Anode composition, anode for lithium secondary battery including the same, and lithium secondary battery including the anode

A partially crosslinked binder polymer for silicon-based electrodes in lithium secondary batteries addresses volume expansion issues, enhancing electrode stability and capacity retention.

JP7575171B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023552557
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-15
Filing Date
2022-12-02
Publication Date
2024-10-29
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

Silicon-based negative electrode active materials in lithium secondary batteries experience significant volume expansion during charging and discharging, leading to conductive path disruption and degradation of battery characteristics, which current binder solutions fail to adequately address.

Method used

A negative electrode composition featuring a (meth)acrylamide group-containing compound, unsaturated organic acid or its salt, α,β-unsaturated nitrile monomer, and diacrylamide or diacrylate-containing compound, forming a partially crosslinked binder polymer to minimize electrode thickness changes and enhance adhesion.

Benefits of technology

The partially crosslinked binder polymer effectively suppresses volumetric expansion and contraction, maintaining electrode integrity and improving capacity retention rates in lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575171000003
    Figure 0007575171000003
  • Figure 0007575171000004
    Figure 0007575171000004
  • Figure 0007575171000001
    Figure 0007575171000001
Patent Text Reader

Abstract

The present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, and a method for producing the lithium secondary battery negative electrode composition including the negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2021-0180143, filed with the Korean Intellectual Property Office on December 15, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, and a lithium secondary battery including the negative electrode. [Background technology]

[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is power generation and storage using electrochemical reactions.

[0004] At present, a representative example of an electrochemical element that utilizes such electrochemical energy is a secondary battery, and the range of its use is tending to expand more and more.

[0005] As technological development and demand for mobile devices increases, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used. In addition, research into a method for manufacturing a high-density electrode with a higher energy density per unit volume as an electrode for such high-capacity lithium secondary batteries is being actively conducted.

[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and removes lithium ions from the positive electrode. Silicon-based particles having a large discharge capacity can be used as the negative electrode active material.

[0007] In particular, in recent years, in response to the demand for high-density energy batteries, active research has been conducted into methods of increasing capacity by using silicon-based compounds such as Si / C and SiOx, which have a capacity 10 times larger than that of graphite-based materials, as negative electrode active materials. However, silicon-based compounds, which are high-capacity materials, have a large capacity compared to the conventionally used graphite, but they have the problem that their volume suddenly expands during charging, cutting off the conductive path and reducing the battery characteristics.

[0008] In order to solve the problems when using silicon-based compounds as negative electrode active materials, various methods for suppressing the volume expansion itself or preventing the conductive path from being broken, such as a method of adjusting the driving potential, a method of further coating a thin film on the active material layer, and a method of adjusting the particle size of the silicon-based compound, have been discussed. However, the above methods have limitations in their application because they may actually degrade the performance of the battery, and there are still limitations in the commercialization of negative electrode batteries with a high content of silicon-based compounds.

[0009] In particular, research is being conducted on the composition of binders that accompany volume expansion, and research is being conducted on the use of binder polymers that have strong lateral stress in order to suppress the volume expansion of negative electrode active materials, which have large volume changes, that accompany charge and discharge. However, these binder polymers alone have limitations in suppressing the increase in electrode thickness due to the contraction and expansion of negative electrode active materials and the resulting deterioration in lithium secondary battery performance.

[0010] In order to solve the above problems, research has been conducted on introducing a crosslinking agent into the binder polymer, but this method can have problems with viscosity change and phase stability of the slurry due to long-term storage of the battery, making it difficult to apply to actual processes.

[0011] Therefore, even when a negative electrode active material with large volume expansion is used, it is necessary to study a negative electrode binder that can minimize the change in thickness of the negative electrode and thereby improve the capacity retention rate. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2009-080971 A Summary of the Invention [Problem to be solved by the invention]

[0013] As a result of research into binders that can be used in silicon-based negative electrodes and have improved slurry dispersibility and excellent adhesion, it was found that the above problems could be solved by changing the polymer binder to a specific composition so that it has a partially cross-linked structure.

[0014] Accordingly, the present application relates to a negative electrode composition, a negative electrode for a lithium secondary battery including the same, and a lithium secondary battery including the negative electrode. [Means for solving the problem]

[0015] One embodiment of the present specification provides a negative electrode composition including a negative electrode binder polymer, a negative electrode active material, and a negative electrode conductive material, in which the negative electrode binder polymer includes a (meth)acrylamide group-containing compound; an unsaturated organic acid or a salt of an unsaturated organic acid; a monomer including an α,β-unsaturated nitrile; and a diacrylamide or diacrylate-containing compound; and the negative electrode composition includes, based on 100 parts by weight of the negative electrode binder polymer, 1 part by weight or more and 30 parts by weight or less of the monomer including an α,β-unsaturated nitrile; and 0.1 parts by weight or more and 15 parts by weight or less of the diacrylamide or diacrylate-containing compound.

[0016] In yet another embodiment, there is provided a negative electrode for a lithium secondary battery, comprising: a negative electrode current collector layer; and a negative electrode active material layer formed on one or both sides of the negative electrode current collector layer, the negative electrode active material layer comprising the negative electrode composition according to the present application.

[0017] Finally, there is provided a lithium secondary battery comprising: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator disposed between the positive electrode and the negative electrode; and an electrolyte. Effect of the Invention

[0018] A negative electrode composition according to one embodiment of the present invention is characterized in that the negative electrode composition contains a negative electrode binder polymer, the negative electrode binder polymer including: a (meth)acrylamide group-containing compound; an unsaturated organic acid or a salt of an unsaturated organic acid; a monomer containing an α,β-unsaturated nitrile; and a diacrylamide or diacrylate-containing compound.

[0019] In particular, the negative electrode binder polymer satisfies the following ratios per 100 parts by weight: 1 to 30 parts by weight of the α,β-unsaturated nitrile-containing monomer, and 0.1 to 15 parts by weight of the diacrylamide or diacrylate-containing compound. As a result, even when a negative electrode active material (especially a silicon-based active material) that exhibits large volume expansion during charging / discharging is used, volume expansion and contraction can be suppressed and thickness changes due to electrode swelling can be minimized, resulting in excellent life performance of the lithium secondary battery.

[0020] The negative electrode binder polymer according to the present invention is characterized in that it contains a specific amount of diacrylamide or diacrylate to partially crosslink linear polymers, thereby forming a partially crosslinked structure.

[0021] In the case where the negative electrode binder polymer having the above-mentioned characteristics is included, the binder itself has a partially crosslinked structure, which reduces the change in electrode thickness during charging and discharging, and improves the capacity retention rate during the life evaluation. At this time, the degree of partial crosslinking of the polymer can be expressed by the content of the diacrylamide or diacrylate-containing compound.

[0022] That is, the negative electrode composition according to one embodiment of the present invention is characterized in that it contains a silicon-based active material with a high theoretical capacity as a negative electrode active material, thereby improving the capacity characteristics, and solves the problem of volume expansion due to charge and discharge, which is a problem of silicon-based active materials, by using a specific negative electrode binder polymer according to the present application. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a diagram showing a laminated structure of a negative electrode for a lithium secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 1 is a diagram showing a layered structure of a lithium secondary battery according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Prior to describing the invention, some terms will first be defined.

[0025] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.

[0026] In this specification, "p to q" means a range of "not less than p and not more than q".

[0027] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mini II manufactured by BEL Japan Co., Ltd. That is, in this application, the BET specific surface area may mean the specific surface area measured by the above-mentioned measurement method.

[0028] In this specification, "Dn" means particle size distribution, and refers to the particle size at the n% point of the cumulative particle number distribution by particle size. That is, D50 is the particle size (average particle size) at the 50% point of the cumulative particle number distribution by particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution by particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution by particle size. On the other hand, the particle size distribution may be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in the diffraction pattern due to the particle size when the particles pass through a laser beam is measured to calculate the particle size distribution.

[0029] In this specification, when a polymer contains a certain monomer or compound as a monomer or compound unit, it means that the monomer or compound is involved in a polymerization reaction and is included as a repeating unit in the polymer. In this specification, when a polymer contains a monomer or compound, this is interpreted as the same as when a polymer contains a monomer or compound as a monomer unit.

[0030] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless otherwise specified as a "homopolymer."

[0031] In this specification, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various polymerization degrees that are commercially available for molecular weight measurement as standard substances. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0032] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in various different forms and is not limited to the following description.

[0033] One embodiment of the present specification provides a negative electrode composition including a negative electrode binder polymer, a negative electrode active material, and a negative electrode conductive material, in which the negative electrode binder polymer includes a (meth)acrylamide group-containing compound; an unsaturated organic acid or a salt of an unsaturated organic acid; a monomer including an α,β-unsaturated nitrile; and a diacrylamide or diacrylate-containing compound; and the negative electrode composition includes, based on 100 parts by weight of the negative electrode binder polymer, 1 part by weight or more and 30 parts by weight or less of the monomer including an α,β-unsaturated nitrile; and 0.1 parts by weight or more and 15 parts by weight or less of the diacrylamide or diacrylate-containing compound.

[0034] The negative electrode binder polymer according to the present application is characterized in that it contains a specific amount of a diacrylamide or diacrylate-containing compound to partially crosslink a linear polymer, forming a partially crosslinked structure. That is, when the negative electrode binder polymer having the above-mentioned characteristics is included, the partially crosslinked structure of the binder itself reduces the change in thickness of the electrode during charging and discharging, and improves the capacity retention rate during the life evaluation.

[0035] In one embodiment of the present application, the negative electrode binder polymer may include a (meth)acrylamide group-containing compound; an unsaturated organic acid or a salt of an unsaturated organic acid; a monomer containing an α,β-unsaturated nitrile; and a diacrylamide or diacrylate-containing compound.

[0036] In one embodiment of the present application, the negative electrode binder may contain 30 parts by weight or more and 80 parts by weight or less of the (meth)acrylamide group-containing compound based on 100 parts by weight of the negative electrode binder polymer.

[0037] In another embodiment, the negative electrode binder may contain 30 parts by weight or more and 80 parts by weight or less, preferably 35 parts by weight or more and 75 parts by weight or less, and more preferably 40 parts by weight or more and 70 parts by weight or less, of the (meth)acrylamide group-containing compound based on 100 parts by weight of the negative electrode binder polymer.

[0038] In one embodiment of the present application, the negative electrode binder polymer may contain 5 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 35 parts by weight or less, and more preferably 15 parts by weight or more and 35 parts by weight or less of the unsaturated organic acid or a salt of the unsaturated organic acid, based on 100 parts by weight of the negative electrode binder polymer.

[0039] In one embodiment of the present application, there is provided a negative electrode composition comprising, based on 100 parts by weight of the negative electrode binder polymer, 1 part by weight or more and 30 parts by weight or less of the α,β-unsaturated nitrile-containing monomer; and 0.1 parts by weight or more and 15 parts by weight or less of the diacrylamide or diacrylate-containing compound.

[0040] In another embodiment, based on 100 parts by weight of the negative electrode binder polymer, the monomer containing an α,β-unsaturated nitrile may be 1 part by weight or more and 30 parts by weight or less, preferably 3 parts by weight or more and 30 parts by weight or less, and more preferably 5 parts by weight or more and 30 parts by weight or less.

[0041] In another embodiment, the amount of the diacrylamide or diacrylate-containing compound may be 0.1 parts by weight or more and 15 parts by weight or less, preferably 0.5 parts by weight or more and 12 parts by weight or less, based on 100 parts by weight of the negative electrode binder polymer.

[0042] The negative electrode binder polymer according to the present application contains four types of monomers as described above, and is characterized by including the above-mentioned content portion in particular. By including the above-mentioned content portion, the negative electrode binder polymer forms a partially crosslinked structure, improving the binding force, and the electrode containing the same has a small change in thickness during charging and discharging, and therefore has an improved capacity retention rate during the progress of a life evaluation.

[0043] In one embodiment of the present application, the specific parts by weight of the composition based on 100 parts by weight of the negative electrode binder polymer may refer to the weight ratio of each component monomer based on the total weight of the monomer group of the negative electrode binder polymer being 100, and this is expressed as parts by weight.

[0044] In one embodiment of the present application, there is provided a negative electrode composition in which the molar ratio of the (meth)acrylamide group-containing compound to the unsaturated organic acid or the salt of the unsaturated organic acid is 1:0.1 to 1:0.6.

[0045] The molar ratio means a ratio of moles contained based on 100 parts by weight of the negative electrode binder polymer according to the present application, and specifically, may mean a ratio of mole %.

[0046] In one embodiment of the present application, the negative electrode binder polymer may contain a (meth)acrylamide group-containing compound.

[0047] In one embodiment of the present application, the (meth)acrylamide may be methacrylamide; or may include acrylamide.

[0048] In one embodiment of the present application, the unsaturated organic acid can be used without limitation as long as it is an organic acid that can be contained in the binder, and specifically, acrylic acid can be used. In this case, the salt of the unsaturated organic acid can mean a salt form containing ions in the unsaturated organic acid, and this can also be used without limitation. In this case, the unsaturated organic acid includes, for example, a carboxylic acid or a salt thereof. The carboxylic acid can be a carboxylic acid monomer or a salt thereof such as (meth)acrylic acid, itaconic acid, fumaric acid, crotonic acid, maleic acid, monomethyl itaconate, methyl fumarate, monobutyl fumarate, etc., and these can be used alone or in combination of two or more kinds.

[0049] In one embodiment of the present application, the α,β-unsaturated nitrile containing monomer may be acrylonitrile.

[0050] In one embodiment of the present application, there is provided a negative electrode composition, wherein the diacrylamide or diacrylate-containing compound is an alkyl diacrylamide; an alkylene oxide diacrylamide; or an alkylene oxide diacrylate.

[0051] Specifically, the diacrylamide or diacrylate containing compound may include N,N-methylenebisacrylamide; or ethylene glycol diacrylate.

[0052] As a result, the negative electrode binder polymer according to the present application contains four components having specific contents and compositions as described above, and even when a negative electrode active material (especially a silicon-based active material) that exhibits large volume expansion during charge / discharge is used, the negative electrode binder polymer can suppress volume expansion and contraction and minimize thickness changes due to electrode swelling, thereby improving the life performance of the lithium secondary battery.

[0053] The four components may be polymerized to form the negative electrode binder polymer.

[0054] In one embodiment of the present application, there is provided a negative electrode composition in which the weight average molecular weight of the negative electrode binder polymer is 100,000 g / mol or more and 3,000,000 g / mol or less.

[0055] In another embodiment, the weight average molecular weight of the negative electrode binder polymer may be in the range of 100,000 g / mol to 3,000,000 g / mol, preferably 200,000 g / mol to 1,500,000 g / mol.

[0056] When the weight average molecular weight of the negative electrode binder polymer satisfies the above range, the negative electrode binder polymer has excellent mechanical strength, high intermolecular interaction, and excellent electrode binding force. In addition, when the weight average molecular weight satisfies the above range, the viscosity of the negative electrode binder can be selected within an appropriate range, and when a negative electrode is manufactured using the negative electrode binder, the negative electrode binder has excellent electrode coating properties.

[0057] In an embodiment of the present application, the negative electrode binder polymer may be included in an amount of 1 part by weight to 20 parts by weight based on 100 parts by weight of the negative electrode composition.

[0058] In another embodiment of the present application, the negative electrode binder polymer may be 1 part by weight or more and 20 parts by weight or less, preferably 3 parts by weight or more and 15 parts by weight or less, and more preferably 4 parts by weight or more and 15 parts by weight or less, based on 100 parts by weight of the negative electrode composition.

[0059] When the content is within the above range, the negative electrode active material can be effectively dispersed, and the negative electrode active material can have high electrode adhesive strength and high binding strength between the active materials inside the electrode against contraction and expansion of the negative electrode active material due to charging and discharging of the lithium secondary battery.

[0060] In one embodiment of the present application, the Young's modulus of the negative electrode binder polymer is 10 3 MPa or more.

[0061] In another embodiment, the negative electrode binder polymer has a Young's modulus of 1×10 3 MPa or more, preferably 2×10 3 MPa, more preferably 5×10 3 MPa or more, and 25×10 3 MPa or less, preferably 22×10 3 MPa or less, more preferably 20×10 3 MPa or less.

[0062] The Young's modulus is measured by placing the negative electrode binder polymer in a coated container and drying it at room temperature for a long time to remove moisture. The film from which moisture has been removed is vacuum dried at 130°C for 10 hours in accordance with the electrode drying temperature to obtain a dried film. The dried film is then cut or punched into a sample shape of 6 mm x 100 mm to obtain a sample, and the tensile strength (Young's modulus) can be measured using a UTM device.

[0063] The Young's modulus of the negative electrode binder polymer varies depending on the measurement method, speed, and measurement condition of the binder, but may refer to a value measured in a dry room with a dew point of -5°C to 10°C and a temperature of about 20°C to 22°C.

[0064] In this application, the dew point means the temperature at which condensation begins when moist air is cooled and the partial pressure of water vapor in the air becomes equal to the saturated vapor pressure of water at that temperature. In other words, it can mean the temperature at which dew begins to appear when the temperature of a gas containing water vapor is lowered at the same temperature, with the relative humidity reaching 100%.

[0065] A room with a dew point of -5°C to 10°C and a temperature of about 20°C to 22°C can generally be defined as a dry room, and the humidity at this time corresponds to a very low level.

[0066] The negative electrode binder polymer has dispersibility for dispersing the negative electrode active material in a negative electrode slurry state containing the negative electrode composition, and adhesive strength for binding the negative electrode current collector layer and the negative electrode active material layer after drying. Also, the adhesive strength is not high. That is, the negative electrode binder polymer according to the present application may mean a binder that satisfies the Young's modulus and has a surface-adhesive form.

[0067] The negative electrode binder polymer is hydrophilic and does not dissolve in an electrolyte or electrolytic solution generally used in a secondary battery. Such a characteristic can provide the negative electrode binder polymer with strong stress or tensile strength when applied to a negative electrode or a lithium secondary battery, thereby effectively suppressing the problem of volume expansion / contraction associated with charge / discharge of a silicon-based active material.

[0068] In one embodiment of the present application, the negative electrode binder polymer may further include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, K, or the like, or may further include various copolymers thereof.

[0069] The negative electrode binder polymer according to one embodiment of the present application serves to hold down the negative electrode active material and the negative electrode conductive material to prevent twisting and deformation of the negative electrode structure due to volume expansion and relaxation of the silicon-based active material.

[0070] In one embodiment of the present application, there is provided a negative electrode composition, wherein the negative electrode active material includes at least one selected from the group consisting of a silicon-based active material and a carbon-based active material.

[0071] In one embodiment of the present application, the negative electrode active material includes at least one selected from the group consisting of silicon-based active materials and carbon-based active materials, and the silicon-based active material may include at least one selected from the group consisting of SiOx (x = 0), SiOx (0 < x < 2), SiC, and Si alloys.

[0072] In one embodiment of the present application, the negative electrode active material includes a silicon-based active material, the silicon-based active material includes at least one selected from the group consisting of SiOx (x = 0) and SiOx (0 < x < 2), and a negative electrode composition is provided in which, based on 100 parts by weight of the silicon-based active material, 70 parts by weight or more of the SiOx (x = 0) is included.

[0073] In one embodiment of the present application, the negative electrode active material consists of a silicon-based active material, the silicon-based active material includes at least one selected from the group consisting of SiOx (x = 0) and SiOx (0 < x < 2), and a negative electrode composition is provided in which, based on 100 parts by weight of the silicon-based active material, 70 parts by weight or more of the SiOx (x = 0) is included.

[0074] In one embodiment of the present application, the silicon-based active material may include at least one selected from the group consisting of SiOx (x = 0), SiOx (0 < x < 2), SiC, and Si alloys.

[0075] The active material of the present invention includes a silicon-based active material. The silicon-based active material may be SiOx, Si / C, or Si. SiOx may include a compound represented by SiOx (0 ≦ x < 2). In the case of SiO2, since it does not react with lithium ions and cannot store lithium, x is preferably within the above range. The silicon-based active material may be Si / C or Si composed of a composite of Si and C. Also, two or more of the above silicon-based active materials may be mixed and used. The negative electrode active material may further include a carbon-based active material together with the above-described silicon-based active material. The carbon-based active material can contribute to improving excellent cycle characteristics or battery life performance of the negative electrode or secondary battery of the present invention.

[0076] Generally, silicon-based active materials are known to have a capacity more than 10 times higher than that of carbon-based active materials. Therefore, when applying silicon-based active materials to the negative electrode, it is expected that electrodes with high-level energy density can be realized even with a thin thickness.

[0077] In one embodiment of the present application, the carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, and soft carbon, and preferably may include at least one selected from the group consisting of artificial graphite and natural graphite.

[0078] In one embodiment of the present application, the negative electrode active material is (1) at least one of artificial graphite, natural graphite, surface-modified graphite, coke, hard carbon, soft carbon, carbon fiber, conductive carbon, and combinations thereof, (2) a silicon-based alloy, (3) i) at least one of artificial graphite, natural graphite, surface-modified graphite, coke, hard carbon, soft carbon, carbon fiber, conductive carbon, and combinations thereof, and ii) a metal complex compound containing or consisting of a metal selected from the group consisting of Al, Ag, Bi, In, Ge, Mg, Pb, Si, Sn, Ti, and combinations thereof, (4) a lithium complex metal oxide, (5) a lithium-containing nitride, (6) silicon-graphene, (7) silicon-carbon nanotube, (8) silicon oxide, (9) silicon, and (10) any substance including combinations thereof.

[0079] In one embodiment of the present application, the silicon-based active material includes at least one selected from the group consisting of SiOx (x = 0) and SiOx (0 < x < 2), and provides a negative electrode composition containing 70 parts by weight or more of the SiOx (x = 0) based on 100 parts by weight of the silicon-based active material.

[0080] In another embodiment, the silicon-based active material may contain 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more of the SiOx (x=0) based on 100 parts by weight of the silicon-based active material, and may contain 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.

[0081] In one embodiment of the present application, the silicon-based active material may be pure silicon (Si) alone. The use of pure silicon (Si) as the silicon-based active material may mean that the silicon-based active material contains pure Si particles (SiOx (x=0)) that are not bonded with other particles or elements, based on 100 parts by weight of the total silicon-based active material, within the above range.

[0082] Silicon-based active materials have a significantly higher capacity than conventional graphite-based active materials, and efforts to use them are increasing. However, because of their high volume expansion during charging and discharging, their use is limited to mixing a small amount with graphite-based active materials.

[0083] Therefore, in the present invention, a silicon-based active material is used as the negative electrode active material to improve capacity performance, while a thermally crosslinkable negative electrode binder solution under specific conditions is used to solve the problems of maintaining the conductive path and maintaining the bond between the conductive material, binder, and active material due to the volume expansion as described above.

[0084] On the other hand, the average particle size (D50) of the silicon-based active material of the present invention may be 5 μm to 10 μm, specifically 5.5 μm to 8 μm, and more specifically 6 μm to 7 μm. When the average particle size is within the above range, the specific surface area of ​​the particles is within an appropriate range, and the viscosity of the negative electrode slurry is formed within an appropriate range. This allows smooth dispersion of the particles constituting the negative electrode slurry. In addition, when the size of the silicon-based active material is equal to or greater than the above lower limit range, the complex of the conductive material and the binder in the negative electrode slurry has an excellent contact area between the silicon particles and the conductive material, and the conductive network is more likely to be maintained, thereby increasing the capacity retention rate. On the other hand, when the average particle size satisfies the above range, silicon particles that are too large are excluded, and the surface of the negative electrode is formed smoothly, thereby preventing the non-uniform phenomenon of current density during charging and discharging.

[0085] In one embodiment of the present application, the silicon-based active material generally has a characteristic BET specific surface area. The BET specific surface area of ​​the silicon-based active material is preferably less than 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m 2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET specific surface area is determined in accordance with DIN 66131 (using nitrogen).

[0086] In one embodiment of the present application, silicon-based active material may be, for example, in crystalline or amorphous form, and is preferably not porous.Silicon particles are preferably spherical or shard particles.Alternatively, but less preferably, silicon particles may have a fibrous structure or be in the form of silicon-containing film or coating.

[0087] In one embodiment of the present application, there is provided a negative electrode composition in which the negative electrode active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0088] In one embodiment of the present application, there is provided a negative electrode composition in which the silicon-based active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

[0089] In another embodiment, the silicon-based active material may be included in an amount of 60 parts by weight or more, preferably 65 parts by weight or more, more preferably 70 parts by weight or more, based on 100 parts by weight of the negative electrode composition, and may be included in an amount of 95 parts by weight or less, preferably 90 parts by weight or less, more preferably 85 parts by weight or less.

[0090] According to the negative electrode composition of the present application, even if a silicon-based active material with extremely high capacity is used within the above range, a specific conductive material and binder that suppress the volume expansion rate during charge and discharge are used, so that even if the above range is included, the performance of the negative electrode is not reduced and the negative electrode has excellent output characteristics during charge and discharge.

[0091] In one embodiment of the present application, the silicon-based active material may have a non-spherical morphology, and the circularity thereof is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.

[0092] In this application, the circularity is determined by the following formula 1-1, where A is the area and P is the perimeter. [Formula 1-1] 4πA / P 2

[0093] In the past, it was common to use only graphite-based compounds as negative electrode active materials, but in recent years, as the demand for high-capacity batteries has increased, there have been increasing attempts to mix silicon-based compounds to increase capacity. However, silicon-based compounds have a limitation in that their volume expands rapidly during the charge / discharge process, damaging the conductive path formed in the negative electrode active material layer and reducing the performance of the battery.

[0094] Therefore, in one embodiment of the present application, the negative electrode composition may use a binder having the above characteristics and simultaneously contain a specific negative electrode conductive material.

[0095] In one embodiment of the present application, there is provided a negative electrode composition in which the negative electrode conductive material includes at least one selected from the group consisting of a dot-like conductive material, a sheet-like conductive material, and a linear conductive material.

[0096] In one embodiment of the present application, the dot-shaped conductive material may be used to improve the conductivity of the negative electrode, and refers to a conductive material that forms conductivity without inducing a chemical change and has a circular or dot-shaped form. Specifically, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and may preferably include carbon black in that it realizes high conductivity and has excellent dispersibility.

[0097] In one embodiment of the present application, the dotted conductive material has a BET specific surface area of ​​40 m 2 / g or more 70m 2 / g or less, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.

[0098] In one embodiment of the present application, the particle diameter of the dotted conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 40 nm to 60 nm.

[0099] In one embodiment of the present application, the conductive material may include a sheet-shaped conductive material.

[0100] The planar conductive material refers to a conductive material that increases surface contact between silicon particles in a negative electrode to improve conductivity and simultaneously suppresses disconnection of a conductive path due to volume expansion. The planar conductive material may be referred to as a plate-shaped conductive material or a bulk-type conductive material.

[0101] In one embodiment of the present application, the sheet conductive material may include at least one selected from the group consisting of platelet graphite, graphene, graphene oxide, and graphite flakes, and may be preferably platelet graphite.

[0102] In one embodiment of the present application, the average particle size (D50) of the sheet conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. If the range is satisfied, the sufficient particle size makes it easy to disperse the negative electrode slurry without causing an excessive increase in viscosity. Therefore, when dispersing using the same equipment and time, the dispersion effect is excellent.

[0103] In one embodiment of the present application, there is provided a negative electrode composition in which the sheet conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 4.0 μm or more and 5.0 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.

[0104] In one embodiment of the present application, the sheet conductive material may be a high-specific surface area sheet conductive material having a high BET specific surface area; or a low-specific surface area sheet conductive material.

[0105] In one embodiment of the present application, the sheet conductive material may be a high-specific surface area sheet conductive material or a low-specific surface area sheet conductive material without any restrictions. However, the sheet conductive material in the present application may be affected to some extent by dispersion in terms of electrode performance, and it may be particularly preferable to use a low-specific surface area sheet conductive material that does not cause dispersion problems.

[0106] In one embodiment of the present application, the sheet conductive material has a BET specific surface area of ​​1 m 2 / g or more.

[0107] In another embodiment, the sheet conductive material has a BET specific surface area of ​​1 m 2 / g or more 500m 2 / g or less, preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 / g or less.

[0108] In another embodiment, the sheet conductive material is a high specific surface area sheet conductive material having a BET specific surface area of ​​50 m 2 / g or more 500m 2 / g or less, preferably 80m 2 / g or more 300m 2 / g or less, more preferably 100m 2 / g or more 250m 2 / g or less.

[0109] In another embodiment, the sheet conductive material is a sheet conductive material having a low specific surface area and a BET specific surface area of ​​1 m 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 / g or less.

[0110] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may include a plurality of carbon nanotube monomers. Specifically, unless otherwise specified, the term "bundle type" refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged side by side or entangled with the longitudinal axes of the carbon nanotube units in substantially the same orientation. The carbon nanotube monomer has a graphite sheet in the form of a cylinder with a nano-sized diameter and has an sp2 bond structure. In this case, the graphite sheet may exhibit conductive or semiconductive properties depending on the angle and structure of the winding. The bundled carbon nanotubes may be uniformly dispersed during the manufacture of the negative electrode compared to entangled type carbon nanotubes, and may smoothly form a conductive network in the negative electrode, thereby improving the conductivity of the negative electrode.

[0111] In one embodiment of the present application, there is provided a negative electrode composition, wherein the negative electrode conductive material includes linear conductive material, and the linear conductive material is a carbon nanotube.

[0112] In one embodiment of the present application, the carbon nanotubes may be SWCNTs and / or MWCNTs. When the linear conductive agent is SWCNTs, the length of the SWCNTs may be 0.5 μm to 100 μm, preferably 1 μm to 80 μm.

[0113] In one embodiment of the present application, there is provided a negative electrode composition in which the negative electrode conductive material is 5 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode composition.

[0114] In another embodiment, the negative electrode conductive material may be included in an amount of 5 parts by weight or more and 40 parts by weight or less, preferably 5 parts by weight or more and 30 parts by weight or less, and more preferably 5 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode composition.

[0115] In one embodiment of the present application, the negative electrode conductive material may include dot-like conductive materials and linear conductive materials, and a ratio of the dot-like conductive materials:linear conductive materials may satisfy 1:0.001 to 1:0.05.

[0116] In one embodiment of the present application, the negative electrode conductive material includes dot-like conductive material and linear conductive material, each of which satisfies the above-mentioned composition and ratio, so that the battery does not have a significant effect on the life characteristics of existing lithium secondary batteries, there are more points at which charging and discharging are possible, and the battery has excellent output characteristics at a high C-rate.

[0117] The negative electrode conductive material according to the present application has a completely different structure from the conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present application plays a role of capturing the contact between the silicon-based active materials, which have a very large volume expansion of the electrodes due to charging and discharging, while the positive electrode conductive material plays a role of providing some conductivity while acting as a buffer when rolled, and has a completely different structure and role from the negative electrode conductive material of the present invention.

[0118] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, in which a rate of change in thickness of a negative electrode active material layer after the negative electrode composition is cured or dried satisfies the following formula 1:

[0119] [Formula 1] 0%≦[(X2-X1) / X1]×100(%)≦15%

[0120] In the above formula 1, X1 is the thickness of the negative electrode active material layer after curing or drying the negative electrode composition at 0 cycle of the negative electrode for lithium secondary battery, X2 is the thickness of the negative electrode active material layer after the negative electrode composition of the lithium secondary battery negative electrode has been cured or dried after 30 cycles.

[0121] The 0 cycle may refer to a state in which the negative electrode for a lithium secondary battery is not yet charged / discharged after being manufactured, and specifically, may refer to the negative electrode for a lithium secondary battery after being manufactured.

[0122] In one embodiment of the present application, the negative electrode composition may contain a solvent for forming a negative electrode slurry to form a negative electrode slurry, and the negative electrode slurry may be applied to a negative electrode current collector layer to form a negative electrode.

[0123] At this time, the solid content of the negative electrode slurry may be 10% to 60%.

[0124] In one embodiment of the present application, the solvent for forming the negative electrode slurry can be used without limitation as long as the negative electrode composition can be dissolved and dispersed therein. Specifically, distilled water or NMP may be used.

[0125] In one embodiment of the present invention, the method for mixing the negative electrode slurry is not particularly limited, and examples thereof include a ball mill, a sand mill, a pigment disperser, an ultrasonic disperser, a homogenizer, a planetary mixer, a Hobart mixer, and the like. It is preferable to use a homogenizer and / or a planetary mixer for kneading.

[0126] In one embodiment of the present application, a means for applying the negative electrode slurry to the negative electrode current collector layer is not particularly limited, and a conventionally known coating device such as a comma coater, a gravure coater, a microgravure coater, a die coater, or a bar coater may be used.

[0127] After the negative electrode slurry is applied, a drying step can be carried out. The drying method is not particularly limited, and the temperature is suitably 60° C. to 200° C., preferably 100° C. to 180° C. The atmosphere can be dry air or an inert atmosphere. The thickness of the electrode (cured coating film) is not particularly limited, but is suitably 5 μm to 300 μm, preferably 10 μm to 250 μm.

[0128] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, comprising: a negative electrode current collector layer; and a negative electrode active material layer formed on one or both sides of the negative electrode current collector layer, the negative electrode active material layer comprising the negative electrode composition according to the present application.

[0129] In one embodiment of the present application, a further negative electrode active material layer may be provided on the surface opposite to the surface in contact with the negative electrode current collector layer of the negative electrode active material layer. In this case, the additional negative electrode active material layer may be a commonly used negative electrode active material layer such as a carbon-based or silicon-based layer.

[0130] 1 is a diagram showing a laminated structure of a negative electrode for a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode for a lithium secondary battery 100 including a negative electrode active material layer 20 on one surface of a negative electrode current collector layer 10 can be seen. Although FIG. 1 shows that the negative electrode active material layer is formed on one surface, the negative electrode active material layer may be formed on both surfaces.

[0131] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative electrode current collector layer is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, the surface may be formed with fine irregularities to strengthen the binding force of the negative electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. Among them, when the electrode active material is used for the negative electrode, copper foil is preferable as the current collector.

[0132] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode current collector layer has a thickness of 1 μm or more and 100 μm or less, and the negative electrode active material layer has a thickness of 20 μm or more and 500 μm or less.

[0133] However, the thickness can be changed in various ways depending on the type and application of the negative electrode used, and is not limited thereto.

[0134] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, in which the thickness change rate of the negative electrode active material layer satisfies the following formula 1:

[0135] [Formula 1] 0%≦[(X2-X1) / X1]×100(%)≦15%

[0136] In the above formula 1, X1 is the thickness of the negative electrode active material layer at 0 cycle of the negative electrode for lithium secondary battery, X2 is the thickness of the negative electrode active material layer of the negative electrode for a lithium secondary battery after 30 cycles.

[0137] The 0 cycle means a state in which the negative electrode for a lithium secondary battery is not yet charged / discharged after it is produced, and specifically may mean the negative electrode for a lithium secondary battery after it is produced.

[0138] The rate of change in thickness means the rate of change in thickness of the negative electrode active material layer after the above-mentioned negative electrode composition is cured or dried.

[0139] That is, the negative electrode for a lithium secondary battery according to the present application is characterized in that the volume expansion of the negative electrode active material is prevented and the change in thickness is small even when the cycles are repeated by using a specific negative electrode binder polymer.

[0140] In one embodiment of the present application, there is provided a lithium secondary battery including: a positive electrode; a negative electrode for a lithium secondary battery according to the present application; a separator provided between the positive electrode and the negative electrode; and an electrolyte.

[0141] 2 is a diagram showing a laminated structure of a lithium secondary battery according to an embodiment of the present application. Specifically, a lithium secondary battery anode 100 including an anode active material layer 20 on one side of an anode current collector layer 10 can be seen, and a lithium secondary battery cathode 200 including a cathode active material layer 40 on one side of a cathode current collector layer 50 can be seen, and the lithium secondary battery anode 100 and the lithium secondary battery cathode 200 are laminated with a separator 30 sandwiched therebetween.

[0142] A secondary battery according to an embodiment of the present specification may include the negative electrode for a lithium secondary battery described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the negative electrode is the same as the negative electrode described above. The negative electrode has been described above, so a detailed description thereof will be omitted.

[0143] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material.

[0144] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0145] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and satisfies 0.01≦c2≦0.3);2-c3 M c3 Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li-metal.

[0146] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material.

[0147] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular restrictions as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or a mixture of two or more of these may be used alone.

[0148] The positive electrode binder serves to improve adhesion between particles of the positive electrode active material and adhesion between the positive electrode active material and the positive electrode current collector.Specific examples of the positive electrode binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.

[0149] The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator that is generally used in secondary batteries can be used without any particular restrictions. In particular, a separator that has low resistance to ion movement of the electrolyte and excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymeric substance may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.

[0150] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in manufacturing lithium secondary batteries, but are not limited to these.

[0151] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0152] Examples of the non-aqueous organic solvent include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0153] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, can be preferably used because they have a high dielectric constant as a high-viscosity organic solvent and dissociate lithium salts well. When such a cyclic carbonate is mixed with a low-viscosity, low-dielectric-constant linear carbonate such as dimethyl carbonate and diethyl carbonate in an appropriate ratio, an electrolyte having high electrical conductivity can be produced, and therefore, it can be used more preferably.

[0154] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 -, (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of:

[0155] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride for the purposes of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.

[0156] The lithium secondary battery according to the present invention is useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), and can be particularly preferably used as a constituent battery of a medium- to large-sized battery module. Thus, the present invention also provides a medium- to large-sized battery module including the above-mentioned lithium secondary battery as a unit cell.

[0157] According to an embodiment of the present invention, there is provided a battery module including the secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate-limiting characteristics and high cycle characteristics, and therefore can be used as a power source for a medium- to large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system. EXAMPLES

[0158] In the following, preferred embodiments are presented to help understand the present invention, but the embodiments are merely illustrative of the present invention, and it is clear to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present invention. It is natural that such changes and modifications fall within the scope of the appended claims.

[0159] <Production Example> <Production of binder polymer> Example 1 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 65 g of acrylamide, 20 g of acrylic acid, 10 g of acrylonitrile, 5 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0160] Example 2 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 60 g of acrylamide, 23 g of acrylic acid, 5 g of acrylonitrile, 12 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0161] Example 3 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 65 g of acrylamide, 20 g of acrylic acid, 10 g of acrylonitrile, 5 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0162] Example 4 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 65 g of acrylamide, 20 g of acrylic acid, 10 g of acrylonitrile, 5 g of ethylene glycol diacrylate, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90° C. and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0163] Comparative Example 1 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 50 g of acrylamide, 35 g of acrylic acid, 15 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0164] Comparative Example 2 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 50 g of acrylamide, 30 g of acrylic acid, 20 g of acrylonitrile, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90° C. and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0165] Comparative Example 3 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 15 g of acrylamide, 20 g of acrylic acid, 60 g of acrylonitrile, 5 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0166] Comparative Example 4 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet was charged with 900 g of water, 45 g of acrylamide, 20 g of acrylic acid, 10 g of acrylonitrile, 25 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0167] Comparative Example 5 A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 45 g of acrylamide, 20 g of acrylic acid, 10 g of acrylonitrile, 17 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer. Comparative Example 6

[0168] A reactor equipped with an agitator, a thermometer, a reflux condenser, and a nitrogen gas inlet pipe was charged with 900 g of water, 40 g of acrylamide, 30 g of acrylic acid, 20 g of hydroxyethyl acrylate (HEA), 5 g of N'N'-methylenebisacrylamide, and 0.5 g of ammonium persulfate as a polymerization initiator, and the temperature was raised to 90°C and polymerization was carried out for 5 hours. The pH was then adjusted to 5 with an aqueous NaOH solution to produce a binder polymer.

[0169] The compositions and contents of the above-prepared Examples 1 to 4 and Comparative Examples 1 to 6 are as shown in Table 1.

[0170] [Table 1]

[0171] <Production of negative electrode slurries in Examples 1, 2, and 4 and Comparative Examples 1 to 6> As the negative electrode active material, 1) artificial graphite with d50=15μm was used, 2) silicon was used SiOx (d50=1-6μm, 0.9≦x≦1.5, specifically x=1.05), and they were mixed in a weight ratio of graphite:silicon=7:3, and the conductive material was used Super-P black and SWCNT (Super-P:SWCNT weight ratio=1:0.005), and the active material:conductive material:binder was mixed in a weight ratio of 85:5:10 to prepare a negative electrode composition. At this time, the content of water as a solvent was adjusted in consideration of the coating property, viscosity, and solid content. The viscosity of the obtained slurry composition was adjusted to be 5,000-6,000cps.

[0172] In this case, the binders prepared in Table 1 were used.

[0173] <Preparation of negative electrode slurry of Example 3> Pure Si (average particle size (D50): 3.5 μm) was used as the silicon-based active material, and Super-P black and SWCNT (Super-P:SWCNT weight ratio = 1:0.005) were used as the conductive material. The active material:conductive material:binder were mixed in a weight ratio of 85:5:10 to prepare a negative electrode composition. The content of water as a solvent was adjusted in consideration of the coating properties, viscosity, and solid content. The viscosity of the obtained slurry composition was adjusted to 5,000 to 6,000 cps.

[0174] In this case, the binder of Example 3 prepared in Table 1 was used as the binder.

[0175] <Battery manufacturing and battery characteristic evaluation> The negative electrode slurries of Examples 1 to 4 and Comparative Examples 1 to 6 were coated on copper foil with a thickness of 18 μm and dried, and a 50 μm-thick active material layer was formed on one side of the copper foil, which was then punched into a circle with a diameter of 14Φ to produce a test electrode (negative electrode). A metallic lithium foil with a thickness of 0.3 mm was used as the positive electrode, a porous polyethylene sheet with a thickness of 0.1 mm was used as the separator, and a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, in which LiPF6 was dissolved as the lithium salt at a concentration of about 1 mol / L, was used as the electrolyte.

[0176] The negative electrode, positive electrode, separator, and electrolyte were sealed in a stainless steel container to prepare a coin cell for evaluation, 2 mm thick and 32 mm in diameter. The evaluation results are shown in Table 2 below.

[0177] [Table 2]

[0178] -Initial efficiency (%): The coin cell was charged at a constant current of 0.05 C until the voltage reached 0.01 V, and then discharged at a constant current of 0.05 C until the voltage reached 1.5 V. The discharge capacity and initial efficiency were calculated and expressed as (discharge capacity / charge capacity) x 100 (%). -Capacity retention rate (%): The coin cell was charged at a constant current of 0.05C until the voltage reached 0.01V, and then discharged at a constant current of 0.05C until the voltage reached 1.5V. The cycle characteristics were then tested at a constant current of 0.2C within the same voltage range as above, and the capacity retention rate was calculated based on 30 cycles. -Thickness increase rate (%): The negative electrode active material layer of the manufactured coin cell was set to a thickness (X1), and the coin cell was charged at a constant current of 0.05 C until the voltage reached 0.01 V, and discharged at a constant current of 0.05 C until the voltage reached 1.5 V. Thereafter, the cycle characteristics were measured at a constant current of 0.2 C within the same voltage range as above, and the thickness (X2) of the negative electrode active material layer was measured from the coin cell after 30 cycles.

[0179] The above Examples 1 to 4 correspond to the cases where the negative electrode binder according to the present invention was used. As a result, even when a negative electrode active material (especially a silicon-based active material) that exhibits large volume expansion during charge / discharge is used, the volume expansion and contraction can be suppressed, and thickness changes due to electrode swelling can be minimized, thereby providing excellent life performance of the lithium secondary battery.

[0180] Specifically, a specific amount of diacrylamide or diacrylate compound is included to partially crosslink the linear polymer, forming a partially crosslinked structure. Due to the partially crosslinked structure of the binder itself, it has been confirmed that the change in electrode thickness during charging and discharging is small, and the capacity retention rate is improved during the life evaluation.

[0181] In particular, in the case of Example 3, the negative electrode uses 100% Si as the negative electrode active material. In the case of pure Si, the volume expansion is intense due to charging and discharging, and it is generally difficult to apply this. However, it was confirmed that the initial efficiency is superior to other Examples 1, 2, and 4 as described above by including a specific binder according to the present invention. The thickness increase is also greater than other Examples 1 and 2 due to the material characteristics because pure Si particles are used, but by applying the binder of the present invention, the thickness increase rate is within the range of 0 to 15%, which corresponds to a level that does not cause a problem when driving the negative electrode. That is, it was confirmed that the negative electrode of Example 3 can easily suppress volume expansion while maximizing the capacity characteristics.

[0182] The comparative examples 1 and 2 are cases where the α,β-unsaturated nitrile-containing monomer or the diacrylamide- or diacrylate-containing compound is not included. In these cases, the initial efficiency is similar to that of the examples, but it is confirmed that the volume expansion of the silicon-based active material cannot be suppressed and the binder cannot function.

[0183] In Comparative Examples 3 to 5, the negative electrode binder polymer contains four compositions as in the present invention, but the content parts are different. In these cases, as in Comparative Examples 1 and 2, it was confirmed that the volume expansion of the silicon-based active material could not be suppressed, the conductive path was damaged, and the battery performance was reduced.

[0184] Furthermore, a monomer containing hydroxyalkyl (meth)acrylate was used in Comparative Example 6. In this case, the initial efficiency was similar to that of the Examples, but it was confirmed that the volume expansion of the silicon-based active material could not be suppressed and the binder could not function.

Claims

1. A negative electrode composition comprising a negative electrode binder polymer, a negative electrode active material, and a negative electrode conductive material, The negative electrode binder polymer comprises: a (meth)acrylamide group-containing compound; an unsaturated organic acid or a salt of an unsaturated organic acid; a monomer containing an α,β-unsaturated nitrile; and a diacrylamide or diacrylate-containing compound; a negative electrode composition comprising, based on 100 parts by weight of the negative electrode binder polymer, 30 parts by weight or more and 80 parts by weight or less of the (meth)acrylamide group-containing compound; 1 part by weight or more and 30 parts by weight or less of the monomer containing an α,β-unsaturated nitrile; and 0.1 parts by weight or more and 15 parts by weight or less of the diacrylamide or diacrylate-containing compound.

2. 2. The anode composition of claim 1, wherein the diacrylamide or diacrylate-containing compound is an alkyl diacrylamide; an alkylene oxide diacrylamide; or an alkylene oxide diacrylate.

3. 2. The negative electrode composition according to claim 1, wherein the molar ratio of the (meth)acrylamide group-containing compound to the unsaturated organic acid or the salt of the unsaturated organic acid is from 1:0.1 to 1:0.

6.

4. The negative electrode composition according to claim 1 , comprising 1 part by weight or more and 20 parts by weight or less of the negative electrode binder polymer based on 100 parts by weight of the negative electrode composition.

5. 2. The negative electrode composition according to claim 1, wherein the weight average molecular weight of the negative electrode binder polymer is 100,000 g / mol or more and 3,000,000 g / mol or less.

6. 2. The negative electrode composition according to claim 1, wherein the negative electrode conductive material is at least one selected from the group consisting of a dot-like conductive material; a sheet-like conductive material; and a linear conductive material.

7. The negative electrode composition according to claim 1 , wherein the negative electrode active material comprises at least one selected from the group consisting of a silicon-based active material and a carbon-based active material.

8. 8. The negative electrode composition according to claim 7, wherein the negative electrode active material comprises a silicon-based active material, the silicon-based active material comprises at least one selected from the group consisting of SiOx (x=0) and SiOx (0<x<2), and the silicon-based active material comprises 70 parts by weight or more of the SiOx (x=0) based on 100 parts by weight of the silicon-based active material.

9. 2. The negative electrode composition according to claim 1, wherein the negative electrode active material is a silicon-based active material, the silicon-based active material includes at least one selected from the group consisting of SiOx (x=0) and SiOx (0<x<2), and the silicon-based active material includes 70 parts by weight or more of the SiOx (x=0) based on 100 parts by weight of the silicon-based active material.

10. The negative electrode composition according to claim 9, wherein the silicon-based active material has an average particle size (D50) of 5 μm to 10 μm.

11. 2. The negative electrode composition according to claim 1, wherein the negative electrode conductive material includes dot-like conductive materials and linear conductive materials, and a ratio of the dot-like conductive materials to the linear conductive materials satisfies 1:0.001 to 1:0.

05.

12. The negative electrode composition of claim 1 , wherein the negative electrode active material is 60 parts by weight or more based on 100 parts by weight of the negative electrode composition.

13. A negative electrode current collector layer; and A negative electrode active material layer comprising the negative electrode composition according to any one of claims 1 to 12, which is formed on one or both sides of the negative electrode current collector layer; A negative electrode for a lithium secondary battery comprising:

14. The thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, 14. The negative electrode for a lithium secondary battery according to claim 13, wherein the negative electrode active material layer has a thickness of 20 μm or more and 500 μm or less.

15. The negative electrode for a lithium secondary battery according to claim 13, wherein the thickness change rate of the negative electrode active material layer satisfies the following formula 1: [Formula 1] 0%≦[(X2-X1) / X1]×100(%)≦15% In the above formula 1, X1 is the thickness of the negative electrode active material layer at 0 cycle of the negative electrode for lithium secondary battery, X2 is the thickness of the negative electrode active material layer of the negative electrode for a lithium secondary battery after 30 cycles.

16. positive electrode; The negative electrode for a lithium secondary battery according to claim 13 ; A separator disposed between the positive electrode and the negative electrode; and an electrolyte.

Citation Information

Patent Citations

  • Preparation method of negative pole piece water-based binder

    CN111057184A

  • Running regulating device for vehicle

    JP1988061655A

  • Anode for lithium ion battery

    JP2009080971A