COMPOSITION, POSITIVE ELECTRODE COMPOSITION, POSITIVE ELECTRODE SLURRY, POSITIVE ELECTRODE, AND SECONDARY BATTERY
A graft copolymer with polyvinyl alcohol and (meth)acrylonitrile units is used as a binder to address performance and high-temperature issues in lithium ion secondary batteries, enhancing stability and resistance.
Patent Information
- Application Number
- JP2022542866
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-12
- Filing Date
- 2021-08-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-08-11
AI Technical Summary
Existing lithium ion secondary batteries face issues with battery performance deterioration, high-temperature storage properties, and DC resistance in high-capacity electrodes, necessitating a composition that can balance these factors.
A graft copolymer with a polyvinyl alcohol structure as the trunk polymer and a branch polymer containing (meth)acrylonitrile and/or (meth)acrylic acid monomer units, with a gel fraction of 30% or more, is used as a binder to form a positive electrode composition, which includes a crosslinking portion and a free polymer, to enhance stability and resistance.
The composition effectively suppresses battery performance deterioration, maintains high-temperature storage characteristics, and balances DC resistance, resulting in improved battery performance and stability.
Smart Images

Figure 0007575464000001 
Figure 0007575464000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition, a positive electrode composition, a positive electrode slurry, a positive electrode, and a secondary battery. [Background technology]
[0002] In recent years, secondary batteries have been used as power sources for electronic devices such as notebook computers and mobile phones, and the development of hybrid and electric vehicles that use secondary batteries as power sources is underway to reduce the environmental impact. These power sources require secondary batteries with high energy density, high voltage, and high durability. Lithium-ion secondary batteries have attracted attention as secondary batteries that can achieve high voltage and high energy density.
[0003] A lithium ion secondary battery is composed of components such as a positive electrode, a negative electrode, an electrolyte, and a separator, and the positive electrode is composed of a positive electrode active material, a conductive assistant, a metal foil, and a binder (Patent Documents 1 to 3).
[0004] As a positive electrode binder for lithium ion secondary batteries, a binder (graft copolymer) containing polyvinyl alcohol and polyacrylonitrile as main components has been disclosed (Patent Document 4).
[0005] In addition, a composition containing a graft copolymer in which a monomer mainly composed of (meth)acrylonitrile and (meth)acrylic acid ester is graft-copolymerized onto a backbone polymer having polyvinyl alcohol has been disclosed as a positive electrode binder for lithium ion secondary batteries (Patent Document 5). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-98123 A [Patent Document 2] JP 2013-84351 A [Patent Document 3] Japanese Patent Application Publication No. 6-172452 [Patent Document 4] International Publication No. 2015 / 053224 [Patent Document 5] International Publication No. 2018 / 230599 Summary of the Invention [Problem to be solved by the invention]
[0007] However, there has been a demand for the development of a composition capable of obtaining a battery that is excellent in balance between suppressing deterioration of battery performance in a high-capacity electrode, high-temperature storage characteristics, and DC resistance, as well as a slurry for a positive electrode, a positive electrode, and a secondary battery that use the composition.
[0008] The present invention has been made in consideration of such problems, and provides a composition that serves as a binder that suppresses deterioration of battery performance in a high-capacity electrode and has an excellent balance between high-temperature storage characteristics and DC resistance, and a positive electrode slurry, a positive electrode, and a secondary battery that use the composition. [Means for solving the problem]
[0009] According to the present invention, there is provided a composition containing a graft copolymer, the graft copolymer having a trunk polymer and a branch polymer, the trunk polymer containing a polyvinyl alcohol structure, the branch polymer containing a first monomer unit containing a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer, the composition having a gel fraction of 30% or more, the gel fraction being expressed as gel fraction %=A×100 / 1 when 1 g of the composition is added to 300 ml of dimethyl sulfoxide, stirred at 60° C. for 15 hours, and filtered through a No. 5C filter paper specified in JIS P 3801, and the insoluble matter remaining as a residue on the filter paper is defined as Ag.
[0010] As a result of intensive research, the inventors have discovered that a binder containing a graft copolymer having a structure in which a first monomer unit, which is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit, is graft-copolymerized onto a backbone polymer having a polyvinyl alcohol structure, and having a gel fraction within a predetermined range, can be obtained that suppresses the deterioration of battery performance in high-capacity electrodes, and has an excellent balance of high-temperature storage characteristics and DC resistance, and have thus completed the present invention.
[0011] Various embodiments of the present invention will be described below. The embodiments described below can be combined with each other. Preferably, the composition further comprises a free polymer, the free polymer having no covalent bond with the graft copolymer, the free polymer comprising at least a polymer comprising a polyvinyl alcohol structure and / or a polymer comprising the first monomer unit. Preferably, the graft copolymer further contains a crosslinked portion derived from a crosslinking agent. Preferably, the cross-linking portion includes an ether structure. Preferably, the composition contains 0.2 to 10 parts by mass of a structure derived from the crosslinking agent when the composition is taken as 100 parts by mass. Preferably, the composition has a swelling ratio of 90 to 230% after immersion in an electrolytic solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 at 25° C. for 15 days. Preferably, the graft ratio of the graft copolymer is 40 to 3000%. Preferably, the degree of saponification of the polyvinyl alcohol structure in the composition is 60 to 100 mol %. Preferably, the average degree of polymerization of the polyvinyl alcohol structure in the composition is 300-4,000. Preferably, the positive electrode composition contains the above composition.
[0012] According to another aspect of the present invention, there is provided a positive electrode slurry containing the positive electrode composition, a positive electrode active material, and a conductive assistant. Preferably, when the total solid content in the positive electrode slurry is 100% by mass, the solid content of the positive electrode composition is 1 to 20% by mass. Preferably, the conductive assistant is at least one selected from the group consisting of fibrous carbon, carbon black, and a carbon composite in which fibrous carbon and carbon black are interconnected. According to another aspect of the present invention, a positive electrode is provided that includes a metal foil and a coating film of the positive electrode slurry described above formed on the metal foil. According to another aspect of the present invention, a secondary battery including the positive electrode described above is provided, and the secondary battery is at least one selected from the group consisting of a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, and a potassium ion secondary battery. According to another aspect of the present invention, the positive electrode active material is LiNi X Mn (2-X) O4 (where 0 < X < 2), Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1), and Li(Ni X Co Y Al Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1), and a secondary battery including at least one of the above and being a lithium ion secondary battery is provided.
Advantages of the Invention
[0013] The present invention provides a composition that serves as a binder excellent in suppressing a decrease in battery performance in a high-capacity electrode, high-temperature storage characteristics, and balance of DC resistance, a positive electrode slurry using the composition, a positive electrode, and a secondary battery.
Embodiments for Carrying Out the Invention
[0014] Hereinafter, embodiments of the present invention will be described. The various characteristic matters shown in the following embodiments can be combined with each other. Also, the invention can be established independently for each of the various characteristic matters.
[0015] 1. Composition The composition according to one embodiment of the present invention can be used as a positive electrode composition. A composition for a positive electrode according to one embodiment of the present invention includes a composition according to one embodiment of the present invention, and preferably consists of a composition according to one embodiment of the present invention. A composition according to one embodiment of the present invention is a composition containing a graft copolymer, and the graft copolymer has a trunk polymer and a branch polymer, and preferably has a trunk polymer and a plurality of branch polymers. Hereinafter, the polymer may be referred to as a copolymer.
[0016] 1-1. Graft copolymer The graft copolymer according to one embodiment of the present invention is synthesized by graft copolymerizing at least a first monomer onto a trunk polymer. The branch polymers produced by the polymerization are grafted, i.e., covalently bonded, to the trunk polymer. At this time, a trunk polymer that is not grafted, or a polymer containing a first monomer that is not grafted to the trunk polymer, i.e., not covalently bonded to the graft copolymer, may be simultaneously produced as a free polymer. Therefore, the composition according to one embodiment of the present invention may contain a graft copolymer and a free polymer.
[0017] The graft copolymer according to one embodiment of the present invention may further include a crosslinking portion derived from a crosslinking agent. The crosslinking portion means a structure derived from a crosslinking agent that crosslinks branch polymers with each other, crosslinks a trunk polymer with a branch polymer, or crosslinks trunk polymers with each other. The graft copolymer according to one embodiment of the present invention can be obtained by graft copolymerizing at least a first monomer onto a trunk polymer and crosslinking either the trunk polymer or the branch polymer with either the trunk polymer or the branch polymer. The composition according to one embodiment of the present invention may also include a polymer including a structure derived from a crosslinking agent as a free polymer, in addition to a polymer including a first monomer.
[0018] The graft copolymer according to one embodiment of the present invention may contain a second monomer unit containing an ether structure and a monomer unit other than the first monomer unit and the second monomer unit, as long as the effect of the present invention is not impaired. The composition according to one embodiment of the present invention may also contain, as the free polymer, a polymer containing the second monomer unit and a polymer containing a monomer unit other than the first monomer unit and the second monomer unit.
[0019] The graft ratio of the graft copolymer is preferably 40 to 3000%, more preferably 150 to 900%. From the viewpoint of solubility, the graft ratio is preferably within the above range. If the graft ratio is equal to or higher than the above lower limit, the solubility in a solvent (e.g., NMP (N-methyl-2-pyrrolidone)) is improved when the polymer is made into a slurry, whereas if the graft ratio is equal to or lower than the above upper limit, the viscosity of the slurry is reduced, improving the fluidity of the slurry.
[0020] 1-2. Trunk polymer The trunk polymer has a polyvinyl alcohol structure. Here, the polyvinyl alcohol structure is, for example, a structure derived from polyvinyl alcohol synthesized by saponifying polyvinyl acetate obtained by polymerizing vinyl acetate monomer. Preferably, the trunk polymer is mostly composed of a polyvinyl alcohol structure. More preferably, the trunk polymer is polyvinyl alcohol.
[0021] The average degree of polymerization of the polyvinyl alcohol structure in the composition is preferably 300 to 4000, more preferably 500 to 2000. When the average degree of polymerization is in this range, the stability of the slurry is particularly high. In addition, the above range is also preferable from the viewpoints of solubility, binding property, and viscosity of the binder. When the average degree of polymerization is 300 or more, the binding property between the binder and the active material and the conductive assistant is improved, and durability is improved. When the average degree of polymerization is 4000 or less, the solubility is improved and the viscosity is reduced, making it easier to manufacture the slurry for the positive electrode. The average degree of polymerization here is a value measured by a method conforming to JIS K 6726. The saponification degree of the polyvinyl alcohol structure in the composition is preferably 60 to 100 mol%, more preferably 80 to 100 mol%. When the saponification degree is within this range, the stability of the slurry is particularly high. The saponification degree referred to here is a value measured by a method according to JIS K 6726.
[0022] 1-3. Branch polymer The branch polymer contains at least a first monomer unit. The branch polymer may contain a second monomer unit and a monomer unit other than the first monomer unit and the second monomer unit, as long as the effect of the present invention is not impaired. Here, the first monomer unit and the second monomer unit are monomer units derived from the first monomer and the second monomer used in the synthesis of the graft copolymer, respectively.
[0023] 1-4.Bridge part The graft copolymer according to one embodiment of the present invention may further include a crosslinking portion. The crosslinking portion is a structure derived from a crosslinking agent, and connects the branch polymers of the graft copolymer to each other, the trunk polymer and the branch polymer, or the trunk polymers of the graft copolymer to each other. The crosslinking portion preferably crosslinks the branch polymers of the graft copolymer to each other. The crosslinking portion preferably includes an ether structure, more preferably includes an alkylene glycol repeating unit, and most preferably includes an ethylene glycol repeating unit.
[0024] The crosslinking agent according to one embodiment of the present invention is a bifunctional or polyfunctional compound, preferably a compound that is soluble in a polar solvent, and preferably a compound that is soluble in the first monomer. The crosslinking agent is not particularly limited as long as it satisfies the above requirements, but examples thereof include alkane polyol-poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, oligoethylene glycol di(meth)acrylate (polyethylene glycol di(meth)acrylate), trimethylolpropane di(meth)acrylate, and trimethylolpropane tri(meth)acrylate, and divinylbenzene. Among these, oligoethylene glycol di(meth)acrylate is preferred. Among the oligoethylene glycol di(meth)acrylates, di(meth)acrylates represented by the following general formula (B) are preferred. H2C=CR 21 -COO-(-CH2CH2O-) n -CO-CR 22 =CH2(B) In the general formula (B), R 21 , R 22 is hydrogen (H) or a methyl group. 21 , R 22 may be the same or different. n is a number of 0 or more. n is preferably 1 or more. n is preferably 30 or less, and more preferably 10 or less. The crosslinking agent preferably contains an ether structure, and more preferably has an ethylene glycol repeating unit. The number of ethylene glycol repeating units is preferably 2 or more and 20 or less, more preferably 5 or more and 15 or less, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15, and may be within a range between any two of the numerical values exemplified here. In the graft copolymer according to one embodiment of the present invention, the gel fraction of the composition can be controlled by adjusting the type and amount of the crosslinked portion.
[0025] 1-4.Free polymer The composition according to one embodiment of the present invention may further include a free polymer. The free polymer is a polymer that does not have a covalent bond with the graft copolymer, and includes at least a polymer containing a polyvinyl alcohol structure and / or a polymer containing the first monomer unit. The polymer having a polyvinyl alcohol structure means a trunk polymer that was not mainly involved in the graft copolymerization. The polymer containing the first monomer unit means a homopolymer of the first monomer, a copolymer containing the first monomer unit and the second monomer unit, a copolymer containing the first monomer and a monomer unit other than the first monomer unit and the second monomer unit, or a polymer containing a copolymer containing a structure derived from the first monomer and a crosslinking agent, which is not copolymerized with the graft copolymer (i.e., the trunk polymer). Furthermore, within the scope of the present invention, the free polymer may include polymers other than the polymer having a polyvinyl alcohol structure and the polymer containing the first monomer unit, such as a homopolymer of the second monomer, a homopolymer of a monomer other than the first monomer and the second monomer, and a polymer containing a structure derived from a crosslinking agent, which is not copolymerized in the graft copolymer (i.e., trunk polymer). The free polymer is preferably a polymer that substantially contains the first monomer unit.
[0026] In addition, the weight average molecular weight of the free polymer other than the trunk polymer, for example, a copolymer containing a homopolymer of the first monomer, is preferably 30,000 to 250,000, more preferably 40,000 to 200,000, and even more preferably 50,000 to 150,000. From the viewpoint of suppressing an increase in viscosity and easily producing a positive electrode slurry, the weight average molecular weight of the free polymer other than the trunk polymer is preferably 300,000 or less, more preferably 200,000 or less, and even more preferably 150,000 or less. The weight average molecular weight of the free polymer other than the trunk polymer can be determined by GPC (gel permeation chromatography), and specifically, can be measured by the method described later.
[0027] 1-6. First monomer unit The first monomer unit is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit. The first monomer unit is more preferably a (meth)acrylonitrile monomer unit, and further preferably an acrylonitrile monomer unit. That is, the first monomer used in synthesizing the graft copolymer is preferably (meth)acrylonitrile and / or (meth)acrylic acid, more preferably (meth)acrylonitrile, and even more preferably acrylonitrile, and therefore the first monomer unit has a structure derived from these.
[0028] 1-7. Second monomer unit The second monomer unit is a structural unit containing an ether structure, and is a structure derived from a monofunctional second monomer. The second monomer unit is a monofunctional compound having an ether structure. The ether structure preferably has at least one selected from a linear polyether structure, a branched polyether structure, and a cyclic ether structure. More preferably, the ether structure has a polyethylene oxide structure. Moreover, the second monomer unit preferably has a structure derived from a monomer which is a (meth)acrylic acid ester derivative, a styrene derivative, a polysubstituted ethylene, or a vinyl ether derivative.
[0029] That is, the second monomer used in synthesizing the graft polymer is a monomer having an ether structure, and is preferably a monomer such as a (meth)acrylic acid ester derivative having an ether structure, a styrene derivative having an ether structure, a polysubstituted ethylene derivative, or a vinyl ether derivative. Among these, a (meth)acrylic acid ester derivative having an ether structure is preferred. Among the (meth)acrylic acid ester derivatives having an ether structure, a (meth)acrylic acid ester derivative represented by the following general formula (A) is preferred.
[0030] [ka] In the general formula (A), Y is preferably -(AO)nR. AO is an oxyalkylene group. The number of carbon atoms in the oxyalkylene group is preferably 1 to 18, more preferably 2 to 10. The oxyalkylene group is most preferably one or more of an ethylene oxide group and a propylene oxide group, and more preferably an ethylene oxide group. n is a number of 0 or more. n is preferably 1 or more. n is preferably 30 or less, more preferably 10 or less. Also, R 1 , R 2 , R 3 R is hydrogen (H), a hydrocarbon group or an ether group which may be substituted, etc. Preferably, the hydrocarbon group or ether group which may be substituted is a hydrocarbon group or ether group having 1 to 20 carbon atoms. Here, the ether group is a functional group having an ether bond, such as an alkyl ether group. R 1 , R 2 , R 3 Preferably, R is unsubstituted. 1 , R 2 , R 3 R may be the same or different. R is preferably a hydrocarbon group. As the hydrocarbon group, one or more of a methyl group and an ethyl group are preferable. As the (meth)acrylic acid ester derivative, alkoxy polyalkylene glycol (meth)acrylate is preferred. Among the alkoxy polyalkylene glycol (meth)acrylates, one or more of alkoxy polyethylene glycol (meth)acrylate and alkoxy polypropylene glycol (meth)acrylate are preferred. More specifically, one or more of (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate, methoxy polyethylene glycol (meth)acrylate (poly:n=23), and methoxy dipropylene glycol (meth)acrylate are preferred. The second monomer is more preferably one or more of (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate and methoxy dipropylene glycol (meth)acrylate, and most preferably (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate. Therefore, the second monomer unit has a structure derived from these.
[0031] 1-8. Content of each component in the composition It is also preferable that the content and characteristics of each component satisfy the following requirements: When the content and characteristics of each component are within the following ranges, it is possible to provide a positive electrode composition that serves as a binder that suppresses deterioration of battery performance in a high-capacity electrode, and has an excellent balance of high-temperature storage characteristics (high-temperature preservation characteristics) and DC resistance.
[0032] In the composition according to one embodiment of the present invention, when the composition is 100 parts by mass, the content of the polyvinyl alcohol structure in the composition is preferably 5 to 70 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 15 to 55 parts by mass, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 parts by mass, and may be within a range between any two of the numerical values exemplified here. By making it equal to or more than the above lower limit, it is possible to obtain a binder having binding properties, and by making it equal to or less than the above upper limit, it is possible to maintain oxidation resistance and flexibility. In this embodiment, the content of the polyvinyl alcohol structure in the composition refers to the total amount of the polyvinyl alcohol structure in the graft copolymer and the polyvinyl alcohol structure in the free polymer containing polyvinyl alcohol contained in the composition.
[0033] In the composition according to one embodiment of the present invention, when the composition is taken as 100 parts by mass, the content of the first monomer unit derived from the first monomer is preferably 3 to 80 parts by mass, more preferably 5 to 70 parts by mass, for example, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80 parts by mass, and may be within a range between any two of the numerical values exemplified here. By setting it to the above lower limit or more, a binder having binding properties can be obtained, and by setting it to the above upper limit or less, oxidation resistance can be maintained. In this embodiment, the content of the first monomer unit in the composition refers to the total amount of the first monomer unit in the graft copolymer and the first monomer unit in the free polymer containing the first monomer unit, which are contained in the composition.
[0034] The composition according to one embodiment of the present invention preferably contains 0.2 to 10 parts by mass of the structure derived from the crosslinking agent, more preferably 0.5 to 8 parts by mass, and particularly preferably 1 to 5 parts by mass, when the composition is taken as 100 parts by mass. The content of the structure derived from the crosslinking agent is, for example, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the numerical values exemplified here. By making it equal to or more than the above lower limit, the composition has a sufficient gel fraction, and by making it equal to or less than the above upper limit, the solubility in a solvent such as NMP can be sufficiently maintained. In this embodiment, the content of the structure derived from the crosslinking agent in the composition refers to the total amount of the structure derived from the crosslinking agent bonded to the graft copolymer contained in the composition and the structure derived from the crosslinking agent in the free polymer.
[0035] In the composition according to one embodiment of the present invention, when the composition is taken as 100 parts by mass, the content of the second monomer unit derived from the second monomer is preferably 0 to 20 parts by mass, more preferably 0 to 15 parts by mass, and may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 parts by mass, and may be within a range between any two of the numerical values exemplified here. The composition according to one embodiment of the present invention may not contain the second monomer unit. By setting the content of the second monomer unit within the above range, a binder having a suitable gel fraction and suitable flexibility can be obtained. In this embodiment, the content of the second monomer unit in the composition refers to the total amount of the second monomer unit in the graft copolymer and the second monomer unit in the free polymer containing the second monomer unit, which are contained in the composition.
[0036] The composition according to one embodiment of the present invention preferably contains 0.1 to 20 parts by mass of the structure derived from the crosslinking agent and the second monomer unit in total, more preferably 0.1 to 15 parts by mass, when the composition is 100 parts by mass. The total content of the structure derived from the crosslinking agent and the second monomer unit is, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 parts by mass, and may be within a range between any two of the numerical values exemplified here. By setting the total content of the structure derived from the crosslinking agent and the second monomer unit within the above range, a binder having appropriate flexibility can be obtained while controlling the gel fraction.
[0037] 1-9. Characteristics of the composition (DMSO soluble fraction (gel fraction)) The composition according to one embodiment of the present invention has a gel fraction of 30% or more. In one aspect, it is preferably 50% or more, more preferably 60% or more, and most preferably 65% or more. The upper limit of the gel fraction can be, for example, 95%. The gel fraction can be, for example, any of 30, 40, 50, 60, 65, 70, 75, 80, 85, 90, and 95%, and may be within a range between any two of the values exemplified here. According to the composition according to one embodiment of the present invention, by controlling the gel fraction within the above range, it is possible to maintain the pore volume while appropriately controlling the electrolyte solution that penetrates into the interior of the composition, and it is presumed that this makes it possible to have high battery characteristics and suppress the decrease in discharge capacity during high-temperature storage.
[0038] As described later, the gel fraction of a composition is an index of the gel content contained in the composition, and is evaluated as the ratio of components in the composition that are insoluble in DMSO when the composition is mixed with DMSO. The gel fraction is related to the type and amount of each component contained in the composition and the structure of the composition, and more specifically, is affected by the graft ratio and the degree of crosslinking, and for example, it is considered that the more crosslinked parts there are, the higher the gel fraction tends to be. Therefore, the gel fraction of the composition can be adjusted by controlling the contents of PVA, the first monomer unit, the second monomer unit and the crosslinking agent and the structure of the composition. Specifically, it can be controlled by adjusting the balance of the types and amounts of the raw materials of the composition, as well as the conditions for graft copolymerization, etc.
[0039] (swelling rate) The composition according to one embodiment of the present invention has a swelling ratio in an electrolytic solution at 25° C. for 15 days of preferably 90 to 230%, more preferably 100 to 220%, and more preferably 105 to 210%. Here, the swelling ratio in an electrolytic solution at 25° C. for 15 days means the swelling ratio after the composition is immersed in an electrolytic solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 at 25° C. for 15 days. The swelling ratio of the composition when immersed in an electrolytic solution at 25° C. for 15 days is, for example, any of 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 150, 160, 170, 180, 190, 200, 210, 220, and 230%, and may be within a range between any two of the numerical values exemplified here. According to the composition of one embodiment of the present invention, by controlling the swelling ratio within the above range, it is possible to maintain the pore volume, particularly in the high rate region, while maintaining appropriate flexibility, and it is presumed that this makes it possible to have excellent battery characteristics and suppress the decrease in discharge capacity during high-temperature storage.
[0040] 1-10.Various measurement / calculation methods (DMSO insoluble matter (gel fraction)) The gel fraction of the composition is evaluated by dissolving the composition in DMSO and stirring the mixture at a predetermined temperature for a predetermined time, based on the insoluble content. Specifically, the gel fraction of the composition can be evaluated by the following method. 1 g of the obtained composition and 300 ml of DMSO are added to a 500 ml beaker and stirred at 60°C for 15 hours. The obtained mixture is then filtered with a Kiriyama funnel using No. 5C filter paper (retention particles 1 μm) specified in JIS P 3801, and the residue remaining on the filter paper is the insoluble part (gel part), and the filtrate is the soluble part. The insoluble part (gel part) is vacuum dried at 100°C for 24 hours and weighed. The insoluble part is taken as Ag, and the gel fraction (%) = A × 100 / 1 is calculated.
[0041] (Swelling ratio of composition (25°C, 15 days)) The swelling ratio of a composition in an electrolyte solution indicates the change in mass before and after a film made of the composition is immersed in an electrolyte solution for a predetermined time at a predetermined temperature. The swelling ratio can be determined, for example, by the following method. The obtained composition is dissolved in NMP to prepare a 4% by mass NMP solution. 5.6 g of the obtained solution is added to a petri dish of PTFE (tetrafluoroethylene) and dried for 8 hours at 105°C with a blower dryer to obtain a film with a thickness of 250 μm. The center part of the obtained film is cut to 5 mm x 5 mm to be used as a test film. The obtained test film is measured for mass, and then immersed in an electrolyte solution in which ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:2. After leaving it at 25°C for 15 days, the liquid on the film surface is wiped off and the mass after immersion is measured. The swelling ratio is calculated from the change in mass before and after immersion using the following formula. The swelling ratio is calculated from the following formula, where WA (g) is the mass before immersion and WB (g) is the mass after immersion. Swelling ratio (25°C, 15 days) (%) = WB × 100 / WA Equation (1) WA: Mass before immersion (g) WB: Mass after immersion (g)
[0042] By changing the conditions for immersion in the electrolyte, it is possible to obtain the swelling ratio under different conditions. For example, by changing the conditions for immersion in the electrolyte to 60°C for 48 hours, the swelling ratio when immersed in the electrolyte at 60°C for 48 hours can be obtained, and the swelling ratio can be evaluated in a short period of time.
[0043] (Content of polyvinyl alcohol structure, first monomer unit, second monomer unit, and structure derived from crosslinking agent) The composition according to one embodiment of the present invention contains a component derived from PVA and a component derived from a first monomer, and optionally contains a component derived from a second monomer and / or a component derived from a crosslinking agent. The content of each component in the composition can be roughly calculated from the amount of the components charged for graft polymerization. More precisely, the content of each component can be calculated by determining the reaction rate of each component by the following method. The content of each component can also be calculated from the integral ratio of the obtained composition by NMR.
[0044] The reaction rate of polyvinyl alcohol can be calculated by the following method. First, the concentration of PVA in the raw material solution is calculated by absorbance. Next, a polymerization reaction is carried out to obtain a polymerization reaction liquid, and 50 g of the obtained polymerization reaction liquid is centrifuged at 3000G for 30 minutes to obtain a supernatant. The absorbance of the supernatant is measured to determine the PVA concentration. The reaction rate of PVA is calculated by {1-(PVA concentration in the supernatant) / (PVA concentration at the time of charging)} x 100. The reaction rates of the first monomer, the second monomer, and the crosslinking agent can be determined by the following method. After the polymerization is completed, the product is precipitated with methanol, and the dried product is dissolved in deuterated DMSO. 1 1H-NMR is measured. From the intensity of the signals in the obtained spectrum corresponding to PVA, the first monomer, the second monomer, and the crosslinking agent, the composition of each component is calculated with PVA as the standard. The composition calculated from NMR is compared with the composition of each component at the time of charging, and the reaction rate is calculated, which indicates the extent to which the first monomer, second monomer, and crosslinking agent are contained in the composition out of the first monomer, second monomer, and crosslinking agent charged.
[0045] (graft rate) When producing a graft copolymer (graft copolymerization), a free polymer containing at least one of the group consisting of the first monomer, the second monomer, and the crosslinking agent may be produced. Calculation of the graft ratio requires a process of separating the free polymer from the graft copolymer. The free polymer dissolves in dimethylformamide (hereinafter sometimes abbreviated as DMF), but PVA and the graft copolymer do not dissolve in DMF. By utilizing this difference in solubility, the free polymer can be separated by an operation such as centrifugation. Where: F: Mass of component dissolved in DMF (g) G: Mass of the composition used in the test (g) H: Total content (mass%) of the first monomer unit and the second monomer unit in the composition Then, the graft ratio can be calculated by the following formula (2). [(GF) / (G×(100-H) / 100)]×100...Equation (2)
[0046] (Molecular weight of free polymer other than trunk polymer) 1.00 g of the composition is weighed out and added to 50 cc of special grade DMF (manufactured by Kokusan Chemical Co., Ltd.), and stirred at 1000 rpm for 24 hours at 80°C. Next, this is centrifuged at 10,000 rpm for 30 minutes in a centrifuge (model: H2000B, rotor: H) manufactured by Kokusan Co., Ltd. The filtrate (DMF soluble matter) is carefully separated and then poured into 1000 ml of methanol to obtain a precipitate. The precipitate is vacuum dried at 80°C for 24 hours, and the weight average molecular weight in terms of standard polystyrene is measured by GPC. The GPC measurement can be performed, for example, under the following conditions. Column: Two GPC LF-804 columns, φ8.0×300 mm (Showa Denko K.K.) were connected in series. Column temperature: 40℃ Solvent: 20mM LiBr / DMF
[0047] 1-11. Method for producing composition containing graft copolymer Although there is no particular limitation on the method for producing the composition including the graft copolymer according to one embodiment of the present invention, the method for producing the composition according to one embodiment of the present invention preferably includes a graft copolymerization step of graft copolymerizing a raw material including at least polyvinyl alcohol and a first monomer. That is, the composition according to one embodiment of the present invention is preferably obtained by a production method including a graft copolymerization step of graft copolymerizing a raw material including at least polyvinyl alcohol and a first monomer. In addition, the production method according to one embodiment of the present invention preferably further includes a vinyl acetate polymerization step of polymerizing vinyl acetate to obtain polyvinyl acetate, and a saponification step of saponifying the obtained polyvinyl acetate to obtain polyvinyl alcohol.
[0048] [Production method of polyvinyl alcohol (PVA)] As a method for polymerizing polyvinyl acetate, any known method such as bulk polymerization or solution polymerization can be used.
[0049] Examples of initiators used in the polymerization of polyvinyl acetate include azo-based initiators such as azobisisobutyronitrile, and organic peroxides such as benzoyl peroxide and bis(4-t-butylcyclohexyl)peroxydicarbonate.
[0050] The saponification reaction of polyvinyl acetate can be carried out, for example, in an organic solvent in the presence of a saponification catalyst.
[0051] Examples of the organic solvent include methanol, ethanol, propanol, ethylene glycol, methyl acetate, ethyl acetate, acetone, methyl ethyl ketone, benzene, toluene, etc. These may be used alone or in combination. Among these, methanol is preferred.
[0052] Examples of the saponification catalyst include basic catalysts such as sodium hydroxide, potassium hydroxide, sodium alkoxide, etc., and acidic catalysts such as sulfuric acid, hydrochloric acid, etc. Among these, sodium hydroxide is preferred from the viewpoint of saponification rate. The degree of polymerization of polyvinyl alcohol can be controlled by adjusting the type and amount of the initiator, and the temperature and time during polymerization, and the degree of saponification of polyvinyl alcohol can be controlled by adjusting the type and amount of the saponification catalyst, and the temperature and time during saponification. The degree of polymerization and the degree of saponification of polyvinyl alcohol are preferably adjusted within the above-mentioned ranges.
[0053] [Method of producing the composition] The manufacturing method according to one embodiment of the present invention preferably includes a step of graft copolymerizing a raw material containing at least polyvinyl alcohol and a first monomer, and the raw material containing at least polyvinyl alcohol and the first monomer may further include a crosslinking agent. Also, the raw material containing at least polyvinyl alcohol and the first monomer may further include a second monomer. In the production method according to one embodiment of the present invention, the gel fraction is adjusted to fall within the above-mentioned range by adjusting the types and amounts of raw materials used in the graft copolymerization, polymerization conditions, and the like. The polyvinyl alcohol used in the graft copolymerization preferably has the above-mentioned degree of polymerization and degree of saponification, and the first monomer, the second monomer, and the crosslinking agent used in the graft copolymerization preferably are the above-mentioned types of the first monomer, the second monomer, and the crosslinking agent. The blending amount during graft copolymerization is preferably adjusted so that the content of each component in the composition of the graft copolymerization satisfies the requirements for the content of each component in the composition described above. For example, when the raw material to be subjected to graft copolymerization is 100 parts by mass, the raw material to be subjected to graft copolymerization preferably contains 0.2 to 10 parts by mass of the crosslinking agent, more preferably contains 0.5 to 8 parts by mass, and particularly preferably contains 1 to 5 parts by mass. The content of the crosslinking agent in the raw material to be subjected to graft copolymerization is, for example, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0054] The method for graft-copolymerizing a monomer onto polyvinyl alcohol includes, for example, a solution polymerization method, and examples of the solvent used include water, dimethyl sulfoxide, and N-methylpyrrolidone.
[0055] As the initiator used in the graft copolymerization, a peroxide is preferable. Examples of the peroxide include organic peroxides such as benzoyl peroxide and inorganic peroxides. Among the peroxides, inorganic peroxides are preferable. Examples of the inorganic peroxides that can be used include potassium persulfate and ammonium persulfate. Among the inorganic peroxides, ammonium persulfate is preferable.
[0056] The graft copolymer according to one embodiment of the present invention can be used by dissolving it in a solvent. Examples of the solvent include dimethyl sulfoxide, N-methylpyrrolidone, etc. The composition and the slurry for the positive electrode described below may contain these solvents.
[0057] 1-12.Other The composition according to one embodiment of the present invention may contain other components, such as resins, within a range that does not impair the effects of the present invention. Examples of such resins include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene, styrene-butadiene copolymers (styrene butadiene rubber, etc.), and acrylic copolymers. Among these, fluororesins, particularly polyvinylidene fluoride, are preferred from the viewpoint of stability.
[0058] 2. Positive electrode slurry The positive electrode slurry according to one embodiment of the present invention includes the above composition and has excellent stability. The positive electrode slurry according to one embodiment of the present invention includes the above composition and can produce a positive electrode with excellent rate characteristics. The positive electrode slurry may include the composition and a conductive assistant, or may include the composition, a positive electrode active material, and a conductive assistant.
[0059] In the positive electrode slurry according to one embodiment of the present invention, the solid content of the positive electrode (binder) composition is preferably 0.1 to 20 mass %, and more preferably 1 to 10 mass %, relative to the total amount of solids in the positive electrode slurry.
[0060] 3. Lithium-ion secondary battery A secondary battery is preferred as a battery having a positive electrode according to an embodiment of the present invention. The secondary battery is preferably one or more selected from a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, and a potassium ion secondary battery, and more preferably a lithium ion secondary battery. The positive electrode according to one embodiment of the present invention and the lithium ion secondary battery including the positive electrode can be produced using a positive electrode slurry containing the above composition. Preferably, the positive electrode, the negative electrode, the separator, and the electrolyte solution (hereinafter, also referred to as electrolyte or electrolyte solution) are included.
[0061] [Positive electrode] The positive electrode according to one embodiment of the present invention can be produced by applying a positive electrode slurry containing a composition, a conductive assistant, and a positive electrode active material used as necessary onto a current collector such as aluminum foil, removing the solvent contained in the slurry by heating, and then pressing the current collector and the electrode mixture layer together by a roll press or the like to make them adhere to each other. That is, a positive electrode is obtained that includes a metal foil and a coating of the positive electrode slurry formed on the metal foil.
[0062] [Conductive additive] The conductive aid is preferably at least one selected from the group consisting of (i) fibrous carbon, (ii) carbon black, and (iii) a carbon composite in which fibrous carbon and carbon black are interconnected. Examples of the fibrous carbon include vapor-grown carbon fiber, carbon nanotube, and carbon nanofiber. Examples of the carbon black include acetylene black, furnace black, and Ketjenblack (registered trademark). These conductive aids may be used alone or in combination of two or more. Among these, from the viewpoint of high effect of improving the dispersibility of the conductive aid, one or more selected from acetylene black, carbon nanotube, and carbon nanofiber are preferable. The slurry for the positive electrode according to one embodiment of the present invention preferably has a solid content of the conductive aid of 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, based on the total solid content in the slurry for the positive electrode.
[0063] [Positive electrode active material] A positive electrode active material may be used as necessary. The positive electrode active material is preferably a positive electrode active material capable of reversibly occluding and releasing cations. The positive electrode active material is preferably a lithium-containing composite oxide or a lithium-containing polyanion compound containing Mn with a volume resistivity of 1×10 4 Ω·cm or more. For example, LiCoO2, LiMn2O4, LiNiO2, LiMPO4, Li2MSiO4, LiNi X Mn (2-X) O4, Li(Co X Ni Y Mn Z )O2, Li(Ni X Co Y Al Z )O2, or XLi2MnO3-(1-X)LiMO2, etc. are mentioned. However, X in LiNi X Mn (2-X) O4 satisfies the relationship of 0 < X < 2, and in Li(Co X Ni Y Mn Z )O2 or Li(Ni X Co Y Al Z) X, Y, and Z in O2 satisfy the relationship X + Y + Z = 1 and the relationships 0 < X < 1, 0 < Y < 1, 0 < Z < 1. X in XLi2MnO3-(1-X)LiMO2 satisfies the relationship 0 < X < 1. Further, in LiMPO4, Li2MSiO4, or XLi2MnO3-(1-X)LiMO2, M is preferably one or more elements selected from Fe, Co, Ni, and Mn. Among the cathode active materials, LiNi X Mn (2-X) O4 (where 0 < X < 2), Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) and Li(Ni X Co Y Al Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) is preferably selected, and one or more selected from LiNi X Mn (2-X) O4 (where 0 < X < 2) and Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) is more preferably selected. The slurry for the cathode according to one embodiment of the present invention preferably has a solid content of the cathode active material of 50 to 99.8% by mass, more preferably 80 to 99.5% by mass, and most preferably 95 to 99.0% by mass, based on the total solid content of the slurry for the cathode.
[0064] [Negative electrode] The negative electrode used in the lithium ion secondary battery according to one embodiment of the present invention can be manufactured using a negative electrode slurry containing a negative electrode active material, although it is not particularly limited. This negative electrode can be manufactured, for example, using a metal foil for a negative electrode and a negative electrode slurry provided on the metal foil. The negative electrode slurry preferably contains a negative electrode binder (a negative electrode composition), a negative electrode active material, and the above-mentioned conductive assistant. The negative electrode binder is not particularly limited, but for example, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene copolymer (styrene butadiene rubber, etc.), acrylic copolymer, etc. can be used. The negative electrode binder is preferably a fluorine-based resin. As the fluorine-based resin, one or more of the group consisting of polyvinylidene fluoride and polytetrafluoroethylene is more preferable, and polyvinylidene fluoride is most preferable.
[0065] Examples of the negative electrode active material used in the negative electrode include carbon materials such as graphite, polyacene, carbon nanotubes, and carbon nanofibers, alloy materials such as tin and silicon, and oxide materials such as tin oxide, silicon oxide, and lithium titanate. These may be used alone or in combination. The metal foil for the negative electrode is preferably copper foil, and the thickness is preferably 5 to 30 μm from the viewpoint of workability. The negative electrode can be manufactured using the negative electrode slurry and the negative electrode metal foil by a method similar to the above-mentioned method for manufacturing the positive electrode.
[0066] [Separator] The separator can be made of an electrically insulating porous film, net, nonwoven fabric, fiber, or the like, as long as it has sufficient strength. In particular, it is preferable to use a separator that has low resistance to ion movement of the electrolyte and excellent solution retention. The material is not particularly limited, but examples include inorganic fibers such as glass fibers or organic fibers, olefins such as polyethylene and polypropylene, synthetic resins such as polyester, polytetrafluoroethylene, and polyflon, or layered composites thereof. From the viewpoint of binding and stability, olefins or layered composites thereof are preferred. As the olefin, one or more members of the group consisting of polyethylene and polypropylene are preferred.
[0067] [Electrolytes] As the electrolyte, any known lithium salt can be used, for example, LiClO4, LiBF4, LiBF6, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiI, LiB(C2H5)4, LiCF3SO3, LiCH3SO3, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiC(CF3SO2)3, and lithium lower fatty acid carboxylates.
[0068] [Electrolyte] The electrolyte in which the electrolyte is dissolved is not particularly limited. Examples of the electrolyte include carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate, lactones such as γ-butyrolactone, ethers such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, and 2-methyltetrahydrofuran, sulfoxides such as dimethyl sulfoxide, oxolanes such as 1,3-dioxolane and 4-methyl-1,3-dioxolane, nitrogen-containing compounds such as acetonitrile, nitromethane, and N-methyl-2-pyrrolidone, methyl formate, methyl acetate, and the like. Examples of the electrolyte include esters such as ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, and phosphoric acid triesters, inorganic acid esters such as sulfates, nitrates, and hydrochlorides, amides such as dimethylformamide and dimethylacetamide, glymes such as diglyme, triglyme, and tetraglyme, ketones such as acetone, diethyl ketone, methyl ethyl ketone, and methyl isobutyl ketone, sulfolanes such as sulfolane, oxazolidinones such as 3-methyl-2-oxazolidinone, and sultones such as 1,3-propane sultone, 4-butane sultone, and naphtha sultone. At least one of these electrolytes can be used. The electrolyte preferably contains a carbonate, and more preferably contains ethylene carbonate or diethyl carbonate.
[0069] Among the above electrolytes and electrolytic solutions, an electrolytic solution in which LiPF6 is dissolved in a carbonate is preferred, an electrolytic solution in which LiPF6 is dissolved in a mixed solution containing ethylene carbonate and diethyl carbonate is more preferred, and an electrolytic solution in which LiPF6 is dissolved in a mixed solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 is even more preferred. The concentration of the electrolyte in the solution varies depending on the electrode and electrolytic solution used, but is preferably 0.5 to 3 mol / L.
[0070] Applications of the lithium ion secondary battery according to the embodiment of the present invention are not particularly limited, and examples thereof include portable AV devices such as digital cameras, video cameras, portable audio players, and portable LCD televisions, portable information terminals such as notebook personal computers, smartphones, and mobile PCs, as well as a wide range of other fields such as portable game devices, power tools, electric bicycles, hybrid automobiles, electric automobiles, and power storage systems. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples. These are merely illustrative examples and do not limit the scope of the present invention. Data are shown in Table 1.
[0072] [Example 1] The PVA used was PVA (B-17) manufactured by Denka Co., Ltd. The average polymerization degree and saponification degree of the obtained PVA are shown in Table 1. The average polymerization degree and saponification degree of PVA were measured in accordance with JIS K 6726.
[0073] <Preparation of Composition> A reaction vessel was charged with 1,804 parts by mass of pure water, and after deoxygenation by bubbling nitrogen gas, 100 parts by mass of partially saponified PVA (saponification degree 85.6%, polymerization degree 1700) was charged at room temperature and dissolved by heating to 90°C. The reaction vessel was adjusted to 60°C, and 170 parts by mass of a 10% aqueous solution of ammonium persulfate that had been deoxygenated by bubbling nitrogen gas separately was added all at once, followed by 96 parts by mass of acrylonitrile and the crosslinking agent oligoethylene glycol diacrylate (the number of ethylene glycol repeats in general formula (B) is n = 9, R 21 , R 22 is hydrogen.) (manufactured by Shin-Nakamura Chemical Co., Ltd., product name: A-400) 8 parts by mass of the mixed solution was added over 5 hours to polymerize. 100 parts by mass of the obtained polymerization solution was added to 300 parts by mass of methanol, and the precipitate was filtered under reduced pressure and dried at 40°C for 12 hours to obtain a resin composition. The composition of the obtained composition containing the graft copolymer is shown in Table 1.
[0074] <Composition ratio> The composition ratio of each component of the obtained composition was calculated based on the reaction rate of Example 2 described later. This composition ratio includes the free polymer (homoPAN), which is a homopolymer of the first monomer. The results are shown in Table 1.
[0075] <Evaluation method> (DMSO insoluble matter (gel fraction)) 1 g of the obtained composition and 300 ml of DMSO were added to a 500 ml beaker and stirred at 60° C. for 15 hours. The obtained mixture was then filtered with a Kiriyama funnel using No. 5C filter paper specified in JIS P 3801, and the residue remaining on the filter paper was taken as the insoluble part (gel content), and the filtrate was taken as the soluble part. The insoluble part (gel content) was vacuum dried at 100° C. for 24 hours and weighed. The insoluble part was taken as Ag, and the gel fraction (%) was calculated as A×100 / 1.
[0076] (graft rate) 1.00 g of the obtained composition containing the graft copolymer was weighed out and added to 50 cc of special grade DMF (manufactured by Kokusan Chemical Co., Ltd.), and stirred at 1000 rpm for 24 hours at 80°C. Next, this was centrifuged at 10000 rpm for 30 minutes in a centrifuge (model: H2000B, rotor: H) manufactured by Kokusan Co., Ltd. The filtrate (DMF soluble matter) was carefully separated, and the DMF insoluble matter was vacuum dried at 100°C for 24 hours, and the graft ratio was calculated using the following formula. [(GF) / (G×(100-H) / 100)]×100...Equation (3) F: Mass of component dissolved in DMF (g) G: Mass of the composition used in the test (g) H: Total content (mass%) of the first monomer unit and the second monomer unit in the composition
[0077] (Swelling ratio of composition (25°C, 15 days)) The obtained composition was dissolved in NMP to prepare 4% by mass NMP. 5.6 g of the obtained solution was added to a petri dish of PTFE (tetrafluoroethylene) and dried at 105 ° C. for 8 h with a blower dryer to obtain a film with a thickness of 250 μm. The center part of the obtained film was cut to 5 mm × 5 mm to be used as a test film. The obtained test film was measured for mass, and then immersed in an electrolyte solution in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed at a volume ratio of 1:2. After leaving it at 25 ° C. for 15 days, the liquid on the film surface was wiped off and the mass after immersion was measured. The swelling ratio was calculated from the change in mass before and after immersion using the following formula. The swelling ratio was calculated from the following formula, with the mass before immersion being WA (g) and the mass after immersion being WB (g). Swelling ratio (25°C, 15 days) (%) = WB × 100 / WA Equation (4) WA: Mass before immersion (g) WB: Mass after immersion (g)
[0078] (Swelling ratio of composition (60°C, 48 hours)) The swelling ratio when immersed in the electrolyte at 60°C for 48 hours was determined in the same manner as in (Swelling ratio of composition (25°C, 15 days)), except that the immersion conditions in the electrolyte were set to 60°C for 48 hours.
[0079] <Preparation of slurry> A mixture of 1 part by mass of the obtained binder, 2 parts by mass of acetylene black (manufactured by Denka Co., Ltd., Denka Black (registered trademark) "Li435"), and NMC532 (LiNi 0.5 Mn 0.3 Co 0.2 O2 (Umicore, TX-10) (97 parts by mass) was dissolved in 66 parts by mass of N-methyl-2-pyrrolidone (hereinafter abbreviated as NMP) to prepare a slurry for forming a positive electrode.
[0080] <Preparation of positive electrode> The prepared positive electrode slurry was applied to an aluminum foil with a thickness of 20 μm at a rate of 140 g / m using an automatic coater. 2The coating was applied so that the thickness of the positive electrode plate was 75 μm, and the positive electrode plate was pre-dried at 105°C for 30 minutes. The positive electrode plate was then pressed with a roll press at a linear pressure of 0.1 to 3.0 ton / cm, and the thickness of the positive electrode plate was adjusted to 75 μm. The positive electrode plate was then punched out into a circle of 13 mm in diameter. In order to completely remove volatile components such as residual solvent and adsorbed moisture, the positive electrode was obtained by drying at 170°C for 6 hours. The electrode area density was 29.0 mg / cm. 2 , volume density is 3.4g / cm 3 It was.
[0081] <Production of lithium-ion secondary battery> A 2032-type coin cell was fabricated using the obtained positive electrode and metallic lithium as a counter electrode. An electrolyte (a mixed solution of ethylene carbonate / diethyl carbonate = 1 / 2 (volume ratio)) in which LiPF6 was dissolved at a concentration of 1 mol / L was used as the electrolyte. A 15Φmm nonwoven fabric made of olefin fiber was used as a separator to electrically isolate them. The battery performance of the fabricated lithium-ion secondary battery was evaluated by the following method.
[0082] <Battery characteristics> The battery characteristics of the obtained battery were evaluated under the following measurement conditions. Charging conditions: CC-CV method, CC current = 0.2C, CV voltage = 4.2V, cutoff current = 1 / 20C Discharge conditions: CC method, CC current = 0.2, 0.5, 1.0, 2.0, 2.8C, cutoff voltage = 3.0V Temperature conditions: 25℃ After first charging the battery, confirm that the charge / discharge efficiency is close to 100%, then charge at 0.20mA / cm 2 The discharge capacity was measured when constant current discharge was performed at a current density of 100 V to 3.0 V, and the capacity density (mAh / g) was calculated by dividing the capacity by the amount of positive electrode active material. The current value at which this capacity (mAh) can be charged and discharged in 1 hour was defined as "1C."
[0083] <DC resistance> Currents of 0.2, 0.4, 0.6, 0.8, and 1.0 mmA were applied to an electrode of φ13 mm × 75 μm prepared in the same manner as the positive electrode described above, and the voltage was read after 10 seconds, and the resistance value was calculated using Ohm's law. Volume resistivity (Ω cm) was measured using the two-terminal method. It can be expressed by the following formula, where V is the potential difference, S is the cross-sectional area, I (A) is the current, and L (cm) is the electrode thickness. Volume resistivity (Ω cm) = (V×S) / (I×L) Formula (3)
[0084] <High temperature storage characteristics> The obtained lithium secondary battery was charged to 4.3 V at a constant current of 0.2 C (fully charged). It was placed in an environmental test chamber at 60° C. and stored for 30 days. After 30 days, it was discharged to 3.0 V at a constant current of 0.2 C at 25° C., and the high-temperature storage characteristics were calculated using the following formula. The high temperature storage characteristic (%) was calculated as follows: [(discharge capacity after storage)÷(charge capacity before storage)]×100. The obtained high-temperature storage characteristics were compared with those of a lithium secondary battery using PVDF as a positive electrode binder according to Reference Example 1 described later, and evaluated according to the following criteria. The results are shown in Table 1. ○: Equivalent to a lithium secondary battery using PVDF as a positive electrode binder △: Compared to the lithium secondary battery using PVDF as the positive electrode binder, the high-temperature storage characteristics are poor, and the difference is within 5%. X: Compared to a lithium secondary battery using PVDF as a positive electrode binder, the high-temperature storage characteristics are poor, and the difference is more than 5% and less than 15%.
[0085] [Example 2] <Preparation of polyvinyl alcohol (PVA)> The PVA used was PVA (B-24) manufactured by Denka Co., Ltd. The average polymerization degree and saponification degree of the PVA are shown in Table 1.
[0086] <Preparation of Composition> A composition was obtained in the same manner as in Example 1, except that the blending amounts were as shown in Table 1. The results are shown in Table 1.
[0087] <Reaction rate and composition ratio> For the resulting composition, the reaction rate of each raw material and the composition ratio of each component were calculated. The reaction rate of polyvinyl alcohol was determined by the following method. First, the concentration of PVA in the raw material solution was determined by absorbance. Next, 50 g of the polymerization reaction solution obtained in the polymerization reaction was centrifuged at 3000G for 30 minutes to obtain a supernatant. The absorbance of the supernatant was measured to determine the PVA concentration. The reaction rate of PVA was calculated by {1-(PVA concentration in the supernatant) / (PVA concentration at the time of charging)}×100. The reaction rate of PVA was 93%.
[0088] The reaction rates of the first monomer and the crosslinking agent were determined by the following method. After the polymerization was completed, the product was precipitated with methanol, and the dried product was dissolved in deuterated DMSO. 1 H-NMR was measured. From the intensity of the signals corresponding to PVA, the first monomer, and the crosslinking agent in the obtained spectrum, the composition of each component was calculated with PVA as the standard. Signals from PVA, PAN and vinyl acetate, PAN, and the crosslinking agent were observed at 1 to 1.7 ppm, 1.7 to 2.3 ppm, 3 to 3.2 ppm, and 3.5 to 3.7 ppm, respectively. The reaction rate was calculated by comparing the composition calculated from NMR with the composition of each component at the time of charging. The reaction rate indicates the extent to which the first monomer and crosslinking agent are contained in the composition out of the first monomer and crosslinking agent charged. The reaction rate of the first monomer was 98%, and the reaction rate of the crosslinking agent was 100%.
[0089] In addition, the composition ratio of each component of the composition according to Example 2 was calculated from the reaction rate. When the composition was 100 parts by mass, the content of the polyvinyl alcohol structure was 47.7 parts by mass, the content of the first monomer unit was 48.2 parts by mass, and the content of the structure derived from the crosslinking agent was 4.2 parts by mass. This composition ratio includes a free polymer that is a homopolymer of the first monomer.
[0090] [Comparative Example 1] <Preparation of polyvinyl alcohol (PVA)> The PVA used was PVA (F-12) manufactured by Denka Co., Ltd. The average polymerization degree and saponification degree of the PVA are shown in Table 1.
[0091] <Preparation of Composition> A composition was obtained in the same manner as in Example 1, except that the amount of acrylonitrile added to the PVA was as shown in Table 1.
[0092] <Reaction rate and composition ratio> The reaction rate of each raw material and the composition ratio of each component were calculated in the same manner as in Example 2. The results are shown in Table 1.
[0093] [Reference example 1] Polyvinylidene fluoride resin (HSV900: manufactured by Arkema) was used as the positive electrode composition. The results are shown in Table 1.
[0094] The abbreviations used in the following tables represent the following compounds. The monomer units represent the monomers from which the monomer units are derived. AN: Acrylonitrile OEG: Oligoethylene glycol diacrylate
[0095] [Table 1]
Claims
1. A composition containing a graft copolymer, The graft copolymer has a trunk polymer and a branch polymer, the trunk polymer comprises a polyvinyl alcohol structure, the branch polymer comprises a first monomer unit comprising a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer; The first monomer unit includes a (meth)acrylonitrile monomer unit, The composition has a gel fraction of 30% or more, The gel fraction is calculated by adding 1 g of the composition to 300 ml of dimethyl sulfoxide, stirring at 60° C. for 15 hours, filtering through No. 5C filter paper specified in JIS P 3801, and expressing the insoluble matter remaining as a residue on the filter paper as Ag, as follows: gel fraction %=A×100 / 1.
2. The composition further comprises a free polymer; the free polymer has no covalent bond to the graft copolymer; The free polymer includes at least a polymer including a polyvinyl alcohol structure and / or a polymer including the first monomer unit; The composition of claim 1.
3. The composition according to claim 1 or claim 2, wherein the graft copolymer further comprises a crosslinked portion derived from a crosslinking agent.
4. The composition according to claim 3 , wherein the crosslinking portion comprises an ether structure.
5. The composition according to claim 3 or claim 4, wherein the composition contains 0.2 to 10 parts by mass of a structure derived from the crosslinking agent when the composition is taken as 100 parts by mass.
6. The composition according to any one of claims 1 to 5, wherein the composition has a swelling ratio of 90 to 230% after immersion in an electrolytic solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 at 25°C for 15 days.
7. The composition according to any one of claims 1 to 6, wherein the graft ratio of the graft copolymer is 40 to 3000%.
8. The composition according to any one of claims 1 to 7, wherein the degree of saponification of the polyvinyl alcohol structure in the composition is 60 to 100 mol %.
9. The composition according to any one of claims 1 to 8, wherein an average degree of polymerization of the polyvinyl alcohol structure in the composition is from 300 to 4,000.
10. A positive electrode composition comprising the composition according to any one of claims 1 to 9.
11. A positive electrode slurry comprising the positive electrode composition according to claim 10, a positive electrode active material, and a conductive assistant.
12. The positive electrode slurry according to claim 11, wherein the solid content of the positive electrode composition is 1 to 20 mass% when the total amount of solids in the positive electrode slurry is 100 mass%.
13. 13. The positive electrode slurry according to claim 11 or 12, wherein the conductive assistant is at least one selected from the group consisting of fibrous carbon, carbon black, and a carbon composite in which fibrous carbon and carbon black are mutually bonded.
14. A positive electrode comprising a metal foil and a coating of the positive electrode slurry according to any one of claims 11 to 13 formed on the metal foil.
15. 15. A secondary battery comprising the positive electrode according to claim 14, wherein the secondary battery is one or more types selected from the group consisting of a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, or a potassium ion secondary battery.
16. The positive electrode active material is LiNi X Mn (2-X) O 4 (where 0<X<2), Li(Co X Ni Y Mn Z ) O 2 (where 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1), and Li(Ni X Co Y A Z ) O 2 (wherein 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1), and the secondary battery is a lithium ion secondary battery.
Citation Information
Patent Citations
Vinylidene fluoride-based copolymer
JP1994172452A
Wrinkled absorbent particles with highly available surface area for fast absorption
JP1994506252A
Production of water absorptive gel solution
JP2000095823A
Binder for lithium ion secondary battery electrode and its utlization