Nickel particles and their uses
By attaching amine, nitrile, and/or amide compounds to nickel particles, the dispersibility of conductive pastes is enhanced, addressing aggregation issues and improving their performance in miniaturized electronic components.
Patent Information
- Application Number
- JP2022046168
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-23
AI Technical Summary
Conductive pastes containing nickel particles with small particle sizes tend to aggregate, necessitating improved dispersibility for effective use in miniaturized electronic components like multilayer ceramic capacitors.
Nickel particles with an amine compound, nitrile compound, and/or amide compound attached to their surface, with at least 40% by weight of the amine compound, enhance dispersibility, as confirmed by GCMS analysis.
The modified nickel particles significantly improve the dispersibility of conductive pastes, reducing agglomeration and enhancing their suitability for forming internal electrodes in miniaturized MLCCs.
Smart Images

Figure 0007575419000003 
Figure 0007575419000001 
Figure 0007575419000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to nickel particles and uses thereof. [Background technology]
[0002] In recent years, there has been a demand for further miniaturization of electronic components (e.g., multilayer ceramic capacitors: MLCCs). For example, in order to miniaturize MLCCs, it is necessary to thin the internal electrodes of the MLCCs, and it is considered preferable that the conductive paste used to form such internal electrodes contains conductive particles with small particle sizes (typically, an average particle size of about 150 nm or less). The following Patent Document 1 discloses a technology related to nickel particles that are suitable for use in a conductive paste for forming internal electrodes of MLCCs. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6799936 Summary of the Invention [Problem to be solved by the invention]
[0004] However, according to the study by the present inventor, it was found that in a conductive paste containing nickel particles having a small particle size as described above, the nickel particles in the conductive paste tend to aggregate with each other. Therefore, in a conductive paste having such a composition, it is required to further improve the dispersibility of the nickel particles.
[0005] The present disclosure has been made in consideration of the above circumstances, and a main object of the present disclosure is to provide a technique capable of suitably improving the dispersibility of a conductive paste. [Means for solving the problem]
[0006] In order to achieve this object, the present disclosure provides nickel particles containing nickel as a main constituent element. An amine compound, a nitrile compound and / or an amide compound are attached to the surface of the nickel particles, and when the total weight of the amine compound, the nitrile compound and / or the amide compound is taken as 100% by weight based on GCMS analysis, the amine compound is attached at 40% by weight or more. Details will be described later, but nickel particles having such a configuration can suitably improve the dispersibility of a conductive paste.
[0007] In a preferred embodiment of the nickel particles disclosed herein, the CuNi core-shell particles have a CV value of 0.2 or less. For example, in CuNi core-shell particles having a CV value of 0.2 or less, the dispersibility of the conductive paste can be more suitably improved, which is preferable.
[0008] In a preferred embodiment of the nickel particles disclosed herein, the CuNi core-shell particles have an average particle size of 150 nm or less. As described above, particles having an average particle size of 150 nm or less are preferred because they can be suitably used for forming an internal electrode of a miniaturized MLCC.
[0009] In one embodiment of the nickel particles disclosed herein, two or more types of amine compounds are attached to the surface of the nickel particles.
[0010] In another aspect, the present disclosure provides a powder material containing any of the nickel particles disclosed herein. By using the powder material containing the nickel particles disclosed herein, a conductive paste with excellent dispersibility can be obtained.
[0011] In another aspect, the present disclosure provides a conductive paste comprising any of the nickel particles disclosed herein and a medium for dispersing the nickel particles. The conductive paste comprising the nickel particles disclosed herein has excellent dispersibility and can be preferably used. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a flow chart showing the steps of a method for producing nickel particles according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Preferred embodiments of the present disclosure will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure can be understood as design matters for a person skilled in the art based on the conventional technology in the field. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The following embodiments are not intended to limit the technology disclosed herein. In this specification and claims, when a certain numerical range is described as A to B (A and B are arbitrary numerical values), it means A or more and B or less. Therefore, it includes the case where it is greater than A and less than B.
[0014] In addition, in the present specification and claims, "nickel particles" refers to a group of many fine particles (i.e., particles), except when referring to a single particle. In Japanese, it is unclear whether to use the singular or plural form, so the above definition is used to clarify the meaning of "nickel particles." In addition, in the present specification and claims, "conductive paste" can be a concept that includes a slurry composition and an ink composition.
[0015] 1. Nickel particles The nickel particles disclosed herein are nickel particles whose main constituent element is nickel (Ni). An amine compound, a nitrile compound and / or an amide compound are attached to the surface of the nickel particles. The nickel particles are characterized in that, based on GCMS analysis (gas chromatography mass spectrometry), when the total weight of the amine compound, the nitrile compound and / or the amide compound is taken as 100% by weight, the amine compound is attached in an amount of 40% by weight or more.
[0016] The reason why the above-mentioned configuration achieves the effects of the technology disclosed herein is considered to be as follows, although it is not particularly limited to the above. That is, for example, in the production of nickel particles, nickel ions (Ni 2+ When R is reduced to metallic nickel (Ni), a nitrile compound can be produced from a portion of the amine compound added as a reducing agent by the reaction shown in the following formula (I) (R represents hydrogen or a hydrocarbon group).
[0017] [ka]
[0018] In addition, an amide compound may be produced by reacting a part of the amine compound with the carboxylic acid attached to the nickel salt using the nickel particles as a catalyst. For example, when an amine compound, a nitrile compound, or an amide compound (particularly an amine compound) is attached to the surface of a nickel particle, these compounds are said to play a role as a dispersant. On the other hand, according to the study by the present inventor, when nickel particles are synthesized by a conventional method, the amine compound is not attached to the surface of the nickel particles after synthesis (even if it is attached, it is not attached in sufficient amount), and it was found that mainly a nitrile compound and / or an amide compound is attached. And, when a conductive paste is prepared by performing a dispersion treatment in such a state, it was found that a large amount of aggregated particles is generated. Therefore, as a result of the intensive study by the present inventor, it was found that the amine compound can be suitably attached to the surface of the nickel particles by adding an amine compound to the nickel particles after synthesis and performing heating and stirring. Furthermore, according to the study of the present inventors, when the total weight of the amine compound and the nitrile compound and / or amide compound is taken as 100% by weight based on GCMS analysis, nickel particles having 40% by weight or more of the amine compound attached to the surface can suitably suppress the generation of aggregated particles even when a conductive paste is prepared by performing a dispersion treatment, and the present disclosure has been completed. Note that the above explanation is the inventors' consideration based on the experimental results, and the technology disclosed here is not to be interpreted as being limited to the above mechanism. Each component will be explained below.
[0019] Nickel particles are particles whose main constituent element is nickel. Here, in the present specification and claims, "whose main constituent element is nickel" means that, among the components constituting the nickel particles, the component that is contained most in a mole percent basis is nickel. The nickel particles are preferably particles containing nickel at, for example, 50 mole % or more, 60 mole % or more, 70 mole % or more, 80 mole % or more, 90 mole % or more, or 95 mole % or more (may be 100 mole %), when the amount of substance of all metal elements contained in the nickel particles is 100 mole %. The nickel particles may contain various metal elements (e.g., gold (Au), platinum (Pt), silver (Ag), palladium (Pd), copper (Cu)) and nonmetal elements (e.g., hydrogen (H), carbon (C), nitrogen (N), oxygen (O), sulfur (S), phosphorus (P)) as unavoidable impurities. In addition, the nickel particles may be, for example, nickel alloys or core-shell particles in which the inside (core) is made of a metal other than nickel and the shell covering at least a part of the surface of the core is made of nickel. In the case of core-shell particles, examples of the metal other than nickel include copper (Cu), silver (Ag), gold (Au), platinum (Pt), and palladium (Pd). The core-shell particles are a typical example of the "nickel particles" referred to here. In addition, examples of such nickel alloys include alloys of nickel and at least one metal selected from the group consisting of the metals other than nickel. The nickel particles may be used alone from the above-mentioned ones, or two or more kinds may be used in combination.
[0020] Here, when the nickel particles are core-shell particles, the shape of the core particles is not particularly limited as long as the effect of the technology disclosed herein is exhibited, and may be spherical or non-spherical. From the viewpoint of ease of handling, the core particles are preferably spherical. The average particle diameter of the core particles may be about 1 nm to 100 nm (for example, about 10 nm to 50 nm). The thickness of the nickel shell may be about 1 nm to 100 nm (for example, about 10 nm to 50 nm). The thickness of the nickel shell can be determined, for example, by observing the cross section of the core-shell particle with a transmission electron microscope (TEM). The thickness of the nickel shell can be calculated, for example, as the average value when the thickness of the nickel shell is measured at five random points. In addition, when the total weight of the nickel particles is 100% by weight, the weight ratio of the nickel shell can be typically about 0.5 to 95% by weight (for example, about 50 to 95% by weight). However, the weight ratio of the nickel shell is not limited to these.
[0021] In this specification and claims, the term "average particle size" may refer to the particle size (hereinafter also referred to as "D50") that corresponds to 50% of the cumulative particle size from the smallest particle size in the particle size distribution based on the number of particles measured by a field emission scanning electron microscope (FE-SEM). Such measurements can be performed using, for example, a commercially available device, S-4700 manufactured by Hitachi High-Technologies Corporation.
[0022] The nickel particles disclosed herein have an amine compound, a nitrile compound and / or an amide compound attached to their surfaces. Based on GCMS analysis, the total weight of the amine compound, the nitrile compound and / or the amide compound is taken as 100% by weight, and the amine compound is attached at 40% by weight or more. The amounts of the amine compound, the nitrile compound and the amide compound attached to the surface of the nickel particles can be calculated using a calibration curve created based on the GCMS analysis. For details, please refer to the examples described later. As described above, the present inventor has found that the nickel particles having such a configuration can suitably improve the dispersibility of the conductive paste.
[0023] The type of the amine compound is not particularly limited as long as the effect of the technology disclosed herein is exerted. The amine compound is preferably, for example, a monoamine compound that does not contain a secondary or tertiary amino group. Examples of such amine compounds include linear amine compounds such as n-propylamine, n-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-dodecylamine, stearylamine, and oleylamine; branched amine compounds such as 2-ethylhexylamine; cyclic amine compounds such as cyclopropylamine, cyclobutylamine, cyclopentylamine, cyclohexylamine, cycloheptylamine, and cyclooctylamine; and the like. The carbon number of the amine compound is preferably 6 or more, more preferably 7 or more, and more preferably 8 or more. The nickel particles may have one or more of the above-mentioned amine compounds attached thereto. Alternatively, as long as the effect of the technology disclosed herein is exerted, in addition to the above-mentioned amine compounds, amine compounds other than the above-mentioned amine compounds may be attached thereto. In one embodiment of the nickel particles disclosed herein, two or more kinds of amine compounds are attached to the surface of the nickel particles. An example of a method for synthesizing nickel particles having such a configuration is a method using different amine compounds in steps S1 and S3 described below. The amine compounds attached to the surface of the nickel particles can be identified, for example, by pyrolysis GCMS spectrum.
[0024] As described above, the nitrile compound may be, for example, a nickel ion (Ni 2+) is reduced to metallic nickel, it may be generated from a part of the amine compound added as a reducing agent. Examples of such nitrile compounds include nitrile compounds generated from the amine compounds based on the above formula (I). The nickel particles may have one or more of the above-mentioned nitrile compounds attached thereto. Alternatively, in addition to the above-mentioned nitrile compounds, nitrile compounds other than the above-mentioned nitrile compounds may be attached thereto, as long as the effects of the technology disclosed herein are exhibited. The nitrile compounds attached to the surface of the nickel particles can be identified, for example, by pyrolysis GCMS spectrum.
[0025] As described above, the amide compound may be produced by, for example, a reaction between a carboxylic acid and an amine compound attached to a nickel salt using nickel particles as a catalyst. Examples of such amide compounds include amide compounds of the amine compound and a carboxylic acid (for example, formic acid or carboxylic acid) attached to a nickel salt. The nickel particles may have one or more of the above-mentioned amide compounds attached thereto. Alternatively, in addition to the above-mentioned amide compounds, amide compounds other than the above-mentioned amide compounds may be attached thereto, as long as the effect of the technology disclosed herein is exhibited. The amide compounds attached to the surface of the nickel particles can be identified, for example, by pyrolysis GCMS spectrum.
[0026] The nickel particles disclosed herein are characterized in that, based on GCMS analysis, when the total weight of the amine compound and the nitrile compound and / or amide compound is taken as 100% by weight, the amine compound is adhered at 40% by weight or more. As described above, nickel particles having such a configuration can suitably improve the dispersibility of the conductive paste. Here, the amount of the amine compound adhered is preferably, for example, 45% by weight or more, 50% by weight or more, 55% by weight or more, or 60% by weight or more. In addition, the upper limit of the amount of the amine compound adhered is not particularly limited as long as the effect of the technology disclosed herein is exhibited, but it is generally 90% by weight or less, and can be, for example, 80% by weight or less, 70% by weight or less, or 65% by weight or less.
[0027] The amount of the nitrile compound attached to the surface of the nickel particles is not particularly limited as long as the effects of the technology disclosed herein are exhibited, and can be about 0 to 50% by weight (e.g., about 20 to 45% by weight).The amount of the amide compound attached to the surface of the nickel particles is not particularly limited as long as the effects of the technology disclosed herein are exhibited, and can be about 0 to 20% by weight (e.g., about 5 to 15% by weight).
[0028] The amount of the amine compound, nitrile compound, and amide compound attached to the nickel surface can be easily changed, for example, by the following method. The amount of the amine compound attached to the nickel surface can be changed, for example, by adjusting the amount of the amine compound added to the nickel particles after synthesis and the conditions of the heat treatment (heating time, heating temperature, etc.). Typically, the amount of the amine compound attached to the nickel particle surface can be increased by increasing the amount of the amine compound added, the heating time, and the heating temperature. In addition, the amount of the nitrile compound or amide compound attached to the nickel surface can be changed, for example, by adjusting the conditions of the reduction reaction shown in the above formula (I) (reaction time, reaction temperature, etc.). Typically, the amount of the nitrile compound or amide compound attached to the nickel particle surface can be increased by increasing the reaction time and reaction temperature of the reduction reaction shown in the above formula (I). However, it is not intended to be limited to these.
[0029] The average particle size of the nickel particles is not particularly limited as long as the effects of the technology disclosed herein are exhibited. The lower limit of the average particle size of the nickel particles is generally 10 nm or more, and from the viewpoint of easily controlling the aggregation of particles, it is preferably 20 nm or more, more preferably 30 nm or more, and more preferably 40 nm or more. On the other hand, the upper limit of the nickel particles is generally 200 nm or less, and from the viewpoint of use in forming an internal electrode of a miniaturized MLCC, it is preferably 150 nm or less, and more preferably 100 nm or less (for example, 60 nm or less or 50 nm or less).
[0030] The CV value of the nickel particles is not particularly limited as long as the effect of the technology disclosed herein is exhibited. Here, the CV value (coefficient of variation) means the ratio of the standard deviation σ to the average particle size of the nickel particles (standard deviation σ / average particle size), and it can be said that the smaller the CV value, the more uniform the particles. In addition, nickel particles with a small CV value (in other words, uniform particles) are preferable because they can suitably suppress the aggregation of particles. The CV value of the nickel particles is generally 0.5 or less, and from the viewpoint of suitably suppressing the aggregation of particles, it is preferably 0.2 or less, more preferably 0.18 or less, and more preferably 0.15 or less.
[0031] The crystal structure of the nickel particles is not particularly limited as long as the effect of the technology disclosed herein is exhibited. Here, examples of the crystal structure of the nickel particles include fcc (face-centered cubic) and hcp (hexagonal close-packed). From the viewpoint of stability, etc., it is preferable that at least a part of the crystal structure of the nickel particles is fcc, and more preferably the whole is fcc. In addition, such a crystal structure can be confirmed by peak analysis based on XRD (X-ray Diffraction), for example.
[0032] 2. Nickel particle manufacturing method Next, a preferred example of the method for producing nickel particles disclosed herein will be described. The method for producing nickel particles disclosed herein is characterized in that an amine compound is added to the synthesized nickel particles and heat treatment is performed (see step S3). This allows the amount of the amine compound attached to the nickel particle surface to be suitably increased. The process before the amine compound is added later may be the same as the conventional process. In the following, a method for producing copper-nickel core-shell particles (CuNi core-shell particles) consisting of a core particle made of copper and a nickel shell covering at least a part of the surface of the core particle will be described as the nickel particles. In the following description, the method for producing CuNi core-shell particles is not intended to be limited to the following manufacturing method. In the following, the description will be made with reference to FIG. 1 as appropriate.
[0033] Fig. 1 is a general flow diagram showing the steps of a method for producing nickel particles (here, CuNi core-shell particles) according to one embodiment. As shown in Fig. 1, the steps include producing nickel seed particles (step S1); producing nickel particles (step S2); adding an amine compound (step S3); and recovering the nickel particles (step S4). Each step will be described below.
[0034] First, in step S1, nickel seed particles (hereinafter also simply referred to as "seed particles") are prepared. Here, the seed particles are capable of functioning as nuclei for the growth of nickel. Such seed particles can be synthesized, for example, by using nickel salt and copper salt as raw materials and carrying out wet reduction by heating in the presence of an amine compound. According to this method, due to the difference in standard potential between copper and nickel, copper particles that serve as nuclei are first generated, and then a nickel coating is formed on the surface of the copper particles, thereby obtaining the seed particles.
[0035] Specifically, a nickel-amine complex is synthesized by adding a predetermined amount of nickel salt (e.g., about 0.005 to 0.1 molar equivalent) to an amine compound and heating at a predetermined temperature (e.g., about 100 to 150°C) for a predetermined time (e.g., about 60 to 120 minutes). A copper-amine complex is then added to the nickel-amine complex in a predetermined amount (e.g., about 0.0005 to 0.01 molar equivalent), and heating at a predetermined temperature (e.g., about 50 to 100°C) for a predetermined time (e.g., about 30 to 60 minutes) to synthesize a copper-amine complex. After that, seed particles (seed particle slurry) can be synthesized by heating at a predetermined temperature (e.g., about 150 to 200°C) for a predetermined time (e.g., about 10 to 30 minutes) in a nitrogen atmosphere.
[0036] As the amine compound, for example, the amine compounds described above can be used. As these amine compounds, for example, commercially available ones can be used without any particular limitation.
[0037] Examples of the nickel salt include nickel carboxylate, nickel chloride, nickel carbonate, nickel nitrate, and nickel hydroxide. Among these, nickel carboxylate, which has a relatively low decomposition temperature during reduction, can be preferably used. Examples of such nickel carboxylate include nickel formate and nickel acetate. The nickel carboxylate may be anhydride or hydrate. Examples of such hydrate include nickel formate dihydrate and nickel acetate tetrahydrate. As the nickel salt, for example, commercially available ones can be used without any particular limitation.
[0038] As the copper salt, a copper carboxylate having a relatively low decomposition temperature during reduction can be preferably used. Examples of such copper carboxylates include copper formate and copper acetate. Such copper carboxylates may be anhydrides or hydrates. An example of such hydrates is copper acetate tetrahydrate. As the copper salt, for example, commercially available products can be used without any particular limitations.
[0039] Next, in step S2, nickel particles are produced. In step S2, nickel salt is added to the seed particle slurry obtained in step S1, and wet reduction is performed by heating. This allows a Ni shell to grow around the seed particles as nuclei. In this way, by growing a Ni shell around the seed particles as nuclei, uniform nickel particles with a low CV value can be obtained, which is preferable.
[0040] Specifically, a nickel salt is first added to the seed particle slurry obtained in step S1 in a predetermined amount (e.g., about 1 to 45 molar equivalents), and the mixture is heated at a predetermined temperature (e.g., about 100 to 150°C) for a predetermined time (60 to 120 minutes) to synthesize a nickel-amine complex. Then, the mixture is heated in a nitrogen atmosphere at a predetermined temperature (e.g., about 150 to 200°C) for a predetermined time (30 to 60 minutes) to synthesize nickel particles (nickel particle slurry). Here, the nickel salt may be, for example, one as described in the nickel salt section of step S1.
[0041] Subsequently, in step S3, an amine compound is added, which makes it possible to suitably increase the amount of the amine compound attached to the surface of the nickel particles. Specifically, the supernatant of the nickel particle slurry obtained in step S2 is removed, and the above-mentioned amine compound is added. Then, the mixture is heated in a nitrogen atmosphere at a predetermined temperature (e.g., about 50 to 150° C.) for a predetermined time (e.g., about 30 to 60 minutes) to obtain nickel particles (nickel particle slurry).
[0042] Next, in step S4, the nickel particles are collected. Specifically, first, the supernatant of the nickel particle slurry obtained in step S3 is removed. Then, a suitable washing solvent (e.g., isobornyl acetate, etc.) is added, and the mixture is dispersed using an ultrasonic cleaner or the like, after which the supernatant is removed. This operation is repeated multiple times (e.g., about 2 to 5 times), and then the mixture is dried in a dryer at a predetermined temperature (e.g., about 100 to 150°C) for a predetermined time (e.g., about 30 to 60 minutes) to obtain nickel particles (powder).
[0043] In addition to the nickel particles disclosed herein, a binder (e.g., acrylic resin, epoxy resin, phenol resin, amine resin, alkyd resin, cellulose resin such as ethyl cellulose), conductive material, other powder material (e.g., barium titanate), etc. can be added as necessary to obtain powder materials for various applications. For example, a powder material can be obtained by mixing and grinding nickel particles and the above-mentioned materials. Since such a powder material contains nickel particles as described above, the use of the powder material can favorably achieve both the dispersibility of the conductive paste and the reduction in the shrinkage rate of the conductive layer obtained after firing. The content of nickel particles in the powder material is not particularly limited, but is preferably about 50 to 95% by weight (e.g., about 60 to 90% by weight) when the entire powder material is 100% by weight.
[0044] In addition, the nickel particles disclosed herein can be dispersed in a dispersion medium (medium) made of an appropriate aqueous or organic solvent to obtain a dispersion (conductive paste) for various applications. For example, nickel particles are dispersed in a predetermined organic solvent, and components such as a binder (see those listed in the description of the powder material), a conductive material, other powder materials, a dispersant (e.g., a carboxylic acid-based dispersant), and a viscosity modifier are added as necessary to obtain a composition (conductive paste) prepared in a paste form. As described above, such a conductor paste contains nickel particles, and therefore can favorably achieve both excellent dispersibility and a reduced shrinkage rate of the conductive layer obtained after firing.
[0045] The dispersion medium used in the conductive paste may be any one that can disperse this type of conductive powder material well, and any one used in the preparation of conventionally known conductive pastes may be used without any particular limitation. Examples of organic solvents include one or more combinations of high-boiling organic solvents such as mineral spirits and other petroleum-based hydrocarbons (particularly aliphatic hydrocarbons), ethylene glycol and diethylene glycol derivatives, toluene, xylene, butyl carbitol (BC), isobornyl acetate, and terpineol. Here, the content of nickel particles in the conductive paste is not particularly limited, but is preferably about 30 to 70% by weight (for example, about 40 to 60% by weight) when the entire conductive paste is taken as 100% by weight. The content of the dispersion medium in the conductive paste is not particularly limited, but is preferably about 30 to 70% by weight (for example, about 40 to 60% by weight) when the entire conductive paste is taken as 100% by weight. The viscosity of the conductive paste is not particularly limited, but is preferably about 10 to 100 mPa·s (for example, about 20 to 50 mPa·s). The viscosity can be measured, for example, by a commercially available viscometer.
[0046] The above-mentioned technology can be utilized in the field of electronic materials to realize miniaturization of electronic components and thinning of electrodes.
[0047] Hereinafter, test examples relating to the nickel particles disclosed herein will be described, but it is not intended that the present disclosure be limited to such test examples. In addition, the following will describe the case where CuNi core-shell particles are used as an example of nickel particles.
[0048] <Synthesis of nickel particles> First, the synthesis of nickel particles according to Examples 1 to 6 will be described.
[0049] (Synthesis of nickel seed particle slurry) Nickel formate dihydrate (Fujifilm Wako Pure Chemical Industries, Ltd., hereinafter the same) was added to 319.2 g of oleylamine (Fujifilm Wako Pure Chemical Industries, Ltd., hereinafter the same) and heated at 120°C for 120 minutes to synthesize a nickel formate-oleylamine complex. Next, 0.23 g of copper formate tetrahydrate (Fujifilm Wako Pure Chemical Industries, Ltd., hereinafter the same) was added to the nickel formate-oleylamine complex and heated at 60°C for 30 minutes to synthesize a copper formate-oleylamine complex. After that, nickel seed particle slurry was synthesized by heating at 190°C for 10 minutes under a nitrogen atmosphere.
[0050] (Synthesis of nickel particle slurry) To the nickel seed particle slurry synthesized above, 114.0 g of nickel acetate tetrahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., the same applies below) was added, and the mixture was heated at 135°C for 120 minutes to synthesize a nickel acetate-oleylamine complex. After that, the mixture was heated at 200°C for 30 minutes in a nitrogen atmosphere to synthesize a nickel particle slurry.
[0051] Synthesis of nickel particle slurry according to Example 1 The supernatant of the nickel particle slurry synthesized above was removed, and 200 mL of oleylamine was added to the slurry, followed by heating and stirring at 100° C. for 30 minutes to synthesize the nickel particle slurry according to Example 1.
[0052] Synthesis of nickel particle slurry according to Example 2 The supernatant of the nickel particle slurry synthesized above was removed, and 100 mL of oleylamine was added to the slurry, followed by heating and stirring at 100° C. for 30 minutes to synthesize a nickel particle slurry according to Example 2.
[0053] Synthesis of nickel particle slurry according to Example 3 The supernatant of the nickel particle slurry synthesized above was removed, and 200 mL of oleylamine was added to the slurry, followed by heating and stirring at 50° C. for 60 minutes to synthesize a nickel particle slurry according to Example 3.
[0054] Synthesis of nickel particle slurry according to Example 4 The supernatant of the nickel particle slurry synthesized above was removed, and 200 mL of 2-ethylhexylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the slurry, and the mixture was heated and stirred at 100° C. for 30 minutes to synthesize the nickel particle slurry of Example 4.
[0055] Synthesis of nickel particle slurry according to Example 5 The supernatant of the nickel particle slurry synthesized above was removed, and 100 mL of oleylamine was added to the slurry, followed by heating and stirring at 50° C. for 60 minutes to synthesize the nickel particle slurry according to Example 1.
[0056] Synthesis of nickel particle slurry according to Example 6 The supernatant liquid of the nickel particle slurry synthesized above was removed. The resulting slurry was used as the nickel particle slurry of Example 5.
[0057] The supernatant of the nickel particle slurry according to each example synthesized above was removed. Then, isobornyl acetate was added, dispersed in an ultrasonic cleaner, and the supernatant was removed. This process was repeated three times, and then dried in a dryer at 120°C for 60 minutes to obtain a powder material made of nickel particles according to each example.
[0058] <Evaluation test>
[0059] (1) Characteristics of nickel particles The nickel particles in the powder material were observed using a field emission scanning electron microscope (FE-SEM: S-4700 manufactured by Hitachi High-Technologies Corporation). Specifically, five images were extracted from a 50,000x field of view, and 200 nickel particles were randomly extracted to determine their projected areas. The diameter of a circle having the same area (Heywood diameter) was measured. The cumulative 50% particle diameter (D50) in the number-based particle size distribution was calculated as the average particle diameter (nm). The coefficient of variation (CV) of the average particle diameter was also calculated. Here, the CV value means the ratio of the standard deviation σ to the average particle diameter of the nickel particles (standard deviation σ / average particle diameter). The average particle diameter of the nickel particles in each example was about 50 nm, and the CV value was about 0.15.
[0060] (2) Analysis of organic matter on the surface of nickel particles 0.6mL of methanol was added to 500mg of nickel particles according to each of the above synthesis examples, and ultrasonic irradiation was performed for 1 hour using an ultrasonic cleaner. The supernatant liquid after collecting the particles with a magnet was used as an extract, and was measured with a GCMS device (Shimadzu Corporation's GCMS-QP-2010Ultra) to analyze the organic matter attached to the surface of the nickel particles. Specifically, the organic matter attached to the surface of the nickel particles was identified, and the amount of attachment (wt%) of amine compounds, nitrile compounds, and amide compounds was calculated when the total weight of the organic matter was taken as 100 wt%. The amount of attachment was calculated using a calibration curve based on the peak area and sample concentration of GCMS. The measurement results are shown in the corresponding columns of Table 1.
[0061] Although not shown in Table 1, it was confirmed that oleylamine, oleylnitrile, and an amide compound of oleylamine and acetic acid (or formic acid) were adhered to the surfaces of the nickel particles according to Examples 1 to 3, 5, and 6. It was also confirmed that oleylamine, 2-ethylhexylamine, oleylnitrile, 2-ethylhexylnitrile, an amide compound of oleylamine and acetic acid (or formic acid), and an amide compound of 2-ethylhexylamine and acetic acid (or formic acid) were adhered to the surfaces of the nickel particles according to Example 4.
[0062] (Preparation of conductive paste) The nickel particles (powder material) obtained above, commercially available barium titanate powder, ethyl cellulose resin, carboxylic acid dispersant, and isobornyl acetate were mixed and dispersed using a triple roll to prepare a conductive paste. The blending amounts of each raw material, when the entire conductive paste is taken as 100% by weight, were 45% by weight of nickel particles, 4.5% by weight of barium titanate, 2% by weight of ethyl cellulose resin, 2% by weight of carboxylic acid dispersant, and the remainder is isobornyl acetate. The viscosity of the conductive paste was about 20 to 50 mPa·s at 25°C and 100 rpm (measured with a Brookfield DV viscometer).
[0063] (3) Evaluation of dispersibility The conductive paste obtained above was applied to a substrate in a film thickness of 2 μm and dried at 120° C. for 5 minutes. Next, the coating film was observed in a total of three fields of view using an optical microscope (ECLIPSE LV150 manufactured by Nikon Solutions Corporation), and the presence or absence of aggregated particles was confirmed from the obtained observation images. Here, such aggregated particles are observed as white lumps in optical microscope observation. Dispersibility was evaluated as “○” when the number of aggregated particles per field was 10 or less, and dispersibility was evaluated as “×” when the number of aggregated particles per field was more than 10. The evaluation results are shown in the corresponding columns in Table 1.
[0064] [Table 1]
[0065] As shown in Table 1, the conductive pastes containing nickel particles (nickel powder) according to Examples 1 to 5, which are nickel particles having nickel as a main constituent element, have an amine compound, a nitrile compound and / or an amide compound attached to the surface of the nickel particles, and have 40% by weight or more of the amine compound attached when the total weight of the amine compound, the nitrile compound and / or the amide compound is taken as 100% by weight based on GCMS analysis, were confirmed to have excellent dispersibility. On the other hand, the conductive paste containing nickel particles according to Example 6, in which the amount of the amine compound attached is outside the above range, was confirmed to have poor dispersibility.
[0066] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above.
Claims
1. Nickel particles containing nickel as a main component, an amine compound and a nitrile compound and / or an amide compound are attached to the surface of the nickel particles; Here, when the total weight of the amine compound and the nitrile compound and / or the amide compound is taken as 100% by weight, the amine compound adheres to the nickel particles in an amount of 40% by weight or more and 65% by weight or less based on GCMS analysis.
2. The nickel particles according to claim 1, wherein the CV value of the nickel particles is 0.2 or less.
3. The nickel particles according to claim 1 or 2, wherein the average particle size of the nickel particles is 150 nm or less.
4. The nickel particles according to any one of claims 1 to 3, wherein two or more types of amine compounds are attached to the surface of the nickel particles.
5. A powder material comprising nickel particles according to any one of claims 1 to 4.
6. The nickel particles according to any one of claims 1 to 4, A medium for dispersing the nickel particles; A conductive paste comprising:
Citation Information
Patent Citations
Metal microparticle and method for producing the same, metal paste containing the metal microparticle, and metal coat made of the metal paste
JP2013072091A
Nickel particle, conductive paste, internal electrode and laminate ceramic capacitor
JP2017179551A
Coated copper nanoparticle, coated copper nanoparticle-containing composition, and article
JP2021031738A
Nickel particles, conductive paste, internal electrodes and multilayer ceramic capacitors
JP6799936B2
Electroconductive adhesive