Non-oriented polypropylene film
The unstretched polypropylene film with a specific resin composition addresses the challenge of high sealing strength and lack of transparency in biomass-derived films by incorporating biomass-derived polyethylene and propylene/α-olefin random copolymer, ensuring both heat-sealing strength and easy-opening properties while maintaining transparency and impact resistance.
Patent Information
- Application Number
- JP2021021422
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-22
- Filing Date
- 2021-02-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-02-15
AI Technical Summary
Conventional resin films containing biomass-derived polyethylene have high sealing properties and heat-sealing strength, making them difficult to open, and lack transparency and impact resistance necessary for packaging materials.
An unstretched polypropylene film with a base layer of polypropylene resin, an intermediate layer of biomass-derived polyethylene resin, and a sealant layer composed of 40 to 70% polyethylene resin and 30 to 60% propylene/α-olefin random copolymer, with a molecular weight distribution of 3.5 or less, achieving both heat-sealing strength and easy-opening properties.
The film achieves both heat-sealing strength and easy-opening properties while maintaining transparency and impact resistance, contributing to environmental sustainability by using biomass-derived materials.
Smart Images

Figure 0007575291000004 
Figure 0007575291000001 
Figure 0007575291000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented polypropylene film containing a biomass-derived polyethylene resin for reducing the environmental load. [Background technology]
[0002] Polypropylene-based films are extremely useful as packaging materials because of their excellent heat resistance, chemical resistance, heat sealing properties, etc. Packaging bags for packaging foods and other items in pillow packaging or the like are made of sealant films that can be fused by heat sealing or the like. These packaging bags are required to have a hermetic film due to the need to prevent leakage of contents and to maintain hygiene during packaging. However, if the adhesive strength of the sealed portion is high, it may be difficult for weak consumers such as children and the elderly to open the bag, or excessive force may be applied when opening the bag, resulting in unintended breakage, etc.
[0003] In recent years, the increase in the concentration of carbon dioxide in the atmosphere has been cited as a major cause of global warming, and carbon neutrality is being sought in various fields to reduce the environmental burden. For example, synthetic resin materials that make up resin films are generally produced from petroleum and other raw materials, but in recent years, the use of biomass resources has been attracting attention from the perspective of carbon neutrality.
[0004] Therefore, in the field of resin films, the demand for carbon neutrality has led to the development of resin films using biomass resources, and for example, a resin film containing 5% by mass or more of biomass-derived polyethylene is known (see, for example, Patent Document 1). Biomass-derived polyethylene is produced using biomass-derived ethanol obtained from plant raw materials as a raw material, and therefore the amount of conventional petroleum-derived (fossil fuel)-derived materials used can be reduced. Therefore, by incorporating a large amount of biomass-derived polyethylene into a resin film, the contribution to reducing the environmental load can be further increased.
[0005] However, conventional resin films containing biomass-derived polyethylene have poor ease of opening because of their tight sealing properties and high heat seal strength. In addition, the films do not provide satisfactory transparency or impact resistance, which are necessary functions for the films. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-251006 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above-mentioned points, and provides a non-oriented polypropylene film that contains a biomass-derived polyethylene resin while achieving both the heat seal strength and easy-openability required for a packaging material, and also has appropriate transparency and impact resistance. [Means for solving the problem]
[0008] That is, the invention of claim 1 relates to a non-oriented polypropylene-based film having a base layer, an intermediate layer, and a sealant layer, wherein the base layer is made of a polypropylene-based resin, the intermediate layer is made of a biomass-derived polyethylene-based resin and a polypropylene-based resin, and has a composition in which the biomass-derived polyethylene-based resin is 60% by weight or less, and the sealant layer is made of 40 to 70% by weight of a polyethylene-based resin having a molecular weight distribution (Mw / Mn) of 3.5 or less in a molecular weight distribution curve obtained by GPC measurement in accordance with JIS K 7252-1 (2008), and 30 to 60% by weight of a propylene-α-olefin random copolymer.
[0009] The invention of claim 2 relates to the non-oriented polypropylene film according to claim 1, wherein the polypropylene resin of the base layer is made of a propylene homopolymer. Effect of the Invention
[0010] According to the invention of claim 1, the non-oriented polypropylene-based film has a base layer, an intermediate layer, and a sealant layer, the base layer is a polypropylene-based resin, the intermediate layer is composed of a biomass-derived polyethylene-based resin and a polypropylene-based resin, and the biomass-derived polyethylene-based resin is 60% by weight or less, and the sealant layer is composed of 40 to 70% by weight of a polyethylene-based resin having a molecular weight distribution (Mw / Mn) of 3.5 or less in a molecular weight distribution curve obtained by GPC measurement in accordance with JIS K 7252-1 (2008) and 30 to 60% by weight of a propylene-α-olefin random copolymer. Therefore, while containing a biomass-derived polyethylene-based resin, it is possible to achieve both heat seal strength and easy opening properties required for a packaging material, and to obtain transparency and impact resistance suitable for a packaging material.
[0011] According to the non-oriented polypropylene film of the invention of claim 2, in the invention of claim 1, the polypropylene resin of the base layer is made of a propylene homopolymer, so that the transparency can be further improved. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of a non-stretched polypropylene film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] 1 according to one embodiment of the present invention is a film having a base layer 20, an intermediate layer 30, and a sealant layer 40, and from the viewpoint of carbon neutrality, the intermediate layer 30 contains a biomass-derived polyethylene resin. The unstretched polypropylene film 10 is produced to a predetermined thickness by melting the resins constituting each layer and using a known production method such as a T-die method.
[0014] The unstretched polypropylene-based film 10 is preferably used as a packaging material for food packaging bags for fresh foods, processed foods, confectionery, etc., packaging materials for packaging bags for detergents, cosmetics, other medicines, etc., and appropriate industrial film products. As a packaging material for food packaging bags, it can be widely used in heat-resistant applications such as packaging materials (sealant films) for retort foods that are filled with various foods, sealed, and then boiled or retorted. The polypropylene-based film 10 as this type of packaging material can form a packaging bag by itself. In addition, the polypropylene-based film 10 may be laminated with a polyamide film, a polyester film, or even an aluminum foil, etc., as necessary.
[0015] The base layer 20 is a layer that becomes the surface of the polypropylene-based film 10, and is made of a polypropylene-based resin. The polypropylene-based resin is selected from general polypropylene-based resins. For example, it is selected from at least one of propylene homopolymer, propylene-α-olefin random copolymer such as propylene-ethylene random copolymer and propylene-ethylene-butene random copolymer, or propylene-ethylene block copolymer. The polypropylene-based resin may be one type or a mixture of two or more types. In addition, the polypropylene-based resin of the base layer 20 is a propylene homopolymer, so that the transparency can be further improved. In addition, as a catalyst used in producing the polypropylene-based resin, a Ziegler-Natta catalyst containing a solid titanium catalyst component and an organometallic compound catalyst component, or a metallocene catalyst can be used.
[0016] The intermediate layer 30 is composed of a biomass-derived polyethylene resin and a polypropylene resin, and is composed of a composition in which the biomass-derived polyethylene resin is 60% by weight or less. The biomass-derived polyethylene resin is a polyethylene resin obtained by processing a plant raw material. Specifically, ethanol is produced from a sugar liquid extracted from a plant raw material such as sugar cane through alcohol fermentation by yeast, and after ethylene is produced, polyethylene is produced through a known resinification process. This biomass-derived polyethylene resin contributes to reducing the environmental load of the final product, so that the contribution to reducing the environmental load is increased by increasing the weight blending ratio. In addition, the polypropylene resin used in the intermediate layer 30 is selected from general polypropylene resins, and may be the same as or different from the resin used in the base layer 20.
[0017] In the intermediate layer 30, as described above, the higher the blending ratio of the biomass-derived polyethylene resin, the greater the contribution to reducing the environmental load. However, if the blending ratio is too high, there is a risk that the performance such as easy opening, transparency, and impact resistance may not be sufficiently obtained. In addition, the contribution to reducing the environmental load is sufficient if the biomass-derived polyethylene resin is contained in a small amount (not 0% by weight). The lower the blending ratio of the biomass-derived polyethylene resin, the more the effect on the film performance tends to be suppressed, and if it is less than a certain ratio (for example, 5% by weight), the effect on the film performance is not observed. Therefore, the blending ratio of the biomass-derived polyethylene resin is appropriately set based on the balance between the contribution to reducing the environmental load and the desired film performance.
[0018] The sealant layer 40 is a layer that becomes the heat seal surface of the polypropylene film 10, and is composed of 40 to 70% by weight of polyethylene resin and 30 to 60% by weight of propylene-α-olefin random copolymer.
[0019] The polyethylene resin used for the sealant layer 40 has a molecular weight distribution (Mw / Mn) of 3.5 or less in the molecular weight distribution curve obtained by GPC measurement in accordance with JIS K 7252-1 (2008). If the molecular weight distribution (Mw / Mn) value of the molecular weight distribution curve of the polyethylene resin is too large (the molecular weight distribution is too broad), the transparency may decrease.
[0020] The type of polyethylene resin of the sealant layer 40 is not particularly limited as long as it satisfies the above molecular weight distribution value. As the polyethylene resin having the above molecular weight distribution (Mw / Mn) of 3.5 or less, for example, petroleum-derived polyethylene resin is preferable because it is easily available. Petroleum-derived polyethylene resin is a known polyethylene resin produced from petroleum or the like as a raw material, and examples thereof include linear low-density polyethylene resin (LLDPE), high-density polyethylene (HDPE), and low-density polyethylene (LDPE). Linear low-density polyethylene resin is a random copolymer of ethylene and an α-olefin having 3 to 8 carbon atoms, and is excellent in terms of tensile strength, tear resistance, impact strength, seal strength, stress cracking resistance, etc. High-density polyethylene is excellent in terms of tensile strength, tear resistance, impact strength, seal strength, heat resistance, etc. The use of the above resins depends on the application, etc.
[0021] The polyethylene resin of the sealant layer 40 is preferably a linear low density polyethylene from the viewpoints of transparency, flexibility, moldability, etc. The melt flow rate of the linear low density polyethylene resin is not particularly limited, but may be, for example, 0.1 to 30 g / 10 min, preferably 1 to 10 g / 10 min, as measured under conditions of 190°C and a load of 2.16 kg as described in JIS K 7210. The density of the linear low density polyethylene resin is not particularly limited, but may be, for example, 0.865 g / cm, as measured under conditions as described in JIS K 7112. 3 ~0.965g / cm 3 Less than 0.885 g / cm 3 ~0.945g / cm 3Examples of the metallocene catalyst include the following. The method for producing the ethylene-α-olefin copolymer is not particularly limited, and the copolymer can be produced by, for example, a gas phase polymerization reaction, a liquid phase polymerization reaction, or the like, using a known catalyst such as a Ziegler catalyst or a metallocene catalyst. Among these, the use of a metallocene catalyst is preferred because it allows the ethylene-α-olefin copolymer having the desired physical properties to be easily produced. As the metallocene catalyst, a known catalyst can be used, such as a metallocene compound made of a transition metal of Group 4 of the periodic table activated with an organoaluminum compound and / or an ionic compound.
[0022] Propylene-α-olefin random copolymer is a resin that plays a role in ensuring heat sealability. Examples of the propylene-α-olefin random copolymer include propylene-ethylene-butene random copolymer, propylene-ethylene random copolymer, and propylene-butene copolymer. The melt flow rate of the propylene-α-olefin random copolymer is not particularly limited, but may be, for example, 0.1 to 20 g / 10 min, preferably 3 to 15 g / 10 min, as measured at 230° C. and a load of 2.16 kg as described in JIS K 7210.
[0023] In the sealant layer 40, if the blending ratio of the polyethylene resin is too low, i.e., if the blending ratio of the propylene-α-olefin random copolymer is too high, the heat seal strength may become too high and easy opening may not be obtained. Also, if the blending ratio of the polyethylene resin is too high, the transparency may decrease and the blending ratio of the propylene-α-olefin random copolymer may become too low, and sufficient heat seal strength may not be obtained.
[0024] In each of the base layer 20, the intermediate layer 30, and the sealant layer 40, various additives such as lubricants, antiblocking agents, heat stabilizers, antioxidants, light stabilizers, crystal nucleating agents, and ultraviolet absorbers may be added as necessary.
[0025] The thickness of the non-stretched polypropylene film 10 is not particularly limited, but is usually 20 to 200 μm, and preferably 20 to 150 μm. The thickness ratio of the base layer 20, intermediate layer 30, and sealant layer 40 of the non-stretched polypropylene film 10 is in the range of 10% to 33.3%: 33.4% to 80%: 10% to 33.3%. EXAMPLES
[0026] [Film Creation] For the films of prototypes 1 to 19, the raw resins were melted and kneaded based on the resin blending ratio (weight %) described below, co-extruded by a T-die film molding machine, and cooled by a cooling roll to produce a non-oriented polypropylene film. The raw materials used to compose each layer were blended in proportions that totaled 100% by weight. The non-oriented polypropylene films of each prototype were produced under the same settings, and all films had a thickness of 30 μm, with a thickness ratio of the base layer, intermediate layer, and sealant layer of 1:3:1.
[0027] [Polypropylene resin material] The polypropylene resins used were the following resins (A1) to (A3). ·Resin (A1): Density 0.9g / cm 3 Homopolypropylene resin (Japan Polypropylene Corporation, "FB3B") ·Resin (A2): Density 0.9g / cm 3 Random polypropylene resin (Japan Polypropylene Corporation, "WFW4M") ·Resin (A3): Density 0.9g / cm 3 Random polypropylene resin (Japan Polypropylene Corporation, "FW3GT") ·Resin (A4): Density 0.9g / cm 3 Random polypropylene resin (Japan Polypropylene Corporation, "WXK1233")
[0028] [Biomass-derived polyethylene resin material] The biomass-derived polyethylene resins used were the following resins (B1) to (B3). ·Resin (B1): Density 0.916g / cm 3 Biomass-derived polyethylene resin (manufactured by Braskem SA, "SLH218") ·Resin (B2): Density 0.918g / cm 3 Biomass-derived polyethylene resin (Braskem SA, "SLL318") ·Resin (B3): Density 0.961g / cm 3 Biomass-derived polyethylene resin (manufactured by Braskem SA, "SGM9460")
[0029] [Petroleum-derived polyethylene resin material] The petroleum-derived polyethylene resin used was the following resin (C1). ·Resin (C1): Density 0.919g / cm 3 Petroleum-derived polyethylene resin (Ube Maruzen Polyethylene Co., Ltd., "2040F")
[0030] [Prototype 1] The unstretched polypropylene film of prototype 1 was produced with a base layer of 100% resin (A1), an intermediate layer of 97% resin (A2) and 3% resin (B1), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0031] [Prototype 2] The unstretched polypropylene film of prototype 2 was produced using a base layer of 100% resin (A1), an intermediate layer of 95% resin (A2) and 5% resin (B1), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0032] [Prototype 3] The unstretched polypropylene film of prototype 3 was produced using a base layer of 100% resin (A1), an intermediate layer of 40% resin (A2) and 60% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0033] [Prototype 4] The unstretched polypropylene film of prototype 4 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0034] [Prototype 5] The unstretched polypropylene film of prototype 5 was produced using a base layer of 100% resin (A1), an intermediate layer of 90% resin (A1) and 10% resin (B1), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0035] [Prototype 6] The unstretched polypropylene film of prototype 6 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A1) and 20% resin (B1), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0036] [Prototype 7] The unstretched polypropylene film of prototype 7 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A1), 10% resin (B1), and 10% resin (B2), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0037] [Prototype 8] The unstretched polypropylene film of prototype 8 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A1), 10% resin (B1), and 10% resin (B3), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0038] [Prototype 9] The unstretched polypropylene film of prototype 9 was produced using a base layer of 100% resin (A1), an intermediate layer of 60% resin (A1) and 40% resin (B1), and a sealant layer of 40% resin (A2) and 60% resin (C1).
[0039] [Prototype 10] The unstretched polypropylene film of prototype 10 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 30% resin (A2) and 70% resin (C1).
[0040] [Prototype example 11] The unstretched polypropylene film of prototype 11 was produced using a base layer of 100% resin (A3), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0041] [Prototype 12] The unstretched polypropylene film of prototype 12 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 100% resin (A4).
[0042] [Prototype 13] The unstretched polypropylene film of prototype 13 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (B1).
[0043] [Prototype 14] The unstretched polypropylene film of prototype 14 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (B2).
[0044] [Prototype 15] The unstretched polypropylene film of prototype 15 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (B3).
[0045] [Prototype 16] The unstretched polypropylene film of prototype 16 was produced using a base layer of 100% resin (A1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A1) and 40% resin (C1).
[0046] [Prototype 17] The unstretched polypropylene film of prototype 17 was produced using a base layer of 100% resin (A1), an intermediate layer of 20% resin (A2) and 80% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0047] [Prototype 18] The unstretched polypropylene film of prototype 18 was produced using a base layer of 100% resin (A1), an intermediate layer of 100% resin (A1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0048] [Prototype Example 19] The unstretched polypropylene film of prototype 19 was produced using a base layer of 100% resin (C1), an intermediate layer of 80% resin (A2) and 20% resin (B1), and a sealant layer of 60% resin (A2) and 40% resin (C1).
[0049] [GPC measurement of polyethylene resin] Biomass-derived polyethylene resins (resins B1 to B3) and polyethylene resin (resin C1) were measured by gel permeation chromatography (GPC). In accordance with JIS K 7252-1 (2008), the measurement was performed using a Tosoh Corporation "HLC-8321GPC / HT" measuring device, two columns, "TSKgel guardcolumn HHR(S)" and "GMHHR-H(S)HT", and a differential refractometer as a detector. In addition, the concentration of the resin sample was adjusted to 0.1 wt / vol% using o-dichlorobenzene as the eluent and completely dissolved, and the temperature setting of the column and injector was set to 145°C, and the flow rate was set to 1.0 mL / min. In addition, polystyrene was used as the standard substance for molecular weight conversion.
[0050] For the biomass-derived polyethylene resins (resins B1 to B3) and the polyethylene resin (resin C1), the molecular weight distribution (Mw / Mn) of the molecular weight distribution curve obtained from the GPC measurement was 4.6 for resin (B1), 4.6 for resin (B2), 13.3 for resin B3, and 2.9 for resin C1.
[0051] [Evaluation of the performance of non-oriented polypropylene films] Using the laminated films corresponding to prototypes 1 to 19, the haze (%), dart impact strength (J), and heat seal strength (N / 15 mm) of the non-oriented polypropylene-based film were tested, and the performance was evaluated based on the results. In addition, in the overall evaluation of the performance of the non-oriented polypropylene-based film, if it was judged to be "good" or better in all tests, it was rated as "good (◯)", and if it was judged to be "poor" in any test, it was rated as "poor (×)". The results are shown in Tables 1 to 3 below.
[0052] [Haze measurement] Haze (%) is an index of transparency, and was measured in accordance with JIS K 7136 (2000) using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) For the unstretched polypropylene films of prototypes 1 to 19, from the viewpoint of transparency required for packaging materials, a measurement result of 6% or less was rated as "good (◯)", particularly when it was 5.5% or less, it was rated as "excellent (◎)", and when it was more than 6%, it was rated as "unacceptable (×)".
[0053] [Measurement of dart impact strength] The dart impact strength (J) is an index of penetration destruction, and was measured in accordance with JIS K 7124-1 (1999) using a dart impact tester with a low temperature chamber (manufactured by Toyo Seiki Seisakusho). In this measurement, the films of prototypes 1 to 19 were fixed horizontally by a fixing device, and a dart (hemispherical metal penetration part: diameter 25.4 mm) with an adjusted mass was dropped to break and penetrate the film, and the breaking energy (J) was obtained. From the viewpoint of the impact resistance required for packaging materials, the dart impact strength (J) was evaluated as "good (◯)" when the measurement result was 0.4 (J) or more, and "unacceptable (×)" when it was less than 0.4 (J).
[0054] [Heat seal strength measurement] The heat seal strength (N / 15mm) is one of the indices of adhesive suitability, and was measured using a tensile tester (Shimadzu Corporation's "EZ-SX") in accordance with JIS Z 0238 (1998). In this measurement, the heat seal layers (40) of the films of prototypes 1 to 19 were overlapped with each other and heat sealed at a temperature of 125°C, a pressure of 0.2 MPa, and a sealing time of 0.5 seconds using a thermal gradient tester (Toyo Seiki Seisakusho). The film was cut into a width of 15 mm and the heat seal portion was peeled off at a peeling speed of 200 mm / min using a tensile tester to determine the heat seal strength. From the viewpoint of the heat seal strength and ease of opening required for packaging materials, the heat seal strength (N / 15mm) was evaluated as "good (◯)" when it was in the range of 3 to 7 (N / 15mm), and as "bad (×)" when it was less than 3 (N / 15mm) or more than 7 (N / 15mm).
[0055] [Table 1]
[0056] [Table 2]
[0057] [Table 3]
[0058] [Results and Discussion] As shown in Tables 1 to 3, prototypes 1 to 11 received an overall rating of "good (◯)," while prototypes 12 to 19 received an overall rating of "poor (×)." Prototype 12, which received an overall rating of "poor," differs from prototypes 4 and 10, which received an overall rating of "good," in that the sealant layer does not contain a polyethylene-based resin. As a result, since the heat seal strength was high in prototype 12, it was found that easy opening cannot be achieved unless the sealant layer contains a polyethylene-based resin.
[0059] Samples 13 to 15, which were given an overall rating of "poor," differ from Sample 4, which was given an overall rating of "good," in the density of the polyethylene resin contained in the sealant layer and the molecular weight distribution (Mw / Mn) value of the molecular weight distribution curve obtained from the GPC measurement. 3 Resin C1 has a molecular weight distribution (Mw / Mn) of 2.9, and prototype 13 has a density of 0.916 g / cm 3 Resin B1 has a molecular weight distribution (Mw / Mn) of 4.6, and prototype 14 has a density of 0.918 g / cm 3 Resin B2 has a molecular weight distribution (Mw / Mn) of 4.6, and prototype 15 has a density of 0.961 g / cm 3 and resin B3 having a molecular weight distribution (Mw / Mn) of 13.3.
[0060] All of the prototypes 13 to 15 had higher haze values than the prototype 4, and the haze value was particularly high in the prototype 15, which contained the resin B3, whose molecular weight distribution value was significantly larger than the other resins (B1, B2, C1). This shows that the larger the molecular weight distribution (Mw / Mn) value of the molecular weight distribution curve obtained from the GPC measurement, the higher the haze value and the less transparent the resin becomes. Therefore, it is considered that the preferable molecular weight distribution (Mw / Mn) of the polyethylene resin contained in the sealant layer is 3.5 or less. In addition, as can be seen from the prototype 15, it was found that if the molecular weight distribution (Mw / Mn) value is too large, the dart impact strength and heat seal strength decrease.
[0061] Sample 16, which received an overall rating of "Fail," differs from Sample 4, which received an overall rating of "Good," in the type of polypropylene-based resin contained in the sealant layer. That is, Sample 4 is a propylene-α-olefin random copolymer, while Sample 16 is a propylene homopolymer. As a result, Sample 16 had a significantly lower heat seal strength and a higher haze value than Sample 4. From this, it is considered that the polypropylene-based resin contained in the sealant layer is preferably a propylene-α-olefin random copolymer.
[0062] Furthermore, when the blending ratio of the resins constituting the sealant layer is examined, as can be seen from the above-mentioned prototype 12, it is not preferable to not include a polyethylene-based resin, since easy opening cannot be obtained. In prototypes 1 to 11, which were given an overall rating of "good," the blending ratio of the polyethylene-based resin in the sealant layer was the minimum of 40% by weight for prototypes 3, 4, and 11, and the maximum of 70% by weight for prototype 10. From this, it is considered that the preferable blending ratio of the polyethylene-based resin and propylene-α-olefin random copolymer in the sealant layer is 40 to 70% by weight of the polyethylene-based resin and 30 to 60% by weight of the propylene-α-olefin random copolymer.
[0063] In prototype 17, which received an overall rating of "poor," the mixing ratio of the biomass-derived polyethylene resin and the polypropylene resin in the intermediate layer is different from prototypes 3 and 4, which received an overall rating of "good." In prototype 17, the mixing ratio of resin B1 (biomass-derived polyethylene resin) was 80% by weight, and the haze value exceeded 6%, resulting in insufficient transparency. On the other hand, in prototype 3, the mixing ratio of resin B1 was 60% by weight, and the haze value was 6% or less, and in prototype 4, the mixing ratio of resin B1 was 20% by weight, and both had haze values of 6% or less. In addition, when comparing the relationship between the mixing ratio of resin B1 and the haze value in prototypes 3 and 4, the haze value of prototype 3, which had a high mixing ratio of resin B1, was higher than that of prototype 4. From this, it was found that when the mixing ratio of the biomass-derived polyethylene resin contained in the intermediate layer increased, the haze value increased and transparency was insufficient.
[0064] Sample 18, which received an overall rating of "poor," differs from Samples 3 and 4, which received an overall rating of "good," in that the intermediate layer does not contain biomass-derived polyethylene resin (the blending ratio of polypropylene resin is 100% by weight), and the dart impact strength was insufficient at 0.3 J. On the other hand, the dart impact strength of Sample 3, which has a high blending ratio of Resin B1, was 1.6 J, which was higher than that of Sample 4, which had a lower blending ratio. This shows that the dart impact strength decreases as the blending ratio of biomass-derived polyethylene resin in the intermediate layer decreases.
[0065] Here, the blending ratio of the resin constituting the intermediate layer will be considered. As can be seen from Prototype 1, when the blending ratio of the biomass-derived polyethylene resin is small, the overall evaluation was "good". On the other hand, as can be seen from Prototype 17, if the blending ratio of the biomass-derived polyethylene resin is too high, the transparency is insufficient, which is not preferable. In Prototypes 1 to 11, which were given an overall evaluation of "good", the blending ratio of the biomass-derived polyethylene resin in the intermediate layer was maximum at 60% by weight in Prototype 3.
[0066] As can be seen from the above prototype 1, if even a small amount (not 0% by weight) of biomass-derived polyethylene resin is blended in the intermediate layer, a film that has good film performance and can contribute to reducing the environmental load can be obtained. Also, as can be seen from the above prototype 3, when considering the impact on film performance, blending a large amount of biomass-derived polyethylene resin increases the haze value and causes insufficient transparency. Therefore, from the viewpoint of film performance and reducing the environmental load, it is considered that the blending ratio of biomass-derived polyethylene resin in the intermediate layer is preferably 60% by weight or less, more preferably 3 to 40% by weight.
[0067] Sample 19, which received an overall rating of "Fail," differs from Samples 4 and 11, which received an overall rating of "Good," in the type of resin that constitutes the base layer. That is, Samples 4 and 11 are polypropylene-based resins, while Sample 19 is polyethylene-based resin. As a result, in Sample 19, the film melted during heat sealing and adhered to the seal bar, making it impossible to measure the heat seal strength. For this reason, it is considered preferable for the base layer to be made of a polypropylene-based resin.
[0068] Furthermore, comparing prototype 4 and prototype 11, the difference is that the base layer of prototype 4 is made of a propylene homopolymer, while the base layer of prototype 11 is made of a propylene random copolymer. Since prototype 4 has a haze of 5.2%, which is "excellent," and prototype 11 has a haze of 5.7%, which is "good," it is believed that transparency is improved by forming the base layer from a propylene homopolymer.
[0069] As shown and described above, the non-stretched polypropylene resin film of the present invention containing biomass-derived polyethylene resin has a base layer composed of a polypropylene resin, an intermediate layer composed of a biomass-derived polyethylene resin and a polypropylene resin, the biomass-derived polyethylene resin being 60% by weight or less, and a sealant layer composed of 40 to 70% by weight of a polyethylene resin having a molecular weight distribution (Mw / Mn) of 3.5 or less in a molecular weight distribution curve obtained by GPC measurement in accordance with JIS K 7252-1 (2008), and 30 to 60% by weight of a propylene-α-olefin random copolymer. As a result, while containing a biomass-derived polyethylene resin, it is possible to achieve both heat seal strength and easy opening properties required for packaging materials, and further to obtain transparency and impact resistance suitable for packaging materials. [Industrial Applicability]
[0070] The non-oriented polypropylene film of the present invention is a polypropylene film containing a biomass-derived polyethylene resin, and is capable of achieving both the heat seal strength and easy opening required for use as a packaging material, and furthermore, is capable of obtaining appropriate transparency and impact resistance. Therefore, it is expected to be used as a new packaging material, etc., and is advantageous in utilizing biomass resources. [Explanation of symbols]
[0071] 10 Non-oriented polypropylene resin film 20 Base material layer 30 Middle Class 40 Sealant Layer
Claims
1. A non-oriented polypropylene film having a base layer, an intermediate layer, and a sealant layer, The base layer is made of a polypropylene-based resin, The intermediate layer is made of a biomass-derived polyethylene-based resin and a polypropylene-based resin, and the biomass-derived polyethylene-based resin is contained in an amount of 60% by weight or less. The sealant layer was composed of 40 to 70% by weight of a polyethylene resin having a molecular weight distribution (Mw / Mn) of 3.5 or less in a molecular weight distribution curve obtained by GPC measurement in accordance with JIS K 7252-1 (2008) and 30 to 60% by weight of a propylene-α-olefin random copolymer. A non-oriented polypropylene film.
2. 2. The non-oriented polypropylene film according to claim 1, wherein the polypropylene resin of the base layer is a propylene homopolymer.
Citation Information
Patent Citations
Resin composition for laminate and laminate and method for producing the same
JP2001200114A
Multi-layer polyolefin film and package
JP2002210899A
Polyolefin resin film
JP2012251006A
Sealant film
JP2016049727A
Unstretched polypropylene-based resin film
JP2020075400A