount of remaining excrement in the secondary dehydrated superabsorbent polymer and, in turn, in the superabsorbent recycled polymer can be further reduced. In addition, when the secondary dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method is contacted with an alkali metal ion source to form the superabsorbent recycled polymer, the amount of the alkali metal ion source used can be reduced.

[0018] [Aspect 6] A method according to any one of aspects 1 to 5, wherein in the preparation step, the primarily dehydrated superabsorbent polymer has a moisture content of more than 80.0% by mass and not more than 97.0% by mass.

[0019] In the above-mentioned manufacturing method, since the first dehydrated superabsorbent polymer has a predetermined moisture content in the preparation step, it is easy to reduce the moisture content of the second dehydrated superabsorbent polymer (the amount of remaining excrement is easy to reduce), and thus the amount of remaining excrement in the superabsorbent recycled polymer can be reduced. In addition, the second dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method can be easily formed into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like.

[0020] [Aspect 7] The method according to any one of aspects 1 to 6, further comprising a primary dehydration step, prior to the preparation step, of immersing the sanitary product constituent material in the acid-containing aqueous solution to form the primarily dehydrated superabsorbent polymer and separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material.

[0021] The above-mentioned manufacturing method further includes a predetermined first dehydration step, so that the amount of excrement remaining in the second dehydrated superabsorbent polymer, and therefore in the superabsorbent recycled polymer, can be reduced. In addition, the second dehydrated superabsorbent polymer formed by the above-mentioned manufacturing method can be easily formed into a superabsorbent recycled polymer by contacting it with an alkali metal ion source or the like.

[0022] [Aspect 8] The method according to any one of aspects 1 to 7, further comprising, after the second dehydration step, mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regenerating solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer.

[0023] The above-mentioned manufacturing method further includes a predetermined step of forming a highly absorbent recycled polymer, and can easily form a highly absorbent recycled polymer that has a small amount of remaining excrement.

[0024] [Aspect 9] The method according to aspect 8, wherein the alkali metal ion source is (i) a hydroxide of an alkali metal having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion, (ii) a salt of a hydroxide of an alkali metal having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion and an acid having a larger acid dissociation constant than the acid group of the superabsorbent polymer, or (iii) an oxide of an alkali metal having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion.

[0025] In the above-mentioned manufacturing method, since the alkali metal source is selected from a predetermined source, the polyvalent metal ions crosslinking the acid groups of the secondary dehydrated superabsorbent polymer can be easily replaced with alkali metal ions, and the superabsorbent recycled polymer has excellent water absorption properties. As a result, a superabsorbent recycled polymer with excellent water absorption properties and a small amount of residual excrement can be easily formed.

[0026] [Aspect 10] 10. The method of embodiment 9, wherein the alkali metal ions are selected from the group consisting of lithium ions, sodium ions, and potassium ions, and any combination thereof.

[0027] In the above-mentioned manufacturing method, the alkali metal ions are selected from predetermined ones, so that a highly water-absorbent recycled polymer having excellent water absorbency and a small amount of residual excrement can be easily formed.

[0028] [Aspect 11] A method for producing a recycled superabsorbent polymer, comprising the steps of: a preparation step of preparing a second dehydrated superabsorbent polymer obtained by immersing a sanitary product constituent material that constitutes a sanitary product, the second dehydrated superabsorbent polymer being obtained by immersing the sanitary product constituent material, the sanitary product constituent material including pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution that contains an acid to form a first dehydrated superabsorbent polymer, separating the first dehydrated superabsorbent polymer from the sanitary product constituent material, and contacting the first dehydrated superabsorbent polymer with a polyvalent metal ion supply source capable of supplying polyvalent metal ions to further dehydrate the first dehydrated superabsorbent polymer; a step of forming the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer by mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution; The above method, comprising:

[0029] The above-mentioned manufacturing method can easily form a highly water-absorbent recycled polymer that leaves a small amount of excrement behind.

[0030] [Aspect 12] A method for producing a recycled superabsorbent polymer from a used sanitary product containing pulp fibers and a superabsorbent polymer having acid groups, comprising the steps of: a primary dehydration step of immersing a sanitary product constituent material that constitutes the sanitary product, the sanitary product constituent material including the pulp fiber and the superabsorbent polymer, in an acid-containing aqueous solution that contains an acid to form a primarily dehydrated superabsorbent polymer, and separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material; a secondary dehydration step of contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the primarily dehydrated superabsorbent polymer to form a secondarily dehydrated superabsorbent polymer; a step of forming the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer by mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution; The above method, comprising:

[0031] The above-mentioned manufacturing method can easily form a highly water-absorbent recycled polymer that leaves a small amount of excrement behind.

[0032] The following provides a detailed description of (i) a method for producing a secondarily dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer (hereinafter, may be referred to as a "method for producing a secondarily dehydrated superabsorbent polymer"), (ii) a method for producing a superabsorbent recycled polymer (hereinafter, may be referred to as a "method for producing a superabsorbent recycled polymer"), and (iii) a method for producing a superabsorbent recycled polymer from used sanitary products that contain pulp fibers and a superabsorbent polymer having acid groups (hereinafter, may be referred to as a "method for producing a superabsorbent recycled polymer from used sanitary products"), which relate to the present disclosure.

[0033] For ease of explanation, the following will be explained in the order of (iii) a method for producing a highly absorbent recycled polymer from used sanitary products, (i) a method for producing a secondarily dehydrated highly absorbent polymer, and (ii) a method for producing a highly absorbent recycled polymer. The above three methods may be collectively referred to as "the method of the present disclosure."

[0034] <<Production method of highly absorbent recycled polymer from used sanitary products>> The disclosed method for producing a highly absorbent recycled polymer from used sanitary products includes the following steps. A primary dehydration step (hereinafter sometimes referred to as the "primary dehydration step") in which a sanitary product component material that constitutes the sanitary product, which comprises the pulp fiber and the superabsorbent polymer, is immersed in an acid-containing aqueous solution that contains an acid to form a primarily dehydrated superabsorbent polymer, and the primarily dehydrated superabsorbent polymer is separated from the sanitary product component material. A secondary dehydration step (hereinafter sometimes referred to as the "secondary dehydration step") in which the primarily dehydrated superabsorbent polymer is further dehydrated by contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to form the secondarily dehydrated superabsorbent polymer. A step of forming a superabsorbent recycled polymer by mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer (hereinafter, may be referred to as a "superabsorbent recycled polymer formation step").

[0035] [First dehydration step] In the primary dehydration step, a sanitary product constituent material containing pulp fibers and a superabsorbent polymer having acid groups is immersed in an acid-containing aqueous solution containing acid to form a primarily dehydrated superabsorbent polymer, and the primarily dehydrated superabsorbent polymer is separated from the sanitary product constituent material.

[0036] In the first dehydration step, the acid groups of the superabsorbent polymer are converted from a salt state (e.g., sodium salt) with a component in the body fluid (e.g., sodium ion) to a free acid state, and the water absorption of the superabsorbent polymer decreases. When the superabsorbent polymer that has absorbed water is placed in an acid-containing aqueous solution, negatively charged hydrophilic groups (e.g., -COO - ) turns into positively charged hydrogen ions (H + ) (e.g., -COOH), the ionic repulsion of the hydrophilic groups is weakened, the water absorption capacity is reduced, and the superabsorbent polymer is dehydrated.

[0037] The acid is not particularly limited, and examples thereof include inorganic acids and organic acids. When the superabsorbent polymer is dehydrated (inactivated) using an acid, ash is less likely to remain in the pulp fibers compared to when the superabsorbent polymer is dehydrated (inactivated) using a polyvalent metal ion source capable of supplying polyvalent metal ions, such as lime, calcium chloride, magnesium sulfate, magnesium chloride, aluminum sulfate, aluminum chloride, etc.

[0038] Examples of the inorganic acid include sulfuric acid, hydrochloric acid, and nitric acid, and sulfuric acid is preferred as the inorganic acid from the viewpoints of not containing chlorine, cost, etc. Examples of the organic acid include those having an acid group, such as a carboxyl group or a sulfo group. An organic acid having a sulfo group is called a sulfonic acid, and an organic acid having a carboxyl group but not a sulfo group is called a carboxylic acid. From the viewpoint of protecting the equipment, the organic acid is preferably an organic acid having a carboxyl group, particularly a carboxylic acid.

[0039] When the organic acid has a carboxyl group, the organic acid may have one or more carboxyl groups per molecule, and preferably has more than one carboxyl group, which makes it easier for the organic acid to form a chelate complex with a divalent or higher metal, such as calcium, contained in excrement, and when recycled pulp fibers are formed from used sanitary products, the ash content of the resulting recycled pulp fibers is easier to reduce.

[0040] Examples of the organic acids include citric acid, tartaric acid, malic acid, succinic acid, oxalic acid (all of which are carboxylic acids having multiple carboxyl groups), gluconic acid (C6), pentanoic acid (C5), butanoic acid (C4), propionic acid (C3), glycolic acid (C2), acetic acid (C2), glacial acetic acid, formic acid (C1) (all of which are carboxylic acids having one carboxyl group), methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid (all of which are sulfonic acids), and the like.

[0041] The acid-containing aqueous solution preferably has a predetermined pH, and the predetermined pH is preferably 4.5 or less, more preferably 4.0 or less, even more preferably 3.5 or less, and even more preferably 3.0 or less. If the predetermined pH is too high, the primary dehydration of the superabsorbent polymer is not sufficiently carried out, and the primarily dehydrated superabsorbent polymer tends to be difficult to separate from the pulp fibers.

[0042] Moreover, the predetermined pH is preferably 0.5 or more, and more preferably 1.0 or more. If the predetermined pH is too low, the recycled pulp fibers may be damaged when they are formed from used sanitary products. In this specification, pH refers to the value at 25° C. In addition, pH can be measured, for example, using a twin pH meter AS-711 manufactured by Horiba, Ltd.

[0043] In the manufacturing method of the present disclosure, it is preferable that the acid-containing aqueous solution at least satisfies the above-mentioned predetermined pH at the start of the primary dehydration step, for example, when the sanitary product constituent material is immersed in the acid-containing aqueous solution. This is to perform the primary dehydration of the superabsorbent polymer, and if the primary dehydration of the superabsorbent polymer is insufficient, the discharge of liquids such as body fluids held by the superabsorbent polymer tends to be insufficient, and the primary dehydrated superabsorbent polymer tends to be difficult to separate from pulp fibers, etc. In the production method of the present disclosure, it is preferable to satisfy the above-mentioned predetermined pH at the end of the primary dehydration step, from the viewpoint of maintaining the state of the superabsorbent polymer after the primary dehydration.

[0044] The superabsorbent polymer is not particularly limited as long as it is used in the art as a superabsorbent polymer having an acid group, and examples thereof include those containing a carboxyl group, a sulfo group, etc., and those containing a carboxyl group are preferred. Examples of highly water-absorbent polymers containing a carboxyl group include polyacrylates and polymaleic anhydrides, and examples of highly water-absorbent polymers containing a sulfo group or the like include polysulfonates. The pulp fibers are not particularly limited as long as they can be contained in sanitary products.

[0045] In order to efficiently perform the primary dehydration of the superabsorbent polymer, the acid dissociation constant (pK a , in water) a , in water).

[0046] When the acid has multiple acid groups, for example when the acid is a dibasic or tribasic acid, the acid dissociation constant (pK a , in water) has the largest acid dissociation constant (pK a , in water) is the acid dissociation constant (pK a In the case where the highly water-absorbent polymer has a plurality of acid groups, the acid dissociation constant (pK a , in water) has the largest acid dissociation constant (pK a , in water) is the smallest acid dissociation constant (pK a , in water) from the viewpoint of the efficiency of the primary dehydration of the highly water-absorbent polymer.

[0047] As used herein, the acid dissociation constant (pK a , in water), the values ​​described in the Electrochemical Handbook compiled by the Electrochemical Society can be used. According to the Electrochemical Handbook, the acid dissociation constants (pK a , in water, at 25°C) is as follows. [Organic acid] ·Tartaric acid: 2.99 (pK a1 ), 4.44(pK a2 ) Malic acid: 3.24 (pK a1 ), 4.71(pK a2 ) Citric acid: 2.87 (pK a1 ), 4.35(pK a2 ), 5.69(pK a3 ) [Inorganic acid] ·Sulfuric acid: 1.99(pK a2 )

[0048] Acid dissociation constants (pK a The acid dissociation constant (pK aAn example of an instrument capable of measuring the physical properties of compounds (in water) is the Sirius T3 Compound Property Evaluation and Analysis System.

[0049] In the manufacturing method disclosed herein, the specific technique is not particularly limited as long as the sanitary product constituent materials can be immersed in the acid-containing aqueous solution. For example, the sanitary product constituent materials may be placed in a tank containing the acid-containing aqueous solution, and the acid-containing aqueous solution may be placed in the tank in which the sanitary product constituent materials are placed.

[0050] The sanitary product is not particularly limited as long as it contains pulp fibers and a highly absorbent polymer, and examples thereof include disposable diapers, disposable shorts, sanitary napkins, panty liners, urine pads, bed sheets, pet sheets, and the like. The sanitary product may, for example, include a product including a liquid-permeable sheet, a liquid-impermeable sheet, and an absorbent body (absorbent core and core wrap) therebetween.

[0051] In the method of the present disclosure, the sanitary product component in the first dehydration step can be a mixture of pulp fibers and a superabsorbent polymer, such as an absorbent core taken from a used sanitary product. The sanitary product component can also be the sanitary product itself.

[0052] When the sanitary product constituent materials to be immersed in the acid-containing aqueous solution include, in addition to pulp fibers and superabsorbent polymers (hereinafter sometimes referred to as "specific materials"), additional materials (hereinafter sometimes referred to as "non-specific materials"), such as a liquid-permeable sheet, a liquid-impermeable sheet, etc., for example, the sanitary product itself may be immersed in the acid-containing aqueous solution as the sanitary product constituent materials.

[0053] In the primary dehydration step, for example, the sanitary product constituent materials are stirred in a primary dehydration tank containing an acid-containing aqueous solution for about 5 to 60 minutes, depending on the temperature, to primarily dehydrate the superabsorbent polymer and form a primarily dehydrated superabsorbent polymer.

[0054] The acid-containing aqueous solution in the first dehydration step may or may not be heated. The temperature of the acid-containing aqueous solution in the primary dehydration step can be, for example, room temperature (25° C.) to 40° C., or less than 60° C., when not heated. When the acid-containing aqueous solution in the primary dehydration step is heated, the temperature is preferably higher than room temperature, more preferably 60 to 100° C., even more preferably 70 to 95° C., and even more preferably 80 to 90° C. By doing so, the acid contained in the acid-containing aqueous solution can easily kill bacteria derived from excrement and the like contained in the acid-containing aqueous solution.

[0055] In the primary dehydration step, the primary dehydration is preferably performed so that the primarily dehydrated superabsorbent polymer has a moisture content of preferably more than 80.0 mass% and not more than 97.0 mass%, more preferably 85.0 to 96.0 mass%, and even more preferably 87.0 to 95.0 mass%, which makes it easier to reduce the moisture content of the secondary dehydrated superabsorbent polymer.

[0056] In this specification, the moisture content is measured using an infrared moisture meter FD-720 manufactured by Kett Co., Ltd. Specifically, about 5 g of a sample is placed on the sample tray of the FD-720, the temperature is set to 150° C., the automatic stop mode is selected, and the moisture content is measured.

[0057] <Secondary dehydration step> In the secondary dehydration step, the primary dehydrated superabsorbent polymer is further dehydrated by contacting the primary dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to form a secondary dehydrated superabsorbent polymer.

[0058] In the secondary dehydration step, the acid groups (e.g., -COOH) of the superabsorbent polymer having acid groups are crosslinked with polyvalent metal ions (e.g., calcium ions), and the primarily dehydrated superabsorbent polymer is further dehydrated to form a secondary dehydrated superabsorbent polymer.

[0059] Examples of the polyvalent metal ion include alkaline earth metal ions and transition metal ions. Examples of the alkaline earth metal ions include beryllium ions, magnesium ions, calcium ions, strontium ions, and barium ions. Examples of the transition metal ions include iron ions, cobalt ions, nickel ions, and copper ions.

[0060] When the polyvalent metal ion is an alkaline earth metal ion, examples of a polyvalent metal ion source capable of supplying the polyvalent metal ion include alkaline earth metal hydroxides (e.g., calcium hydroxide, magnesium hydroxide), alkaline earth metal hydroxide and acid salts (e.g., calcium chloride, calcium nitrate, magnesium chloride, magnesium nitrate), alkaline earth metal oxides (e.g., calcium oxide, magnesium oxide), etc., with calcium chloride being preferred. Examples of the acid include the acids for the acid-containing aqueous solution described in the "primary dehydration step" section.

[0061] When the polyvalent metal ion is a transition metal ion, examples of a polyvalent metal ion source capable of supplying the polyvalent metal ion include transition metal hydroxides (e.g., iron hydroxide, cobalt hydroxide, nickel hydroxide, copper hydroxide), transition metal hydroxide and acid salts, transition metal oxides (e.g., iron oxide, cobalt oxide, nickel oxide, copper oxide), etc. Examples of the acid include the acids for the acid-containing aqueous solution described in the section "primary dehydration step."

[0062] Specific examples of the hydroxides and acid salts of the transition metals include inorganic acid salts or organic acid salts. Examples of the inorganic acid salts include iron salts such as iron chloride, iron sulfate, iron phosphate, and iron nitrate, cobalt salts such as cobalt chloride, cobalt sulfate, cobalt phosphate, and cobalt nitrate, nickel salts such as nickel chloride and nickel sulfate, and copper salts such as copper chloride and copper sulfate. Examples of the organic acid salts include iron lactate, cobalt acetate, cobalt stearate, nickel acetate, and copper acetate.

[0063] In the secondary dehydration step, for example, the primary dehydrated superabsorbent polymer can be directly contacted with a polyvalent metal ion source capable of supplying polyvalent metal ions to form a secondary dehydrated superabsorbent polymer. In addition, in the secondary dehydration step, the primary dehydrated superabsorbent polymer can be secondarily dehydrated by stirring the primary dehydrated superabsorbent polymer for about 5 to 60 minutes, depending on the temperature, in a secondary dehydration tank containing an aqueous solution containing a polyvalent metal ion source capable of supplying polyvalent metal ions, thereby forming a secondary dehydrated superabsorbent polymer.

[0064] The aqueous solution containing the polyvalent metal ion source in the second dehydration step may or may not be heated. In the secondary dehydration step, the temperature of the aqueous solution containing a polyvalent metal ion source is not particularly limited if it is not heated, and can be, for example, room temperature (25°C) to 40°C, or less than 60°C.

[0065] When the aqueous solution containing the polyvalent metal ion source in the secondary dehydration step is heated, the temperature is preferably higher than room temperature, more preferably 60 to 100° C., even more preferably 70 to 95° C., and even more preferably 80 to 90° C. When the polyvalent metal ion source has low solubility in water, heating can efficiently supply polyvalent metal ions from the polyvalent metal ion source and promote the formation of a highly water-absorbent polymer by secondary dehydration.

[0066] In the secondary dehydration step, the primary dehydrated superabsorbent polymer is secondarily dehydrated so that the secondary dehydrated superabsorbent polymer has a moisture content of preferably 50 to 80% by mass, more preferably 50 to 75% by mass, and even more preferably 50 to 67% by mass. This can reduce the amount of excrement remaining in the secondary dehydrated superabsorbent polymer, and also makes it easier to form a superabsorbent recycled polymer from the secondary dehydrated superabsorbent polymer. If the moisture content of the secondary dehydrated superabsorbent polymer is too low, the secondary dehydrated superabsorbent polymer is less likely to react with the alkali metal ion source in the subsequent superabsorbent recycled polymer formation step, and it tends to be difficult to form a superabsorbent recycled polymer.

[0067] In the secondary dehydration step, when the primarily dehydrated superabsorbent polymer is contacted with a polyvalent metal ion source-containing aqueous solution containing a polyvalent metal ion source, for example, when the primarily dehydrated superabsorbent polymer is put into the polyvalent metal ion source-containing aqueous solution, the concentration of the polyvalent metal ion source in the polyvalent metal ion source-containing aqueous solution is preferably 1.0 to 30.0% by mass, more preferably 3.0 to 25.0% by mass, and more preferably 5.0 to 20.0% by mass. This makes it easier for the secondarily dehydrated superabsorbent polymer to have a desired moisture content.

[0068] <Additional drying step> In the method of the present disclosure, after the secondary dehydration step, the secondary dehydrated superabsorbent polymer is formed, a drying step may be further included in which the secondary dehydrated superabsorbent polymer is dried to form a dried secondary dehydrated superabsorbent polymer.

[0069] In the drying step, the secondarily dehydrated superabsorbent polymer is preferably dried so that the dried secondarily dehydrated superabsorbent polymer has a moisture content of preferably 10 to 30% by mass, and more preferably 15 to 25% by mass. This makes it possible to reduce the amount of alkali metal ion source used in forming the superabsorbent recycled polymer, and to maintain the water absorption of the formed superabsorbent recycled polymer.

[0070] In the drying step, the secondarily dehydrated superabsorbent polymer is dried at a drying temperature of preferably room temperature (e.g., 25° C.) to 120° C., more preferably 30 to 80° C., and more preferably 40 to 60° C. If the drying temperature is lower, the drying time tends to be longer, and if the drying temperature is higher, the acid groups of the superabsorbent recycled polymer after drying may undergo dehydration condensation, etc., resulting in a decrease in the water absorbency of the superabsorbent recycled polymer after drying. The drying step can be carried out for, for example, 30 to 300 minutes.

[0071] <Highly absorbent recycled polymer formation step> In the superabsorbent recycled polymer formation step, the second dehydrated superabsorbent polymer and an alkali metal ion source capable of supplying alkali metal ions are mixed in an aqueous regeneration solution, and a superabsorbent recycled polymer is formed from the second dehydrated superabsorbent polymer. In this specification, a superabsorbent polymer obtained by recycling a second-dehydrated superabsorbent polymer may be referred to as a "recycled superabsorbent polymer."

[0072] The alkali metal ion source is not particularly limited as long as it can supply alkali metal ions, and examples thereof include alkali metal hydroxides, salts of alkali metal hydroxides and acids (hereinafter sometimes simply referred to as "salts"), and alkali metal oxides.

[0073] The alkali metal ions include lithium ions, sodium ions, and potassium ions, and any combination thereof. The alkali metal hydroxides include lithium hydroxide, sodium hydroxide, and potassium hydroxide, and any combination thereof.

[0074] The above salt may be an acid salt, a basic salt, or the like. The alkali metal hydroxides in the above salts include lithium hydroxide, sodium hydroxide, and potassium hydroxide, and any combination thereof. The acid in the salt is not particularly limited, and examples thereof include acids for the acid-containing aqueous solution (eg, hydrochloric acid, sulfuric acid), carbonic acid, and the like, which are explained in the section "primary dehydration step." The alkali metal oxides include lithium oxide, sodium oxide, and potassium oxide, and any combination thereof.

[0075] The alkali metal ion source and the polyvalent metal ion source have a relationship in which the difference in standard electrode potential between the alkali metal ion constituting the alkali metal ion source and the polyvalent metal ion constituting the polyvalent metal ion source is preferably 2.0 or less, more preferably 1.6 or less, even more preferably 1.0 or less, and even more preferably 0.5 or less, which makes it easier to replace the polyvalent metal ion crosslinking the acid groups of the secondary dehydrated highly absorbent polymer with the alkali metal ion, and thus the highly absorbent recycled polymer has excellent water absorption properties.

[0076] The acid dissociation constant (pK a , in water) a In this way, the acid group of the highly water-absorbent polymer can easily form an alkali metal salt.

[0077] When the acid has multiple acid groups, for example when the acid is a dibasic or tribasic acid, the acid dissociation constant (pK a , in water) has the smallest acid dissociation constant (pK a , in water) is the acid dissociation constant (pK a In the case where the highly water-absorbent polymer has a plurality of acid groups, the acid dissociation constant (pK a , in water) has the smallest acid dissociation constant (pK a , in water) is the largest acid dissociation constant (pK a , in water) from the viewpoint of facilitating conversion of the acid groups of the highly water-absorbent polymer into alkali metal salts.

[0078] Carbonic acid is preferred as the acid because carbonic acid is unlikely to remain in the aqueous solution for regeneration and can be easily removed by heating or the like. In addition, although it depends on the pH of the superabsorbent recycled polymer, for example, when the superabsorbent recycled polymer is at an acidic pH, the superabsorbent recycled polymer can be imparted with antibacterial properties.

[0079] Examples of the above salts include lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium chloride, sodium chloride, potassium chloride, and the like.

[0080] In the superabsorbent recycled polymer formation step, the recycled aqueous solution can be acidic (pH < 7.0), neutral (pH = 7.0), or alkaline (7.0 < pH), preferably neutral or alkaline, and more preferably alkaline. This is from the perspective of the effects of the present disclosure.

[0081] In order to make the recycled aqueous solution acidic, neutral, or alkaline, the recycled aqueous solution may contain an acidic substance, an alkaline substance, or a buffering substance (buffer solution), and the above alkali metal ion source may contain an acidic substance, an alkaline substance, or a buffering substance (buffer solution). The above acidic substance, alkaline substance, or buffering substance (buffer solution) is preferable when it is difficult for the alkali metal ion source to change the pH of the recycled aqueous solution (for example, when the alkali metal ion source is lithium chloride, sodium chloride, potassium chloride, etc.), or when it is not desired to change the pH of the recycled aqueous solution.

[0082] The above acidic substance is not particularly limited as long as it can make the pH of deionized water acidic (pH < 7.0), and those known in the art can be adopted. For example, the acids for acid-containing aqueous solutions, carbonic acid, etc. described in the section of "primary dehydration step" can be mentioned. The above-mentioned alkaline substance is not particularly limited as long as it can make the pH of deionized water alkaline (7.0 < pH), and those known in the art can be adopted. For example, hydroxides of alkali metals or their salts, hydroxides of alkaline earth metals or their salts, etc. can be mentioned. From the viewpoint of making it difficult to inactivate the superabsorbent polymer, it is preferably a hydroxide of an alkali metal or its salt. The hydroxide of an alkali metal or its salt is as described above. Examples of the above-mentioned buffer substance (buffer solution) include a carbonate-bicarbonate buffer solution containing sodium carbonate, sodium bicarbonate and water.

[0083] The above-mentioned regeneration aqueous solution is not particularly limited as long as it contains water, and can generally be a neutral aqueous solution (for example, tap water, deionized water, etc.), an acidic aqueous solution (aqueous solution with pH < 7.0), for example, the acid-containing aqueous solution used in the primary dehydration step, the acid for the acid-containing aqueous solution described in the section of "primary dehydration step", for example, an aqueous solution containing an inorganic acid or an organic acid, or an alkaline aqueous solution (aqueous solution with 7.0 < pH), for example, an aqueous solution containing the above-mentioned alkali metal ion source.

[0084] By adjusting the pH of the regeneration aqueous solution, the water absorption of the superabsorbent recycled polymer can be adjusted to a predetermined range. The above-mentioned pH is not particularly limited as long as the superabsorbent recycled polymer can achieve a predetermined water absorption (absorption magnification), but it can be in any of the acidic pH region (pH < 7.0), neutral pH (pH = 7.0), and alkaline pH region (7.0 < pH), and the above-mentioned pH is preferably 5.0 to 14.0.

[0085] When adjusting the above-mentioned pH within the acidic pH region, the above-mentioned regeneration aqueous solution is preferably an acidic aqueous solution, and it is preferable to form a superabsorbent recycled polymer by adding an alkali metal ion source as it is or as an aqueous solution to the regeneration aqueous solution that is an acidic aqueous solution.

[0086] When the pH is adjusted to within the range of neutral or alkaline pH, the regenerating aqueous solution can be an acidic aqueous solution, a roughly neutral aqueous solution, or an alkaline aqueous solution, and is preferably a roughly neutral aqueous solution or an alkaline aqueous solution, from the viewpoint of efficiently using the alkali metal ion source for the formation of the highly water-absorbent recycled polymer. It is also preferred to form the highly water-absorbent recycled polymer by adding an alkali metal ion source as it is or as an aqueous solution to the regenerating aqueous solution, which is a substantially neutral aqueous solution or an alkaline aqueous solution.

[0087] The source of alkali metal ions may be present in the aqueous regenerating solution as described above, and the source of alkali metal ions may be added neat or as an aqueous solution to the aqueous regenerating solution. When an alkali metal hydroxide is added to the regenerating aqueous solution as an alkali metal ion source, the alkali metal hydroxide is preferably in the form of an aqueous solution, and the aqueous solution is added to the regenerating aqueous solution at a hydroxide ion concentration of preferably 0.1 to 5.0 mol / L, more preferably 0.3 to 3.0 mol / L, and more preferably 0.4 to 1.0 mol / L, from the viewpoint of ease of adjustment of the pH of the regenerating aqueous solution and, in turn, the water absorbency of the highly water absorbent recycled polymer.

[0088] The highly water-absorbent recycled polymer formation step can be carried out by, for example, stirring the regenerating aqueous solution at a predetermined temperature, for example, 2 to 80° C., for a predetermined time, for example, 5 to 60 minutes.

[0089] <Additional drying step> The process of the present disclosure may further include a drying step after the superabsorbent recycled polymer forming step. In the drying step, the highly absorbent recycled polymer formed in the highly absorbent recycled polymer formation step (hereinafter, for the sake of distinction, may be referred to as the "highly absorbent recycled polymer before drying") is dried to form a highly absorbent recycled polymer having a predetermined water absorbency (hereinafter, for the sake of distinction, may be referred to as the "highly absorbent recycled polymer after drying").

[0090] The above-mentioned predetermined water absorption is not particularly limited, but taking into consideration the practicality of the highly water absorbent recycled polymer after drying, the water absorption ratio is preferably 100 times (g / g) or more, more preferably 200 times (g / g) or more, and even more preferably 300 times (g / g) or more relative to deionized water.

[0091] The above-mentioned predetermined water absorbency is not particularly limited, but taking into consideration the gel strength of the highly water absorbent recycled polymer when swollen after drying, the water absorption capacity is preferably 500 times (g / g) or less, more preferably 450 times (g / g) or less, and even more preferably 400 times (g / g) or less relative to deionized water.

[0092] As used herein, water absorption capacity is measured as follows. (1) The sample (highly absorbent recycled polymer) is placed in a mesh and hung for 5 minutes to remove the moisture adhering to the surface, and its mass before drying: m1 (g) is measured. (2) The sample whose mass before drying was measured is dried at 120°C for 120 minutes, and its mass after drying: m2 (g) is measured. (3) Water absorption capacity (g / g) is calculated using the following formula: Water absorption capacity (g / g)=m1 / m2 It is calculated as follows.

[0093] In the drying step, the aqueous regenerating solution containing the pre-dried highly absorbent recycled polymer obtained in the highly absorbent recycled polymer formation step can be directly dried to obtain a dried highly absorbent recycled polymer. In addition, the highly absorbent recycled polymer before drying can be separated from the aqueous regeneration solution containing the highly absorbent recycled polymer using an apparatus capable of solid-liquid separation, and then the highly absorbent recycled polymer after drying can be obtained.

[0094] The separated highly absorbent recycled polymer before drying may be washed with tap water, deionized water, etc. before drying to remove the regenerating aqueous solution adhering to the surface of the highly absorbent recycled polymer before drying. In addition, the separated highly absorbent recycled polymer before drying can be brought into contact with a hydrophilic organic solvent (e.g., immersed in a hydrophilic organic solvent) before drying to remove water contained in the separated highly absorbent recycled polymer to a water absorption ratio of preferably 100 times (g / g) or less, more preferably 70 times (g / g) or less, and even more preferably 50 times (g / g) or less. By doing so, the drying temperature and / or drying time can be reduced.

[0095] The hydrophilic organic solvent is preferably one that is miscible with water, and examples thereof include alcohol solvents (e.g., methanol, ethanol, propyl alcohol and its isomers, butyl alcohol and its isomers), ketone solvents (e.g., acetone, methyl ethyl ketone), and nitrile solvents (e.g., acetonitrile).

[0096] In the drying step, the highly absorbent recycled polymer is dried at a drying temperature of preferably room temperature (e.g., 25° C.) to 120° C., more preferably 30 to 80° C., and more preferably 40 to 60° C. If the drying temperature is lower, the drying time tends to be longer, and if the drying temperature is higher, the acid groups of the highly absorbent recycled polymer after drying may undergo dehydration condensation, etc., resulting in a decrease in the water absorption of the highly absorbent recycled polymer after drying. When the separated highly water-absorbent recycled polymer before drying is brought into contact with a hydrophilic organic solvent before drying, the drying temperature can be low, for example, from room temperature to 60°C.

[0097] The drying step may be carried out under reduced pressure, for example at least 0.1 kPa and less than 100 kPa. The drying step can be carried out for, for example, 30 to 300 minutes. The drying step is preferably carried out so that the weight loss of the highly absorbent recycled polymer is preferably 15% or less (2.0 g, 105° C., 3 hours) from the viewpoint of utilization of the highly absorbent recycled polymer after drying. The loss on drying is measured in accordance with "7. Test method for loss on drying" under "2. General testing methods" in the "Standards for materials for sanitary treatment products" attached as an appendix to the "Standards for materials for sanitary treatment products" notified by the Ministry of Health, Labour and Welfare as Yakusho Licensing and Evaluation Division No. 0325-24 on March 25, 2015.

[0098] After the drying step, if the dried highly absorbent recycled polymer is stuck or integrated, the dried highly absorbent recycled polymer may be pulverized, classified, or the like.

[0099] <<Secondary dehydration superabsorbent polymer manufacturing method>> The method for making the secondarily dehydrated superabsorbent polymer of the present disclosure includes the following steps. A preparation step (hereinafter sometimes referred to as the "preparation step") of preparing the primarily dehydrated superabsorbent polymer obtained by immersing a sanitary product component material that constitutes a sanitary product, the superabsorbent polymer including pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution that includes an acid to form a primarily dehydrated superabsorbent polymer, and separating the primarily dehydrated superabsorbent polymer from the sanitary product component material. A secondary dehydration step (hereinafter sometimes referred to as the "secondary dehydration step") in which the primarily dehydrated superabsorbent polymer is further dehydrated by contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to form the secondarily dehydrated superabsorbent polymer.

[0100] <Preparation steps> The primarily dehydrated superabsorbent polymer in the preparation step can be prepared, for example, by carrying out the "primary dehydration step" in the "method for producing a superabsorbent recycled polymer from used sanitary products".

[0101] <Secondary dehydration step> The secondary dehydration step is the same as the "secondary dehydration step" in the "Method for producing highly absorbent recycled polymers from used sanitary products," so a description thereof will be omitted.

[0102] <<Manufacturing method for highly absorbent recycled polymers>> The method for producing the superabsorbent recycled polymer of the present disclosure includes the following steps. a preparation step (hereinafter sometimes referred to as the "preparation step") of preparing the second dehydrated superabsorbent polymer obtained by immersing a sanitary product component material constituting a sanitary product, the superabsorbent polymer including pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution containing an acid to form a primarily dehydrated superabsorbent polymer, separating the primarily dehydrated superabsorbent polymer from the sanitary product component material, and contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the primarily dehydrated superabsorbent polymer; A step of forming a superabsorbent recycled polymer by mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer (hereinafter, may be referred to as a "superabsorbent recycled polymer formation step").

[0103] <Preparation steps> The secondarily dehydrated superabsorbent polymer in the preparation step can be prepared, for example, by carrying out the "primary dehydration step" and "secondary dehydration step" in the "method for producing superabsorbent recycled polymer from used sanitary products."

[0104] <Highly absorbent recycled polymer formation step> The step of forming a highly absorbent recycled polymer is the same as the "step of forming a highly absorbent recycled polymer" in the "Method of producing a highly absorbent recycled polymer from used sanitary products", and therefore a description thereof will be omitted.

[0105] The highly absorbent recycled polymer can be used for any application in which a highly absorbent polymer is used, without any particular limitation. Examples of the applications include sanitary products (e.g., disposable diapers, incontinence pads (e.g., light incontinence pads), disposable shorts, sanitary napkins, panty liners, bed sheets), pet sheets, cat litter, soil conditioners, etc. EXAMPLES

[0106] [Example 1] Physiological saline was absorbed into 100 g of a polyacrylic acid-based highly water-absorbent polymer (AQUAKEEP, unused product, manufactured by Sumitomo Seika Chemicals, hereafter referred to as "SAP"), and then the polymer was filtered through a 200-mesh filter to prepare simulated used SAP No. 1 with a moisture content of 97.5% by mass. The simulated used SAP No. 1 was stirred for 5 minutes in 4,000 mL of an aqueous solution of 1.0 mass% citric acid as an acid-containing aqueous solution, allowed to stand for 20 minutes, and then filtered through a 200-mesh filter to form primarily dehydrated SAP No. 1. The moisture content of the primarily dehydrated SAP No. 1 was 95.0 mass%.

[0107] The first dehydrated SAP No.1 was stirred for 5 minutes in 4,000 mL of a 10.0% by mass dispersion of calcium hydroxide as a polyvalent metal ion source, left to stand for 1 hour, filtered through a 200 mesh filter, and then dehydrated for 5 minutes at 150G using a centrifugal dehydrator to form the second dehydrated SAP No.1. The 10.0% by mass dispersion of calcium hydroxide (Ca(OH)2) also contained solid calcium hydroxide, but it was confirmed that the solid calcium hydroxide was removed by filtering through a 200 mesh filter and then dehydrating using a centrifugal dehydrator. The moisture content of the second dehydrated SAP No.1 was 69.0% by mass.

[0108] The secondarily dehydrated SAP No. 1 was dried at 120° C. for 120 minutes to obtain dried secondarily dehydrated SAP No. 1. The drying properties of the secondary dehydrated SAP after drying were judged according to the following criteria. The results are shown in Table 1. [Drying] ◯: The secondary dehydrated SAP after drying is sufficiently dried and is in a powder form or can be easily made into a powder form. ×: The secondary dehydrated SAP after drying is insufficiently dried and is in the form of lumps.

[0109] [Examples 2 to 4] The acid-containing aqueous solution and the polyvalent metal ion source were changed as shown in Table 1 to prepare primary dehydrated SAP No. 2 to No. 4 and secondary dehydrated SAP No. 2 to No. 4, and their moisture contents were measured. In addition, secondary dehydrated SAP No. 2 to No. 4 were prepared after drying, and their drying properties were evaluated. The results are shown in Table 1.

[0110] [Comparative Example 1] The simulated used SAP No. 1 was stirred for 5 minutes in 4,000 mL of an aqueous solution of 1.0 mass% sulfuric acid as an acid-containing aqueous solution, allowed to stand for 20 minutes, and then filtered through a 200-mesh filter to form primarily dehydrated SAP No. 5. The moisture content of the primarily dehydrated SAP No. 5 was 90.0 mass%. The primarily dehydrated SAP No. 5 was dried at 120° C. for 120 minutes to obtain the dried primarily dehydrated SAP No. 5, and its drying properties were evaluated. The results are shown in Table 1.

[0111] [Comparative Example 2] The simulated used SAP No. 1 was stirred for 5 minutes in 4,000 mL of a 10.0% by mass dispersion solution of calcium hydroxide as a polyvalent metal ion source, allowed to stand for 1 hour, passed through a 200 mesh filter, and then dehydrated for 5 minutes at 150 G using a centrifugal dehydrator to form primarily dehydrated SAP No. 6. The moisture content of the primarily dehydrated SAP No. 6 was 73.0% by mass. The primarily dehydrated SAP No. 6 was dried at 120° C. for 120 minutes to obtain the dried primarily dehydrated SAP No. 6, and its drying properties were evaluated. The results are shown in Table 1.

[0112] [Table 1]

[0113] The secondarily dehydrated SAPs No. 1 to No. 4 were immersed in an aqueous sodium hydroxide solution to form a highly absorbent recycled polymer. Compared with the firstarily dehydrated SAPs No. 5 and No. 6, (i) a low concentration of an aqueous sodium hydroxide solution and (ii) a small amount of an aqueous sodium hydroxide solution were used to form a highly absorbent recycled polymer.

[0114] In addition, the dried secondarily dehydrated SAP Nos. 1 to 4 were immersed in an aqueous sodium hydroxide solution to form a highly absorbent recycled polymer. Compared with the secondarily dehydrated SAP Nos. 1 to 4, (i) a low concentration of aqueous sodium hydroxide solution and (ii) a small amount of aqueous sodium hydroxide solution were used to form a highly absorbent recycled polymer.

[0115] [Example 5] A mixture of 100g of polyacrylic acid-based superabsorbent polymer (Sumitomo Seika Chemicals, AQUAKEEP, unused product, hereafter referred to as "SAP") and 100g of pulp fiber (softwood pulp fiber) was allowed to absorb 4,000mL of saline solution, resulting in the swollen SAP and the pulp fiber becoming integrated. The mixture that had absorbed the saline solution was filtered through a 200 mesh filter to remove the remaining saline solution from the mixture.

[0116] The mixture from which the saline was removed was stirred for 5 minutes in 4,000 mL of an aqueous solution of 1.0 mass% citric acid as an acid-containing aqueous solution, and then allowed to stand for 20 minutes, and then the pulp fibers and the first dehydrated SAP were separated. The first dehydrated SAP remaining in the pulp fibers was decomposed with an ozone-containing gas according to the oxidizing agent treatment step P19 of Patent Document 1, to obtain recycled pulp fiber No. 1. The ash content of recycled pulp fiber No. 1 was 0.12 mass%.

[0117] [Example 6] Recycled pulp fiber No. 2 was obtained in the same manner as in Example 5, except that "4,000 mL of 1.0 mass% aqueous solution of citric acid" was changed to "4,000 mL of 1.0 mass% aqueous solution of sulfuric acid." The ash content of recycled pulp fiber No. 2 was 0.15 mass%.

[0118] [Comparative Example 3] Recycled pulp fiber No. 3 was obtained in the same manner as in Example 5, except that "4,000 mL of 1.0 mass% aqueous solution of citric acid" was changed to "4,000 mL of 10.0 mass% dispersion solution of calcium hydroxide." The ash content of recycled pulp fiber No. 3 was 12.1 mass%.

Claims

1. A method for producing a second dehydrated superabsorbent polymer for use in a superabsorbent recycled polymer, comprising: a preparation step of preparing a primarily dehydrated superabsorbent polymer by immersing a sanitary product constituent material, which comprises pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution containing an acid to form a primarily dehydrated superabsorbent polymer, and separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material; a secondary dehydration step of contacting the first dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the first dehydrated superabsorbent polymer to form the second dehydrated superabsorbent polymer; The method according to claim 1, further comprising:

2. 2. The method of claim 1, wherein in the second dehydration step, the first dehydrated superabsorbent polymer is further dehydrated to a moisture content of 50.0 to 80.0% by mass to form the second dehydrated superabsorbent polymer.

3. 3. The method according to claim 1, wherein the polyvalent metal ion source is an alkaline earth metal salt or a hydroxide of a transition metal, a salt of an alkaline earth metal salt or a hydroxide of a transition metal and an acid, or an alkaline earth metal salt or an oxide of a transition metal.

4. 4. The method according to claim 1, wherein in the second dehydration step, the first dehydrated superabsorbent polymer is contacted with the polyvalent metal ion source or an aqueous solution of the polyvalent metal ion source to form the second dehydrated superabsorbent polymer.

5. The method according to claim 4 , wherein the secondary dehydration step further comprises a drying step of drying the secondary dehydrated superabsorbent polymer.

6. The method according to any one of claims 1 to 5, wherein in the preparation step, the primarily dehydrated superabsorbent polymer has a moisture content of more than 80.0 mass% and not more than 97.0 mass%.

7. The method according to any one of claims 1 to 6, further comprising a primary dehydration step of forming the primarily dehydrated superabsorbent polymer by immersing the sanitary product constituent material in the acid-containing aqueous solution prior to the preparation step, and separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material.

8. The method according to any one of claims 1 to 7, further comprising, after the second dehydration step, mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regenerating solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer.

9. The method according to claim 8, wherein the alkali metal ion source is (i) a hydroxide of an alkali metal having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion, (ii) a salt of an alkali metal hydroxide having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion and an acid having a larger acid dissociation constant than the acid group of the superabsorbent polymer, or (iii) an oxide of an alkali metal having a standard electrode potential difference of 2.0 or less with the polyvalent metal ion.

10. 10. The method of claim 9, wherein the alkali metal ions are selected from the group consisting of lithium ions, sodium ions, and potassium ions, and any combination thereof.

11. A method for producing a recycled superabsorbent polymer, comprising the steps of: a preparation step of preparing a second dehydrated superabsorbent polymer obtained by immersing a sanitary product constituent material constituting a sanitary product, the sanitary product containing pulp fibers and a superabsorbent polymer having an acid group, in an acid-containing aqueous solution containing an acid to form a primarily dehydrated superabsorbent polymer, separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material, and contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion supply source capable of supplying polyvalent metal ions to further dehydrate the primarily dehydrated superabsorbent polymer; a step of mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer; The method according to claim 1, further comprising:

12. A method for producing a recycled superabsorbent polymer from a used sanitary product containing pulp fibers and a superabsorbent polymer having acid groups, comprising the steps of: a primary dehydration step of immersing a sanitary product constituent material that constitutes the sanitary product, the sanitary product constituent material including the pulp fiber and the superabsorbent polymer, in an acid-containing aqueous solution that contains an acid to form a primarily dehydrated superabsorbent polymer, and separating the primarily dehydrated superabsorbent polymer from the sanitary product constituent material; a secondary dehydration step of contacting the primarily dehydrated superabsorbent polymer with a polyvalent metal ion source capable of supplying polyvalent metal ions to further dehydrate the primarily dehydrated superabsorbent polymer to form a secondarily dehydrated superabsorbent polymer; a step of mixing the second dehydrated superabsorbent polymer with an alkali metal ion source capable of supplying alkali metal ions in an aqueous regeneration solution to form the superabsorbent recycled polymer from the second dehydrated superabsorbent polymer; The method according to claim 1, further comprising:

Citation Information

Patent Citations

  • Method for regenerating used highly water-absorbent polymer

    JP2013198862A

  • Method of treating water-absorbing resin

    JP2015004034A

  • Method for producing recycled pulp from used sanitary product

    JP2015086483A

  • Water-absorbing resin processing method

    JP2015120834A

  • Method for producing recycled pulp from used sanitary product

    JP2016000881A