Laminate
A laminate with an aliphatic polyamide and modified polyolefin layers addresses the barrier and resistance issues in automotive applications, ensuring robust performance under varying temperatures and chemical exposure.
Patent Information
- Application Number
- JP2021512080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Existing laminates used in automotive applications, particularly for transporting refrigerants like R-1234yf, face challenges with insufficient barrier properties against chemical permeation and high-temperature resistance, especially when the polyolefin layer is thick, leading to potential leaks and adverse effects on vehicle components.
A laminate structure comprising an aliphatic polyamide composition layer and a modified polyolefin layer, where the modified polyolefin includes units derived from α-olefins with specific functional groups, providing excellent low-temperature impact resistance and high-temperature fracture pressure strength, even when the modified polyolefin layer is thick.
The laminate exhibits superior low-temperature impact resistance and high-temperature burst pressure strength, effectively preventing chemical permeation and maintaining structural integrity under demanding conditions.
Smart Images

Figure 0007574795000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate. [Background technology]
[0002] Many types of hoses and tubes are used in automobiles, including various pressure tubes such as hydraulic tubes and water pressure tubes, vacuum tubes, and fuel piping tubes, brake tubes, coolant hoses, air conditioner piping tubes, SCR (diesel engine exhaust gas removal system) tubes, and control cable liners. These hoses and tubes transport chemicals such as coolants (alcohol and water), refrigerants, oils, and urea solutions. The various hoses and tubes used in the automotive industry are required to have extremely high performance, including high burst pressure strength at high temperatures, long-term heat resistance, chemical resistance, water vapor and chemical barrier properties, and flexibility.
[0003] In particular, when the circulating fluid is a coolant (LLC) mainly made of ethylene glycol to prevent freezing in winter, a urea solution filled as a catalyst to remove NOx emitted from diesel engines, or a refrigerant such as carbon dioxide, fluorocarbon, alternative fluorocarbon, propane, or water used in air conditioners and radiators, if the barrier properties against these chemicals are insufficient, the cooling effect and catalytic effect cannot be fully demonstrated during actual use. In addition, with the tightening of regulations on the evaporation of ozone-depleting gases, the requirements for the refrigerant barrier properties of refrigerant transport tubes used in automobiles and other devices are becoming stricter.
[0004] On the other hand, in recent years, the quality of refrigerants used in automobiles and the like has been improved in line with the strengthening of regulations on the evaporation of ozone-depleting gases. For example, R-1234yf refrigerant was developed as an alternative refrigerant to HFC-134a refrigerant, and has a lower ozone depletion potential and global warming potential than HFC-134a refrigerant, making it an extremely environmentally friendly refrigerant. However, R-1234yf refrigerant in particular is prone to hydrolysis when in contact with water in a high-temperature environment, generating acid (formic acid, etc.), which can cause some materials in contact with chemicals to be easily hydrolyzed or deteriorated, and in the worst case, cracks can occur, causing fluid leakage and making it impossible to fulfill the purpose of transporting the fluid. Alternatively, chemicals or water can permeate the tube body, adversely affecting the parts in contact with it.
[0005] Conventionally used single-layer tubes made solely of polyamide resins, particularly polyamide 11 or polyamide 12, which are excellent in strength, toughness, chemical resistance, flexibility, etc., do not have sufficient long-term durability and barrier properties against the above-mentioned chemical solutions.
[0006] Fluorine-based resins such as ethylene / tetrafluoroethylene copolymer (ETFE) are excellent in resistance to various chemicals and are considered to be one of the materials having barrier properties against water vapor. In recent years, there has been active development of fluorine-based resins having adhesive properties with polyamide (see Patent Documents 1 to 3). However, from the viewpoint of environmental friendliness, the use of halogen-containing materials is being avoided, and there are problems such as high specific gravity and high cost. Therefore, there is a demand for the development of a piping system that uses halogen-free materials, has excellent barrier properties against chemicals, and has resistance to various chemicals.
[0007] On the other hand, polyolefin is inexpensive and has excellent chemical permeation prevention properties and long-term chemical resistance. For example, a cooling pipe composed of an outer layer made of polyamide and an inner layer made of crosslinked polyethylene has been proposed (see Patent Document 4). Also, a cooling pipe composed of an outer layer made of polyamide and an inner layer made of polypropylene having a certain thickness or more and containing a specific additive has been proposed (see Patent Document 5). Similarly, a cooling pipe composed of an inner layer that is inactive and non-swellable with respect to a coolant and an outer layer made of polyamide, the inner layer being composed of halogenated or non-halogenated homopolyolefin or copolyolefin, and manufactured by extrusion blow molding, the wall thickness of the layer differs over the length of the conduit, and the polymers of the inner layer and the outer layer have clearly different flexibility has been proposed (see Patent Document 6). Also, a multilayer tube composed of an inner layer of polyolefin, a first intermediate layer based on an adhesive, a second intermediate layer of an ethylene / vinyl alcohol copolymer, a third intermediate layer of polyamide, and an outer protective layer from the inside to the outside has been proposed (see Patent Document 7). Furthermore, a fuel cell pipe has also been proposed, in which an outer layer is made of an outer layer material whose essential components are a polyamide resin and a styrene-isobutylene block copolymer, and an inner layer is made of an inner layer material whose essential components are a polyolefin resin and a styrene-isobutylene block copolymer (see Patent Document 8). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2001 / 058686 [Patent Document 2] International Publication No. 2001 / 060606 [Patent Document 3] JP 2004-301247 A [Patent Document 4] Japanese Patent Application Publication No. 9-29869 [Patent Document 5] Special Publication No. 2008-507436 [Patent Document 6] Japanese Patent Application Publication No. 7-214647 [Patent Document 7] JP 2006-116966 A [Patent Document 8] JP 2005-216725 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0009] The thicknesses of the polyamide layer and the polyolefin layer can be varied depending on the requirements for use, and it is required that any layer thickness exhibits excellent mechanical properties at high and low temperatures. However, in the pipe disclosed in Patent Document 4, when polyethylene is used as the inner layer, the long-term resistance at high temperatures and the physical properties of the tube are poor. Furthermore, as the polyolefin layer becomes thicker, it becomes difficult to achieve both high and low temperature mechanical strength, but Patent Documents 5 to 8 do not provide any specific technical data or suggestions. In particular, electric vehicles and other applications require further improvements in the barrier properties and high-temperature resistance of LLC. There is a demand for increasing the thickness of inexpensive polyolefins that have excellent barrier properties and high-temperature resistance in laminates, while at the same time there is a demand for both high pressure resistance that can withstand the internal pressure of LLC in a high-temperature atmosphere and impact resistance at low temperatures.
[0010] An object of the present invention is to solve the above problems and to provide a laminate which is excellent in low-temperature impact resistance and burst pressure strength at high temperatures even when the modified polyolefin layer is thick. [Means for solving the problem]
[0011] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and found that a laminate having a layer containing an aliphatic polyamide resin composition and a layer containing a modified polyolefin having specific mechanical properties and material characteristics has excellent low-temperature impact resistance and burst pressure strength at high temperatures even in a configuration in which the modified polyolefin is thick.
[0012] That is, the present invention provides a laminate of two or more layers including layer (a) and layer (b), The (a) layer comprises an aliphatic polyamide composition (A), The (b) layer contains a modified polyolefin (B), The modified polyolefin (B) contains units derived from a monomer based on an α-olefin having from 2 to 10 carbon atoms, and units derived from an unsaturated compound having at least one functional group selected from the group consisting of an unsaturated compound having at least one group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, an amino group, an amide group, an imide group, a nitrile group, a thiol group, and an isocyanate group, and a derivative of an unsaturated compound having a carboxyl group, and the modified polyolefin (B) is a laminate having a Shore hardness (D scale) of 30 to 61 measured in accordance with ASTM D2240.
[0013] Preferred embodiments of the laminate are shown below. A plurality of preferred embodiments can be combined. [1] A laminate, wherein the aliphatic polyamide composition (A) comprises a polyamide (A1), and the polyamide (A1) is an aliphatic polyamide having a ratio of the number of methylene groups to the number of amide groups of 7.0 or more. [2] A laminate, wherein the polyamide (A1) is at least one homopolymer selected from the group consisting of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, and polyamide 1212, and / or at least one copolymer using several raw material monomers forming these. [3] A laminate, wherein the aliphatic polyamide composition (A) further comprises one or more additional components selected from the group consisting of plasticizers, impact resistance agents, and heat resistance agents. [4] A laminate, wherein the layer (a) and the layer (b) are adjacent to each other. [5] A laminate, wherein the modified polyolefin (B) has a tensile stress at yield, measured in accordance with ASTM D638, of 23 MPa or less, and a tensile stress at break, measured in accordance with ASTM D638, of 25 MPa or more. [6] A laminate, wherein the modified polyolefin (B) has an MFR (230°C, 2,160 g) measured in accordance with ASTM D1238 of 3.5 g / 10 min or more. [7] The modified polyolefin (B) has a wave number of 710 cm in FT-IR measurement. -1 More than 740cm -1 The wavenumber showing the maximum absorption intensity below is 721. cm -1 This is the laminate. [8] The modified polyolefin (B) is produced by melting a polyolefin before modification, adding the unsaturated compound having a functional group, and carrying out graft copolymerization. [9] A laminate, wherein the modified polyolefin (B) is a maleic anhydride modified polypropylene.
[10] A laminate consisting of only the (a) layer and the (b) layer.
[11] A laminate produced by a coextrusion molding method.
[12] The above Laminate A laminated blown molded body comprising .
[13] A laminated hollow molding body in which the layer (a) and the layer (b) are disposed in this order from the outside.
[14] A laminated blown molding, in which the layer (b) is disposed as an innermost layer.
[15] A laminated hollow molding comprising an innermost layer and an additional layer.
[16] A laminated hollow molding which is a tube. Effect of the Invention
[0014] According to the present invention, even in a configuration in which the modified polyolefin layer is thick, it is possible to provide a laminate which is excellent in low-temperature impact resistance and burst pressure strength at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The laminate is two or more layers including layer (a) and layer (b), The (a) layer comprises an aliphatic polyamide composition (A), the (b) layer contains a modified polyolefin (B), the modified polyolefin (B) containing a unit derived from a monomer based on an α-olefin having from 2 to 10 carbon atoms, and a unit derived from at least one unsaturated compound selected from the group consisting of an unsaturated compound having at least one group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, an amino group, an amide group, an imide group, a nitrile group, a thiol group, and an isocyanate group, and a derivative of an unsaturated compound having a carboxyl group; The modified polyolefin (B) has a Shore hardness (D scale) of 30 or more and 61 or less, measured in accordance with ASTM D2240. The laminate is a layer of modified polyolefin. Thickness Even in the case of such a configuration, the material has excellent low-temperature impact resistance and high-temperature burst pressure strength.
[0016] 1.(a) layer The (a) layer of the laminate comprises an aliphatic polyamide composition (A).
[0017] <Aliphatic polyamide composition (A)> The aliphatic polyamide composition (A) is not particularly limited as long as it is a composition containing an aliphatic polyamide having an amide bond (-CONH-) in the main chain. Examples of the aliphatic polyamide include polyamide 6 (polycaproamide), polyamide 11 (polyundecane amide), polyamide 12 (polydodecanamide), polyamide 26 (polyethylene adipamide), polyamide 44 (polytetramethylene succinamide), polyamide 45 (polytetramethylene glutamide), polyamide 46 (polytetramethylene adipamide), polyamide 48 (polytetramethylene suberamide), polyamide 49 (polytetramethylene azelamide), polyamide 410 (polytetramethylene ceramide), polyamide 420 (polytetramethylene ceramide), polyamide 430 (polytetramethylene ceramide), polyamide 440 (polytetramethylene ceramide), polyamide 450 (polytetramethylene glutamide), polyamide 460 (polytetramethylene adipamide), polyamide 480 (polytetramethylene suberamide), polyamide 490 (polytetramethylene azelamide), polyamide 410 (polytetramethylene ceramide), polyamide 420 (polytetramethylene ceramide), polyamide 420 (polytetramethylene ceramide), polyamide 430 (polytetramethylene ceramide), polyamide 440 (polytetramethylene ceramide), polyamide 440 (polytetramethylene ceramide), polyamide 450 (polytetramethylene glutamide), polyamide 460 (polytetramethylene adipamide), polyamide 480 (polytetramethylene suberamide), polyamide 490 (polytetramethylene azelamide), polyamide 410 (polytetramethylene ceramide), polyamide 420 (polytetramethylene ceramide), polyamide 430 (polytetramethylene ceramide), polyamide 440 (polytetramethylene ceramide), polyamide 440 (polytetramethylene polypentamethylene sebacamide (polyamide 510), polypentamethylene dodecamide (polyamide 512), polyhexamethylene succinamide (polyamide 64), polyhexamethylene succinamide (polyamide 65), polyamide 55 (polypentamethylene glutamide), polyamide 56 (polypentamethylene adipamide), polyamide 58 (polypentamethylene adipamide), polypentamethylene azelamide (polyamide 59), polypentamethylene sebacamide (polyamide 510), polypentamethylene dodecamide (polyamide 512), polyhexamethylene succinamide (polyamide 64), polyhexamethylene succinamide (polyamide 65 ... Polyhexamethylene glutamide (polyamide 65), polyhexamethylene adipamide (polyamide 66), polyhexamethylene suberamide (polyamide 68), polyhexamethylene azelamide (polyamide 69), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polyhexamethylene tetradecamide (polyamide 614), polyhexamethylene hexadecamide (polyamide 616), polyhexamethylene octadecamide (polyamide 618), polynonamethylene Adipamide (Polyamide 96), Polynonamethylene Suberamide (Polyamide 98), Polynonamethylene Azelamide (Polyamide 99), Polynonamethylene Sebacamide (Polyamide 910), Polynonamethylene Dodecamide (Polyamide 912), Polydecamethylene Adipamide (Polyamide 106), Polydecamethylene Suberamide (Polyamide 108), Polydecamethylene Azelamide (Polyamide 109), Polydecamethylene Sebacamide (Polyamide 1010), Polydecamethylene Dodecamide (Polyamide 1012),Examples of such polymers include homopolymers such as polydodecamethylene adipamide (polyamide 126), polydodecamethylene suberamide (polyamide 128), polydodecamethylene azelamide (polyamide 129), polydodecamethylene sebacamide (polyamide 1210), and polydodecamethylene dodecamide (polyamide 1212), as well as copolymers using several kinds of the raw monomers that form these polymers. The aliphatic polyamide composition (A) preferably contains a polyamide (A1).
[0018] [Polyamide (A1)] The polyamide (A1) is an aliphatic polyamide having a ratio of the number of methylene groups to the number of amide groups (hereinafter, sometimes referred to as [CH2] / [NHCO]) of 7.0 or more (hereinafter, sometimes referred to as polyamide (A1)). By using an aliphatic polyamide having a [CH2] / [NHCO] of 7.0 or more, various physical properties such as mechanical properties of the laminate can be made excellent. The upper limit of [CH2] / [NHCO] is not particularly limited, but is practically 11.0 or less.
[0019] Examples of polyamide (A1) include polyamide 11 ([CH2] / [NHCO]=10.0), polyamide 12 ([CH2] / [NHCO]=11.0), polyamide 412 ([CH2] / [NHCO]=7.0), polyamide 512 ([CH2] / [NHCO]=7.5), polyamide 610 ([CH2] / [NHCO]=7.0), polyamide 6 ... O] = 8.0), polyamide 614 ([CH2] / [NHCO] = 9.0), polyamide 616 ([CH2] / [NHCO] = 10.0), polyamide 618 ([CH2] / [NHCO] = 11.0), polyamide 98 ([CH2] / [NHCO] = 7.5), polyamide 99 ([CH2] / [NHCO] = 8.0), polyamide 910 ([CH2] / [NHCO] = 8.5), polyamide Amide 912 ([CH2] / [NHCO]=9.5), Polyamide 106 ([CH2] / [NHCO]=7.0), Polyamide 108 ([CH2] / [NHCO]=8.0), Polyamide 109 ([CH2] / [NHCO]=8.5), Polyamide 1010 ([CH2] / [NHCO]=9.0), Polyamide 1012 ([CH2] / [NHCO]=10.0), Polyamide 126 ( Examples of such copolymers include homopolymers such as polyamide 128 ([CH2] / [NHCO]=8.0), polyamide 128 ([CH2] / [NHCO]=9.0), polyamide 129 ([CH2] / [NHCO]=9.5), polyamide 1210 ([CH2] / [NHCO]=10.0), and polyamide 1212 ([CH2] / [NHCO]=11.0), and / or copolymers using several types of raw material monomers to form these.
[0020] As the polyamide (A1), from the viewpoint of ensuring sufficient physical properties such as mechanical properties and heat resistance of the laminate, and from the viewpoints of economy and ease of availability, it is preferable to use at least one homopolymer selected from the group consisting of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, and polyamide 1212, and / or at least one copolymer using several raw material monomers forming these.
[0021] [Characteristics of Polyamide (A1)] The relative viscosity of the polyamide (A1), measured in accordance with JIS K-6920 under conditions of 96% sulfuric acid, a polymer concentration of 1%, and 25°C, is preferably 1.5 or more and 5.0 or less, and more preferably 2.0 or more and 4.5 or less, from the viewpoints of ensuring the mechanical properties of the laminate and of ensuring desirable moldability of the laminate by keeping the viscosity at the time of melting in an appropriate range.
[0022] When the terminal amino group concentration per 1 g of polyamide (A1) is [A] (μeq / g) and the terminal carboxyl group concentration per 1 g of polyamide (A1) is [B] (μeq / g), from the viewpoint of ensuring sufficient interlayer adhesion of the laminate, it is preferable that [A]>[B]+5, more preferably [A]>[B]+10, and particularly preferably [A]>[B]+15. Furthermore, from the viewpoint of the melt stability of the polyamide and the suppression of the generation of gel-like matter, it is preferable that [A]>20, and particularly preferably 30<[A]<120.
[0023] Here, the terminal amino group concentration [A] (μeq / g) can be measured by dissolving the polyamide in a phenol / methanol mixed solution and titrating with 0.05 N hydrochloric acid. The terminal carboxyl group concentration [B] (μeq / g) can be measured by dissolving the polyamide in benzyl alcohol and titrating with 0.05 N sodium hydroxide solution.
[0024] As long as the above-mentioned terminal group concentration is satisfied, the polyamide (A1) is also preferably an aliphatic polyamide mixture consisting of two or more aliphatic polyamides having different terminal amino group concentrations and / or terminal carboxyl group concentrations. In this case, the terminal amino group concentration and / or terminal carboxyl group concentration of the aliphatic polyamide mixture is determined by the terminal amino group concentration and terminal carboxyl group concentration of the aliphatic polyamides constituting the mixture, and the blending ratio thereof.
[0025] [Production method of polyamide (A1)] Polyamide (A1) is produced by polymerizing or copolymerizing a polyamide raw material in the presence of an amine by a known method such as melt polymerization, solution polymerization, solid-phase polymerization, or a combination thereof. Alternatively, polyamide (A1) is produced by polymerizing the polyamide raw material and then melt-kneading it in the presence of an amine. Here, the polymerization of the polyamide raw material can be carried out by repeating normal pressure, reduced pressure, and increased pressure operations.
[0026] The raw materials for the polyamide (A1) include aliphatic lactams, aliphatic aminocarboxylic acids, or combinations of aliphatic diamines and aliphatic dicarboxylic acids.
[0027] Examples of the aliphatic lactam include caprolactam, enantholactam, undecane lactam, dodecane lactam, α-pyrrolidone, α-piperidone, etc. These can be used alone or in combination of two or more.
[0028] Examples of the aliphatic aminocarboxylic acid include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, etc. These may be used alone or in combination of two or more.
[0029] Examples of aliphatic diamines include 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentadecanediamine, and 1,16-hexadecanediamine. Examples of the diamine include 1,17-heptadecanediamine, 1,18-octadecanediamine, 1,19-nonadecanediamine, 1,20-eicosanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, and 5-methyl-1,9-nonanediamine. These may be used alone or in combination.
[0030] Examples of the aliphatic dicarboxylic acid include glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane diacid, etc. These may be used alone or in combination of two or more.
[0031] The amines include monoamines, diamines, triamines, and polyamines. These can be used alone or in combination of two or more. However, when the raw material for the polyamide (A1) is a combination of an aliphatic diamine and an aliphatic dicarboxylic acid, the amines do not include an aliphatic diamine.
[0032] Examples of monoamines include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, 2-ethylhexylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, octadecylamine, octadecyleneamine, eicosylamine, and docosylamine; alicyclic monoamines such as cyclohexylamine and methylcyclohexylamine; benzylamine, β-phenylamine, and the like. Examples of such amines include aromatic monoamines such as methylamine, symmetric secondary amines such as N,N-dimethylamine, N,N-diethylamine, N,N-dipropylamine, N,N-dibutylamine, N,N-dihexylamine, and N,N-dioctylamine, and mixed secondary amines such as N-methyl-N-ethylamine, N-methyl-N-butylamine, N-methyl-N-dodecylamine, N-methyl-N-octadecylamine, N-ethyl-N-hexadecylamine, N-ethyl-N-octadecylamine, N-propyl-N-hexadecylamine, and N-propyl-N-benzylamine. These amines may be used alone or in combination.
[0033] Diamines include 1,2-ethanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentanediamine, 1,16-pentane ...17-pentanediamine, 1,18-pentanediamine, 1,19-pentanediamine, 1,20-pentanediamine, 1,21-pentanediamine, 1,22-pentanediamine, 1,23-pentanediamine, 1,24-pentanediamine, 1,25-pentanediamine, 1,26-pentanediamine, 1,27-pentanediamine, 1,28-pentanediamine, 1,29-pentanediamine, 1,30-pentanediamine, 1,31-pentanediamine, 1,32-pentanediamine, 1,33-pentanediamine, 1,34-pentanediamine, 1,35-pentanediamine, 1,36-pentanediamine, 1,37-pentanediamine, 1 Aliphatic diamines such as tadecanediamine, 1,16-hexadecanediamine, 1,17-heptadecanediamine, 1,18-octadecanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, and 5-methyl-1,9-nonanediamine. alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(3-methyl-4-aminocyclohexyl)propane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, 2,5-bis(aminomethyl)norbornane, 2,6-bis(aminomethyl)norbornane, 3,8-bis(aminomethyl)tricyclodecane, and 4,9-bis(aminomethyl)tricyclodecane; aromatic diamines such as m-xylylenediamine and p-xylylenediamine. These may be used alone or in combination.
[0034] The amines can be added at any stage during the polymerization of the polyamide raw material, or at any stage during melt-kneading after the polymerization of the polyamide raw material, but in consideration of the interlayer adhesion of the laminate, it is preferable to add them at the polymerization stage. In addition, in order to satisfy the above-mentioned condition of the terminal amino group concentration, it is preferable to add diamines and / or polyamines during the polymerization of the polyamide raw material, and from the viewpoint of suppressing gel generation, it is particularly preferable to add at least one selected from the group consisting of aliphatic diamines, alicyclic diamines, and polyalkyleneimines during the polymerization of the polyamide raw material.
[0035] Furthermore, carboxylic acids such as monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, etc. may be added as necessary within the range that satisfies the above-mentioned terminal group concentration. In this case, the amines and the carboxylic acids may be added simultaneously or separately.
[0036] Examples of carboxylic acids include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, capric acid, pelargonic acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, myristoleic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, arachic acid, behenic acid, and erucic acid; alicyclic monocarboxylic acids such as cyclohexane carboxylic acid and methylcyclohexane carboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, ethylbenzoic acid, and phenylacetic acid; malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane diacid, dodecanedioic acid, hexadecanedioic acid, hexadecenedioic acid, octadecanedioic acid, octadecenedioic acid, eicosane diacid, and eicosenedioic acid. aliphatic dicarboxylic acids such as docosanedioic acid, diglycolic acid, 2,2,4-trimethyladipic acid, and 2,4,4-trimethyladipic acid; alicyclic dicarboxylic acids such as 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and norbornanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, m-xylylenedicarboxylic acid, p-xylylenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid; and tricarboxylic acids such as 1,2,4-butanetricarboxylic acid, 1,3,5-pentanetricarboxylic acid, 1,2,6-hexanetricarboxylic acid, 1,3,6-hexanetricarboxylic acid, 1,3,5-cyclohexanetricarboxylic acid, and trimesic acid. These may be used alone or in combination.
[0037] The amount of amines used is appropriately determined by a known method, taking into consideration the terminal amino group concentration, terminal carboxyl group concentration, and relative viscosity of polyamide (A1). Usually, the amount of amines added per mole of polyamide raw material (1 mole of monomer or monomer unit constituting a repeating unit) is preferably 0.5 meq / mol or more and 20 meq / mol or less, more preferably 1.0 meq / mol or more and 10 meq / mol or less, from the viewpoint of obtaining sufficient reactivity and facilitating the production of polyamide having a desired viscosity. Here, the equivalent (eq) of amino group is defined as the amount of amino group that reacts with carboxyl group in a 1:1 ratio to form an amide group.
[0038] Examples of the polyamide (A1) production apparatus include known polyamide production apparatuses, such as batch reaction vessels, single- or multi-vessel continuous reaction apparatuses, tubular continuous reaction apparatuses, kneading reaction extruders such as single-screw kneading extruders and twin-screw kneading extruders.
[0039] [Additional ingredients] The aliphatic polyamide composition (A) may contain further components as necessary. Such further components include polyamides other than the polyamide (A1), such as aliphatic polyamides having a [CH2] / [NHCO] ratio of less than 7.0, polyamide resins having an alicyclic or aromatic group in the main chain or side chain, impact resistance agents, plasticizers, heat resistance agents selected from antioxidants and heat stabilizers, ultraviolet absorbers, light stabilizers, lubricants, inorganic fillers, antistatic agents, flame retardants, crystallization accelerators, colorants, etc. As further components, it is preferable to include at least one selected from the group consisting of plasticizers, impact resistance agents, and heat resistance agents. These may be used alone or in combination.
[0040] [Impact resistance agent] From the viewpoint of imparting impact resistance to the laminate, the aliphatic polyamide composition (A) preferably contains an impact resistant agent. The impact resistant agent is not a modified polyolefin (B). That is, the impact resistant agent has a Shore hardness (D scale) measured in accordance with ASTM D2240 of less than 30, preferably less than 20. The lower limit of the Shore hardness (D scale) measured in accordance with ASTM D2240 of the impact resistant agent is not particularly limited and can be 0.5 or more. The impact resistant agent includes an elastomer polymer having a constitutional unit derived from an unsaturated compound having a carboxyl group and / or an acid anhydride group and having a Shore hardness (D scale) measured in accordance with ASTM D2240 of less than 30.
[0041] Examples of the elastomeric polymer include (ethylene and / or propylene) / α-olefin copolymers, (ethylene and / or propylene) / (α,β-unsaturated carboxylic acid ester) copolymers, and the like, and these can be used alone or in combination of two or more kinds.
[0042] The (ethylene and / or propylene) / α-olefin copolymer is a polymer obtained by copolymerizing ethylene and / or propylene with an α-olefin having 3 or more carbon atoms. Examples of the α-olefin having 3 or more carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1- Examples of such olefins include heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene. These olefins may be used alone or in combination. Also, conjugated dienes such as 1,3-butadiene; 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, Polyenes such as non-conjugated dienes, such as cyclohexadiene, cyclooctadiene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,5-norbornadiene, may be copolymerized. These may be used alone or in combination.
[0043] The (ethylene and / or propylene) / (α,β-unsaturated carboxylate) copolymer is a polymer obtained by copolymerizing ethylene and / or propylene with an α,β-unsaturated carboxylate monomer. Examples of the α,β-unsaturated carboxylate monomer include methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, pentyl acrylate, pentyl methacrylate, hexyl acrylate, hexyl methacrylate, heptyl acrylate, heptyl methacrylate, octyl acrylate, octyl methacrylate, nonyl acrylate, nonyl methacrylate, decyl acrylate, decyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, monomethyl maleate, monomethyl itaconate, dimethyl maleate, and dimethyl itaconate. These can be used alone or in combination of two or more.
[0044] Examples of the unsaturated compound having a carboxyl group in the elastomer polymer include α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, mesaconic acid, citraconic acid, glutaconic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic acid, and metal salts of these carboxylic acids. Examples of the unsaturated compound having an acid anhydride group include dicarboxylic acid anhydrides having an α,β-unsaturated bond such as maleic anhydride, itaconic anhydride, citraconic anhydride, and endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride. These can be used alone or in combination. Among these, dicarboxylic acid anhydrides having an α,β-unsaturated bond are preferred, and maleic anhydride and itaconic anhydride are more preferred.
[0045] The carboxyl group and / or acid anhydride group concentration in the elastomeric polymer is preferably 25 μeq / g or more and 200 μeq / g or less, and more preferably 50 μeq / g or more and 150 μeq / g or less, from the viewpoint of exhibiting good compatibility with the polyamide (A1) and the flowability of the aliphatic polyamide composition (A).
[0046] The carboxyl group and / or acid anhydride group concentration in an elastomeric polymer can be measured by dissolving the elastomeric polymer in a toluene solution, adding ethanol to prepare a sample solution, and titrating the solution with a 0.1 N KOH ethanol solution using phenolphthalein as an indicator.
[0047] [Plasticizer] The aliphatic polyamide composition (A) preferably contains a plasticizer from the viewpoint of imparting flexibility to the laminate. Examples of the plasticizer include N-butylbenzenesulfonamide, p-hydroxybenzoic acid 2-hexyldecyl ester, etc. These can be used alone or in combination.
[0048] [Heat-resistant agent] The aliphatic polyamide composition (A) preferably contains a heat resistant agent selected from an antioxidant and a heat stabilizer. Examples of the antioxidant include phenolic compounds. The heat stabilizer is also called a processing stabilizer, and examples of the heat stabilizer include thioether-based, phosphorus-based and metal halide-based compounds, and preferably phosphorus-based compounds. The antioxidant and heat stabilizer may be used alone or in combination.
[0049] [Characteristics of Aliphatic Polyamide Composition (A)] The aliphatic polyamide composition (A) preferably has a flexural modulus of 400 MPa to 1,000 MPa, more preferably 450 MPa to 950 MPa, and particularly preferably 500 MPa to 900 MPa, as measured in accordance with ISO 178. When the flexural modulus of the aliphatic polyamide composition (A) is within the above range, the laminate can have excellent flexibility while maintaining its burst pressure strength at high temperatures. The flexural modulus of the aliphatic polyamide composition (A) can be adjusted by appropriately changing the amount of impact resistance agent and plasticizer added.
[0050] [Composition of Aliphatic Polyamide Composition (A)] The content of polyamide (A1) in the aliphatic polyamide composition (A) is preferably 55% by mass or more and 95% by mass or less, more preferably 60% by mass or more and 95% by mass or less, and particularly preferably 70% by mass or more and 89% by mass or less, based on 100% by mass of the aliphatic polyamide composition (A). When the content of polyamide (A1) in the aliphatic polyamide composition (A) is within the above range, the laminate can have sufficiently excellent properties such as burst pressure strength at high temperatures. In addition, when the content of polyamide (A1) is equal to or more than the lower limit, the laminate can have a sufficient burst pressure strength at high temperatures. When the content of polyamide (A1) is equal to or less than the upper limit, the laminate can have sufficient flexibility and low-temperature impact resistance.
[0051] The content of the impact resistant agent in the aliphatic polyamide composition (A) is preferably 5% by mass or more and 30% by mass or less, more preferably 7% by mass or more and 25% by mass or less, and particularly preferably 10% by mass or more and 20% by mass or less, based on 100% by mass of the aliphatic polyamide composition (A). By the content of the impact resistant agent in the aliphatic polyamide composition (A) being within the above range, the flexibility and low-temperature impact resistance of the laminate can be improved while maintaining the mechanical properties. In addition, when the content of the impact resistant agent is equal to or more than the lower limit, the flexibility and low-temperature impact resistance of the laminate can be sufficiently obtained. When the content of the impact resistant agent is equal to or less than the upper limit, the burst pressure strength and other mechanical properties of the laminate at high temperatures can be sufficiently obtained.
[0052] The content of the plasticizer in the aliphatic polyamide composition (A) is preferably 0% by mass or more and 15% by mass or less, and particularly preferably 1% by mass or more and 10% by mass or less, based on 100% by mass of the aliphatic polyamide composition (A). By having the content of the plasticizer within the above range, the flexibility of the laminate can be excellent while maintaining the burst pressure strength of the laminate at high temperatures. In addition, when the content of the plasticizer is equal to or less than the upper limit, the burst pressure strength of the laminate at high temperatures can be sufficiently obtained.
[0053] The content of the heat-resistant agent in the aliphatic polyamide composition (A) is preferably 0% by mass or more and 5% by mass or less, and particularly preferably 0.5% by mass or more and 2% by mass or less, based on 100% by mass of the aliphatic polyamide composition (A). When the content of the heat-resistant agent is within the above range, the mechanical properties, heat resistance, etc. of the laminate can be well balanced.
[0054] The contents of further components other than the impact resistance agent, plasticizer and heat resistance agent in the aliphatic polyamide composition (A) can be appropriately set depending on the required properties.
[0055] [Method for producing aliphatic polyamide composition (A)] The method for producing the aliphatic polyamide composition (A) is not particularly limited, and various conventionally known methods can be adopted. For example, the polyamide (A1), impact resistance agent, plasticizer, and heat resistance agent are mixed together with other components added as necessary in a tumbler or mixer to uniformly dry blend the pellets to the above-mentioned mixing ratio; the polyamide (A1), impact resistance agent, plasticizer, and heat resistance agent are mixed together with other components added as necessary in advance, and then melt-kneaded; the polyamide (A1), impact resistance agent, plasticizer, and heat resistance agent are mixed together with other components added as necessary in advance, and then each of these is fed separately and melt-kneaded. The melt-kneading can be carried out using a kneader such as a single-screw extruder, a twin-screw extruder, a kneader, or a Banbury mixer.
[0056] 2.(b) layer The (b) layer of the laminate contains a modified polyolefin (B).
[0057] <Modified polyolefin (B)> The modified polyolefin (B) is a polymer containing units derived from a monomer based on an α-olefin having 2 to 10 carbon atoms and units derived from an unsaturated compound having at least one functional group selected from the group consisting of an unsaturated compound having at least one group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, an amino group, an amide group, an imide group, a nitrile group, a thiol group, and an isocyanate group, and a derivative of an unsaturated compound having a carboxyl group, and having a Shore hardness (D scale) of 30 to 61 measured in accordance with ASTM D2240 (hereinafter, this may be referred to as modified polyolefin (B)).
[0058] [α-olefin-based monomers with 2 to 10 carbon atoms] The polyolefin (B1) constituting the modified polyolefin (B) contains units derived from a monomer based on an α-olefin having from 2 to 10 carbon atoms.
[0059] Examples of monomers based on α-olefins having 2 to 10 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, and 3-ethyl-1-hexene. These may be used alone or in combination. Among these, from the viewpoint of making the mechanical properties and flexibility of the laminate particularly excellent, monomers based on α-olefins having 2 to 8 carbon atoms are preferred.
[0060] [Other monomers] The polyolefin (B1) may contain other monomers, such as styrenes, conjugated dienes such as 1,3-butadiene, non-conjugated dienes, cyclic olefins, oxygen atom-containing olefins, etc., other than the monomers based on α-olefins having from 2 to 10 carbon atoms and unsaturated compounds having functional groups, so long as the excellent properties of the laminate are not impaired. Examples of styrenes include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,5-dimethylstyrene, 2,4-dimethylstyrene, vinylnaphthalene, vinylanthracene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, etc. Examples of non-conjugated dienes include 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, and 4,8-dimethyl-1,4,8-decatriene (DMDT). Examples of cyclic olefins include dicyclopentadiene, cyclohexadiene, cyclooctadiene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,5-norbornadiene, etc. Examples of oxygen atom-containing olefins include hexenol, hexenoic acid, methyl octenate, etc.
[0061] As the polyolefin (B1), crystalline polyolefins such as polyethylene, polypropylene, polybutene-1, poly(4-methylpentene-1), ethylene, propylene, 1-butene, or α-olefin copolymers of 4-methylpentene-1 with other monomers are preferred. These may be used alone or in combination of two or more.
[0062] [Composition of polyolefin (B1)] In the polyolefin (B1), the content of units derived from a monomer based on an α-polyolefin having 2 to 10 carbon atoms is preferably 60 mol% or more, more preferably 70 mol% or more, and particularly preferably 90 mol% or more, based on 100 mol% of all polymerized units of the polyolefin (B1). When the content of units derived from a monomer based on an α-polyolefin having 2 to 10 carbon atoms is equal to or more than the above value, the mechanical properties and flexibility of the laminate are further improved. In addition, in the polyolefin (B1), the content of units derived from other monomers is preferably less than 40 mol%, more preferably less than 30 mol%, and particularly preferably less than 10 mol%, based on 100 mol% of all polymerized units of the polyolefin (B1).
[0063] Therefore, the polyolefin (B1) is more preferably a polypropylene homopolymer, a random copolymer of propylene and 20 mol % or less of other α-olefin, or a block copolymer of propylene and 30 mol % or less of other α-olefin.
[0064] [Production method of polyolefin (B1)] The polyolefin (B1) can be produced by any conventional method, for example, by polymerization using a titanium catalyst, a vanadium catalyst, a metallocene catalyst, etc. The polyolefin (B1) may be in the form of either a resin or an elastomer, and both an isotactic structure and a syndiotactic structure may be used, and there is no particular restriction on the stereoregularity. When the polyolefin (B1) is a copolymer, it may be any of an alternating copolymer, a random copolymer, and a block copolymer.
[0065] [Unsaturated compounds with functional groups] The modified polyolefin (B) contains a unit derived from an unsaturated compound having at least one type of group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, an amino group, an amide group, an imide group, a nitrile group, a thiol group, and an isocyanate group, and an unsaturated compound having at least one type of functional group selected from the group consisting of a derivative of an unsaturated compound having a carboxyl group. By containing a unit derived from an unsaturated compound having a functional group (i.e., an unsaturated compound having at least one type of group selected from the group consisting of a specific group and / or a derivative of an unsaturated compound having a carboxyl group), the interlayer adhesion between the (a) layer and the (b) layer can be improved, and the durability of the laminate can be improved.
[0066] Examples of unsaturated compounds having a carboxyl group include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid, and endo-bicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic acid. These may be used alone or in combination.
[0067] Derivatives of unsaturated compounds having a carboxyl group include, for example, acid anhydrides, acid halides, amides, imides and / or esters of the unsaturated compounds having a carboxyl group. Derivatives of unsaturated compounds having a carboxyl group include, for example, malenyl chloride, malenylimide, maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride, endo-bicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, dimethyl maleate, monomethyl maleate, diethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalate, dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate, etc. These can be used alone or in combination.
[0068] Examples of unsaturated compounds having a hydroxyl group include hydroxyl group-containing (meth)acrylic acid esters such as hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, glycerin mono(meth)acrylate, and pentaerythritol mono(meth)acrylate, 10-undecen-1-ol, 1-octen-3-ol, glycerin monoallyl ether, allyl alcohol, and 2-butene-1,4-diol. These may be used alone or in combination of two or more.
[0069] Examples of the unsaturated compound having an epoxy group include glycidyl esters of unsaturated carboxylic acids such as glycidyl acrylate and glycidyl methacrylate, monoglycidyl esters of unsaturated dicarboxylic acids such as maleic acid and fumaric acid (the alkyl group in the case of monoglycidyl esters has 1 to 12 carbon atoms), alkyl glycidyl esters of p-styrene carboxylic acid, 2-methylallyl glycidyl ether, 3,4-epoxy-1-butene, 3,4-epoxy-3-methyl-1-butene, 3,4-epoxy-1-pentene, 3,4-epoxy-3-methyl-1-pentene, 5,6-epoxy-1-hexene, vinylcyclohexene monoxide, etc. These can be used alone or in combination.
[0070] Examples of unsaturated compounds having an amino group include aminoalkyl ester derivatives of acrylic acid or methacrylic acid such as aminomethyl acrylate, aminomethyl methacrylate, dimethylaminoethyl methacrylate, aminopropyl acrylate, aminopropyl methacrylate, and cyclohexylaminoethyl methacrylate, and vinylamine derivatives such as N-vinyldiethylamine and N-acetylvinylamine. These may be used alone or in combination of two or more.
[0071] Examples of unsaturated compounds having an amide group include acrylamide derivatives such as acrylamide, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, N,N-dimethylaminopropylacrylamide, etc. These can be used alone or in combination of two or more.
[0072] Examples of unsaturated compounds having an imide group include N-acryloyloxyethyl-1,2,3,6-tetrahydrophthalimide (manufactured by Toagosei Co., Ltd., trade name: Aronix TO-1428), N-acryloyloxyethylhexahydrophthalimide (manufactured by Toagosei Co., Ltd., trade name: Aronix TO-1429), and N-acryloyloxyethyl-3,4,5,6-tetrahydrophthalimide (manufactured by Toagosei Co., Ltd., trade name: Aronix TO-1534). These may be used alone or in combination of two or more.
[0073] Examples of unsaturated compounds having a nitrile group include acrylonitrile, methacrylonitrile, 5-hexenenitrile, 5-methyl-5-hexenenitrile, methyl-2-cyanoacrylate, ethyl-2-cyanoacrylate, butyl-2-cyanoacrylate, cyclohexyl-2-cyanoacrylate, 2-ethylhexyl-2-cyanoacrylate, ethoxyethyl-2-cyanoacrylate, etc. These can be used alone or in combination of two or more.
[0074] Examples of unsaturated compounds having a thiol group include esters of aliphatic or aromatic mercaptoalcohols or thiol group-containing compounds such as dithiols, such as 2-mercaptoethanol, ethanedithiol, 1,2-propanedithiol, 1,3-propanedithiol, parahydroxythiophenol, 3-mercapto-1,2-propanedithiol, 1,4-butanedithiol, 2-mercaptoethyl ether, and 2-mercaptoethyl sulfide, and acrylic acid or methacrylic acid. These may be used alone or in combination.
[0075] Examples of unsaturated compounds having an isocyanate group include 2-methacryloyloxyethyl isocyanate (manufactured by Showa Denko K.K., product name: Karenz MOI (registered trademark)), 2-acryloyloxyethyl isocyanate (manufactured by Showa Denko K.K., product name: Karenz AOI (registered trademark)), etc. These can be used alone or in combination of two or more.
[0076] The unsaturated compound having a functional group is preferably maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, glycidyl methacrylate, or aminopropyl methacrylate, more preferably a dicarboxylic acid anhydride such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, or endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, and particularly preferably maleic anhydride.
[0077] The modified polyolefin (B) is preferably a maleic anhydride modified polypropylene from the viewpoint of obtaining a laminate having good mechanical properties, long-term resistance to chemical solutions, and good interlayer adhesion.
[0078] [Characteristics of modified polyolefin (B)] From the viewpoint of obtaining a laminate having mechanical properties and flexibility at low temperatures, the upper limit of the Shore hardness (D scale) of the modified polyolefin (B) measured in accordance with ASTM D2240 is 61 or less, and preferably 59 or less. From the viewpoint of mechanical strength of the laminate, the lower limit of the Shore hardness (D scale) measured in accordance with ASTM D2240 is 30 or more, preferably 45 or more, and particularly preferably 50 or more.
[0079] From the viewpoint of obtaining a laminate having mechanical properties and flexibility at low temperatures, the modified polyolefin (B) preferably has a tensile stress at yield measured according to ASTM D638 of 23 MPa or less, particularly preferably 21 MPa or less, and from the same viewpoint, preferably has a tensile stress at break measured according to ASTM D638 of 25 MPa or more, particularly preferably 27 MPa or more.
[0080] The modified polyolefin (B) preferably has an MFR value of 3.5 g / 10 min to 10.0 g / 10 min, more preferably 4.0 g / 10 min to 7.0 g / 10 min, measured in accordance with ASTM D1238 under conditions of 230° C. / 2,160 g. When the MFR value of the modified polyolefin (B) is within the above range, the impact resistance at low temperatures is excellent, and the molding stability of the laminate can be improved.
[0081] Generally, in FT-IR measurement of polyolefins, the wave number is 710 cm -1 From 740cm -1 The maximum absorption of the 710 cm -1 The closer it is to a homopolymer, the closer it is to 740cm -1 The closer the wavelength is to a random copolymer, the closer the structure is to a random copolymer. -1 More than 740cm -1 The wavenumber showing the maximum absorption intensity below is 721. cm -1 Within such a range, a laminate tube excellent in flexibility and excellent in impact resistance at low temperatures can be obtained.
[0082] [Composition of modified polyolefin (B)] In the modified polyolefin (B), the content of the unsaturated compound having a functional group is preferably an amount equivalent to the graft amount of the unsaturated compound having a functional group, which will be described later, relative to 100% by mass of the modified polyolefin (B). When the modified polyolefin (B) is maleic anhydride-modified polypropylene, the content of polypropylene in the maleic anhydride-modified polypropylene is preferably 50% by mass or more and 99.5% by mass or less, more preferably 60% by mass or more and 97% by mass or less, and particularly preferably 70% by mass or more and 95% by mass or less, relative to 100% by mass of the maleic anhydride-modified polypropylene. By making the content of polypropylene in the maleic anhydride-modified polypropylene equal to or more than the above value, the flexibility of the laminate can be sufficiently ensured, while the resistance to the elution of low molecular weight substances and ions can be further improved. Here, the content of polypropylene in the maleic anhydride-modified polypropylene can be measured in the same manner as the graft amount of the unsaturated compound having a functional group, which will be described later.
[0083] [Production method of modified polyolefin (B)] The modified polyolefin (B) can be produced by a known method for introducing the unit derived from the unsaturated compound having the functional group into the polyolefin (B1). For example, the method includes graft copolymerizing the unsaturated compound having the functional group into the polyolefin (B1) and radical copolymerizing an olefin monomer and the unsaturated compound having the functional group, and the method of graft copolymerizing the unsaturated compound having the functional group into the polyolefin (B1) is preferred.
[0084] In addition, various known methods can be adopted as a method for graft copolymerizing the unsaturated compound having the functional group to the polyolefin (B1). For example, a method of melting the polyolefin before modification and adding the unsaturated compound having the functional group to perform graft copolymerization, or a method of dissolving the polyolefin before modification in a solvent and adding a graft monomer to perform graft copolymerization, etc. can be mentioned. In either case, it is preferable to carry out the reaction in the presence of a radical polymerization initiator in order to efficiently graft polymerize the unsaturated compound having the functional group.
[0085] The radical polymerization initiator is not particularly limited as long as it promotes the reaction between the polyolefin main chain and the unsaturated compound having the functional group, but organic peroxides and organic peresters are preferred. Specifically, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, 1,4-bis(t-butylperoxyisopropyl)benzene, lauroyl peroxide, t-butyl peracetate, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butyl benzoate, t-butyl perphenyl acetate, t-butyl perisobutyrate, t-butyl per-sec-octoate, t-butyl perpivalate, cumyl perpivalate, t-butyl perdiethyl acetate, and other azo compounds such as azobis-isobutylnitrile, dimethylazoisobutylnitrile, etc. These can be used alone or in combination. Among these, dialkyl peroxides such as dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3,2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 1,4-bis(t-butylperoxyisopropyl)benzene are more preferred.
[0086] The radical polymerization initiator is preferably used in an amount of about 0.001 to 10 parts by mass per 100 parts by mass of the polyolefin (B1). The graft amount of the unsaturated compound having a functional group is preferably 0.05% by mass or more and 20% by mass or less, more preferably 0.05% by mass or more and 10% by mass or less, even more preferably 0.05% by mass or more and 5% by mass or less, and particularly preferably 0.05% by mass or more and 3% by mass or less, based on 100% by mass of the polyolefin (B1). The graft amount of the polyolefin (B1) is the net graft amount measured after removing the unsaturated compound having a functional group from the polyolefin (B1). The graft amount is 13 C-NMR, 1 It can be measured by known means such as H-NMR measurement. When a monomer having an acidic functional group, such as an unsaturated carboxylic acid or its acid anhydride, is used as the unsaturated compound having a functional group, it is also possible to use, for example, an acid value as a measure of the amount of functional group introduced into the polyolefin (B1). When maleic anhydride is used as the unsaturated compound having a functional group, it is usually measured by an infrared spectrophotometer at 1780 to 1790 cm -1 The amount of grafting can also be determined based on the absorption spectrum of the carbonyl group of maleic anhydride detected nearby.
[0087] The modified polyolefin (B) can be used in combination with various additives as necessary. In this case, the (b) layer contains various additives in addition to the modified polyolefin. The additives include conductive fillers, antioxidants, heat stabilizers, UV absorbers, light stabilizers, lubricants, inorganic fillers, antistatic agents, flame retardants, crystallization promoters, plasticizers, colorants, lubricants, and other thermoplastic resins. These can be used alone or in combination of two or more.
[0088] 3.Layered structure The laminate includes two or more layers, layer (a) and layer (b).
[0089] By including layer (a) in the laminate, it is possible to obtain a laminate having excellent mechanical properties, chemical resistance, and flexibility. Also, by including layer (b) in the laminate, the laminate has good chemical barrier properties, particularly barrier properties against water vapor, coolant (LLC), and urea solution, and long-term chemical resistance.
[0090] The laminate is preferably arranged in the order of layer (a) and layer (b) from the outside to the inside. This effectively imparts both mechanical properties and other properties provided by layer (a) and chemical barrier properties and other properties provided by layer (b). Here, when the laminate is in the form of a sheet, for example, and two or more surfaces of the laminate are in contact with air and not with a chemical solution, any surface that is in contact with air and not with a chemical solution is defined as the outside, and the opposite surface is defined as the inside. In addition, when the laminate is a hollow laminate, the inside of the laminate means the side of the laminate that is in contact with a chemical solution, and the outside means the side of the laminate that is in contact with air and not with a chemical solution.
[0091] In the laminate, the (a) layer and the (b) layer are preferably adjacent to each other, which makes it possible to obtain a laminate having excellent interlayer adhesion.
[0092] The laminate preferably consists of only the (a) layer and the (b) layer. This allows the effects of the (a) layer and the (b) layer to be efficiently exerted. In this case, each of the (a) layer and the (b) layer may be one layer or two or more layers.
[0093] In the laminate, it is more preferable that layer (a) is disposed as the outermost layer of the laminate. By disposing layer (a) as the outermost layer, it is possible to obtain a laminate having superior burst pressure strength at high temperatures. In the laminate, it is more preferable that layer (b) is disposed as the innermost layer of the laminate. By disposing layer (b) as the innermost layer, it is possible to further suppress deterioration of mechanical properties due to contact with a chemical solution.
[0094] The laminate may have one or more additional layers in order to provide additional functions or to obtain an economically advantageous laminate other than the two layers of layer (a) and layer (b). Examples of such additional layers include layers containing other thermoplastic resins and / or layers of any substrate other than thermoplastic resins. When the laminate includes additional layers, it is preferable that the laminate includes the additional layer in the innermost layer. By including the additional layer in the innermost layer of the laminate, the function of the additional layer can be efficiently provided.
[0095] Examples of the thermoplastic resin constituting the layer containing another thermoplastic resin include polyamide-based resins, fluorine-containing polymers, polyester-based resins, polyether-based resins, polysulfone-based resins, polythioether-based resins, polyketone-based resins, polynitrile-based resins, polymethacrylate-based resins, polyvinyl ester-based resins, polyvinyl chloride-based resins, cellulose-based resins, polycarbonate-based resins, polyimide-based resins, and thermoplastic polyurethane-based resins.
[0096] It is also possible to laminate any substrate other than thermoplastic resins, such as paper, metal-based materials, unstretched, uniaxially or biaxially stretched plastic films or sheets, woven fabrics, nonwoven fabrics, metallic cotton, wood, etc. Examples of metal-based materials include metals such as aluminum, iron, copper, nickel, gold, silver, titanium, molybdenum, magnesium, manganese, lead, tin, chromium, beryllium, tungsten, cobalt, etc., and / or metal compounds thereof, as well as alloys consisting of two or more of these metals, such as stainless steel alloys, aluminum alloys, copper alloys such as brass and bronze, and nickel alloys.
[0097] The total number of layers in the laminate is not particularly limited, as long as it is at least two layers, including at least one (a) layer and at least one (b) layer. The total number of layers in the laminate is preferably 8 layers or less, and more preferably 2 layers or more and 7 layers or less, in consideration of the mechanism of the laminate manufacturing device. In addition, due to the limitations of material management and the molding and manufacturing device of the laminate, it is particularly preferable that the total number of layers in the laminate is 2 layers.
[0098] The shape of the laminate is arbitrary, and may be a sheet or a hollow shape (a shape with a hollow interior, such as a tube or bottle shape). As a hollow shape, a tube shape is preferable. The laminate may have a corrugated region. The corrugated region is a region formed in a corrugated shape, a bellows shape, an accordion shape, a corrugated shape, or the like. The corrugated region may not only be present over the entire length of the laminate, but may also be present partially in an appropriate region along the way. Specific embodiments of the laminate include a laminated blown molded article, a laminated film, and a laminated plate, and a laminated blown molded article is preferred. A specific embodiment of the laminated blown molded article is a laminated tube.
[0099] The thickness of layer (a) in the laminate is preferably 30% to 95% of the total thickness of the laminate, more preferably 40% to 85%, and particularly preferably 45% to 80%. By having the layer thickness of layer (a) within the above range, the above-mentioned properties can be effectively exhibited. The thickness of layer (b) in the laminate is preferably more than 5% and less than 70% of the total thickness of the laminate, more preferably more than 15% and less than 60%, and particularly preferably more than 20% and less than 55%. By having the layer thickness of layer (b) within the above range, the above-mentioned properties can be effectively exhibited. The total thickness of the laminate is preferably 0.5 mm or more and 25 mm or less.
[0100] When the laminate is a laminate tube, the outer diameter of the laminate tube is designed in consideration of the flow rate of circulating liquid medicine and / or gas (e.g., engine coolant), etc., and the wall thickness is designed to be such that the permeability of the liquid medicine does not increase, the burst pressure of a normal tube can be maintained, and flexibility is maintained to a degree that makes the tube easy to assemble and provides good vibration resistance during use, but is not limited thereto. The outer diameter is preferably 4 mm or more and 300 mm or less, the inner diameter is preferably 3 mm or more and 250 mm or less, and the wall thickness is preferably 0.5 mm or more and 25 mm or less.
[0101] The laminate can be produced by melt extrusion using an extruder corresponding to the number of layers or materials, laminating simultaneously inside or outside a die (co-extrusion molding method), or by first producing a single-layer tube or a laminate produced by the above method, and then laminating the resin on the outside in sequence, if necessary, using an adhesive to integrate the resin (coating method). The laminate is preferably produced by the co-extrusion method in which various materials are co-extruded in a molten state and heat-sealed (melted and bonded) to produce a tube with a laminated structure in one step. That is, the laminate production method preferably includes co-extrusion molding.
[0102] Furthermore, when the laminate has a complex shape or is to be subjected to a heat bending process after molding to form a molded product, in order to remove residual distortion in the molded product, it is also possible to obtain the desired molded product by heat treating the laminate after formation for 0.01 to 10 hours at a temperature lower than the lowest melting point of the resins constituting the laminate in order to obtain the desired molded product.
[0103] A laminate having a corrugated region can be easily formed by first forming a straight tubular laminate, and then molding it to a desired corrugated shape. By having such a corrugated region, it has shock absorbing properties and is easy to install. Furthermore, it is possible to add necessary parts such as connectors, or to bend it into an L-shape, U-shape, or the like.
[0104] Taking into consideration stone chipping, abrasion with other parts, and flame resistance, the entire or part of the outer periphery of the laminate thus molded is coated with natural rubber (NR), butadiene rubber (BR), isoprene rubber (IR), butyl rubber (IIR), chloroprene rubber (CR), carboxylated butadiene rubber (XBR), carboxylated chloroprene rubber (XCR), epichlorohydrin rubber (ECO), acrylonitrile butadiene rubber (NBR), hydrogenated acrylonitrile butadiene rubber (HNBR), carboxylated acrylonitrile butadiene rubber (XNBR), a mixture of NBR and polyvinyl chloride, acrylonitrile isoprene rubber (NIR), chlorinated polyethylene rubber (CM), chlorosulfonated polyethylene rubber (CSM), ethylene propylene rubber (E A solid or sponge-like protective member (protector) made of thermoplastic elastomers such as ethylene propylene diene rubber (PR), ethylene vinyl acetate rubber (EPDM), ethylene vinyl acetate rubber (EVM), a mixture of NBR and EPDM rubber, acrylic rubber (ACM), ethylene acrylic rubber (AEM), acrylate butadiene rubber (ABR), styrene butadiene rubber (SBR), carboxylated styrene butadiene rubber (XSBR), styrene isoprene rubber (SIR), styrene isoprene butadiene rubber (SIBR), urethane rubber, silicone rubber (MQ, VMQ), fluororubber (FKM, FFKM), fluorosilicone rubber (FVMQ), vinyl chloride-based, olefin-based, ester-based, urethane-based, and amide-based, can be provided. The protective member may be a sponge-like porous body by a known method. By making it a porous body, a lightweight protective part with excellent heat insulation can be formed. In addition, material costs can be reduced. Alternatively, glass fibers or the like may be added to improve its strength. The shape of the protective member is not particularly limited, but it is usually a cylindrical member or a block-shaped member having a recess for receiving a laminate tube, which is one aspect of the laminate. In the case of a cylindrical member, the laminate tube can be inserted into a previously prepared cylindrical member, or the cylindrical member can be coated and extruded onto the laminate tube to bond the two together. To bond the two together, an adhesive is applied to the inner surface or the concave surface of the protective member as necessary, and the laminate tube is inserted or fitted into this, and the two are bonded together to form an integrated structure of the laminate tube and the protective member.It is also possible to reinforce it with metal or the like.
[0105] [Applications of laminates] The laminates can be used for a variety of applications, including automobile parts, internal combustion engine applications, mechanical parts such as power tool housings, industrial materials, industrial supplies, electrical and electronic parts, medical, food, household and office supplies, building material-related parts, and furniture parts.
[0106] In addition, the laminate has excellent resistance to permeation of chemicals, and is therefore suitable for use as a chemical transport tube. Examples of chemicals include aromatic hydrocarbon solvents such as benzene, toluene, xylene, and alkylbenzenes; alcohols such as methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, diethylene glycol, phenol, cresol, polyethylene glycol, polypropylene glycol, and polyalkylene glycol; phenol solvents; dimethyl ether, dipropyl ether, methyl t-butyl ether, ethyl t-butyl ether, dioxane, tetrahydrofuran, Ether solvents such as polyol esters and polyvinyl ethers; HFC-23, HFC-32, HFC-41, HFC-123, HFC-125, HFC-134, HFC-134a, HFC-143, HFC-143a, HFC-152, HFC-152a, HFC-161, HFC-227ea, HFC-227ca, HFC-236fa, HFC-236ea, HFC-236cb, HFC-236ca, HFC-245ca, HFC-245ea, HFC-245eb, HFC-245fa, HFC-245cb, HFC -254eb, HFC-254cb, HFC-254ca, HFC-263fb, HFC-263ca, HFC-272fb, HFC-272ea, HFC-272fa, HFC-272ca, HFC-281fa, HFC-281ea, HFC-329p, HFC -329mmz, HFC-338mf, HFC-338mcc, HFC-338pcc, HFC-347s, HFC-365mfc, HFC-4310mee, HFC-1123, HFC-1132a, FC-1216, HFC-1223, HFC-1225zc, H FC-1225ye, HFC-1225yc, HFC-1232xf, HFC-1234ye, HFC-1234ze, HFC-1234yf, HFC-1234yc, HFC-1234zc, HFC-1243yf, HFC-1243zc, HFC-1243ye , HFC-1243ze, HFC-1243zf, HFC-1243yc, HFC-1261yf, FC-1318my, FC-1318cy, HFC-1327my, HFC-1327ye, HFC-1327py, HFC-1327et, HFC-1327cz,HFC-1327cye、HFC-1327cyc、HFC-1336yf、HFC-1336ze、HFC-1336eye、HFC-1336eyc、HFC-1336pyy、HFC-1336pz、HFC-1336mzy、HFC-1336mzz、HFC-1336qc、HFC-1336pe、HFC-1336ft、HFC-1345qz、HFC-1345mzy、HFC-1345fz、HFC-1345mzz、HFC-1345sy、HFC-1345fyc、HFC-1345pyz、HFC-1345cyc、HFC-1345pyy、HFC-1345eyc、HFC-1345ctm、HFC-1345ftp、HFC1345fye、HFC-1345eyf、HFC-1345eze、HFC-1345ezc、HFC-1345eye、HFC-1354fzc、HFC-1354ctp、HFC-1354etm、HFC-1354tfp、HFC-1354my、HFC-1354mzy、FC-141-10myy、FC-141-10cy、HFC-1429mzt、HFC-1429myz、HFC-1429mzy、HFC-1429eyc、HFC-1429czc、HFC-1429cycc、HFC-1429pyy、HFC-1429myyc、HFC-1429myye、HFC-1429eyym、HFC-1429cyzm、HFC-1429mzt、HFC-1429czym、HFC-1438fy、HFC-1438eycc、HFC-1438ftmc(、HFC-1438czzm、HFC-1438ezym、HFC-1438ctmf、HFC-1447fzy、HFC-1447fz、HFC-1447fycc、HFC-1447cz、HFC-1447mytm、HFC-1447fyz、HFC-1447ezz、HFC-1447qzt、HFC-1447syt、HFC-1456szt、HFC-1456szy、HFC-1456mstz、HFC-1456fzce、HFC-1456ftmf、FC-151-12c、FC-151-12mcy、FC-151-12mmtt、FC-151-12mmzz、HFC-152-11mmtz、HFC-152-11mmyyz、HFC-152-11mmyyz、HFC-1549fz(PFBE)、HFC-1549fztmm、HFC-1549mmtts、HFC-1549fycz, HFC-1549myts, HFC-1549mzzz, HFC-1558szy, HFC-1558fzccc, HFC-1558mmtzc, HFC-1558ftmf, HF C-1567fts, HFC-1567szz, HFC-1567fzfc, HFC-1567sfyy, HFC-1567fzfy, HFC-1567myzzm(, HFC-1567mmtyf, FC-1 61-14myy, FC-161-14mcyy, HFC-162-13mzy, HFC162-13myz, HFC-162-13mczy, HFC-162-13mcyz, CFC-11(, CFC-11 4, CFC-114a, CFC-115, HCFC-21, HCFC-22, HCFC-122, HCFC-123, HCFC-124, HCFC-124a, HCFC-132, HCFC-133a, HCF C-141b, HCFC-142, HCFC-142b, HCFC-225ca, HCFC-225cb, HCFC-240db, HCFC-243db, HCFC-243ab, HCFC-244eb, HC FC-244bb, HCFC-244db, HCFC-1111, HCFC-1113, HCFC-1223xd, HCFC-1224xe, HCFC-1232xf, HCFC-1233xf, HCFC-1 haloolefins such as 233zd and mixtures thereof; ketone solvents such as acetone, methyl ethyl ketone, diethyl ketone, acetophenone; mineral oils, silicone oils, natural paraffins, naphthenes, synthetic paraffins, polyalphaolefins, gasoline, kerosene, diesel gasoline, rapeseed oil methyl ester, soybean oil methyl ester, palm oil methyl ester, coconut oil methyl ester, gas to liquid (Gas To Liquid: GTL), coal to liquid (Coal To Liquid: CTL), biomass to liquid (Biomass To Liquid: BTL), alcohol-containing gasoline, ethyl-t-butyl ether blend oxygen-containing gasoline, amine-containing gasoline, sour gasoline, compressed natural gas (CNG), liquefied petroleum gas (LPG), liquefied hydrocarbon gas (LHG), liquefied natural gas (LNG), fuel dimethyl ether (DME), castor oil-based brake fluid, glycol ether-based brake fluid, borate ester-based brake fluid, brake fluid for extremely cold regions,Examples of the brake fluids include silicone oil-based brake fluids, mineral oil-based brake fluids, power steering oils, hydrogen sulfide-containing oils, windshield washer fluids, engine coolants, urea solutions, pharmaceuticals, inks, and paints.
[0107] The laminate is suitable as a tube for transporting the chemical liquid, and specifically, it is preferably used as a fuel tube such as a feed tube, a return tube, an evaporative tube, a fuel filler tube, an ORVR tube, a reserve tube, or a vent tube, an oil tube, an oil drilling tube, an air pressure or hydraulic tube, a clutch tube, a brake tube, a brake negative pressure tube, a suspension tube, an air tube, a turbo air tube, an air duct tube, a blow-by tube, an EGR valve control tube, a windshield washer fluid tube, a coolant liquid (LLC) cooler tube, a reservoir tank tube, a urea solution transport tube, a battery cooling and heating tube, a fuel cell tube, an air conditioner tube, a heater tube, a radiator tube, a road heating tube, a floor heating tube, an infrastructure supply tube, a fire extinguisher and a fire extinguishing equipment tube, a medical cooling equipment tube, an ink or paint spraying tube, or other chemical liquid tube, and it is particularly preferable that the laminate is used as a coolant liquid (LLC) cooler tube, a urea solution transport tube, a battery cooling and heating tube, or an air conditioner tube. EXAMPLES
[0108] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto. First, the analytical and property measurement methods in the examples and comparative examples, and the materials used in the examples and comparative examples will be described.
[0109] 1. The properties of polyolefin were measured by the following methods.
[0110] [Shore hardness (D scale)] Shore hardness (D scale) was measured in accordance with ASTM D2240.
[0111] [Tensile test] Tensile stress at yield and at break were measured according to ASTM D638.
[0112] [MFR (Melt Flow Rate)] The MFR was measured at 230°C and 2,160g in accordance with ASTM D1238.
[0113] [FT-IR] 4000cm using JASCO FT / IR-4700 -1 From 650cm -1 Measured in the range of 710cm -1 From 740cm -1 The maximum wavenumber of absorption within the range was investigated.
[0114] 2. The physical properties of the laminate were measured by the following methods. [Low temperature impact resistance] An impact test was carried out on 10 laminated tubes at −40° C. according to the method described in SAE J 2260 7.5. Thereafter, the laminated tubes were checked for the presence or absence of breakage.
[0115] [High temperature burst pressure strength] A burst pressure strength test was carried out on five laminated tubes according to the method described in SAE J 2260 7.2, except that the test temperature was changed to 125° C. The average values of the measured burst pressure strengths are shown in Table 1.
[0116] 3. Materials used in the Examples and Comparative Examples (1) Aliphatic polyamide (A1) [Production of Polyamide 12 (A1-1)] In a 70-liter pressure-resistant reactor equipped with a stirrer, 19.73 kg (100.0 mol) of dodecane lactam, 45.0 g (0.264 mol) of 5-amino-1,3,3-trimethylcyclohexanemethylamine, and 0.5 L of distilled water were charged, and the inside of the polymerization vessel was replaced with nitrogen, and then the vessel was heated to 180°C, and stirred at this temperature so that the reaction system was in a homogeneous state. Next, the temperature inside the polymerization vessel was raised to 270°C, and polymerization was carried out for 2 hours under stirring while adjusting the pressure inside the vessel to 3.5 MPa. Thereafter, the pressure was released to normal pressure (0.1 MPa) over about 2 hours, and then reduced to 53 kPa, and polymerization was carried out under reduced pressure for 5 hours. Next, nitrogen was introduced into the autoclave, and after the pressure was restored to normal pressure, the mixture was extracted as a strand from the lower nozzle of the reaction vessel, and cut to obtain pellets. The pellets were dried under reduced pressure to obtain polyamide 12 with a relative viscosity of 2.20, a terminal amino group concentration of 48 μeq / g, and a terminal carboxyl group concentration of 24 μeq / g (hereinafter, this polyamide 12 is referred to as (A1-1)). The ratio [CH2] / [NHCO] of the number of methylene groups to the number of amide groups in polyamide 12 (A1-1) was 11.0, which satisfies 7.0 or more. In addition, the terminal amino group concentration [A] (μeq / g) and the terminal carboxyl group concentration [B] (μeq / g) of polyamide 12 (A1-1) satisfied [A]>[B]+5.
[0117] (2) Impact resistant agent (A2) Maleic anhydride modified ethylene / 1-butene copolymer (A2-1) (Mitsui Chemicals, Inc., TAFMER (registered trademark) MH5020, acid anhydride group concentration: 100 μeq / g, Shore hardness (D scale): <20)
[0118] (3) Plasticizer (A3) N-Butylbenzenesulfonamide (A3-1) (Proviplast (registered trademark) 024, manufactured by Proviron Co., Ltd.)
[0119] (4) Aliphatic polyamide composition (A) [Production of Aliphatic Polyamide Composition (A-1)] Polyamide 12 (A1-1) was mixed with maleic anhydride-modified ethylene / 1-butene copolymer (A2-1) as an impact resistance agent, N-butylbenzenesulfonamide (A3-1) as a plasticizer, triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate] (BASF Japan, IRGANOX® 245) as an antioxidant, and tris(2,4-di-t-butylphenyl)phosphite (BASF Japan, IRGAFOS168) as a phosphorus-based processing stabilizer. The mixture was mixed in advance and fed to a twin-screw melt kneader (manufactured by Japan Steel Works, Ltd., model: TEX (registered trademark) 44), melt-kneaded at a cylinder temperature of 180°C to 270°C, and the molten resin was extruded in the form of strands, which were then introduced into a water tank, cooled, cut, and vacuum dried to obtain pellets of an aliphatic polyamide composition (A-1) consisting of 0.8 parts by mass of antioxidant and 0.2 parts by mass of phosphorus-based process stabilizer per 100 parts by mass of polyamide 12 (A1-1) / impact resistance agent (A2-1) / plasticizer (A3-1) = 85.0 / 10.0 / 5.0 (mass%) in total.
[0120] (5) Modified polyolefin (B) Modified polyolefin (B-1) Maleic anhydride modified polypropylene (Mitsui Chemicals, Inc., Admer (registered trademark) QF551, Shore hardness (D scale): 58, tensile yield stress: 19 MPa, tensile break stress: 31 MPa, MFR: 5.2 g / 10 min, FT-IR measurement: wave number 710 cm -1 More than 740cm -1 The wavenumber showing the maximum absorption intensity at: 722.2 cm -1 ) Modified polyolefin (B-2) Maleic anhydride modified polypropylene (Mitsui Chemicals, Inc., Admer (registered trademark) QB516, Shore hardness (D scale): 62, tensile yield stress: 23 MPa, tensile break stress: 25 MPa, MFR: 2.8 g / 10 min, FT-IR measurement: wave number 710 cm -1 More than 740cm -1 The wavenumber showing the maximum absorption intensity is: 720.3 cm -1 ) Modified polyolefin (B-3) Maleic anhydride modified polypropylene (Mitsui Chemicals, Inc., Admer (registered trademark) QF500, Shore hardness (D scale): 66, tensile yield stress: 24 MPa, tensile break stress: 38 MPa, MFR: 3.5 g / 10 min, FT-IR measurement: wave number 710 cm -1 More than 740cm -1 The wavenumber showing the maximum absorption intensity is 718.4 cm -1 ) Modified polyolefin (B-4) Maleic anhydride modified polypropylene (Mitsui Chemicals, Inc., Admer (registered trademark) QB510, Shore hardness (D scale): 65, tensile yield stress: 28 MPa, tensile break stress: 33 MPa, MFR: 2.7 g / 10 min) Modified polyolefin (B-5) Maleic anhydride modified polypropylene (Mitsui Chemicals, Inc., Admer (registered trademark) QB520E, Shore hardness (D scale): 64, tensile yield stress: 24 MPa, tensile break stress: 35 MPa, MFR: 1.8 g / 10 min)
[0121] 4. Manufacturing of laminates (Example 1-1) Using the above-mentioned aliphatic polyamide composition (A-1) and modified polyolefin (B-1), (A-1) was melted at an extrusion temperature of 270°C and (B-1) was melted at an extrusion temperature of 220°C separately in a PAL32 (Milpha Co., Ltd.) two-layer tube molding machine, and the discharged molten resin was merged by an adapter and molded into a laminated tubular body. Subsequently, the tube was cooled by a sizing die for controlling dimensions, and taken up. When layer (a) (outermost layer) was made of (A-1) and layer (b) (innermost layer) was made of (B-1), a laminated tube with a layer structure of (a) / (b)=0.80mm / 0.20mm, an inner diameter of 6.0mm, and an outer diameter of 8.0mm was obtained. The physical property measurement results of the laminated tube (i.e., the high-temperature burst pressure strength results for five laminated tubes and the low-temperature impact resistance test results for ten laminated tubes) are shown in Table 1.
[0122] (Example 1-2) A laminated tube having a layer structure of (a) / (b)=0.65 mm / 0.35 mm, an inner diameter of 6.0 mm, and an outer diameter of 8.0 mm was obtained in the same manner as in Example 1-1, except that the layer thickness was changed. The physical property measurement results of the laminated tube are shown in Table 1.
[0123] (Examples 1-3) A laminated tube having a layer structure of (a) / (b)=0.50 mm / 0.50 mm, an inner diameter of 6.0 mm, and an outer diameter of 8.0 mm was obtained in the same manner as in Example 1-1, except that the layer thickness was changed. The physical property measurement results of the laminated tube are shown in Table 1.
[0124] (Comparative Example 1-1) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-1, except that the modified polyolefin (B-1) in Example 1-1 was changed to (B-2). The physical property measurement results of the laminated tube are shown in Table 1.
[0125] (Comparative Example 1-2) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-2, except that the modified polyolefin (B-1) in Example 1-2 was changed to (B-2). The physical property measurement results of the laminated tube are shown in Table 1.
[0126] (Comparative Example 1-3) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-3, except that the modified polyolefin (B-1) in Example 1-3 was changed to (B-2). The physical property measurement results of the laminated tube are shown in Table 1.
[0127] (Comparative Example 2-1) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-1, except that the modified polyolefin (B-1) in Example 1-1 was changed to (B-3). The results of measuring the physical properties of the laminated tube are shown in Table 1.
[0128] (Comparative Example 2-2) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-2, except that the modified polyolefin (B-1) in Example 1-2 was changed to (B-3). The physical property measurement results of the laminated tube are shown in Table 1.
[0129] (Comparative Example 2-3) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-3, except that the modified polyolefin (B-1) in Example 1-3 was changed to (B-3). The physical property measurement results of the laminated tube are shown in Table 1.
[0130] (Comparative Example 3-1) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-1, except that the modified polyolefin (B-1) in Example 1-1 was changed to (B-4). The physical property measurement results of the laminated tube are shown in Table 1.
[0131] (Comparative Example 3-2) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-2, except that the modified polyolefin (B-1) in Example 1-2 was changed to (B-4). The physical property measurement results of the laminated tube are shown in Table 1.
[0132] (Comparative Example 3-3) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-3, except that the modified polyolefin (B-1) in Example 1-3 was changed to (B-4). The physical property measurement results of the laminated tube are shown in Table 1.
[0133] (Comparative Example 4-1) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-1, except that the modified polyolefin (B-1) in Example 1-1 was changed to (B-5). The physical property measurement results of the laminated tube are shown in Table 1.
[0134] (Comparative Example 4-2) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-2, except that the modified polyolefin (B-1) in Example 1-2 was changed to (B-5). The physical property measurement results of the laminated tube are shown in Table 1.
[0135] (Comparative Example 4-3) A laminated tube having a layer structure shown in Table 1 was obtained in the same manner as in Example 1-3, except that the modified polyolefin (B-1) in Example 1-3 was changed to (B-5). The physical property measurement results of the laminated tube are shown in Table 1.
[0136] [Table 1]
[0137] It is clear from Table 1 that the laminated tubes of the examples have excellent low-temperature impact resistance and high-temperature burst pressure strength even when the layer of modified polyolefin is thick.
Claims
1. A laminate of two or more layers including layer (a) and layer (b), The (a) layer comprises an aliphatic polyamide composition (A), The (b) layer contains a modified polyolefin (B), the (a) layer and the (b) layer are adjacent to each other, The modified polyolefin (B) contains a unit derived from a monomer based on an α-olefin having from 2 to 10 carbon atoms, and a unit derived from an unsaturated compound having at least one functional group selected from the group consisting of an unsaturated compound having at least one group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, an amino group, an amide group, an imide group, a nitrile group, a thiol group, and an isocyanate group, and a derivative of an unsaturated compound having a carboxyl group, and the modified polyolefin (B) has a Shore hardness (D scale) of from 30 to 61 as measured in accordance with ASTM D2240, wherein the aliphatic polyamide composition (A) comprises a polyamide (A1) and an impact resistance agent, The polyamide (A1) is an aliphatic polyamide having a ratio of the number of methylene groups to the number of amide groups of 7.0 or more, the impact resistance agent is an elastomer polymer having a structural unit derived from an unsaturated compound having a carboxyl group and / or an acid anhydride group, and having a Shore hardness (D scale) measured in accordance with ASTM D2240 of less than 30; A laminate, wherein the thickness of layer (a) is 50% or more and 80% or less of the total thickness of the laminate, the thickness of layer (b) is 20% or more and 50% or less of the total thickness of the laminate, and the total thickness of the laminate is 0.5 mm or more and 25 mm or less.
2. The laminate according to claim 1, wherein the polyamide (A1) is at least one homopolymer selected from the group consisting of polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, and polyamide 1212, and / or at least one copolymer using several raw material monomers forming these.
3. 3. The laminate according to claim 1 or 2, wherein the aliphatic polyamide composition (A) comprises one or more further components selected from the group consisting of plasticizers and heat stabilizers.
4. The laminate according to any one of claims 1 to 3, wherein the modified polyolefin (B) has a tensile stress at yield measured in accordance with ASTM D638 of 23 MPa or less and a tensile stress at break measured in accordance with ASTM D638 of 25 MPa or more.
5. The laminate according to any one of claims 1 to 4, wherein the modified polyolefin (B) has an MFR (230°C, 2,160 g) measured in accordance with ASTM D1238 of 3.5 g / 10 min or more.
6. The modified polyolefin (B) has a wave number of 710 cm in FT-IR measurement. -1 740cm or more -1 The wave number showing the maximum absorption intensity is 721 cm -1 The laminate according to any one of claims 1 to 5, wherein
7. The laminate according to any one of claims 1 to 6, wherein the modified polyolefin (B) is produced by a method in which a polyolefin before modification is melted, an unsaturated compound having a functional group is added, and the melted polyolefin is subjected to graft copolymerization.
8. The laminate according to claim 1 , wherein the modified polyolefin (B) is a maleic anhydride modified polypropylene.
9. The laminate according to claim 1 , which consists of only the layer (a) and the layer (b).
10. 10. The laminate according to claim 1, produced by a coextrusion process.
11. A laminated blown molded article comprising the laminate according to any one of claims 1 to 10.
12. The laminated hollow molded article according to claim 11 , wherein the layer (a) and the layer (b) are disposed in this order from the outside.
13. The laminated hollow molded article according to claim 12, wherein the layer (b) is disposed as an innermost layer.
14. The laminated hollow molded article according to claim 13, further comprising an innermost layer.
15. The laminated blown molded article according to any one of claims 11 to 14, which is a tube.
Citation Information
Patent Citations
Multilayer cooling liquid conduit
JP1995214647A
Line for coolant
JP1997029869A
Fuel hose for automobile
JP2004285905A
Laminated hose
JP2004301247A
Hose for fuel cell
JP2005216725A