Concrete Composition

A concrete composition with controlled water and binder ratios in artificial lightweight fine aggregate addresses moisture-related stress, enhancing frost resistance by minimizing freezing-induced damage.

JP7574129B2Active Publication Date: 2024-10-28SUMITOMO MITSUI CONSTRUCTION CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021059716
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-17
Filing Date
2021-03-31
Publication Date
2024-10-28
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Artificial lightweight fine aggregate in concrete compositions is prone to moisture retention in its voids, leading to repeated freezing and thawing, which causes stress and reduces frost resistance.

Method used

A concrete composition with specific water and binder ratios, using artificial lightweight fine aggregate, is formulated to control water content and minimize moisture retention, thereby enhancing frost resistance.

Benefits of technology

The composition reduces the amount of water that freezes and expands, improving frost resistance and maintaining structural integrity under freezing conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574129000008
    Figure 0007574129000008
  • Figure 0007574129000009
    Figure 0007574129000009
  • Figure 0007574129000010
    Figure 0007574129000010
Patent Text Reader

Abstract

To improve frost damage resistance in a concrete composition containing an artificial lightweight fine aggregate.SOLUTION: A concrete composition of the present invention contains a binder, water, and a fine aggregate, and when assuming a water-binder ratio as W / B (%), W is 110 or more and 150 or less, and W / B is 18 or more and (0.168×(W-110)+20) or less. A concrete composition of other aspects of the present invention contains a binder, water, and a fine aggregate, and the binder contains cement and the fine aggregate contains a lightweight fine aggregate, and when assuming a unit water content of water as W (kg / m3) and a volume ratio of a fine aggregate to a paste as vs / vp, W is 110 or more and 150 or less, and vs / vp is 0.67 or more and 1.00 or less. A concrete composition of yet other aspect of the present invention contains a binder, water, and a fine aggregate, and the fine aggregate contains a lightweight fine aggregate, and when assuming a unit water content of water as W(kg / m3), W is 110 or more and 150 or less, and a unit fine aggregate amount (kg / m3) is 515 or more and 655 or less.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to concrete compositions. [Background technology]

[0002] Artificial lightweight fine aggregate is known to have features such as reducing the weight of concrete compositions and reducing autogenous shrinkage due to the internal curing effect. Patent Document 1 describes a concrete composition containing artificial lightweight fine aggregate and containing 145 to 155 kg / m of water. 3 A concrete composition is disclosed in which the [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6180946 specification Summary of the Invention [Problem to be solved by the invention]

[0004] Artificial lightweight fine aggregate has many voids and is prone to moisture absorption. As a result, the moisture in the voids repeatedly freezes, expands, and melts, subjecting the concrete to repeated stress, which can reduce its frost resistance.

[0005] An object of the present invention is to provide a concrete composition which contains artificial lightweight fine aggregate and has high frost resistance. [Means for solving the problem]

[0006] The concrete composition of one embodiment of the present invention includes a binder, water, and fine aggregate, the fine aggregate includes lightweight fine aggregate, and the water content per unit weight of the water is W (kg / m 3 ), where the water-binder ratio is W / B (%), W is 110 or more, 1 40 or less, and W / B is 18 or more and (0.168×(W−110)+20) or less. A concrete composition according to another embodiment of the present invention includes a binder, water, and fine aggregate, the binder includes cement, the fine aggregate includes lightweight fine aggregate, and the unit water content of water is W (kg / m 3 ), where vs / vp is the volume ratio of fine aggregate to paste, W is 110 or more, 1 4 The concrete composition according to still another embodiment of the present invention includes a binder, water, and fine aggregate, the fine aggregate includes lightweight fine aggregate, and the unit water content of the water is W (kg / m 3 ) is 110 or more, 1 4 0 or less, unit fine aggregate amount (kg / m 3 ) is greater than or equal to 515 and less than or equal to 655. Effect of the Invention

[0007] In the present invention, the unit water amount is 110 to 150 kg / m 3 Therefore, according to the present invention, it is possible to provide a concrete composition containing an artificial lightweight fine aggregate and having high frost resistance. [Brief description of the drawings]

[0008] [Figure 1] 1 is a graph showing the results of a freeze-thaw test for Examples 1 to 3 and Comparative Example 1. [Diagram 2] 1 is a graph showing shrinkage strain in Example 1 and Comparative Example 1. [Diagram 3] 1 is a graph showing shrinkage strain in Examples 4 to 6 and Comparative Examples 2 to 3. [Figure 4] 1 is a graph showing the results of the neutralization acceleration test for Examples 1 and 3 and Comparative Example 1. [Diagram 5] 1 is a graph showing the relationship between material age and compressive strength in Examples 1 to 3 and 7 and Comparative Example 1. [Figure 6] 1 is a graph showing the relationship between compressive strength and Young's modulus in Examples 1 to 3 and 7 and Comparative Example 1. [Figure 7] 1 is a graph showing the compressive strength of Examples 8 to 14 and Comparative Example 4. [Figure 8] 1 is a graph showing the results of a freeze-thaw test (relative dynamic modulus of elasticity) for Examples 8 to 14 and Comparative Example 4. [Figure 9] 1 is a graph showing the results of a freeze-thaw test (mass reduction rate) for Examples 8 to 14 and Comparative Example 4. [Figure 10] 1 is a graph showing the relationship between unit water amount and W / B in Examples 8 to 14 and Comparative Example 4. [Figure 11] 1 is a graph showing the relationship between the air amount and the durability index in Examples 8 to 14 and Comparative Example 4. [Figure 12] 1 is a graph showing the relationship between vs / vp and compressive strength in Examples 8 to 14 and Comparative Example 4. [Figure 13] 1 is a graph showing the relationship between unit fine aggregate content and compressive strength in Examples 8 to 14 and Comparative Example 4. [Figure 14] 1 is a graph showing shrinkage strain in Examples 8 to 11 and Comparative Example 4. [Figure 15] 1 is a graph showing the relationship between unit water content and shrinkage strain in Examples 8 to 11 and Comparative Example 4. [Figure 16] 1 is a graph showing the relationship between W / B and shrinkage strain in Examples 8 to 11 and Comparative Example 4. EXAMPLES

[0009] Hereinafter, the concrete composition of the present invention will be described based on examples and comparative examples. Table 1 shows the mix proportions of the concrete compositions of Examples 1 to 7 and Comparative Examples 1 to 3, Table 2 shows the unit mass and unit volume of the concrete compositions of Examples 1 and 3 and Comparative Example 1, and Table 3 shows the specifications of the materials used in Examples 1 to 7 and Comparative Examples 1 to 3. In Table 3, BET means that the results are measured according to JIS R 1626 "Method for measuring the specific surface area of ​​fine ceramic powder by the gas adsorption BET method."

[0010] [Table 1]

[0011] [Table 2]

[0012] [Table 3]

[0013] FIG. 1(a) shows the relative dynamic modulus of elasticity for Examples 1 to 3 and Comparative Example 1, FIG. 1(b) shows the mass reduction rate for Examples 1 to 3 and Comparative Example 1, and FIG. 1(c) shows the mix ratio for Examples 1 to 3 and Comparative Example 1. The fine aggregate ratio (s / a) is set to 55.0. The relative dynamic modulus of elasticity and the mass reduction rate were determined based on the underwater freeze-thaw test method (Method A) specified in JISA1148:2010 "Freeze-thaw test method for concrete". If the relative dynamic modulus of elasticity is 60% or more of the initial value after 300 cycles, it can be evaluated as having excellent frost resistance. In Comparative Example 1, the relative dynamic modulus of elasticity falls below 60% of the initial value at about 100 cycles, whereas in Examples 1 to 3, it remains at about 80 to 90% of the initial value even after 300 cycles. The mass reduction rate increases rapidly with the number of cycles in Comparative Example 1, but is almost constant in Examples 1 to 3. The concretes of Examples 1 to 3 contain silica fume as a binder, while the concrete of Comparative Example 1 does not contain silica fume as a binder. Silica fume has the effect of increasing the fluidity of concrete.

[0014] FIG. 2(a) shows the shrinkage strain for Example 1 and Comparative Example 1, and FIG. 2(b) shows the mix proportions for Example 1 and Comparative Example 1. Both Example 1 and Comparative Example 1 use artificial lightweight fine aggregate, but the water content (unit water content) W and the water-binder ratio W / B are different. In Example 1, tests were conducted under two conditions: 18-W130-55.0 (20°C) and 18-W130-55.0 (7dry). In 18-W130-55.0 (20°C), the concrete was poured, and then kept sealed (not dried) in a 20°C environment. In 18-W130-55.0 (7dry), the concrete was poured, sealed in a 20°C environment until the material was 7 days old, removed from the form at 7 days old (point A in the figure), and cured in air (dried). In the comparative example, the concrete was poured and then kept sealed at 20°C, as in the case of 18-W130-55.0 (20°C). When the number of days since pouring is short, shrinkage distortion is mainly caused by autogenous shrinkage (shrinkage in the early stage after concrete pouring, which occurs when water in concrete is consumed by cement hydration). In the comparative example and 18-W130-55.0 (20°C), sealing is continued, so drying shrinkage (shrinkage over a long period after concrete pouring, which occurs when water in concrete dissipates into the air) does not occur. From the above, it can be seen that the initial shrinkage distortion due to autogenous shrinkage is suppressed in all cases of 18-W130-55.0 (20°C), 18-W130-55.0 (7dry), and the comparative example. In the case of 18-W130-55.0 (7dry), water evaporation progresses after removal from the form, and shrinkage distortion due to drying shrinkage progresses accordingly.

[0015] FIG. 3(a) shows the shrinkage strain for Examples 4-6 and Comparative Examples 2-3, and FIG. 3(b) shows the mix proportions for Examples 4-6 and Comparative Examples 2-3. The fine aggregate ratio (s / a) is 47.5. In each Example and Comparative Example, the form was removed at 7 days (point A in the figure) and cured in air. In Examples 4-6, artificial lightweight fine aggregate was used as the fine aggregate, and in Comparative Examples 2-3, crushed sand was used as the fine aggregate. The water content (unit water content) W is the same in all cases. In Examples 4-6, both autogenous shrinkage and drying shrinkage are suppressed. In Comparative Examples 2-3, autogenous shrinkage is large, but drying shrinkage is about the same as in Examples 4-6.

[0016] From the above, the following can be understood. First, comparing artificial lightweight fine aggregate with crushed sand, as shown in FIG. 3(a), autogenous shrinkage is suppressed when artificial lightweight fine aggregate is used. This is considered to be because the internal voids of artificial lightweight fine aggregate have high water retention performance, and the autogenous shrinkage suppression effect due to the internal curing effect is large. The autogenous shrinkage suppression effect due to the internal curing effect is a conventionally known feature of artificial lightweight fine aggregate. On the other hand, 18-W130-55.0(20°C) and 18-W130-55.0(7dry) differ only in the presence or absence of sealing after 7 days of age, but as shown in FIG. 2(a), even in 18-W130-55.0(7dry), the shrinkage strain due to drying shrinkage does not increase significantly. This is considered to be because the water content (unit water content) W in Example 1 is low. In other words, water not used in the cement hydration reaction remains in the gaps in the artificial lightweight fine aggregate, which is the cause of drying shrinkage, but because the unit water content W is small, the amount of residual water is reduced, and it is believed that drying shrinkage is suppressed. Furthermore, as a result of the reduction in the amount of residual water, frost resistance is improved. Frost damage occurs when the water contained in the voids in the concrete repeatedly freezes, expands, and melts, causing repeated stress to be applied to the concrete. The reduction in residual water suppresses stress, and it is believed that this suppresses the fluctuations in the relative dynamic modulus of elasticity and mass reduction rate, as shown in Figure 1(a).

[0017] Unit water volume W is 110-140kg / m 3 or about 125-140 kg / m 3 in the range of 130 kg / m 3 ±5kg / m 3 Range of about 125 to 135 kg / m 3It is considered that similar results to those of each Example will be obtained when the water-binder ratio W / B is within the range of 18% to 20%. Examples 1 and 3 differ only in the water-binder ratio W / B, and Example 1 (W / B=18) is slightly better in frost resistance than Example 3 (W / B=20), but both have sufficient frost resistance. Therefore, it is preferable that the water-binder ratio W / B is at least in the range of 18 to 20%. Furthermore, by including PP (polypropylene fiber) (Example 6), the frost resistance is further improved. As the fiber, organic fibers other than polypropylene fiber can also be used. It is preferable that all the fine aggregates are artificial lightweight fine aggregates, but the effects of the present invention can be obtained even if only a part of the fine aggregates is artificial lightweight fine aggregate.

[0018] By using artificial lightweight fine aggregate as fine aggregate, the fluidity is greatly improved compared to the case where crushed sand is used. Table 4 shows the fresh test results of Example 4 and Comparative Example 2. The slump flow value was measured according to JIS A1150:2014 "Concrete Slump Flow Test Method". The 50 cm slump flow passing time is the time from the moment the cone is lifted up until the diameter of the concrete expands to 50 cm, and is one of the indicators of concrete fluidity. There is no measurement value for Comparative Example 2 because the slump flow value did not reach 50 cm. The difference between Example 4 and Comparative Example 2 is the type of fine aggregate. Example 4 uses artificial lightweight fine aggregate as fine aggregate, and Comparative Example 2 uses crushed sand as fine aggregate. Comparative Example 2 uses a larger amount of high performance water reducing agent (SP) than the Examples, but the slump flow value is extremely smaller than the Examples. In other words, extremely high fluidity can be obtained by using artificial lightweight fine aggregate as fine aggregate.

[0019] [Table 4]

[0020] FIG. 4(a) shows the relationship between the accelerated age and the accelerated carbonation depth for Examples 1 and 3 and Comparative Example 1, and FIG. 4(b) shows the mix ratios for Examples 1 and 3 and Comparative Example 1. The accelerated carbonation depth was determined based on JISA1153:2012 "Accelerated carbonation test method for concrete". Concrete is neutralized by the reaction of carbon dioxide in the atmosphere with calcium hydroxide in the concrete. Carbonation of concrete increases the possibility of corrosion of reinforcing bars. Therefore, the resistance of concrete to carbonation is one of the indicators of long-term durability of concrete, similar to frost resistance. If the accelerated carbonation depth is 25 mm or less 26 weeks after the start of the accelerated test, it is evaluated as having sufficient carbonation resistance. Although there is only data up to 13 weeks for Examples 1 and 3, it is considered that they have sufficient carbonation resistance by comparing with Comparative Example 1.

[0021] Fig. 5(a) shows the relationship between age and compressive strength for Examples 1-3, 7 and Comparative Example 1, and Fig. 5(b) shows the mix proportions for Examples 1-3, 7 and Comparative Example 1. Fig. 5(a) shows the relationship between age and compressive strength for standard cured test specimens. Examples 1-3, 7 have greater compressive strength than Comparative Example 1. It is generally believed that the smaller the water-binder ratio W / B, the higher the compressive strength of concrete, and this general tendency was confirmed from Fig. 5(a).

[0022] Fig. 6(a) shows the relationship between compressive strength and Young's modulus for Examples 1 to 3, 7 and Comparative Example 1, and Fig. 6(b) shows the mix proportions for Examples 1 to 3, 7 and Comparative Example 1. Taking into account the design margin, the Young's modulus is often calculated as 0.8 times the value. The specific gravity γ of concrete using artificial lightweight fine aggregate is 2.3t / m 3 In Fig. 6(a), γ = 2.4t / m 3 and 2.1t / m 3 In Examples 1 to 3 and 7, γ is 2.4t / m 3 The Young's modulus exceeds the value obtained by multiplying the calculated value in the case of 0.8. Artificial lightweight aggregate is softer than crushed sand, and the Young's modulus tends to decrease accordingly, but in Examples 1 to 3 and 7, no problem was observed in terms of Young's modulus (rigidity).

[0023] Table 5 shows the mix proportions of the concrete compositions of Examples 8 to 14 and Comparative Example 4, and Table 6 shows the specifications of the materials used in Examples 8 to 14 and Comparative Example 4. Example 8 has a different lot from Example 1, but the mix proportions are the same. The materials used in Examples 8 to 14 and Comparative Example 4 are basically the same as those used in Examples 1 to 7 and Comparative Examples 1 to 3.

[0024] [Table 5]

[0025] [Table 6]

[0026] Table 7 shows the fresh test results of Examples 8 to 14 and Comparative Example 4. The fresh tests were conducted in the same manner as the fresh test shown in Table 4. All of the examples showed better fluidity than Comparative Example 2 in Table 4, and it was confirmed that high fluidity can be obtained by using artificial lightweight fine aggregate as the fine aggregate. As will be described later, it is believed that the fluidity of Comparative Example 4 was reduced because the amount of fine aggregate was greater than the amount of water and binder.

[0027] [Table 7]

[0028] FIG. 7 shows the compressive strengths of Examples 8 to 14 and Comparative Example 4. In the figure, "90°C sealed σ7" means the compressive strength after pouring concrete and sealing it in a 90°C environment for 7 days, "standard σ28" means the compressive strength after pouring concrete and curing it in water for 28 days, and "20°C sealed σ7" means the compressive strength after pouring concrete and sealing it in a 20°C environment for 7 days. In Examples 8 to 14 and Comparative Example 4, a compressive strength of a level that is practically acceptable was obtained. Also, as in FIG. 5, it was confirmed that the smaller the water-binder ratio W / B, the higher the compressive strength of the concrete.

[0029] FIG. 8(a) shows the relative dynamic modulus of elasticity up to 150 cycles for Examples 8 to 14 and Comparative Example 4. For Examples 8 to 11 and Comparative Example 4, the relative dynamic modulus of elasticity was measured up to 300 cycles, and is shown separately in FIG. 8(b). FIG. 9 shows the mass reduction rate for Examples 8 to 14 and Comparative Example 4. The relative dynamic modulus of elasticity and the mass reduction rate were obtained based on the underwater freeze-thaw test method (A method) specified in JISA1148:2010 "Concrete freeze-thaw test method". In Comparative Example 4, the relative dynamic modulus of elasticity fell below 60% of the initial value at about 150 cycles, whereas in Examples 8 to 11, values ​​similar to the initial value were obtained even after 300 cycles. For Examples 12 to 14, only the measurement results up to 150 cycles were obtained, but judging from the tendency up to 150 cycles and FIG. 8(b), it can be evaluated that the relative dynamic modulus of elasticity at 300 cycles is at least 60% or more. In Comparative Example 4, the mass reduction rate decreased around 150 cycles and then tended to recover. In contrast, in Examples 8 to 14, the mass reduction rate was less than 1% or negative (mass increased). Note that Figure 8(b) also shows the data for Example 1, and Examples 1 and 8, which have the same composition, showed almost the same results, confirming the reproducibility of the test results.

[0030] Figure 10 shows the unit amount of water W (kg / m 3 ) and the water-binder ratio W / B (%). Comparing with FIG. 8, in trapezoidal region A defined by W being 110 or more and 150 or less, and W / B being 18 or more and (0.168×(W−110)+20) or less, and preferably in trapezoidal region B defined by W being 110 or more and 140 or less, and W / B being 18 or more and (0.168×(W−110)+20) or less, the relative dynamic modulus of elasticity is 60% or more at 300 cycles. Also, in this region, the mass reduction rate is less than 1% or negative (mass increases) in the range of 0 to 300 cycles. Therefore, the unit amount of water W (kg / m 3 Regarding the relationship between the water-binder ratio W / B (%) and the viscosity coefficient, region A is preferable, and region B is more preferable.

[0031] Figure 11 shows the relationship between air volume and durability index DF. Durability index DF is an index for evaluating the frost resistance of concrete, as defined in JISA1148:2010 "Freezing and thawing test method for concrete." Generally, a value of 60 or higher is considered to be frost resistant.

[0032] Figure 12 shows the relationship between vs / vp and standard σ28. vs indicates the unit absolute volume of fine aggregate, and vp indicates the unit absolute volume of paste. Figure 13 shows the unit fine aggregate volume (kg / m 3 ) and standard σ28. As can be seen from Table 5, Comparative Example 4 has a large amount of fine aggregate and small amounts of cement and water. This is thought to be why sufficient compressive strength was not obtained. From Fig. 11, it can be seen that when W is 110 or more and 150 or less, preferably 110 or more and 140 or less, and vs / vp is 0.67 or more and 1.00 or less, the relative dynamic modulus of elasticity is 60% or more at 300 cycles. From Fig. 12, it can be seen that when W is 110 or more and 150 or less, preferably 110 or more and 140 or less, and vs / vp is 0.67 or more and 1.00 or less, the relative dynamic modulus of elasticity is 60% or more at 300 cycles. 3 When the relative dynamic modulus of elasticity is 515 or more and 655 or less, the relative dynamic modulus of elasticity is 60% or more at 300 cycles. In addition, in these regions, the mass reduction rate is less than 1% or negative (mass increase) in the range of 0 to 300 cycles.

[0033] Fig. 14 shows the shrinkage strain for Examples 8 to 11 and Comparative Example 4. Fig. 14(a) shows the shrinkage strain when sealed at 20°C, and Fig. 14(b) shows the shrinkage strain when sealed at 20°C until the material was 7 days old and then cured in air at 20°C and a relative humidity of 60%. When sealed at 20°C, no shrinkage was observed in Examples 8 to 11 and Comparative Example 4. When sealed at 20°C until the material was 7 days old and then cured in air, the shrinkage strain was 200×10 -6 Although the shrinkage progressed to a certain extent, the shrinkage strain was suppressed compared to the case shown in Figure 3.

[0034] Figure 15 shows the relationship between unit water content and shrinkage strain, and Figure 16 shows the relationship between W / B and shrinkage strain. It can be seen that unit water content and W / B do not have a significant effect on shrinkage strain.

Claims

1. The method includes the steps of: forming a concrete structure using a binder, water, and fine aggregate; and forming a concrete structure using the binder and water; The unit water content of the water is W (kg / m 3 , and a water-binder ratio is W / B (%), W is 110 or more and 140 or less, and W / B is 18 or more and (0.168×(W−110)+20) or less.

2. The method includes the steps of: providing a binder, water, and fine aggregate, the binder including cement, and the fine aggregate including lightweight fine aggregate; The unit water content of the water is W (kg / m 3 ), where vs / vp is a volume ratio of the fine aggregate to the paste, W is 110 or more and 140 or less, and vs / vp is 0.67 or more and 1.00 or less.

3. The method includes the steps of: forming a concrete structure using a binder, water, and fine aggregate; and forming a concrete structure using the binder and water; The unit water content of the water is W (kg / m 3 ) is 110 or more and 140 or less, unit fine aggregate amount (kg / m 3 ) is 515 or more and 655 or less.

4. The concrete composition according to any one of claims 1 to 3, wherein W = 125 to 140.

5. 4. The concrete composition according to claim 1, wherein W=125 to 135.

6. 6. The concrete composition according to claim 1, wherein the fine aggregate comprises an artificial lightweight fine aggregate.

7. The concrete composition of claim 1 , further comprising organic fibers.

8. 8. The concrete composition of claim 1, wherein the binder comprises silica fume.

Citation Information

Patent Citations

  • Image reader

    JP1986080946A

  • Concrete composition reinforced with high-strength fiber, product using the composition and production of the product

    JP1990267146A

  • Vinylon(r) fiber reinforced lightweight concrete

    JP1998114562A

  • Low-shrinking concrete composition

    JP1999092200A

  • Manufacture of lightweight concrete

    JP1999131803A