Polyester resin and laminate
A copolyester resin with a specific composition and isocyanate curing agent addresses the limitations of existing polyester resins by providing low-temperature tackiness and moisture resistance, enabling cost-effective bonding without heating devices.
Patent Information
- Application Number
- JP2020149200
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-04
AI Technical Summary
Existing polyester resins lack low-temperature tackiness and heat-and-moisture resistance, necessitating the use of heating devices for bonding, which increases costs and limits their application in certain environments.
A copolyester resin is developed with a specific composition comprising 85-100 mol% aromatic dicarboxylic acid, 20-40 mol% polyalkylene glycol, and less than 40 mol% neopentyl glycol, with a glass transition temperature of -45°C or lower, and combined with an isocyanate-based curing agent to enhance adhesion and moisture resistance.
The copolyester resin exhibits excellent low-temperature adhesiveness and heat-and-moisture resistance without impairing the adhesive properties, allowing for cost-effective bonding at various temperatures and humidity levels.
Smart Images

Figure 0007575037000001 
Figure 0007575037000002 
Figure 0007575037000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer polyester resin having excellent low-temperature adhesion and wet heat resistance. [Background technology]
[0002] Traditionally, polyester resins have been used in applications such as plastics, plastics manufacturing, and packaging, due to their excellent heat resistance, chemical resistance, durability, and mechanical strength. It is used in a wide range of applications, including film, PET bottles, textiles, toner, and electrical components. In addition, polyester resin has excellent adhesive properties and is used as a hot melt adhesive or hardener. It is also used as a thermosetting adhesive that reacts with heat.
[0003] In order to achieve excellent adhesive properties such as excellent adhesion and durability, these adhesives are It has a glass transition temperature and melting point much higher than the room temperature, and is quite densely crosslinked. The adhesive is very hard at room temperature. However, there was a problem in that a heating device was required for bonding, which increased costs.
[0004] On the other hand, attempts have been made to use polyester resins as adhesives. In Literature 1, in an adhesive composition mainly composed of a polyester resin, a polyester resin having a specific amount of an aliphatic dicarboxylic acid component with a specific carbon number is used, thereby achieving both mechanical strength and flexibility and improving heat resistance and adhesiveness.
[0005] However, the pressure-sensitive adhesive composition as described in Patent Document 1 is insufficient in terms of adhesiveness under lower temperature conditions and in terms of moist heat resistance for use in a humid environment. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-249443 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention solves the above problems and has excellent solvent solubility, making it suitable for use as an adhesive. The object of the present invention is to provide a copolymer polyester resin which is excellent in both low-temperature adhesion and wet heat resistance. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the gist of the present invention is as follows. (1) A copolymer polyester resin comprising an acid component constituting the polyester resin, which contains 85 to 100 mol % of an aromatic dicarboxylic acid relative to the total acid components, and a polyalkylene glycol, a neopentyl glycol, and an alicyclic glycol as glycol components, in which the polyalkylene glycol accounts for 20 mol % or more and the neopentyl glycol accounts for less than 40 mol % of the total glycol components. (2) The copolymer polyester resin of (1) having a glass transition temperature of -45°C or lower. (3) A copolymer polyester resin according to (1) or (2), in which the polyalkylene glycol is polytetramethylene glycol. (4) A copolymer polyester resin according to any one of (1) to (3), in which the alicyclic glycol content is less than 40 mol % based on the total glycol component. (5) A copolymer polyester resin of (1) to (4) wherein the alicyclic glycol is 1,4-cyclohexanedimethanol. (6) A copolymer polyester resin composition containing the copolymer polyester resin of (1) to (5) and a curing agent. (7) The copolymer polyester resin composition according to (6), wherein the curing agent is an isocyanate-based curing agent. (8) A coating film comprising the copolymer polyester resin composition of (6) or (7). (9) A laminate having the coating film of (8). Effect of the Invention
[0009] The copolymer polyester resin of the present invention is a polyester resin having a specific structure, and therefore has excellent low-temperature adhesion and moist heat resistance without impairing the adhesive properties that polyester resins inherently have. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below.
[0011] <Polyester> The copolymer polyester resin of the present invention (hereinafter sometimes referred to as copolymer polyester resin (A)) is obtained by copolymerizing a polyvalent carboxylic acid component and a glycol component as constituent raw materials.
[0012] The copolymerized polyester resin (A) used in the present invention requires an aromatic dicarboxylic acid as a polyvalent carboxylic acid component, and contains 85 mol% or more of aromatic dicarboxylic acid with respect to the total polyvalent carboxylic acid component. The content of aromatic dicarboxylic acid in the acid component must be 85 mol% or more, and is preferably 90 mol% or more, and more preferably 95 to 100 mol%. If the content is too low, the cohesive force of the polyester resin decreases, and the wet heat resistance and holding power become poor. As the aromatic dicarboxylic acid, terephthalic acid is preferable from the viewpoint of adhesion to the substrate and wet heat resistance, and isophthalic acid is preferable from the viewpoint of solvent solubility.
[0013] As the polyvalent carboxylic acid component constituting the copolymer polyester resin (A), there is no particular limitation on the polyvalent carboxylic acid component that can be used other than terephthalic acid and isophthalic acid. Examples of the polyvalent carboxylic acid component that can be used other than terephthalic acid and isophthalic acid include, but are not limited to, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosane diacid, docosane diacid, phthalic acid, and naphthalene. Examples of the dicarboxylic acid include 4,4'-dicarboxybiphenyl, 5-sodium sulfoisophthalic acid, 5-hydroxy-isophthalic acid, fumaric acid, maleic acid, itaconic acid, mesaconic acid, citraconic acid, 1,3,4-benzenetricarboxylic acid, 1,2,4,5-benzenetetracarboxylic acid, pyromellitic acid, trimellitic acid, oxalic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 2,5-norbornenedicarboxylic acid, and anhydrides thereof. Among these, it is preferable to contain 1,4-cyclohexanedicarboxylic acid from the viewpoint of resistance to moist heat.
[0014] The glycol components constituting the copolymer polyester resin (A) each require polyalkylene glycol, neopentyl glycol, and alicyclic glycol, and the content of polyalkylene glycol relative to the total glycol components is 20 mol% or more, and the content of neopentyl glycol is less than 40 mol%. The content of polyalkylene glycol in the glycol components must be 20 mol% or more, and is preferably 20 to 60 mol%, and more preferably 30 to 50 mol%. If the content is less than 20 mol%, low-temperature adhesion and tackiness will be poor. The content of neopentyl glycol must be less than 40 mol%, and is preferably 10 to 40 mol%, and more preferably 20 to 30 mol%. If the content is 40 mol% or more, moist heat resistance and retention will be poor.
[0015] It is necessary to contain an alicyclic glycol. If an alicyclic glycol is not contained, the moist heat resistance is poor. The content of the alicyclic glycol is preferably less than 40 mol%, more preferably 5 to 40 mol%, more preferably 15 to 35 mol%, and even more preferably 20 to 30 mol%. If the content is 40 mol% or more, low-temperature adhesion and tackiness tend to be poor, and if it is less than 5 mol%, moist heat resistance may be poor.
[0016] Examples of polyalkylene glycols that can be used in the present invention include polyethylene glycol, polytetramethylene glycol, polypropylene glycol, polyhexylene glycol, polynonanediol, poly(3-methyl-1,5-pentane)diol, etc., among which polytetramethylene glycol is preferred in terms of adhesive strength and low-temperature adhesiveness. Examples of alicyclic glycols include 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedicarboxylic acid, tricyclodecane dimethanol, spiroglycol, etc., among which 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,2-cyclohexanedicarboxylic acid are preferred in terms of industrial availability, and 1,4-cyclohexanedimethanol is particularly preferred.
[0017] As the glycol component constituting the copolymer polyester resin (A), glycol components that can be used other than polyalkylene glycol, neopentyl glycol, and alicyclic glycol are not particularly limited, and examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 2,2-butylethylpropanediol, 1,2-propanediol, 2-methyl-1,3propanediol, 3-methyl-1,5pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol. Among these, from the viewpoint of solvent solubility, it is preferable to contain 2,2-butylethylpropanediol, 1,2-propanediol, or 2-methyl-1,3 propanediol.
[0018] As the monomer contained in the polyester polymer which is the main chain, if necessary, a monomer component (other monomer component) other than the polyvalent carboxylic acid component and the glycol component may be used within a range that does not impair the effects of the present invention. In addition, in the polyester polymer, the copolymerization ratio of the other monomer component is preferably less than 50 mol% based on the total monomer components contained in the polyester polymer.
[0019] Examples of other monomer components include hydroxycarboxylic acids such as tetrahydrophthalic acid, lactic acid, oxirane, glycolic acid, 2-hydroxybutyric acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxyisobutyric acid, 2-hydroxy-2-methylbutyric acid, 2-hydroxyvaleric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, 6-hydroxycaproic acid, 10-hydroxystearic acid, and 4-(β-hydroxy)ethoxybenzoic acid; and aliphatic lactones such as β-propiolactone, β-butyrolactone, γ-butyrolactone, δ-valerolactone, and ε-caprolactone.
[0020] In addition, as other monomer components, monocarboxylic acids, monoalcohols, etc. may be used. Examples of monocarboxylic acids include lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, benzoic acid, p-tert-butylbenzoic acid, cyclohexanoic acid, and 4-hydroxyphenylstearic acid. Examples of monoalcohols include octyl alcohol, decyl alcohol, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, and 2-phenoxyethanol.
[0021] The copolymer polyester resin (A) of the present invention may contain, if necessary, and within the range that does not impair the effects of the present invention, conventionally known additives such as a heat stabilizer such as phosphoric acid, an antioxidant such as a hindered phenol compound, a crystal nucleating agent such as talc or silica, a lubricant, a pigment such as titanium oxide, a filler, an antistatic agent, a foaming agent, a crosslinking agent, etc. In order to impart flame retardancy, it may also contain a bromine-based flame retardant, a metal hydroxide, a metal oxide such as antimony trioxide, a phosphate, a borate, a metal sulfide, an ammonium salt, an organic nitrogen-based flame retardant, a silicon-based flame retardant, a phosphorus-based flame retardant, etc.
[0022] The number average molecular weight of the copolymerized polyester resin (A) of the present invention is preferably 5000 to 35000, more preferably 8000 to 30000, and further preferably 10000 to 25000. If the number average molecular weight is less than 5000, the adhesive strength may be poor. If the number average molecular weight exceeds 35000, the melt viscosity and solution viscosity of the resulting polyester resin may be high, resulting in poor handleability.
[0023] In the present invention, the molecular weight of the copolymerized polyester resin (A) can be controlled by terminating the polymerization of the polyester melt at a predetermined melt viscosity during polycondensation, by adding a depolymerization agent after once producing a polyester with a high molecular weight, or by adding a monofunctional carboxylic acid or a monofunctional alcohol in advance. In the present invention, the molecular weight can be controlled by any of the above methods, but it is preferable that the trifunctional or higher component is arranged not only at the end of the polyester but also in the molecular chain. When an alcohol component is used as the depolymerization agent, a hydroxyl group can be added to the polyester end, and when an acid component is used, an acid value can be added to the polyester end. Examples of such depolymerization agent components include ethylene glycol, butanediol, sebacic acid, adipic acid, trimethylolpropane, trimellitic anhydride, and pyromellitic acid, but depolymerization by an acid component is preferable from the viewpoint of adhesion to a glass substrate. In this case, the amount of the acid component added is preferably 0.1 to 15 mol%, more preferably 0.5 to 12 mol%, and even more preferably 1.0 to 8 mol%. If the amount of the acid component added is less than 0.1 mol %, the acid value is low and improvement in adhesion to glass may not be expected, whereas if it exceeds 15 mol %, the resistance to moist heat may be poor.
[0024] The copolymer polyester resin (A) of the present invention preferably has a glass transition temperature of −45° C. or lower, more preferably −50° C. to −100° C., and even more preferably −60° C. to −90° C. If the glass transition temperature exceeds −45° C., both the adhesive strength and tackiness may be deteriorated.
[0025] <Hardening agent> As the curing agent in the present invention, a known one can be used. By containing a curing agent, the adhesive strength and moist heat resistance of the obtained adhesive can be improved in a well-balanced manner. The curing agent that can be used is not particularly limited as long as it is a compound that has reactivity with the functional group of the copolymerized polyester resin (A) or the functional group formed by the reaction of the copolymerized polyester resin (A) (e.g., a carboxyl group or its anhydride, a hydroxyl group, an epoxy group, an isocyanate group, etc.), but from the viewpoint of reactivity at low temperature, it is particularly preferable to use an isocyanate-based curing agent.
[0026] Examples of the isocyanate-based curing agent include aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate and tolylene diisocyanate, aliphatic diisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, xylylene diisocyanate and lysine diisocyanate, and alicyclic diisocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group. Among the above isocyanate-based curing agents, aromatic diisocyanates and alicyclic diisocyanates are preferred from the viewpoints of cohesive strength and adhesive strength. Furthermore, among aromatic diisocyanates, tolylene diisocyanate, among alicyclic diisocyanates, isophorone diisocyanate, and adducts, biuret products, and isocyanurates obtained by reacting these with dihydric or trihydric polyhydric alcohols are particularly preferred.
[0027] The content of the curing agent is preferably 1 to 10 parts by mass, more preferably 2 to 9 parts by mass, and even more preferably 3 to 8 parts by mass, based on the copolymer polyester resin (A). If the content of the curing agent (C) is less than 1 part by mass, the curing property is insufficient, and the moist heat resistance and holding power may be poor. On the other hand, if it exceeds 10 parts by mass, the adhesive strength and tackiness may be insufficient.
[0028] Next, the method for producing the copolymer polyester resin (A) of the present invention will be described. First, a combination of monomers such as polycarboxylic acid and glycol is appropriately selected, and these are polymerized by a known polymerization method to obtain a copolymerized polyester resin (A). That is, the raw material monomers are charged into a reactor, and then an esterification reaction is carried out, followed by polycondensation by a known method until the desired molecular weight is reached, thereby producing the copolymerized polyester resin (A). The esterification reaction is carried out, for example, at a temperature of 180°C or higher for 4 hours or more.
[0029] The polycondensation reaction is generally carried out using a polymerization catalyst under reduced pressure of 130 Pa or less at a temperature of 220 to 280°C. Examples of the polymerization catalyst include titanium compounds such as tetrabutyl titanate, metal acetates such as zinc acetate, magnesium acetate, and zinc acetate, and organotin compounds such as antimony trioxide, hydroxybutyltin oxide, and tin octylate. The amount of the polymerization catalyst used is preferably 0.1 to 20 x 10 per mole of the acid component, since a small amount of the polymerization catalyst slows down the reaction and an excessive amount of the polymerization catalyst reduces the color tone of the resulting copolymerized polyester resin (A). -4 It is preferably molar.
[0030] The copolymer polyester resin (A) of the present invention is preferably dissolved in a solvent before use, and the solvent is preferably an organic solvent. The organic solvent is not particularly limited, and examples thereof include aromatic solvents such as toluene, xylene, solvent naphtha, and solvent, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol solvents such as methyl alcohol, ethyl alcohol, isopropyl alcohol, and isobutyl alcohol, ester solvents such as ethyl acetate and normal butyl acetate, and acetate solvents such as cellosolve acetate and methoxy acetate. These solvents may be used alone or in combination of two or more.
[0031] As described above, the copolymerized polyester resin (A) can be dissolved in an organic solvent to form a pressure-sensitive adhesive. The solid content of the adhesive is preferably 5 to 60% by mass, more preferably 10 to 50% by mass, and even more preferably 20 to 40% by mass. If the solid content is less than 5% by mass, the adhesive cannot be applied in a sufficient amount when applied to a substrate as described below. On the other hand, if the solid content exceeds 60% by mass, the solution viscosity of the adhesive becomes too high, and the thickness accuracy decreases when the adhesive is applied to a substrate.
[0032] The polyester resin (A) of the present invention may be combined with a tackifier resin, if necessary.
[0033] The tackifier resin is not particularly limited, and any conventionally known tackifier resin may be used. For example, terpene-based tackifying resins, phenol-based tackifying resins, rosin-based tackifying resins, etc. Adhesive resin, aliphatic petroleum resin, aromatic petroleum resin, copolymer petroleum resin, alicyclic petroleum resin Grease, xylene resin, epoxy tackifier resin, polyamide tackifier resin, ketone adhesive These include tackifying resins and elastomer-based tackifying resins, particularly rosin-based and terephthalic resins derived from plants. It is preferable to use a pen-based tackifier resin. These can be used alone or in combination of two or more.
[0034] Specifically, the terpene resin may be an α-pinene polymer, a β-pinene polymer, a dipentene polymer, or a terpene resin obtained by modifying these polymers with phenol, aromatic groups, hydrogen, or hydrocarbons.
[0035] Specific examples of the phenol-based tackifier resin include phenol, m-cresol, Various phenols such as 3,5-xylenol, p-alkylphenol, and resorcinol Furthermore, the condensation products of the above phenols and hols can be used. resol obtained by addition reaction of phenol with phenol in the presence of an alkali catalyst; Novolak, which is obtained by condensation reaction of phenols and formaldehyde in the presence of an acid catalyst, Phenol is added to modified rosin or its derivatives in the presence of an acid catalyst, followed by thermal polymerization. For example, a rosin-modified phenolic resin obtained by mixing
[0036] Specific examples of the rosin-based tackifier resin include gum rosin, wood rosin, and talline rosin. Unmodified rosin (raw rosin) such as oil rosin, and those that have been hydrogenated, disproportionated, polymerized, or otherwise chemically modified Chemically modified rosins and derivatives thereof can be used.
[0037] The amount of the tackifier resin added is preferably 10 to 100 parts by weight, more preferably 15 to 80 parts by weight, and even more preferably 20 to 60 parts by weight, relative to the polyester resin (A). If the amount is less than 10 parts by weight, the effect of the addition, such as improved adhesive strength, will not be obtained, whereas if it exceeds 100 parts by weight, the cohesive strength of the resin will decrease, which may cause a decrease in holding power and adhesive strength.
[0038] In addition, the polyester resin (A) of the present invention may contain antioxidants, hydrolysis inhibitors, pigments, etc., as necessary. The antioxidants are not particularly limited, but examples thereof include phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. The hydrolysis inhibitors include carbodiimides derived from isocyanates. The pigments include titanium dioxide, zinc oxide, etc.
[0039] In the present invention, the pressure-sensitive adhesive can be coated on, for example, various substrates, and dried as necessary to remove the organic solvent, thereby forming the coating film of the present invention on the substrate.
[0040] In the present invention, the substrate to be coated with the pressure-sensitive adhesive is not particularly limited, and examples thereof include polyester substrates selected from polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and poly 1,4-cyclohexanedimethanol terephthalate (PCT), polycarbonate substrates, polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), polyethylene tetrafluoroethylene (ETFE), polytetrafluoroethylene (PTFE), and tetrafluoroethylene perfluoroalkylvinyl chloride (PTFE). The substrate may be selected from fluorine-based substrates selected from tetrafluoroethylene-hexafluoropropylene copolymers (PFA) and tetrafluoroethylene-hexafluoropropylene copolymers (FEP); acrylic substrates, polyolefin substrates such as cyclic olefins (COC), polyethylene (high density polyethylene, low density polyethylene, linear low density polyethylene), polypropylene, and polybutene; polyvinyl chloride substrates, polystyrene substrates, polyvinylidene chloride substrates, ethylene-vinyl acetate copolymer substrates, polyvinyl alcohol substrates, polyvinyl acetate substrates, acetal substrates, polyamide substrates, and polyarylate substrates, and these substrates may be the same or different.
[0041] In the present invention, the method for coating the substrate with the pressure-sensitive adhesive is not particularly limited, and known methods such as reverse roll coating, gravure coating, die coating, comma coating, and spray coating can be used.
[0042] The copolymerized polyester resin of the present invention has excellent adhesive properties and can be used in various adhesive and pressure-sensitive adhesive applications. In particular, it has excellent low-temperature adhesive properties and wet heat resistance, so it can be applied to a substrate and used as an adhesive or adhesive tape, or can be used for mounting electric and electronic parts. It can also be suitably used for outdoor use, such as building materials. EXAMPLES
[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0044] 1. Evaluation method (1) Composition of copolymer polyester resin 1H-NMR measurement was performed using an NMR measurement device (JNM-LA400 manufactured by JEOL Ltd.), and the resin composition was determined from the integrated intensity of the peaks of the copolymerization components in the obtained chart. Note that deuterated trifluoroacetic acid was used as the measurement solvent.
[0045] (2) Glass transition temperature of copolymer polyester resin Measurements were performed using an input compensation type differential scanning calorimeter (PerkinElmer, Diamond DSC, detection range: -50°C to 200°C) at a heating rate of 10°C / min. The glass transition temperature was determined as the temperature at the intersection of a straight line extending the low-temperature side baseline to the high-temperature side in the obtained heating curve and a tangent drawn at the point where the gradient of the curve in the stepwise change portion of the glass transition was maximum.
[0046] (3) Number average molecular weight of copolymer polyester resin The number average molecular weight in terms of polystyrene was measured by gel permeation chromatography (GPC) under the following conditions. [Liquid delivery unit]: Shimadzu LC-10ADvp [UV-Visible spectrophotometer]: Shimadzu SPD-6AV, detection wavelength: 254 nm [Column]: One Shodex KF-803 and two Shodex KF-804 columns connected in series [Solvent]: Tetrahydrofuran [Measurement temperature]: 40℃
[0047] (4) Acid value of copolymer polyester resin According to JIS K-0070, 0.5 g of the sample was dissolved in 25 ml of dioxane and titrated with 0.1N-KOH using cresol red as an indicator. The titrated value was used to calculate the equivalent number contained in 1 ton of polyester resin, and the acid value was obtained.
[0048] (5) Calculation method of aromatic concentration in the copolyester resin The aromatic ring concentration referred to here is calculated from the resin composition. Calculated with one benzene nucleus (one equivalent), for example, terephthalic acid has one, and naphthalenedicarboxylic acid has two, to calculate how many aromatic rings there are per repeating unit of the polyester resin. Next, calculate how many (how many equivalents) aromatic rings there are per ton of resin. That is, the unit is expressed as the number of equivalents per ton of resin.
[0049] (6) Adhesive strength Cut out the adhesive film into a width of 25 mm, overlap the adhesive surface with a PC board or a glass plate, use a small desktop test laminator (SA-1010 manufactured by Tester Sangyo Co., Ltd.), and press-bond it under the conditions of a temperature of 23 °C, a pressure of 13.5 N / cm, and a speed of 1.0 m / min. The sample aged for 24 hours at 23 °C was used as the test piece. In this test piece, a small desktop tensile tester (EZ-SX manufactured by Shimadzu Corporation) was used to measure the adhesive strength under the conditions of a temperature of 23 °C, a tensile speed of 300 mm / min, and a tensile angle of 180 degrees. <Adhesive strength to PC board> ◎: 20 N / 25 mm or more ○: 10 N / 20 mm or more and less than 20 N / 25 mm △: 5 N / 25 mm or more and less than 10 N / 25 mm ×: Less than 5 N / 15 mm <Adhesive strength to glass plate> ◎: 15 N / 25 mm or more. ○: 5 N / 25 mm or more and less than 15 N / 25 mm △: 3 N / 25 mm or more and less than 5 N / 25 mm ×: Less than 3 N / 25 mm
[0050] (7) Retaining force The adhesive film was cut to a width of 25 mm, and the adhesive surface was placed on a stainless steel plate (SUS304), and the adhesive was pressed using a small tabletop test laminator (SA-1010 manufactured by Tester Sangyo Co., Ltd.) under conditions of temperature 23°C, pressure 13.5 N / cm, speed 1.0 m / min, and adhesive area 25 mm x 25 mm, and aged for 24 hours at 23°C to prepare a test specimen. A load of 1 kg was applied to this test specimen at 23°C, and the distance (mm) at which the displacement occurred after 1 hour was measured. ◎: The deviation is less than 1 mm. ○: The deviation is 1 mm or more and less than 4 mm. △: The deviation is 4 mm or more and less than 6 mm. ×: The deviation is 6 mm or more.
[0051] (8) Tackiness For adhesive films, a ball tack tester (manufactured by Yasuda Seiki Seisakusho) was used to roll a high carbon chromium steel ball on the adhesive layer surface at a temperature of 23°C and an angle of 30°, and the maximum ball number that came to rest was measured. ◎: Ball number is 6 or more. ○: The ball number is 4 or 5. △: The ball number is 3. ×: The ball number is 2 or less.
[0052] (9) Moisture and heat resistance The adhesive film was cut into a width of 25 mm, and the adhesive surface was placed on a stainless steel plate (SUS304). Test pieces were prepared and adhesive strength was measured under the same conditions as in (6), and this was taken as the initial adhesive strength. The test pieces obtained above were also treated for 500 hours under conditions of 85°C x 85% RH, and the adhesive strength of the treated test pieces was measured under the same conditions as in (6). The retention rate was calculated for each piece using the following formula, and evaluated according to the following criteria. Retention rate (%) = Adhesive strength after treatment / Initial adhesive strength x 100 ◎: Retention rate is 90% or more. ○: The retention rate is 80% or more and less than 90%. △: Retention rate is 70% or more and less than 80%. ×: The retention rate is less than 70%.
[0053] (10) Low temperature adhesion The adhesive film was cut to a width of 25 mm, and the adhesive surface was overlapped with a stainless steel plate (SUS304), and the adhesive was pressed using a small tabletop test laminator (SA-1010 manufactured by Tester Sangyo Co., Ltd.) under conditions of a temperature of -15°C, a pressure of 13.5 N / cm, and a speed of 1.0 m / min, and aged for 24 hours at -15°C to prepare a test specimen. The adhesive strength of this test specimen was measured using a small tabletop tensile tester (EZ-SX manufactured by Shimadzu Corporation) under conditions of a temperature of -15°C, a tensile speed of 300 mm / min, and a tensile angle of 180°. ◎: Adhesive strength is 10N / 25mm or more. ○: Adhesive strength is 8N / 25mm or more and less than 10N / 25mm. △: Adhesive strength is 5N / 25mm or more and less than 8N / 25mm. ×: The adhesive strength is less than 5N / 15mm.
[0054] 2. Preparation of Polyester Resin Preparation Example 1 83g (50 mol%) of terephthalic acid, 83g (50 mol%) of isophthalic acid, 17g (28 mol%) of ethylene glycol, 52g (50 mol%) of neopentyl glycol, 36g (25 mol%) of 1,4-cyclohexanedimethanol, 3g (2 mol%) of trimethylolpropane, and 300g (30 mol%) of polytetramethylene glycol having a molecular weight of 1000 were charged into a reactor, and the inside of the system was replaced with nitrogen. Then, while stirring these raw materials at 1000 rpm, the reactor was heated to 250°C and melted. After the temperature inside the reactor reached 250°C, the esterification reaction was allowed to proceed for 3 hours. After 3 hours, 0.2g of tetrabutyl titanate was added as a polymerization catalyst, and the inside of the system was decompressed. After the inside of the system reached a high vacuum (pressure: 20 Pa), the polymerization reaction was carried out for another 2 hours to obtain a copolymer polyester resin (A). The results are shown in Table 1.
[0055] [Table 1]
[0056] The abbreviations in Table 1 stand for the following: TPA: Terephthalic acid IPA: Isophthalic acid DDA: 1,12-dodecanediol EG: Ethylene glycol NPG: Neopentyl glycol CHDM: 1,4-cyclohexanedimethanol TCD: Tricyclodecane dimethanol PTMG1000: Polytetramethylene glycol (molecular weight: 1000) PEG1000: Polyethylene glycol (molecular weight: 1000) TMP: Trimethylolpropane
[0057] Preparation Examples 2 to 23 Polymerization of copolymerized polyester resins was carried out in the same manner as in Preparation Example 1, except that the types and amounts of monomers used and the polymerization reaction time were changed as shown in Table 1. In Preparation Examples 13 and 14, after the polymerization reaction was completed and the reduced pressure was released, a depolymerization agent (isophthalic acid) was added as shown in Table 1, and a depolymerization reaction was carried out at 250°C for 2 hours to obtain copolymerized polyester resins.
[0058] Example 1 The copolymerized polyester resin (A) obtained in Preparation Example 1 was dissolved in ethyl acetate to a solid content concentration of 30% to prepare a resin solution. The resin solution was coated on the corona-treated surface of a biaxially oriented PET film (manufactured by Unitika Co., Ltd., thickness 75 μm) using a tabletop coating device (manufactured by Yasuda Seiki Co., Ltd., film applicator No. 542-AB type, bar coater attached) so that the film thickness after drying would be 25 μm, and the film was dried in a hot air dryer at 100 ° C. for 1 minute, and then aged at 50 ° C. for 4 days to obtain a laminate with a copolymerized polyester resin coating film formed. Various evaluations were performed using the obtained laminate. The results are shown in Table 2.
[0059] [Table 2]
[0060] Examples 2 to 15 The copolymer polyester resins (B) to (O) were used to obtain resin solutions in the same manner as in Example 1. The obtained resin solutions were used to obtain laminates in the same manner as in Example 1, and various evaluations were carried out. The results are shown in Table 2.
[0061] Comparative Examples 1 to 6 The copolymer polyester resins (P) to (U) were used to obtain resin solutions in the same manner as in Example 1. The obtained resin solutions were used to obtain laminates in the same manner as in Example 1, and various evaluations were carried out. The results are shown in Table 3.
[0062] [Table 3]
[0063] Examples 16 to 22 Each of the copolymer polyester resins (A), (B), (C), (E), (F), (I), and (N) was dissolved in ethyl acetate to a solid content concentration of 30%, and then a resin solution was prepared containing 4 parts by mass of an isocyanate-based curing agent (Tosoh Corporation's Coronate L) per 100 parts by mass of the solid content of the copolymer polyester resin. Using the obtained resin solution, a laminate was obtained in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 4.
[0064] [Table 4]
[0065] In Examples 1 to 15, the adhesive strength, holding strength and tackiness were good because a specific copolymer polyester resin was used, and the adhesive strength, holding strength and tackiness were also excellent in terms of resistance to moist heat and low-temperature adhesion.
[0066] In Examples 16 to 22, a curing agent was further added to the specified copolymer polyester resin, and therefore the adhesive strength and holding power were improved compared to the case where the copolymer polyester resin was used alone. In Examples 17 and 18, the moist heat resistance was also improved.
[0067] In Comparative Example 1, the copolymerization ratio of the aromatic dicarboxylic acid was low, and therefore the holding power and the resistance to moist heat were poor.
[0068] In Comparative Example 2, since no alicyclic glycol was contained, the moist heat resistance was poor.
[0069] In Comparative Example 3, the copolymerization ratio of neopentyl glycol was more than 40 mol %, so that the holding power and the resistance to moist heat were inferior.
[0070] In Comparative Example 4, the copolymerization ratio of polyalkylene glycol was less than 20 mol %, so that the tackiness and low-temperature adhesion were poor.
[0071] In Comparative Example 5, the copolymerization ratio of polytetramethylene glycol was less than 20 mol % and the copolymerization ratio of neopentyl glycol was more than 40 mol %, so that the holding power, tackiness, moist heat resistance and low-temperature adhesion were poor.
[0072] In Reference Example 1, the adhesive strength was insufficient, and the wet heat resistance could not be evaluated.
Claims
1. The copolymer polyester resin contains, as acid components constituting the polyester resin, 85 to 100 mol % of an aromatic dicarboxylic acid relative to the total acid components, and as glycol components, polytetramethylene glycol, neopentyl glycol, and 1,4-cyclohexanedimethanol, with polytetramethylene glycol being 20 mol % or more and neopentyl glycol being less than 40 mol % relative to the total glycol components.
2. The copolymer polyester resin according to claim 1, which has a glass transition temperature of -45°C or lower.
3. 3. The copolymer polyester resin according to claim 1, wherein the content of 1,4-cyclohexanedimethanol is less than 40 mol % based on the total glycol components.
4. A copolymer polyester resin composition comprising the copolymer polyester resin according to any one of claims 1 to 3 and a curing agent.
5. 5. The copolymer polyester resin composition according to claim 4, wherein the curing agent is an isocyanate curing agent.
6. A coating film comprising the copolymer polyester resin composition according to claim 4 or 5.
7. A laminate having the coating film according to claim 6.
Citation Information
Patent Citations
Preparation of amorphous polyester
JP1982212228A
Copolyester resin and adhesive using the same
JP2012214558A
Copolyester resin
JP2013249443A