Rare earth sintered magnet and method for manufacturing rare earth sintered magnet

By optimizing carbon, oxygen, and nitrogen concentrations, and using specific lubricants, the method enhances the magnetic properties of R-Fe-B sintered magnets, achieving high residual magnetic flux density and coercive force.

JP7574736B2Active Publication Date: 2024-10-29SHIN ETSU CHEMICAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021080801
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-12
Publication Date
2024-10-29
Estimated Expiration
2041-05-12

AI Technical Summary

Technical Problem

Existing methods for producing R-Fe-B sintered magnets face challenges in achieving high residual magnetic flux density (Br) and coercive force (HcJ) due to issues with impurity control, particularly nitrogen and oxygen concentrations, which affect the orientation and crystal grain size, leading to contradictory effects on magnetic properties.

Method used

The method involves optimizing carbon, oxygen, and nitrogen concentrations, along with controlling the average crystal grain size and orientation degree, using specific lubricants with polar functional groups and cyclohexane skeletons to enhance the magnetic properties of R-Fe-B sintered magnets.

Benefits of technology

This approach results in a rare earth sintered magnet with high Br and stable HcJ, achieving both high performance and stability by optimizing the relationship between crystal grain size and orientation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574736000005
    Figure 0007574736000005
  • Figure 0007574736000001
    Figure 0007574736000001
  • Figure 0007574736000002
    Figure 0007574736000002
Patent Text Reader

Abstract

To provide a high-quality R-Fe-B rare earth sintered magnet having low nitrogen concentration and high orientation even at low oxygen concentration, high Br and stable HcJ.SOLUTION: An R-Fe-B rare earth sintered magnet has a carbon concentration of 800 to 1400 ppm, an oxygen concentration of 1000 ppm or less, and a nitrogen concentration of 800 ppm or less. The average crystal grain size D50 (μm), which is the area average of the equivalent circle diameter in a surface parallel in a magnetization direction is 4.5 μm or less, and the D50, the residual magnetic flux density Br, and the orientation Or (%) defined by the formula [Or=(Br / 4πIs)×100] by the saturation magnetic flux density 4πIs satisfy a relationship of the [Or>0.7×D50+952].SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rare earth sintered magnet having high residual magnetic flux density and stable coercive force, and to a method for producing the same. [Background technology]

[0002] R-Fe-B sintered magnets (hereinafter sometimes referred to as Nd magnets) are essential functional materials for energy conservation and high performance, and their range of applications and production volume are expanding year by year. For example, they are used in drive motors and electric power steering motors in hybrid and electric vehicles, motors for air conditioner compressors, and voice coil motors (VCM) in hard disk drives. In these various applications, the high residual magnetic flux density (hereinafter referred to as Br) of R-Fe-B sintered magnets is a great advantage, but further improvements in Br are required, for example to further miniaturize motors.

[0003] One method to increase the Br of R-Fe-B sintered magnets is to use RFe 14 In order to increase the proportion of B phase, there are methods to reduce the R content while reducing impurities such as oxygen, carbon, and nitrogen, and methods to reduce the R content while increasing the proportion of B phase. 14 Methods for improving the degree of orientation of the B phase are known.

[0004] The main phase is R2Fe 14 One method known to improve the degree of orientation of the B phase is to increase the amount of lubricant added during fine grinding, which is also known to suppress nitridation. However, adding a large amount of lubricant can lead to a decrease in moldability and a decrease in coercivity (hereafter referred to as H) due to an increase in the amount of carbon remaining after sintering. cJ Because of this, lubricants are required to be highly effective in improving orientation and moldability within limited amounts added, and methods have been proposed to use various substances, primarily organic compounds, as lubricants.

[0005] For example, Japanese Patent Laid-Open Publication No. 4-214804 (Patent Document 1) proposes a method of using at least one of solid paraffin and camphor as a lubricant to impart excellent lubricity and reduce friction between the die face and the compact during molding, thereby suppressing scratches, peeling, cracks, etc. on the surface of the compact.

[0006] Furthermore, Japanese Patent Application Laid-Open No. 2002-285208 (Patent Document 2) describes that a solid that sublimes at room temperature is used as a lubricant, which is added to raw alloy coarse powder and then finely ground, so that the lubricant coats the fine powder particles, suppressing the formation of an oxide film and resulting in a fine powder with excellent fluidity.

[0007] Furthermore, JP 2020-31145 A (Patent Document 3) proposes a sintered magnet that has a specific structure and composition, a fine structure with a crystal grain size of 3.5 μm or less, and a high degree of orientation, as well as a manufacturing method thereof in which the raw material powder is nitrided and the compression molding process is omitted. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 4-214804 [Patent Document 2] JP 2002-285208 A [Patent Document 3] JP 2020-31145 A Summary of the Invention [Problem to be solved by the invention]

[0009] As described above, Patent Documents 1 and 2 propose the selection of a lubricant, but neither of them mentions the effect on Br.

[0010] In Patent Document 1, a lubricant is selected to prevent cracking and chipping of the compact due to a reduction in the ejection pressure of the compact and to improve the product yield. 3This is expected to be due to the high molding pressure causing a disturbance in the orientation, which is contrary to the purpose of obtaining a high Br.

[0011] In addition, in Patent Document 2, the effect of suppressing oxidation of fine powder is obtained by coating the surface of the fine powder with a sublimable lubricant, and although there are regulations regarding the oxygen content, there is no mention of the effect of nitrogen concentration due to fine grinding under low oxygen and low moisture conditions, and there is no mention of high Br and H cJ In addition, when a compound that is a solid at room temperature and has sublimation properties is added as a lubricant to a jet mill system, the lubricant concentration in the system increases during the continuous manufacturing process, and there is a risk that the lubricant will precipitate and clog the low-temperature part of the piping, or that the carbon concentration will increase unintentionally, so that equipment measures such as monitoring the lubricant gas concentration in the system are required, which increases manufacturing costs.

[0012] On the other hand, in Patent Document 3, in order to achieve both a high degree of orientation and fine crystal grains, a method is adopted in which the raw material powder is dispersed in nitrogen gas for a certain period of time to perform nitriding. However, in order to obtain a high Br, in order to effectively locate R at the grain boundaries while reducing R, it is necessary to reduce the amount of nitrogen, which is an impurity that forms a compound phase with R, as much as possible and to reduce H. cJ There is a challenge in that it is necessary to ensure

[0013] In addition, in the method of obtaining a high Br by reducing the R content while reducing the impurities contained in the magnet, such as oxygen, carbon, and nitrogen, the nitrogen concentration increases as the oxygen concentration decreases, causing a decrease in coercivity. On the other hand, the H content, which decreases when the R content is reduced to increase Br, cJ If attempts were made to compensate for this by making the crystal grains finer, the nitriding would proceed further and the degree of orientation would also deteriorate, which was a problem.

[0014] The present invention has been made in view of the above problems, and has disclosed an R-Fe-B rare earth sintered magnet having fine crystal grains, which has a low nitrogen concentration and high orientation even at low oxygen concentrations, and has high Br and stable H cJ The object of the present invention is to provide a high-quality R-Fe-B rare earth sintered magnet having the above properties. [Means for solving the problem]

[0015] As a result of intensive research into solving the above problems, the inventors have found that by adjusting the carbon concentration, oxygen concentration, and nitrogen concentration to specific values ​​and optimizing the average crystal grain size D50 in a plane parallel to the magnetization direction and the relationship between the D50 and the degree of orientation Or, it is possible to obtain high Br and H cJ In addition, when the coarsely pulverized alloy powder containing R, Fe, and B is pulverized to obtain fine powder for magnet molding, the lubricant type and the average particle size of the pulverized fine powder can be optimized to obtain a rare earth sintered magnet having high Br and H. cJ The present invention has been accomplished based on the discovery that it is possible to produce a rare earth sintered magnet having the above-mentioned properties.

[0016] That is, the present invention provides the following rare earth magnet and method for producing the same. 1. A rare earth sintered magnet containing R (R is one or more elements selected from rare earth elements, Nd being an essential element), Fe, and B, characterized in that the magnet has a carbon concentration of 800 to 1400 ppm, an oxygen concentration of 1000 ppm or less, a nitrogen concentration of 800 ppm or less, and an average crystal grain size D50 (μm), which is the area average of the equivalent circle diameters of crystal grains in a plane parallel to the magnetization direction, of 4.5 μm or less, and further in that the D50 and the degree of orientation Or (%), which is defined by the following formula (1) using the residual magnetic flux density Br and the saturation magnetic flux density 4πIs, satisfy the relationship of the following formula (2). Or = (Br / 4πIs) × 100 (1) Or>0.7×D50+95 (2) 2. The rare earth sintered magnet of item 1, further comprising 0.05 to 0.5 atomic % of X (X is one or more elements selected from Ti, Zr, Hf, Nb, V, and Ta), wherein the atomic percentages of B and X are [B] and [X], respectively, and the relationship represented by the following formula (3) is satisfied: 4.3<[B]―2[X]<5.5 (3) 3. The rare earth sintered magnet of 1 or 2, wherein the content of R is 12.5 to 15.0 atomic %. 4. The rare earth sintered magnet of any one of 1 to 3, wherein R contains one or more elements selected from Dy, Tb, Gd and Ho in an amount of more than 0 and not more than 1 mass %. 5. A rare earth sintered magnet according to any one of 1 to 4, which contains, as part of R, an R element introduced into the sintered magnet by grain boundary diffusion. 6. A method for producing a rare earth sintered magnet, comprising the steps of: finely pulverizing a coarsely pulverized powder of an alloy containing R, Fe, and B to obtain a fine powder; compacting the fine powder in a magnetic field using a compression molding machine to obtain a molded body; and heat treating the molded body to obtain a sintered body, In the fine pulverization step, a raw material powder obtained by adding a compound having a polar functional group and a cyclohexane skeleton to the coarsely pulverized powder is finely pulverized in an inert gas atmosphere so that the average particle size, which is the median size in the volume-based particle size distribution measured by a laser diffraction / scattering method, is 0.5 to 3.5 μm. In the molding process, the density is 2.8 to 3.6 g / cm 3 Obtain a molded body of The present invention relates to a method for producing a rare earth sintered magnet. 7. The method for producing a rare earth sintered magnet according to claim 6, wherein the compound having a polar functional group and a cyclohexane skeleton is a compound having a molecular weight of 250 or less. 8. The method for producing a rare earth sintered magnet according to 6 or 7, wherein the compound having a polar functional group and a cyclohexane skeleton is added in an amount of 0.08 to 0.3 parts by mass per 100 parts by mass of the coarsely pulverized powder. 9. The method for producing a rare earth sintered magnet according to any one of 6 to 8, wherein the oxygen concentration of the resulting rare earth sintered magnet is 1000 ppm or less. 10. The method for producing a rare earth sintered magnet according to any one of 6 to 9, wherein the nitrogen concentration of the resulting rare earth sintered magnet is 800 ppm or less. 11. The method for producing a rare earth sintered magnet according to any one of 6 to 10, wherein the polar functional group of the compound having a polar functional group and a cyclohexane skeleton is any one of an OH group, a COOH group, a CH3COO group, and an NH2 group. 12 The strength of the molded body is 20 N or more when a push-pull gauge is pressed against the molded body and the force applied to the push-pull gauge when a crack occurs is measured. 111. A method for producing a rare earth sintered magnet according to any one of claims 1 to 9. 13 6 to 7, wherein the vapor pressure of the compound having a polar functional group and a cyclohexane skeleton at 25°C is 15 Pa or less. 12 1. A method for producing a rare earth sintered magnet according to any one of claims 1 to 9. Effect of the Invention

[0017] According to the present invention, high Br and H cJ Thus, a high-performance rare earth sintered magnet having both of these properties can be obtained. [Brief description of the drawings]

[0018] [Figure 1] 1 is a graph showing the relationship between the average crystal grain size D50 and the degree of orientation for the rare earth sintered magnets of Examples 1, and 8 to 10, and Comparative Examples 1, and 8 to 11, when menthol, a compound having a polar functional group and a cyclohexane skeleton, and stearic acid, a linear saturated fatty acid, were used as lubricants. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] As described above, the rare earth sintered magnet of the present invention contains R, Fe, and B, has a carbon concentration of 800 to 1400 ppm, an oxygen concentration of 1000 ppm or less, and a nitrogen concentration of 800 ppm or less, and has a specific relationship between the average crystal grain size D50 (μm) and the degree of orientation Or (%).

[0020] The element R constituting the rare earth sintered magnet alloy of the present invention is one or more elements selected from rare earth elements, preferably Nd, Pr, La, Ce, Gd, Dy, Tb, and Ho, and more preferably Pr, Nd, Dy, and Tb. Note that some of the R elements may be introduced into the sintered magnet by grain boundary diffusion.

[0021] The content of the R element is preferably 12.5 atomic % or more, and more preferably 12.7 atomic % or more, from the viewpoint of suppressing the crystallization of α-Fe in the raw alloy during production and of sufficiently achieving densification. Although it is difficult to eliminate α-Fe even by homogenization, within the above range, the H of the R-Fe-B sintered magnet can be reduced. cJ This also applies when the raw alloy is produced by strip casting, in which crystallization of α-Fe is unlikely to occur. In addition, it is possible to prevent insufficient densification of R-Fe-B sintered magnets, which would otherwise occur due to a decrease in the amount of liquid phase, which is mainly composed of R components and plays a role in promoting densification in the sintering process described below. On the other hand, if the R content exceeds 14 atomic %, the R2Fe 14 From the viewpoint of preventing a decrease in the proportion of the B phase and a decrease in Br, the content is preferably 15.0 atomic % or less, and more preferably 14.0 atomic % or less.

[0022] In addition, the R preferably contains one or more elements selected from Dy, Tb, Gd, and Ho in a range of more than 0% by mass to 1% by mass, and more preferably in a range of more than 0.3% by mass to 0.8% by mass. Dy, Tb, Gd, and Ho can efficiently convert H into H with small amounts of added. cJ It is preferable to add these elements to magnets because they have the effect of improving the magnet's magnetization. However, these elements are rarer and more expensive than Nd, and from the viewpoint of suppressing the decrease in Br due to their addition, it is preferable to limit the content of these elements to 1 mass % or less.

[0023] Furthermore, as described above, the essential elements include Fe and B. Although there are no particular limitations on the contents of these elements, the Fe content is preferably 75 atomic % or more, more preferably 77 atomic % or more, and is preferably 83 atomic % or less, more preferably 81 atomic % or less. The B content is preferably 5.0 to 6.0 atomic %, more preferably 5.3 to 5.7 atomic %.

[0024] In addition, the rare earth sintered magnet of the present invention preferably contains, as X, one or more elements selected from Ti, Zr, Hf, Nb, V, and Ta, and the content is preferably 0.05 atomic % or more, and more preferably 0.1 atomic % or more, from the viewpoint of obtaining a good effect of suppressing abnormal grain growth during the sintering process. 14 The amount of B required to form the B phase is reduced, and the R2Fe 14 The decrease in the B phase ratio leads to a decrease in Br, and thus to a decrease in R2Fe 17 The formation of the phase results in significant H cJ In order to reduce the risk of causing a decrease, it is preferably 0.5 atomic % or less, and more preferably 0.3 atomic % or less. Furthermore, X forms an XB2 phase with B and consumes B, which is a constituent element of the main phase, so that a sufficient amount of the main phase is secured to obtain a high Br while obtaining a high orientation. As for C, which is derived from the lubricant added in large amounts and can partially replace B in the main phase, in order to allow a high carbon concentration, when the atomic percentages of B and X are [B] and [X], respectively, the content of B preferably satisfies the relationship of the following formula (3), and more preferably satisfies the relationship of the following formula (3'). 4.3<[B]―2[X]<5.5 (3) 4.5<[B]―2[X]<5.3 (3')

[0025] As described above, the carbon concentration of the sintered magnet of the present invention is in the range of 800 to 1400 ppm, and more preferably in the range of 900 to 1200 ppm. cJ On the other hand, if the content is less than 800 ppm, it becomes difficult to obtain sufficient orientation.

[0026] From the viewpoint of obtaining a high Br by reducing the amount of R added while reducing impurities, the oxygen concentration in the sintered magnet of the present invention is, as described above, 1000 ppm or less, and more preferably 800 ppm or less. As will be explained in the manufacturing method described later, the oxygen concentration of the sintered body is strongly affected by the presence of oxygen and moisture in the fine grinding process of the raw materials, and if the oxygen concentration exceeds 1000 ppm, oxidation and hydroxylation of the fine powder surface becomes significant, the adsorption sites on the metal surface decrease, and the amount of adsorption of the lubricant decreases, making it impossible to exert a sufficient effect.

[0027] The nitrogen concentration in the sintered magnet of the present invention is good H cJ From the viewpoint of obtaining the above, the concentration is 800 ppm or less, preferably 500 ppm or less, and more preferably 400 ppm or less.

[0028] As described above, the rare earth sintered magnet of the present invention has a specific relationship between the average crystal grain size D50 (μm) and the degree of orientation Or (%). The average crystal grain size is defined as the median value D50 (μm) of the equivalent circle diameter of the crystal grains in a plane parallel to the magnetization direction. In the present invention, this average crystal grain size D50 (μm) is 4.5 μm or less, preferably 4.0 μm or less, and more preferably 3.5 μm or less. If this average crystal grain size D50 exceeds 4.5 μm, sufficient H cJ Although there is no lower limit for the average crystal grain size D50 (μm), in consideration of obtaining a good degree of orientation within an appropriate range of the amount of lubricant added, the average grain size D50 is preferably 1.2 μm or more, and more preferably 1.8 μm or more.

[0029] The average crystal grain size D50 can be measured, for example, by the following procedure. First, a cross section of a sintered magnet parallel to the magnetization direction is polished to a mirror finish, and then, for example, a Virela liquid (e.g., Mixing ratioThe grain boundary phase of the cross section is selectively etched by immersing the sample in an etching solution such as glycerin:nitric acid:hydrochloric acid=3:1:2), and a cross-sectional image is obtained using a laser microscope. Next, the cross-sectional area of ​​each particle is measured based on the obtained cross-sectional image by image analysis, and the diameter is calculated as the circle equivalent diameter. The average crystal grain size is preferably the average of a large number of particles in images of multiple locations, and for example, although not particularly limited, it is preferably measured by a method such as taking the area-based median diameter of a total of about 2000 or more particles in images of 20 or more different locations.

[0030] Moreover, the degree of orientation Or (%) is defined by the residual magnetic flux density Br and the saturation magnetic flux density 4πIs according to the following formula (1), and the residual magnetic flux density Br can be obtained by measuring the magnetic properties of the sintered magnet with a BH tracer. Or = (Br / 4πIs) × 100 (1)

[0031] As described above, in the rare earth sintered magnet of the present invention, the average crystal grain size D50 (μm) and the degree of orientation Or (%) satisfy the relationship of the following formula (2). cJ This makes it possible to achieve both an improvement in the quality and a high Br. Or>0.7×D50+95 (2)

[0032] Next, a method for producing a rare earth sintered magnet of the present invention will be described. The method for producing the rare earth sintered magnet of the present invention is for producing the rare earth sintered magnet of the present invention, and includes a fine grinding step of finely grinding the coarsely ground powder of the alloy containing R, Fe, and B to obtain a fine powder, a molding step of molding the fine powder in a magnetic field to obtain a molded body, and a heat treatment step of heat treating the molded body to obtain a sintered body.

[0033] The individual steps involved in producing an alloy for an R-Fe-B rare earth sintered magnet by the production method of the present invention are basically the same as those in ordinary powder metallurgy and are not particularly limited, but typically include a melting step in which raw materials are melted to obtain a raw material alloy, and a crushing step in which a raw material alloy having a predetermined composition is crushed to prepare an alloy fine powder, and the crushing step includes a coarse crushing step to obtain the coarsely crushed powder and a fine crushing step to obtain the fine powder.

[0034] First, in the melting step, metals or alloys serving as raw materials for each element are weighed so as to obtain the predetermined composition in the present invention described above, and the raw materials are melted, for example, by high-frequency melting, and cooled to produce a raw alloy. The raw alloy is generally cast by a melting casting method in which the alloy is poured into a flat mold or a book mold, or a strip casting method. In addition, the R2Fe, which is the main phase of the R-Fe-B alloy, is melted by melting the raw materials, for example, by high-frequency melting, and cooled to produce a raw alloy. 14 The present invention can also be applied to the so-called two-alloy method, in which an alloy close to the B compound composition and an R-rich alloy that becomes a liquid phase auxiliary at the sintering temperature are separately prepared, coarsely crushed, and then weighed and mixed. However, since the α-Fe phase is easily crystallized in the alloy close to the main phase composition depending on the cooling rate and alloy composition during casting, it is preferable to perform a homogenization treatment for 1 hour or more at 700 to 1200 ° C in a vacuum or Ar atmosphere as necessary in order to homogenize the structure and eliminate the α-Fe phase. Note that when an alloy close to the main phase composition is prepared by a strip casting method, homogenization can be omitted. In addition to the above casting method, the so-called liquid quenching method can also be adopted for the R-rich alloy that becomes a liquid phase auxiliary.

[0035] The above-mentioned pulverization step is a multi-stage process including, for example, a coarse pulverization step and a fine pulverization step. In the coarse pulverization step, for example, a jaw crusher, a Braun mill, a pin mill, or hydrogen pulverization is used. In the case of an alloy produced by strip casting, hydrogen pulverization is usually applied to obtain coarse powder pulverized to, for example, 0.05 to 3 mm, particularly 0.05 to 1.5 mm.

[0036] In the fine pulverization step, a lubricant is added to the coarse powder obtained in the coarse pulverization step, and the coarse powder is finely pulverized using a method such as jet mill pulverization.

[0037] In the manufacturing method of the present invention, in the fine pulverization step, a compound having a polar functional group and a cyclohexane skeleton is used as a lubricant, and fine pulverization is performed so that the average particle size of the fine powder is in the range of 0.5 to 3.5 μm. In this case, the average particle size of the fine powder is more preferably 1.0 to 3.0 μm, and even more preferably 1.5 to 2.8 μm. In this way, a specific compound is used as a lubricant, and the fine powder adjusted to the average particle size in the above range is molded and heat-treated to form a sintered body, thereby obtaining the rare earth sintered magnet of the present invention that exhibits particularly high magnetic properties. The average particle size of the powder refers to the median diameter in the volume-based particle size distribution measured by a laser diffraction / scattering method. The reason why the high magnetic properties are obtained as described above is not necessarily clear, but it can be speculated as follows.

[0038] The compound having a polar functional group and a cyclohexane skeleton used as a lubricant is effectively adsorbed to the fine powder particles due to the polar functional group, and furthermore, since the cyclohexane skeleton has a three-dimensional molecular structure, it is considered that the repulsion between the fine powder particles is strengthened, and the effect of improving the dispersibility of the fine powder particles is improved compared to known lubricants such as linear fatty acid compounds. On the other hand, when a compound having a polar functional group and a cyclohexane skeleton is used as a lubricant, the frictional force between the particles is higher than that of fatty acids having long linear alkyl groups used as conventional lubricants. In particular, when the average particle size of the fine powder is larger than a certain value, that is, when the particle size distribution of the fine powder is wide, the fine powder is likely to be filled into the molding cavity in the molding process of manufacturing rare earth sintered magnets, so that the fine powder particles are likely to come into contact with each other, and the influence of the frictional force between the particles is strong during magnetic field orientation, and the degree of orientation is worse than when a compound having a long linear alkyl group is used as a lubricant. On the other hand, when the fine powder particle size is smaller than a certain value, the particle size distribution of the fine powder is narrow and the fine powder is difficult to pack, resulting in little contact between the particles. It is therefore believed that the effect of improving the dispersibility of the fine powder by using a compound with a three-dimensionally large molecular structure exceeds the effect of increased frictional forces between particles, thereby improving the orientation during molding in a magnetic field.

[0039] As described above, the lubricant compound has a polar functional group for the purpose of promoting chemical adsorption of the lubricant to the surface of the fine powder. We have As the polar functional group, a functional group which is considered to be effective for adsorption to fine powder and which can exist independently at the molecular terminal is preferably an OH group, an NH2 group, a COOH group, or a CH3COO group.

[0040] Specific examples of the lubricant include, but are not limited to, the following compounds. Compounds having a polar functional group and a cyclohexane skeleton include cyclohexanol, cyclohexylamine, cyclohexanone, cyclohexylcarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and methyl cyclohexanecarboxylate. Cyclic terpenes having a cyclohexane skeleton in the molecule include menthol, menthone, camphor, camphorquinone, borneol, isoborneol, isobornyl acetate, and norbornanone. Compounds having optical isomers do not have limited effects due to their three-dimensional structures. In addition, a combination of multiple types of these lubricants may be used within a specified range of addition amount.

[0041] The molecular weight of the lubricant is preferably 250 or less, and more preferably 200 or less, from the viewpoint of the number of molecules required to sufficiently coat the fine powder particles in a given amount of added lubricant.

[0042] In terms of lubricant properties, in order to reduce the risk of precipitation in low-temperature areas due to an increase in the lubricant concentration in the jet mill system when the lubricant is added to the jet mill system together with the coarse powder in the fine pulverization step and a large amount of the lubricant is continuously pulverized, and the risk of the carbon concentration in the sintered magnet increasing excessively, the lubricant preferably has a vapor pressure of 15 Pa or less at 25°C, and more preferably has a vapor pressure of 10 Pa or less. There are no particular limitations on the state of the lubricant at room temperature, but from the viewpoint of the lubricant coating the fine powder more uniformly in the fine pulverization step, the lubricant is preferably a liquid at 25°C.

[0043] The amount of lubricant added is preferably 0.08 parts by mass or more, more preferably 0.10 parts by mass or more, per 100 parts by mass of the coarsely pulverized powder, from the viewpoint of obtaining a sufficient degree of orientation for fine powders having a small particle size of 3.5 μm or less, which are difficult to orient. cJ From the viewpoint of suppressing a decrease in the amount, the amount is preferably 0.3 parts by mass or less, and more preferably 0.2 parts by mass or less.

[0044] The average particle size of the fine powder in the fine pulverization step is, as described above, 0.5 to 3.5 μm, preferably 1.0 to 3.0 μm, and more preferably 1.5 to 2.8 μm. The lower limit of 0.5 μm is set from the viewpoint of suppressing oxidation and nitridation of the fine powder and from the viewpoint of obtaining a good H cJ The upper limit of 3.5μm is set from the viewpoint of obtaining sufficient H cJ This is a setting value based on the viewpoint of obtaining the above.

[0045] The fine powder thus prepared is compacted in an applied magnetic field to obtain a green body, which is then heat-treated to form a sintered body, thereby producing a sintered magnet.

[0046] In the compacting step, a magnetic field of 400 to 1600 kA / m is applied to the alloy powder to orient it in the direction of the easy magnetization axis, and the powder is compacted in a compression molding machine. At this time, the density of the compact is set to 2.8 to 3.6 g / cm. 3 It is preferable to set the density to 3.0 to 3.4 g / cm 3 From the viewpoint of securing the strength of the molded body and obtaining good handling properties, the molded body density is preferably 2.8 g / cm. 3 On the other hand, from the viewpoint of obtaining a suitable Br by ensuring a good grain orientation during compression while obtaining sufficient compact strength, the compact density is preferably 3.6 g / cm 3 Within this range, when the strength of the compact is high, it is possible to suppress a decrease in Br due to the disturbance of the orientation of the fine powder particles aligned in the applied magnetic field direction during compression molding. In addition, it is preferable to perform molding in a gas atmosphere such as nitrogen gas or Ar gas in order to suppress oxidation of the alloy fine powder.

[0047] It has been found that the compacts produced by adding the above-mentioned compounds as lubricants have a higher strength than those produced by using conventional lubricants such as stearic acid due to the increase in friction between the fine powder particles as described above. This is expected to improve productivity by reducing cracks and chips in the compacts, and it also makes it possible to produce compacts with sufficient strength even at lower compacting pressures than before, suppressing the disturbance of orientation during compression molding, and achieving a higher Br.

[0048] Here, the strength of the compact is generally measured by a compression test using a load cell or a bending strength test, but since the compact may ignite in the air, for example, a push-pull gauge installed in a glove box is used to push the gauge into a compact of a given shape from above, and the breaking pressure at the moment when a crack occurs in the compact can be measured and easily evaluated. In the present invention, a digital force gauge RZ-10 and an electric test stand MODEL-2257 manufactured by Aiko Engineering can be used to measure the strength of the compact. Although not particularly limited, from the viewpoint of reducing the deterioration of yield due to damage to the compact due to springback when the compact is removed from the die after powder compaction, crushing when the compact is clamped or held by a vacuum suction pad, and cracking or chipping of the ridge of the compact when the compact is placed in a heat treatment container, the strength of the compact measured by this measurement is preferably 20N or more, more preferably 30N or more.

[0049] In the heat treatment step, the compact obtained in the compacting step is sintered in a high vacuum or a non-oxidizing atmosphere such as Ar gas. In general, the sintering is preferably carried out by holding the compact at a temperature range of 950°C to 1200°C for 0.5 to 10 hours. Cooling after the sintering is completed may be carried out by any of gas quenching (cooling rate: 20°C / min or more), controlled cooling (cooling rate: 1 to 20°C / min), and furnace cooling, and the magnetic properties of the resulting R-Fe-B based sintered magnets will be similar.

[0050] Following the above heat treatment for sintering, the mixture may be subjected to, but is not limited to, HcJ In order to increase the sintering temperature, a heat treatment may be performed at a temperature lower than the sintering temperature. This post-sintering heat treatment may be a two-stage heat treatment consisting of a high-temperature heat treatment and a low-temperature heat treatment, or only a low-temperature heat treatment may be performed. In the high-temperature heat treatment in the post-sintering heat treatment, the sintered body is preferably heat-treated at a temperature of 600 to 950°C, and in the low-temperature heat treatment, the sintered body is preferably heat-treated at a temperature of 400 to 600°C. The cooling may be performed by any of gas quenching (cooling rate: 20°C / min or more), controlled cooling (cooling rate: 1 to 20°C / min), and furnace cooling, and any cooling method will produce an R-Fe-B based sintered magnet with similar magnetic properties.

[0051] Here, regarding the degree of orientation obtained by measuring the magnetic properties of the sintered body obtained after the heat treatment process with a BH tracer, when the average crystal grain size of the conventional sintered body is small, i.e., when the fine powder grain size is small, the magnetic field orientation is difficult in the compacting process and the degree of orientation decreases. However, as described above, when the degree of orientation Or (%) and the average crystal grain size D50 (μm) satisfy the above formula (2) (Or>0.7×D50+95), the H due to the refinement of the crystal grain size can be obtained. cJ In particular, from the viewpoint of obtaining the effect of making the crystal grains fine, the average crystal grain size D50 is 4.5 μm or less as described above, preferably 4.0 μm or less, and more preferably 3.5 μm or less.

[0052] The carbon concentration of the sintered magnet obtained after the heat treatment step depends on the amount of lubricant added during pulverization, and adding a large amount of lubricant to obtain a high Br results in a high carbon concentration and a low HcJ, while adding a small amount of lubricant makes it difficult to obtain sufficient orientation. From the above viewpoints, the carbon concentration of the sintered magnet is set to the range of 800 to 1400 ppm, as described above, and is more preferably set to the range of 900 to 1200 ppm.

[0053] Furthermore, from the viewpoint of obtaining a high Br by reducing the amount of R added while reducing impurities, the oxygen concentration of the sintered magnet obtained after the heat treatment step is set to 1000 ppm or less, as described above, and preferably 800 ppm or less. Furthermore, the oxygen concentration of the sintered body is strongly affected by the presence of oxygen and moisture in the fine grinding step, but if the oxygen concentration exceeds 1000 ppm, oxidation and hydroxylation of the fine powder surface become significant, the adsorption sites on the metal surface decrease, and the amount of adsorption of the lubricant decreases, making it impossible to exert a sufficient effect.

[0054] Furthermore, the nitrogen concentration of the sintered magnet obtained after the heat treatment process is good, as described above. cJ From the viewpoint of obtaining the above, the nitrogen concentration is set to 800 ppm or less, preferably 500 ppm or less, and more preferably 400 ppm or less. When nitrogen is used as an inert gas in the fine pulverization and molding processes, the oxygen and moisture concentrations in the inert gas decrease, and as a result, vacant adsorption sites increase on the surface of the fine powder, which increases the adsorption of nitrogen, causing the nitrogen concentration to increase. However, the increase in the nitrogen concentration of sintered magnets is not due to the H cJ In the present invention, when the average particle size of the fine powder is 3.5 μm or less, the specific surface area increases rapidly with the decrease in the particle size of the fine powder, resulting in a large amount of nitrogen adsorption. However, it has been found that the nitrogen concentration can be reduced compared to conventional lubricants by adding a compound having a polar functional group and a cyclohexane skeleton and then pulverizing the powder.

[0055] The resulting sintered magnet may be subjected to a grain boundary diffusion treatment using Dy or Tb. By reducing the nitrogen concentration to 800 ppm or less as described above, the H after grain boundary diffusion can be reduced. cJ Therefore, stable characteristics can be obtained without reducing the increase in the amount of EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0057] [Examples 1 to 7, Comparative Examples 1 to 4] The raw materials of each element were melted in a high-frequency induction furnace in an Ar gas atmosphere so that Nd: 30.0 mass%, Co: 1.0 mass%, B: 0.9 mass%, Al: 0.1 mass%, Cu: 0.2 mass%, Zr: 0.2 mass%, Ga: 0.1 mass%, and Fe: remainder, and an alloy ribbon was produced by a strip casting method in which the molten alloy was cooled on a water-cooled copper roll. Next, the produced alloy ribbon was coarsely crushed by hydrogenation to obtain a coarse powder, and then 0.15 mass% of menthol (Example 1), cyclohexane carboxylic acid (Example 2), cyclohexanol (Example 3), camphor (Example 4), borneol (Example 5), camphorquinone (Example 6), isobornyl acetate (Example 7), stearic acid (Comparative Example 1), cyclohexane (Comparative Example 2), adamantane (Comparative Example 3), and camphene (Comparative Example 4) having the following molecular structures were added to the obtained coarse powder as a lubricant and mixed. This mixture of coarse powder and lubricant was pulverized in a jet mill in a nitrogen stream in which the oxygen and moisture concentrations were controlled, to a mean particle size of 2.8 μm.

[0058] [ka]

[0059] The resulting fine powder was then loaded into a mold of a molding machine equipped with an electromagnet in a nitrogen atmosphere, and pressure-molded with a load of 10 kN in a direction perpendicular to the magnetic field while being oriented in a magnetic field of 15 kOe (1.19 MA / m). The resulting molded body was sintered in a vacuum at 1050°C for 3 hours, cooled to below 200°C, and then subjected to a high-temperature heat treatment at 900°C for 2 hours and a low-temperature heat treatment at 500°C for 3 hours to obtain a sintered body.

[0060] The center of each of the obtained sintered bodies was cut into a rectangular parallelepiped shape with a size of 18 mm x 15 mm x 12 mm to obtain a sintered magnet, and the magnetic properties of each of the sintered magnets were measured using a BH tracer. Table 1 shows the values ​​of Examples 1 to 7 and Comparative Examples 1 to 4. The oxygen concentration of the sintered magnets was measured by the inert gas fusion infrared absorption method, the nitrogen concentration was measured by the inert gas fusion thermal conduction method, and the carbon concentration was measured by the combustion infrared absorption method. The average crystal grain size D50 (μm) was determined by polishing a cross section parallel to the magnetization direction of the sintered magnet until it became a mirror surface, immersing it in a mixed solution of glycerin: nitric acid: hydrochloric acid = 3: 1: 2 to selectively etch the grain boundary phase of the cross section, and obtaining 25 cross-sectional images in the range of 85 x 85 μm with a laser microscope, and measuring the cross-sectional area of ​​each particle by image analysis based on the obtained cross-sectional images, and obtaining the area average of the diameter of each particle calculated as a circle equivalent diameter.

[0061] [Comparative Example 5] The raw materials of each element were melted in a high-frequency induction furnace in an Ar gas atmosphere so that Nd: 30.0 mass%, Co: 1.0 mass%, B: 0.9 mass%, Al: 0.1 mass%, Cu: 0.2 mass%, Zr: 0.2 mass%, Ga: 0.1 mass%, and Fe: remainder, and an alloy ribbon was produced by a strip casting method in which the molten alloy was cooled on a water-cooled copper roll. Next, the produced alloy ribbon was coarsely pulverized by hydrogenation to obtain a coarse powder, and then 0.15 mass% of menthol was added as a lubricant to the obtained coarse powder and mixed. This mixture of the coarse powder and the lubricant was finely pulverized to an average particle size of 2.8 μm in a jet mill in a nitrogen stream with controlled oxygen and moisture concentrations. At this time, the oxygen content was adjusted to 1500 ppm by adjusting the oxygen concentration in the jet mill system.

[0062] Next, the obtained fine powder was filled into a mold of a molding device equipped with an electromagnet in a nitrogen atmosphere, and while being oriented in a magnetic field of 15 kOe (1.19 MA / m), it was pressure-molded with a load of 10 kN in a direction perpendicular to the magnetic field. The obtained molded body was sintered in a vacuum at 1050°C for 3 hours, cooled to 200°C or less, and then subjected to a high-temperature heat treatment at 900°C for 2 hours and a low-temperature heat treatment at 500°C for 3 hours to obtain a sintered body. Thereafter, the magnetic properties, the content of impurity elements, and the average crystal grain size were measured in the same manner as in Example 1. The results are shown in Table 1.

[0063] [Comparative Examples 6 and 7] The raw materials of each element were melted in a high-frequency induction furnace in an Ar gas atmosphere so that Nd: 30.0 mass%, Co: 1.0 mass%, B: 0.9 mass%, Al: 0.1 mass%, Cu: 0.2 mass%, Zr: 0.2 mass%, Ga: 0.1 wt%, and Fe: remainder, and an alloy ribbon was produced by a strip casting method in which the molten alloy was cooled on a water-cooled copper roll. Next, the produced alloy ribbon was coarsely pulverized by hydrogenation to obtain a coarse powder, and then 0.07 mass% (Comparative Example 6) and 0.32 mass% (Comparative Example 7) of menthol were added as a lubricant to the obtained coarse powder and mixed. Next, the mixture of the coarse powder and the lubricant was finely pulverized to an average particle size of 2.8 μm in a jet mill in a nitrogen stream with controlled oxygen and moisture concentrations.

[0064] Next, the obtained fine powder was filled into a mold of a molding device equipped with an electromagnet in a nitrogen atmosphere, and while being oriented in a magnetic field of 15 kOe (1.19 MA / m), it was pressure-molded with a load of 10 kN in a direction perpendicular to the magnetic field. The obtained molded body was sintered in a vacuum at 1050°C for 3 hours, cooled to 200°C or less, and then subjected to a high-temperature heat treatment at 900°C for 2 hours and a low-temperature heat treatment at 500°C for 3 hours to obtain a sintered body. Thereafter, the magnetic properties, the content of impurity elements, and the average crystal grain size were measured in the same manner as in Example 1. The results are shown in Table 1.

[0065] [Table 1]

[0066] As shown in Table 1, the sintered magnets of Examples 1 to 7 produced by the method satisfying the conditions of the present invention have a higher degree of orientation relative to the crystal grain size and a lower nitrogen concentration, resulting in higher Br and H, compared to Comparative Examples 1 to 7. cJ In Comparative Example 5, the oxygen concentration was as high as 1480 ppm, and the sinterability was reduced, leading to insufficient densification and a reduction in Br. In Comparative Example 6, in which the amount of lubricant added was small, that is, the carbon concentration of the sintered body was reduced, a sufficient degree of orientation was not obtained and Br was reduced. In Comparative Example 7, in which the amount of lubricant added was extremely large, the H cJ A decrease was observed.

[0067] [Examples 8 to 10, Comparative Examples 8 to 11] The raw materials of each element were melted in a high-frequency induction furnace in an Ar gas atmosphere so that Nd: 30.0 mass%, Co: 1.0 mass%, B: 0.9 mass%, Al: 0.1 mass%, Cu: 0.2 mass%, Zr: 0.2 mass%, Ga: 0.1 mass%, and Fe: remainder, and an alloy ribbon was produced by a strip casting method in which the molten alloy was cooled on a water-cooled copper roll. Next, the produced alloy ribbon was coarsely pulverized by hydrogenation to obtain a coarse powder, and then 0.15 mass% of menthol was added as a lubricant to the obtained coarse powder and mixed. Next, the mixture of the coarse powder and the lubricant was finely pulverized by changing the classifier rotation speed in a jet mill in a nitrogen gas flow so that the average particle size was 2.1 μm (Example 8), 3.1 μm (Example 9), 3.5 μm (Example 10), and 4.0 μm (Comparative Example 8). Similarly, 0.15% by mass of stearic acid was added as a lubricant to the coarse powder and mixed, and the mixture was finely pulverized to an average particle size of 2.1 μm (Comparative Example 9), 3.5 μm (Comparative Example 10), or 4.0 μm (Comparative Example 11) by changing the classifier rotation speed in a jet mill in a nitrogen stream with controlled oxygen and moisture concentrations.

[0068] Next, the obtained fine powder was filled into a mold of a molding device equipped with an electromagnet in a nitrogen atmosphere, and while being oriented in a magnetic field of 15 kOe (1.19 MA / m), it was pressure-molded with a load of 10 kN in a direction perpendicular to the magnetic field. The obtained molded body was sintered in a vacuum at 1050°C for 3 hours, cooled to 200°C or less, and then subjected to a high-temperature heat treatment at 900°C for 2 hours and a low-temperature heat treatment at 500°C for 3 hours to obtain a sintered body. Thereafter, the magnetic properties, the content of impurity elements, and the average crystal grain size were measured in the same manner as in Example 1. The results are shown in Table 2. In addition to the results in Table 2, the results of Example 1 and Comparative Example 1 shown in Table 1 are added to the results in Table 2, and a graph showing the relationship between the average crystal grain size D50 and the degree of orientation when menthol, a compound having a polar functional group and a cyclohexane skeleton in the present invention, and stearic acid, a linear saturated fatty acid, are used as lubricants is shown in FIG.

[0069] [Table 2]

[0070] As shown in Fig. 1, it was confirmed that when menthol, a compound having a polar functional group and a cyclohexane skeleton, was used as a lubricant and the average crystal grain size D50 was 4.5 μm or less, it had a higher degree of orientation than stearic acid, which is conventionally used as a lubricant. On the other hand, when the average crystal grain size exceeded 4.5 μm, the highest Br was obtained in Comparative Example 8, which used menthol as a lubricant, but the H cJ From the above results, it can be seen that when the average crystal grain size D50 and the degree of orientation Or are in a relationship of (Or>0.7×D50+95) with D50 being 4.5μm or less, a high degree of orientation and a high H cJ It can be seen that both are possible.

[0071] [Examples 11 to 13, Comparative Examples 12 to 14] The raw materials of each element were melted in a high-frequency induction furnace in an Ar gas atmosphere so that Nd: 30.0 mass%, Co: 1.0 mass%, B: 0.9 mass%, Al: 0.1 mass%, Cu: 0.2 mass%, Zr: 0.2 mass%, Ga: 0.1 mass%, and Fe: remainder, and an alloy ribbon was produced by a strip casting method in which the molten alloy was cooled on a water-cooled copper roll. Next, the produced alloy ribbon was coarsely pulverized by hydrogenation to obtain a coarse powder, and then 0.15 mass% of menthol was added as a lubricant to the obtained coarse powder and mixed. Next, the mixture of the coarse powder and the lubricant was finely pulverized in a jet mill in a nitrogen stream with controlled oxygen and moisture concentrations to an average particle size of 2.9 μm (Examples 11 to 13). Similarly, 0.15% by mass of lauric acid was added as a lubricant to the coarse powder and mixed, and the mixture was finely pulverized to an average particle size of 2.9 μm in a jet mill in a nitrogen stream with controlled oxygen and moisture concentrations (Comparative Examples 12 to 14).

[0072] Next, the fine powder was filled into a mold of a molding device equipped with an electromagnet in a nitrogen atmosphere, and while oriented in a magnetic field of 15 kOe (1.19 MA / m), it was pressure-molded in a direction perpendicular to the magnetic field under the conditions shown in Table 3. The density and strength of the obtained compacts are shown in the same table. The strength of the compacts was measured using a push-pull gauge installed in a glove box, and the gauge was pressed into the compact, and the breaking pressure was taken as the moment when a crack occurred in the compact. The number of samples measured was 8 or more, and the values ​​in the table were the average values ​​excluding the maximum and minimum values. The strength of the compacts was measured using an Aiko Engineering digital force gauge RZ-10 and an electric test stand MODEL-2257.

[0073] In addition, compacts that were not used to measure the compact strength were sintered in a vacuum at 1,050°C for 3 hours, cooled to below 200°C, and then subjected to high-temperature heat treatment at 900°C for 2 hours and low-temperature heat treatment at 500°C for 3 hours to obtain sintered compacts.

[0074] The central portion of each of the obtained sintered bodies was cut into a rectangular parallelepiped shape measuring 18 mm × 15 mm × 12 mm to obtain a sintered magnet, and the magnetic properties (Br) of each of the sintered magnets was measured using a BH tracer. Table 3 shows the respective values ​​of Examples 11 to 13 and Comparative Examples 12 to 14.

[0075] [Table 3]

[0076] As shown in Examples 11 to 13 in Table 3, when menthol is used as a lubricant, high compact strength is obtained even when the compact density is low, the occurrence rate of cracks and chips during handling of the compact is reduced, and the molding yield is expected to be improved, and a high Br is obtained. On the other hand, in Comparative Example 12, a high Br comparable to that of the Examples is obtained, but the handling of the compact is difficult due to the low compact strength, and the molding yield is deteriorated.

Claims

1. A rare earth sintered magnet containing R (R is one or more elements selected from rare earth elements, essentially including Nd), Fe, and B, characterized in that the magnet has a carbon concentration of 800 to 1400 ppm, an oxygen concentration of 1000 ppm or less, a nitrogen concentration of 800 ppm or less, and an average crystal grain size D50 (μm), which is the area average of the equivalent circle diameters of crystal grains in a plane parallel to the magnetization direction, of 4.5 μm or less, and further in that the D50 and the degree of orientation Or (%), which is defined by the following formula (1) using the residual magnetic flux density Br and the saturation magnetic flux density 4πIs, satisfy the relationship of the following formula (2): Or=(Br / 4πIs)×100...(1) Or>0.7×D50+95...(2)

2. The rare earth sintered magnet according to claim 1, further comprising 0.05 to 0.5 atomic % of X (X is one or more elements selected from Ti, Zr, Hf, Nb, V, and Ta), and satisfying the relationship of the following formula (3), where the atomic percentages of B and X are [B] and [X], respectively: 4.3<[B]-2[X]<5.5...(3)

3. 3. The rare earth sintered magnet according to claim 1, wherein the content of R is 12.5 to 15.0 atomic %.

4. The rare earth sintered magnet according to any one of claims 1 to 3, wherein R contains one or more elements selected from Dy, Tb, Gd, and Ho in an amount of more than 0 to 1 mass %.

5. The rare earth sintered magnet according to any one of claims 1 to 4, wherein part of the R comprises an R element introduced into the sintered magnet by grain boundary diffusion.

6. A method for producing a rare earth sintered magnet, comprising the steps of: finely pulverizing a coarsely pulverized powder of an alloy containing R, Fe, and B to obtain a fine powder; compacting the fine powder in a magnetic field using a compression molding machine to obtain a molded body; and heat treating the molded body to obtain a sintered body, The method for producing a rare earth sintered magnet is characterized in that in the fine pulverizing step, a raw material powder obtained by adding a compound having a polar functional group and a cyclohexane skeleton to the coarsely pulverized powder is finely pulverized in an inert gas atmosphere to an average particle size of 0.5 to 3.5 μm, which is the median size in a volume-based particle size distribution measured by a laser diffraction / scattering method, and in the molding step, a molded body having a density of 2.8 to 3.6 g / cm3 is obtained.

7. 7. The method for producing a rare earth sintered magnet according to claim 6, wherein the compound having a polar functional group and a cyclohexane skeleton has a molecular weight of 250 or less.

8. The method for producing a rare earth sintered magnet according to claim 6 or 7, wherein the compound having a polar functional group and a cyclohexane skeleton is added in an amount of 0.08 to 0.3 parts by mass per 100 parts by mass of the coarsely pulverized powder.

9. The method for producing a rare earth sintered magnet according to any one of claims 6 to 8, wherein the oxygen concentration of the resulting rare earth sintered magnet is 1000 ppm or less.

10. The method for producing a rare earth sintered magnet according to any one of claims 6 to 9, wherein the nitrogen concentration of the resulting rare earth sintered magnet is 800 ppm or less.

11. The polar functional group of the compound having a polar functional group and a cyclohexane skeleton is an OH group, a COOH group, a CH 3 COO group, NH 2 The method for producing a rare earth sintered magnet according to any one of claims 6 to 10, wherein the compound is any one of the groups.

12. A method for manufacturing a rare earth sintered magnet described in any one of claims 6 to 11, wherein the strength of the compact is 20 N or more when a push-pull gauge is pressed against the compact and the force applied to the push-pull gauge is measured when a crack occurs.

13. The method for producing a rare earth sintered magnet according to claim 6, wherein the compound having a polar functional group and a cyclohexane skeleton has a vapor pressure of 15 Pa or less at 25° C.

Citation Information

Patent Citations

  • Organic binder of fine pulverous powder for powder metallurgy

    JP1984143002A

  • Method for molding alloy powder for rare earth-iron-boron based permanent magnet

    JP1992214804A

  • Method for preparing rare earth alloy powder material, and method for manufacturing rare earth alloy sintered compact using the same

    JP2002285208A

  • Manufacturing method of rare earth permanent magnet

    JP2003068551A

  • Method and apparatus for manufacturing magnetically anisotropic rare earth sintered magnet

    JP2007134353A