Composition, resin composition, composition for positive electrode, slurry for positive electrode, positive electrode, and secondary battery

A binder composition with controlled molecular mobility addresses battery performance and high-temperature storage issues in lithium ion secondary batteries by optimizing component ratios and relaxation times, enhancing stability and resistance.

JP7575465B2Active Publication Date: 2024-10-29DENKA CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2022542867
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-12
Filing Date
2021-08-11
Publication Date
2024-10-29
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face issues with battery performance deterioration, high-temperature storage properties, and DC resistance, particularly in high-capacity electrodes.

Method used

A binder composition with specific component ratios and relaxation times, as determined by pulsed NMR, is used to enhance the balance of molecular mobility and electrolyte control, maintaining pore volume and reducing discharge capacity decline.

Benefits of technology

The composition effectively suppresses battery performance deterioration and maintains high-temperature storage characteristics and DC resistance, ensuring stable battery operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575465000001
    Figure 0007575465000001
  • Figure 0007575465000002
    Figure 0007575465000002
Patent Text Reader

Abstract

Provided are a composition serving as a binder having an excellent balance of suppressing deterioration of battery performance in a high-capacity electrode, high-temperature storage characteristics, and direct current resistance, and a slurry for a positive electrode, a positive electrode, and a secondary battery using said composition. Provided according to the present invention is a composition in which the component ratio of the component S180 is from 10% to 80% and the relaxation time of the component S180 is 500 μsec or longer when the free induction decay curve of the composition measured at 180°C by the solid echo method using pulse NMR is separated into three components: component S180, component M180, and component H180.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition, a resin composition, a composition for a positive electrode, a slurry for a positive electrode, a positive electrode, and a secondary battery. [Background technology]

[0002] In recent years, secondary batteries have been used as power sources for electronic devices such as notebook computers and mobile phones, and the development of hybrid and electric vehicles that use secondary batteries as power sources is underway to reduce the environmental impact. These power sources require secondary batteries with high energy density, high voltage, and high durability. Lithium-ion secondary batteries have attracted attention as secondary batteries that can achieve high voltage and high energy density.

[0003] A lithium ion secondary battery is composed of components such as a positive electrode, a negative electrode, an electrolyte, and a separator, and the positive electrode is composed of a positive electrode active material, a conductive assistant, a metal foil, and a binder (Patent Documents 1 to 3).

[0004] As a positive electrode binder for lithium ion secondary batteries, a binder (graft copolymer) containing polyvinyl alcohol and polyacrylonitrile as main components has been disclosed (Patent Document 4).

[0005] In addition, a composition containing a graft copolymer in which a monomer mainly composed of (meth)acrylonitrile and (meth)acrylic acid ester is graft-copolymerized onto a backbone polymer having polyvinyl alcohol has been disclosed as a positive electrode binder for lithium ion secondary batteries (Patent Document 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2013-98123 A [Patent Document 2] JP 2013-84351 A [Patent Document 3] Japanese Patent Application Publication No. 6-172452 [Patent Document 4] International Publication No. 2015 / 053224 [Patent Document 5] International Publication No. 2018 / 230599 Summary of the Invention [Problem to be solved by the invention]

[0007] However, there has been a demand for the development of a composition capable of obtaining a battery that is excellent in balance between suppressing deterioration of battery performance in a high-capacity electrode, high-temperature storage characteristics, and DC resistance, as well as a slurry for a positive electrode, a positive electrode, and a secondary battery that use the composition.

[0008] The present invention has been made in consideration of such problems, and provides a composition that serves as a binder that suppresses deterioration of battery performance in a high-capacity electrode and has an excellent balance between high-temperature storage characteristics and DC resistance, and a positive electrode slurry, a positive electrode, and a secondary battery that use the composition. [Means for solving the problem]

[0009] According to the present invention, the free induction decay curve of the composition measured at 180° C. by the Solid Echo method using pulse NMR is 180 , component M 180 , component H 180 When the mixture is separated into the three components S 180 The component ratio of the component S is 10% or more and 80% or less. 180 The relaxation time is 500 μs or more. A composition is provided.

[0010] The present inventors have conducted extensive research and found that the free induction decay curve of the composition measured at 180° C. by the Solid Echo method using pulsed NMR was 180 , component M 180 , component H 180 When the spectrum is separated into three components, the component S has a relaxation time of 500 μs or more. 180The inventors have found that by setting the component ratio within a predetermined range, when the composition is used as a binder for a positive electrode, it becomes a binder that suppresses the deterioration of battery performance in a high-capacity electrode, and has an excellent balance of high-temperature storage characteristics and DC resistance, and have thus completed the present invention.

[0011] Various embodiments of the present invention will be described below. The embodiments described below can be combined with each other. Preferably, said component H 180 The component ratio of said component H is 20% or more and 80% or less. 180 The relaxation time is less than 100 μsec. Preferably, the free induction decay curve of the composition measured at 27° C. using pulse NMR by the Solid Echo method is 27 , component M 27 , component H 27 When the mixture is separated into the three components H 27 The component ratio of said component H is 60% or more and less than 100%. 27 The relaxation time is less than 50 μsec. Preferably, said component M 180 The component ratio of said component M is 30% or more. 180 The relaxation time of the component S is more than 100 μsec and less than 500 μsec. 180 The component ratio of said component H is 50% or less. 180 The component ratio is 60% or less. Preferably, said component S 180 The component ratio of the component M 180 The sum of the component ratios of the components H 180 is greater than the component ratio. Preferably, the composition contains a graft copolymer, the graft copolymer having a trunk polymer and a branch polymer, the trunk polymer comprising a polyvinyl alcohol structure, and the branch polymer comprising a first monomer unit comprising a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer. Preferably, the composition further comprises a free polymer, the free polymer having no covalent bond with the graft copolymer, the free polymer comprising at least a polymer comprising the first monomer unit. Preferably, the graft copolymer further includes a crosslinked portion derived from a crosslinking agent. Preferably, when the composition is 100 parts by mass, the composition contains 0.2 to 10 parts by mass of a structure derived from the crosslinking agent. Preferably, the graft ratio of the graft copolymer is 40 to 3000%. Preferably, the degree of saponification of the polyvinyl alcohol structure in the composition is 60 to 100 mol%. Preferably, the average degree of polymerization of the polyvinyl alcohol structure in the composition is 300 to 4000. Preferably, it is a resin composition containing the composition. Preferably, it is a composition for a positive electrode containing the composition.

[0012] According to another aspect of the present invention, there is provided a slurry for a positive electrode containing the composition, a positive electrode active material, and a conductive assistant. Preferably, in the slurry for a positive electrode, when the total solid content in the slurry for a positive electrode is 100% by mass, the solid content of the composition is 1 to 20% by mass. Preferably, the conductive assistant is one or more selected from the group consisting of fibrous carbon, carbon black, and a carbon composite in which fibrous hydrocarbon and carbon black are interconnected. According to another aspect of the present invention, there is provided a positive electrode including a metal foil and a coating film of the slurry for a positive electrode according to any one of the above on the metal foil. According to another aspect of the present invention, there is provided a secondary battery including the positive electrode described above, wherein the secondary battery is one or more selected from the group consisting of a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, and a potassium ion secondary battery. Preferably, the positive electrode active material is LiNi X Mn (2-X) O4 (where 0 < X < 2), Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1), and Li(Ni XCo Y Al Z )O2 (provided that 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1), and a secondary battery is provided, where the secondary battery is a lithium-ion secondary battery.

Advantages of the Invention

[0013] The present invention provides a composition that, when used as a binder for a positive electrode, suppresses a decrease in battery performance in a high-capacity electrode, has excellent high-temperature storage characteristics, and is a binder with an excellent balance of DC resistance, a slurry for a positive electrode using the composition, a positive electrode, and a secondary battery.

Embodiments for Carrying Out the Invention

[0014] Hereinafter, embodiments of the present invention will be described. The various characteristic matters shown in the following embodiments can be combined with each other. Also, the invention can be achieved independently for each of the various characteristic matters.

[0015] 1. Composition The composition according to an embodiment of the present invention can be a resin composition. The resin composition according to an embodiment of the present invention includes the composition according to an embodiment of the present invention, and preferably consists of the composition according to an embodiment of the present invention. Also, the composition according to an embodiment of the present invention can be used as a composition for a positive electrode. The composition for a positive electrode according to an embodiment of the present invention includes the composition according to an embodiment of the present invention, and preferably consists of the composition according to an embodiment of the present invention. The composition according to an embodiment of the present invention, when using pulsed NMR and the Solid Echo method, measures the free induction decay curve of the composition at 180°C. When the curve is separated into three components: component S 180 , component M 180 , and component H 180 , the component ratio of component S 180 is 10% or more and 80% or less, and the relaxation time of component S 180 is 500 μs or more.

[0016] In general, the NMR method is known as a method for analyzing the structure of molecules. In particular, the pulsed NMR method makes it possible to evaluate the mobility of molecules from the relaxation time. When a magnetic field is applied as a pulse to a sample such as a resin composition, the nuclear spins of the protons in the sample are excited in a uniform direction. Here, the process in which this returns to the original random ground state is called relaxation, and the time required for this process is called relaxation time. The relaxation time depends on the molecular mobility of the sample, and a sample with high molecular mobility has a long relaxation time, while a sample with low molecular mobility has a short relaxation time. The free induction decay curve obtained by measuring a sample such as a resin composition by pulsed NMR can be separated into three components: a component S (a component with high molecular mobility) with a long relaxation time, a component M (a component with medium molecular mobility) with a medium relaxation time, and a component H (a component with low molecular mobility) with a short relaxation time. In other words, the measured component is the integrated value of the free induction decay curve derived from these multiple components. In addition, by performing pulse NMR measurements of resin compositions, etc. at high temperatures, the crystalline components in the composition are relaxed, and it is believed that it is possible to obtain information regarding the molecular mobility inside the structure, which is difficult to see at room temperature, in particular information regarding the soft components with high molecular mobility.

[0017] The composition according to one embodiment of the present invention has a free induction decay curve measured at 180° C. in which component S 180 The component ratio and relaxation time of the component S are within a predetermined range. 180 The component ratio is an index of the amount of molecules with high mobility. Since the composition according to one embodiment of the present invention has a predetermined amount of molecular structures with high mobility in the composition, it is presumed that the composition can maintain the pore volume while appropriately controlling the electrolyte solution that penetrates into the composition, has high battery characteristics, and can suppress the decrease in discharge capacity during high-temperature storage.

[0018] The composition according to one embodiment of the present invention is characterized in that the free induction decay curve of the composition measured at 180° C. using pulse NMR by the Solid Echo method is 180 , component M 180 , component H 180 When separated into three components, component S 180The component ratio of is 10% or more and 80% or less, and component S 180 The relaxation time of component S is 500 μs or more. 180 The ratio of component S is preferably 15% or more and 70% or less, and more preferably 20% or more and 60% or less. 180 The component ratio of component S may be, for example, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70, or 80%, or may be within a range between any two of the values ​​exemplified here. 180 The relaxation time is preferably 500 to 1500 μsec, and more preferably 550 to 1400 μsec.

[0019] The composition according to one embodiment of the present invention comprises component H 180 The component ratio is 20% or more and 80% or less, Component H 180 The relaxation time of component H is preferably 100 μsec or less. 180 The component ratio of component H is preferably 20% or more and 70% or less, and more preferably 20% or more and 60% or less. 180 The component ratio of component H may be, for example, 20, 25, 30, 35, 40, 45, 50, 60, 70, or 80%, or may be within a range between any two of the values ​​exemplified here. 180 The relaxation time is preferably 10 to 100 μsec, and more preferably 20 to 90 μsec. The composition according to one embodiment of the present invention has a free induction decay curve measured at 180° C. in which component H 180 It is presumed that by having the component ratio and relaxation time within a predetermined range and having an appropriate molecular structure with low mobility in the composition, it is possible to maintain the pore volume while more appropriately controlling the electrolyte that penetrates into the composition, thereby providing high battery characteristics and suppressing a decrease in discharge capacity during storage at high temperatures.

[0020] The composition according to one embodiment of the present invention comprises component M 180 The component ratio of component M is 30% or more. 180 The relaxation time of component M is preferably more than 100 μsec and less than 500 μsec. 180The component ratio of component M is preferably 30% or more and 70% or less, and more preferably 30% or more and 60% or less. 180 The relaxation time is preferably 110 to 400 μsec, and more preferably 120 to 300 μsec. In addition, component M 180 When the component ratio of is within the above range, component S 180 The component ratio of is 50% or less, and component H 180 The component ratio can be set to 60% or less.

[0021] The composition according to one embodiment of the present invention comprises component S 180 Component ratio and component M 180 The sum of the component ratios of 180 This is believed to result in a composition with an excellent balance between molecules with high mobility and components with low mobility, which is believed to result in better battery characteristics and suppress the decrease in discharge capacity during high-temperature storage.

[0022] The composition according to one embodiment of the present invention is characterized in that the free induction decay curve of the composition measured at 27° C. by the Solid Echo method using pulsed NMR is 27 , component M 27 , component H 27 When separated into three components, component H 27 The component ratio of is 60% or more but less than 100%, and component H 27 It is preferable that the relaxation time of component H is 50 μsec or less. 27 The ratio of component H is preferably 70% or more and less than 100%, and more preferably 80% or more and less than 100%. 27 The relaxation time is preferably 1 to 50 μsec, and more preferably 3 to 30 μsec.

[0023] The composition according to one embodiment of the present invention comprises component M 27 The component ratio of is more than 0% and less than 40%, and component M 27 The relaxation time of component M is preferably 100 μsec or more. 27The component ratio of is preferably more than 0% and not more than 30%, and more preferably more than 0% and not more than 20%. 27 The relaxation time is preferably 100 to 500 μsec, and more preferably 150 to 400 μsec. The composition according to one embodiment of the present invention comprises component S 27 Here, the component S 27 The component corresponding to is preferably a component having a relaxation time of 500 μsec or more.

[0024] The composition according to one embodiment of the present invention is characterized in that the free induction decay curve of the composition measured at 150° C. using pulse NMR by the Solid Echo method is 150 , component M 150 , component H 150 When separated into three components, component S 150 Preferably, the component corresponds to: 150 The component corresponding to is preferably a component having a relaxation time of 500 μsec or more. 150 The component ratio of is 3% or more and 40% or less, component S 150 The relaxation time of component M is 500 to 1500 μs. 150 The component ratio of is 20% or more and 60% or less, component M 150 The relaxation time of component H is more than 100 and less than 500 μsec. 150 The component ratio of is 20% or more and 60% or less, component H 150 The relaxation time of component S is preferably 10 to 100 μsec. 150 The component ratio is 5% or more and 35% or less, and component S 150 The relaxation time of component M is 500-1000 μs. 150 The component ratio of is 25% or more and 55% or less, component M 150 The relaxation time of component H is 110-400 μs. 150 The component ratio of is 25% or more and 55% or less, component H 150 It is more preferable that the relaxation time is 20 to 90 μsec.

[0025] The composition according to one embodiment of the present invention is characterized in that the free induction decay curve of the composition measured at 120° C. by the Solid Echo method using pulse NMR is 120 , component M 120 , component H 120 When separated into three components, component S 120 Preferably, the component corresponds to: 120 The component corresponding to is preferably a component having a relaxation time of 500 μsec or more. 120 The component ratio of is 1% or more and 40% or less, component S 120 The relaxation time of component M is 500 to 1500 μs. 120 The component ratio of is 20% or more and 60% or less, component M 120 The relaxation time of component H is more than 50 and less than 500 μs. 120 The component ratio of is 20% or more and 60% or less, component H 120 The relaxation time of component S is preferably 10 to 50 μsec. 120 The component ratio is 5% or more and 35% or less, and component S 120 The relaxation time of component M is 500-1000 μs. 120 The component ratio of is 25% or more and 55% or less, component M 120 The relaxation time of component H is 55 to 400 μs. 120 The component ratio of is 25% or more and 55% or less, component H 120 It is more preferable that the relaxation time is 10 to 50 μsec.

[0026] The composition according to one embodiment of the present invention is preferably a composition containing a graft copolymer, and is a resin composition. The graft copolymer has a trunk polymer and a branch polymer, and preferably has a trunk polymer and a plurality of branch polymers. Hereinafter, the polymer may be referred to as a copolymer.

[0027] 1-1. Graft copolymer The graft copolymer according to one embodiment of the present invention can be synthesized by graft copolymerizing at least a first monomer onto a trunk polymer. The branch polymers produced by polymerization are grafted, i.e., covalently bonded, to the trunk polymer. At this time, a trunk polymer that is not grafted, or a polymer containing a first monomer that is not grafted to the trunk polymer, i.e., not covalently bonded to the graft copolymer, may be simultaneously produced as a free polymer. Therefore, the resin composition according to one embodiment of the present invention may contain the graft copolymer and the free polymer.

[0028] The graft copolymer according to one embodiment of the present invention may further include a crosslinking portion derived from a crosslinking agent. The crosslinking portion means a structure derived from a crosslinking agent that crosslinks branch polymers with each other, crosslinks a trunk polymer with a branch polymer, or crosslinks trunk polymers with each other. The graft copolymer according to one embodiment of the present invention can be obtained by graft copolymerizing at least a first monomer onto a trunk polymer and crosslinking either the trunk polymer or the branch polymer with either the trunk polymer or the branch polymer. The composition according to one embodiment of the present invention may also include a polymer including a structure derived from a crosslinking agent as a free polymer, in addition to a polymer including a first monomer.

[0029] The graft copolymer according to one embodiment of the present invention may contain a second monomer unit containing an ether structure and a monomer unit other than the first monomer unit and the second monomer unit, as long as the effect of the present invention is not impaired. The composition according to one embodiment of the present invention may also contain, as the free polymer, a polymer containing the second monomer unit and a polymer containing a monomer unit other than the first monomer unit and the second monomer unit.

[0030] The graft ratio of the graft copolymer is preferably 40 to 3000%, more preferably 150 to 900%. From the viewpoint of solubility, the graft ratio is preferably within the above range. If the graft ratio is equal to or higher than the above lower limit, the solubility in a solvent (e.g., NMP (N-methyl-2-pyrrolidone)) is improved when the polymer is made into a slurry, whereas if the graft ratio is equal to or lower than the above upper limit, the viscosity of the slurry is reduced, improving the fluidity of the slurry.

[0031] 1-2. Trunk polymer The trunk polymer has a polyvinyl alcohol structure. Here, the polyvinyl alcohol structure is, for example, a structure derived from polyvinyl alcohol synthesized by saponifying polyvinyl acetate obtained by polymerizing vinyl acetate monomer. Preferably, the trunk polymer is mostly composed of a polyvinyl alcohol structure. More preferably, the trunk polymer is polyvinyl alcohol.

[0032] The average degree of polymerization of the polyvinyl alcohol structure in the resin composition is preferably 300 to 4000, more preferably 500 to 2000. When the average degree of polymerization is in such a range, the stability of the slurry is particularly high. In addition, the above range is also preferable from the viewpoints of solubility, binding property, and viscosity of the binder. When the average degree of polymerization is 300 or more, the binding property between the binder and the active material and the conductive assistant is improved, and durability is improved. When the average degree of polymerization is 4000 or less, the solubility is improved and the viscosity is reduced, making it easier to manufacture the slurry for the positive electrode. The average degree of polymerization here is a value measured by a method conforming to JIS K 6726. The saponification degree of the polyvinyl alcohol structure in the composition is preferably 60 to 100 mol%, more preferably 80 to 100 mol%. When the saponification degree is within this range, the stability of the slurry is particularly high. The saponification degree referred to here is a value measured by a method according to JIS K 6726.

[0033] 1-3. Branch polymer The branch polymer contains at least a first monomer unit. The branch polymer may contain a second monomer unit and a monomer unit other than the first monomer unit and the second monomer unit, as long as the effect of the present invention is not impaired. Here, the first monomer unit and the second monomer unit are monomer units derived from the first monomer and the second monomer used in the synthesis of the graft copolymer, respectively.

[0034] 1-4.Bridge part The graft copolymer according to one embodiment of the present invention may further include a crosslinking portion. The crosslinking portion is a structure derived from a crosslinking agent, and connects the branch polymers of the graft copolymer to each other, the trunk polymer and the branch polymer, or the trunk polymers of the graft copolymer to each other. The crosslinking portion preferably crosslinks the branch polymers of the graft copolymer to each other. The crosslinking portion preferably includes an ether structure, more preferably includes an alkylene glycol repeating unit, and most preferably includes an ethylene glycol repeating unit.

[0035] The crosslinking agent according to one embodiment of the present invention is a bifunctional or polyfunctional compound, preferably a compound that is soluble in a polar solvent, and preferably soluble in the first monomer. The crosslinking agent is not particularly limited as long as it satisfies the above requirements, but examples thereof include alkane polyol-poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, oligoethylene glycol di(meth)acrylate (polyethylene glycol di(meth)acrylate), trimethylolpropane di(meth)acrylate, and trimethylolpropane tri(meth)acrylate, and divinylbenzene. Among these, oligoethylene glycol di(meth)acrylate is preferred. Among the oligoethylene glycol di(meth)acrylates, di(meth)acrylates represented by the following general formula (B) are preferred. H2C=CR 21 -COO-(-CH2CH2O-) n -CO-CR 22 =CH2(B) In general formula (B), R21 , R 22 is hydrogen (H) or a methyl group. 21 , R 22 may be the same or different. n is a number of 0 or more. n is preferably 1 or more. n is preferably 30 or less, and more preferably 10 or less. The crosslinking agent preferably contains an ether structure, and more preferably has an ethylene glycol repeating unit. The number of ethylene glycol repeating units is preferably 2 or more and 20 or less, more preferably 5 or more and 15 or less, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15, and may be within a range between any two of the numerical values ​​exemplified here. In the graft copolymer according to one embodiment of the present invention, the ratio of components with high mobility and components with low mobility in the resin composition can be controlled, for example, by adjusting the type and amount of crosslinked moieties.

[0036] 1-4.Free polymer The resin composition according to one embodiment of the present invention may further include a free polymer. The free polymer is a polymer that does not have a covalent bond with the graft copolymer, and includes at least a polymer containing a polyvinyl alcohol structure and / or a polymer containing the first monomer unit. The polymer having a polyvinyl alcohol structure means a trunk polymer that is not mainly involved in the graft copolymerization. The polymer containing the first monomer unit means a homopolymer of the first monomer, a copolymer containing the first monomer unit and the second monomer unit, a copolymer containing the first monomer and a monomer unit other than the first monomer unit and the second monomer unit, or a polymer containing a copolymer containing a structure derived from the first monomer and a crosslinking agent, and is not copolymerized with the graft copolymer (i.e., the trunk polymer). Furthermore, within the scope of the present invention, the free polymer may include polymers other than the polymer having a polyvinyl alcohol structure and the polymer containing the first monomer unit, such as a homopolymer of the second monomer, a homopolymer of a monomer other than the first monomer and the second monomer, and a polymer containing a structure derived from a crosslinking agent, which is not copolymerized in the graft copolymer (i.e., trunk polymer). The free polymer is preferably a polymer that substantially contains the first monomer unit.

[0037] In addition, the weight average molecular weight of the free polymer other than the trunk polymer, for example, a copolymer containing a homopolymer of the first monomer, is preferably 30,000 to 250,000, more preferably 40,000 to 200,000, and even more preferably 50,000 to 150,000. From the viewpoint of suppressing an increase in viscosity and easily producing a positive electrode slurry, the weight average molecular weight of the free polymer other than the trunk polymer is preferably 300,000 or less, more preferably 200,000 or less, and even more preferably 150,000 or less. The weight average molecular weight of the free polymer other than the trunk polymer can be determined by GPC (gel permeation chromatography), and specifically, can be measured by the method described later.

[0038] 1-6. First monomer unit The first monomer unit is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit. The first monomer unit is more preferably a (meth)acrylonitrile monomer unit, and further preferably an acrylonitrile monomer unit. That is, the first monomer used in synthesizing the graft copolymer is preferably (meth)acrylonitrile and / or (meth)acrylic acid, more preferably (meth)acrylonitrile, and even more preferably acrylonitrile, and therefore the first monomer unit has a structure derived from these.

[0039] 1-7. Second monomer unit The second monomer unit is a structural unit containing an ether structure, and is a structure derived from a monofunctional second monomer. The second monomer unit is a monofunctional compound having an ether structure. The ether structure preferably has at least one selected from a linear polyether structure, a branched polyether structure, and a cyclic ether structure. More preferably, the ether structure has a polyethylene oxide structure. Moreover, the second monomer unit preferably has a structure derived from a monomer which is a (meth)acrylic acid ester derivative, a styrene derivative, a polysubstituted ethylene, or a vinyl ether derivative.

[0040] That is, the second monomer used in synthesizing the graft polymer is a monomer having an ether structure, and is preferably a monomer such as a (meth)acrylic acid ester derivative having an ether structure, a styrene derivative having an ether structure, a polysubstituted ethylene derivative, or a vinyl ether derivative. Among these, a (meth)acrylic acid ester derivative having an ether structure is preferred. Among the (meth)acrylic acid ester derivatives having an ether structure, a (meth)acrylic acid ester derivative represented by the following general formula (A) is preferred.

[0041] [ka] In the general formula (A), Y is preferably -(AO)nR. AO is an oxyalkylene group. The number of carbon atoms in the oxyalkylene group is preferably 1 to 18, more preferably 2 to 10. The oxyalkylene group is most preferably one or more of an ethylene oxide group and a propylene oxide group, and more preferably an ethylene oxide group. n is a number of 0 or more. n is preferably 1 or more. n is preferably 30 or less, more preferably 10 or less. Also, R 1 , R 2 , R 3 R is hydrogen (H), a hydrocarbon group or an ether group which may be substituted, etc. Preferably, the hydrocarbon group or ether group which may be substituted is a hydrocarbon group or ether group having 1 to 20 carbon atoms. Here, the ether group is a functional group having an ether bond, such as an alkyl ether group. R 1 , R 2 , R 3 Preferably, R is unsubstituted. 1 , R 2 , R 3 R may be the same or different. R is preferably a hydrocarbon group. As the hydrocarbon group, one or more of a methyl group and an ethyl group are preferable. As the (meth)acrylic acid ester derivative, alkoxy polyalkylene glycol (meth)acrylate is preferred. Among the alkoxy polyalkylene glycol (meth)acrylates, one or more of alkoxy polyethylene glycol (meth)acrylate and alkoxy polypropylene glycol (meth)acrylate are preferred. More specifically, one or more of (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate, methoxy polyethylene glycol (meth)acrylate (poly:n=23), and methoxy dipropylene glycol (meth)acrylate are preferred. The second monomer is more preferably one or more of (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate and methoxy dipropylene glycol (meth)acrylate, and most preferably (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate. Therefore, the second monomer unit has a structure derived from these.

[0042] 1-8. Content of each component in the resin composition It is also preferable that the content and properties of each component satisfy the following requirements: When the content and properties of each component are within the following ranges, it is possible to provide a resin composition that serves as a binder with an excellent balance of the ratio of high-mobility components and low-mobility components in the resin composition, suppresses the deterioration of battery performance in a high-capacity electrode, and has an excellent balance of high-temperature storage properties (high-temperature preservation properties) and DC resistance.

[0043] In the resin composition according to one embodiment of the present invention, when the resin composition is taken as 100 parts by mass, the content of the polyvinyl alcohol structure in the resin composition is preferably 5 to 70 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 15 to 55 parts by mass, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. By making it equal to or more than the above lower limit, a binder having binding properties can be obtained, and by making it equal to or less than the above upper limit, oxidation resistance and flexibility can be maintained. In this embodiment, the content of the polyvinyl alcohol structure in the resin composition refers to the total amount of the polyvinyl alcohol structure in the graft copolymer and the polyvinyl alcohol structure in the free polymer containing polyvinyl alcohol contained in the resin composition.

[0044] In the resin composition according to one embodiment of the present invention, when the resin composition is taken as 100 parts by mass, the content of the first monomer unit derived from the first monomer is preferably 3 to 80 parts by mass, more preferably 5 to 70 parts by mass, for example, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. By making it equal to or more than the above lower limit, a binder having binding properties can be obtained, and by making it equal to or less than the above upper limit, oxidation resistance can be maintained. In this embodiment, the content of the first monomer unit in the resin composition indicates the total amount of the first monomer unit in the graft copolymer and the first monomer unit in the free polymer containing the first monomer unit, which are contained in the resin composition.

[0045] The resin composition according to one embodiment of the present invention preferably contains 0.2 to 10 parts by mass of the structure derived from the crosslinking agent, more preferably 0.5 to 8 parts by mass, and particularly preferably 1 to 5 parts by mass, when the resin composition is taken as 100 parts by mass. The content of the structure derived from the crosslinking agent is, for example, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. By setting it to the above lower limit or more, the resin composition has a moderate amount of highly mobile components, and by setting it to the above upper limit or less, the solubility in a solvent such as NMP can be sufficiently maintained. In this embodiment, the content of the structure derived from the crosslinking agent in the resin composition refers to the total amount of the structure derived from the crosslinking agent bonded to the graft copolymer contained in the resin composition and the structure derived from the crosslinking agent in the free polymer.

[0046] The resin composition according to one embodiment of the present invention may contain 0 to 20 parts by mass of the second monomer unit derived from the second monomer when the resin composition is taken as 100 parts by mass. The resin composition according to one embodiment of the present invention may not contain the second monomer unit. In this embodiment, the content of the second monomer unit in the resin composition refers to the total amount of the second monomer unit in the graft copolymer and the second monomer unit in the free polymer containing the second monomer unit, both of which are contained in the resin composition.

[0047] 1-9. Characteristics of the composition (swelling rate) The composition according to one embodiment of the present invention has a swelling ratio in an electrolytic solution at 25° C. for 15 days of preferably 90 to 230%, more preferably 100 to 220%, and more preferably 105 to 210%. Here, the swelling ratio in an electrolytic solution at 25° C. for 15 days means the swelling ratio after the composition is immersed in an electrolytic solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 at 25° C. for 15 days. The swelling ratio of the composition when immersed in an electrolytic solution at 25° C. for 15 days is, for example, any of 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 150, 160, 170, 180, 190, 200, 210, 220, and 230%, and may be within a range between any two of the numerical values ​​exemplified here. According to the composition of one embodiment of the present invention, by controlling the swelling ratio within the above range, it is possible to maintain the pore volume, particularly in the high rate region, while maintaining appropriate flexibility, thereby providing better battery characteristics and suppressing the decrease in discharge capacity during high temperature storage.

[0048] (DMSO soluble fraction (gel fraction)) The composition according to one embodiment of the present invention preferably has a gel fraction of 30% or more. In one aspect, it is more preferably 50% or more, most preferably 60% or more, and even more preferably 65% ​​or more. The upper limit of the gel fraction can be, for example, 95%. The gel fraction can be, for example, any of 30, 40, 50, 60, 65, 70, 80, 90, and 95%, and may be within a range between any two of the values ​​exemplified here. According to the composition according to one embodiment of the present invention, by controlling the gel fraction within the above range, it is possible to maintain the pore volume while appropriately controlling the electrolyte solution that penetrates into the interior of the composition, and therefore it is possible to have better battery characteristics and suppress the decrease in discharge capacity during high-temperature storage.

[0049] 1-10.Various measurement / calculation methods (Pulsed NMR) The free induction decay curve of the composition and the components contained in the free induction decay curve can be evaluated by the following method. First, the free induction decay curve of the composition under each temperature condition is obtained by the Solid Echo method using pulse NMR. An example of the analysis conditions is shown below. Measurement equipment: JEOL JNM-MU25 (25MHz) Observed nucleus: 1H Measurement: T2 Measurement method: Solid echo method Pulse width: 90° pulse, 25μs Pulse interval: 10μs Number of times: 8 Measurement temperature: 27℃, 120℃, 150℃, 180℃ (The measurement temperature is the temperature inside the sample. After the device temperature reaches the set temperature, adjust the device temperature so that the internal temperature of the sample reaches the measurement temperature 5 minutes later, and then start the measurement.) Repeat time: 4s

[0050] The free induction decay curve obtained by the above method is analyzed by the following method to determine the component ratio and relaxation time of each component. Analysis method: Using equation (1), fitting is performed using analysis software (built-in NM-MU25), and the obtained free induction decay curve is approximated to three components. The ^ in equation (1) indicates exponentiation. M(t) = Σ(M(0) i × exp((-t / T 2i )^w i ))...Equation (1) M(t): signal strength at time t t: time T 2i :Relaxation time of each component M(0)i: Signal intensity at t=0 for each component wi: Weibull coefficient

[0051] (Swelling ratio of composition (25°C, 15 days)) The swelling ratio of a composition in an electrolyte solution indicates the change in mass before and after a film made of the composition is immersed in an electrolyte solution for a predetermined time at a predetermined temperature. The swelling ratio can be determined, for example, by the following method. The obtained composition is dissolved in NMP to prepare a 4% by mass NMP solution. 5.6 g of the obtained solution is added to a petri dish of PTFE (tetrafluoroethylene) and dried for 8 hours at 105 ° C. with a blower dryer to obtain a film with a thickness of 250 μm. The center part of the obtained test film is cut to 5 mm × 5 mm to be used as a test film. The obtained test film is measured for mass, and then immersed in an electrolyte solution in which ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:2. After leaving it at 25 ° C. for 15 days, the liquid on the film surface is wiped off and the mass after immersion is measured. The swelling ratio is calculated from the change in mass before and after immersion using the following formula. The swelling ratio is calculated from the following formula, where WA (g) is the mass before immersion and WB (g) is the mass after immersion. Swelling ratio (25°C, 15 days) (%) = WB × 100 / WA Equation (2) WA: Mass before immersion (g) WB: Mass after immersion (g)

[0052] By changing the conditions for immersion in the electrolyte, it is possible to obtain the swelling ratio under different conditions. For example, by changing the conditions for immersion in the electrolyte to 60°C for 48 hours, the swelling ratio when immersed in the electrolyte at 60°C for 48 hours can be obtained, and the swelling ratio can be evaluated in a short period of time.

[0053] (DMSO insoluble matter (gel fraction)) The gel fraction of the composition is evaluated by dissolving the composition in DMSO and stirring the mixture at a predetermined temperature for a predetermined time, based on the insoluble content. Specifically, the gel fraction of the composition can be evaluated by the following method. 1 g of the obtained composition and 300 ml of DMSO are added to a 500 ml beaker and stirred at 60°C for 15 hours. The obtained mixture is then filtered with a Kiriyama funnel using No. 5C filter paper specified in JIS P 3801, and the residue remaining on the filter paper is the insoluble part (gel part), and the filtrate is the soluble part. The insoluble part (gel part) is vacuum dried at 100°C for 24 hours and weighed. The insoluble part is taken as Ag, and the gel fraction (%) = A x 100 / 1 is calculated.

[0054] (Content of first monomer unit, second monomer unit, and crosslinking portion) The resin composition according to one embodiment of the present invention contains a component derived from PVA and a component derived from a first monomer, and optionally contains a component derived from a second monomer and / or a component derived from a crosslinking agent. The content of each component in the resin composition can be roughly calculated from the amount of the components charged for graft polymerization. More precisely, the content of each component can be calculated by determining the reaction rate of each component by NMR using the following method. The content of each component can also be calculated from the integral ratio of the obtained composition by NMR.

[0055] The reaction rate of polyvinyl alcohol can be calculated using the following method. First, the concentration of PVA in the raw material solution is calculated from absorbance. Next, a polymerization reaction is carried out to obtain a polymerization reaction liquid, and 50 g of the resulting polymerization reaction liquid is centrifuged at 3000G for 30 minutes to obtain a supernatant. The absorbance of the supernatant is measured to determine the PVA concentration. The reaction rate of PVA (%) is calculated using the formula {1-(PVA concentration in the supernatant) / (PVA concentration at the time of charging)} x 100. The reaction rates of the first monomer, the second monomer, and the crosslinking agent can be determined by the following method. After the polymerization is completed, the product is precipitated with methanol, and the dried product is dissolved in deuterated DMSO. 1 1H-NMR is measured. From the intensity of the signals in the obtained spectrum corresponding to PVA, the first monomer, the second monomer, and the crosslinking agent, the composition of each component is calculated with PVA as the standard. The composition calculated from NMR is compared with the composition of each component at the time of charging, and the reaction rate is calculated, which indicates the extent to which the first monomer, second monomer, and crosslinking agent are contained in the composition out of the first monomer, second monomer, and crosslinking agent charged.

[0056] (graft rate) When producing a graft copolymer (graft copolymerization), a free polymer containing at least one of the group consisting of the first monomer, the second monomer, and the crosslinking agent may be produced. Calculation of the graft ratio requires a process of separating the free polymer from the graft copolymer. The free polymer dissolves in dimethylformamide (hereinafter sometimes abbreviated as DMF), but PVA and the graft copolymer do not dissolve in DMF. By utilizing this difference in solubility, the free polymer can be separated by an operation such as centrifugation. Where: F: Mass of component dissolved in DMF (g) G: Mass of the composition used in the test (g) H: Total content (mass%) of the first monomer unit and the second monomer unit in the composition Then, the graft ratio can be calculated by the following formula (3). [(GF) / (G×(100-H) / 100)]×100...Equation (3)

[0057] (Molecular weight of free polymer other than trunk polymer) Weigh out 1.00 g of the resin composition, add it to 50 cc of special grade DMF (manufactured by Kokusan Chemical Co., Ltd.), and stir at 1000 rpm for 24 hours at 80°C. Next, centrifuge it at 10000 rpm for 30 minutes in a centrifuge (model: H2000B, rotor: H) manufactured by Kokusan Co., Ltd. Carefully separate the filtrate (DMF soluble matter) and then pour it into 1000 ml of methanol to obtain a precipitate. The precipitate is vacuum dried at 80°C for 24 hours, and the weight average molecular weight in terms of standard polystyrene is measured by GPC. The GPC measurement can be performed under the following conditions, for example. Column: Two GPC LF-804 columns, φ8.0×300 mm (Showa Denko K.K.) were connected in series. Column temperature: 40℃ Solvent: 20mM LiBr / DMF

[0058] 1-11. Manufacturing method of the composition Although there is no particular limitation on the method for producing the composition according to one embodiment of the present invention, in one example of the resin composition according to one embodiment of the present invention, the method for producing the resin composition containing the graft copolymer according to one embodiment of the present invention preferably includes a graft copolymerization step of graft copolymerizing a raw material containing at least polyvinyl alcohol and a first monomer. That is, the resin composition according to one embodiment of the present invention can be obtained by a production method including a graft copolymerization step of graft copolymerizing a raw material containing at least polyvinyl alcohol and a first monomer. In addition, the production method according to one embodiment of the present invention preferably further includes a vinyl acetate polymerization step of polymerizing vinyl acetate to obtain polyvinyl acetate, and a saponification step of saponifying the obtained polyvinyl acetate to obtain polyvinyl alcohol.

[0059] [Production method of polyvinyl alcohol (PVA)] As a method for polymerizing polyvinyl acetate, any known method such as bulk polymerization or solution polymerization can be used.

[0060] Examples of initiators used in the polymerization of polyvinyl acetate include azo-based initiators such as azobisisobutyronitrile, and organic peroxides such as benzoyl peroxide and bis(4-t-butylcyclohexyl)peroxydicarbonate.

[0061] The saponification reaction of polyvinyl acetate can be carried out, for example, in an organic solvent in the presence of a saponification catalyst.

[0062] Examples of the organic solvent include methanol, ethanol, propanol, ethylene glycol, methyl acetate, ethyl acetate, acetone, methyl ethyl ketone, benzene, toluene, etc. These may be used alone or in combination. Among these, methanol is preferred.

[0063] Examples of the saponification catalyst include basic catalysts such as sodium hydroxide, potassium hydroxide, sodium alkoxide, etc., and acidic catalysts such as sulfuric acid, hydrochloric acid, etc. Among these, sodium hydroxide is preferred from the viewpoint of saponification rate. The degree of polymerization of polyvinyl alcohol can be controlled by adjusting the type and amount of the initiator, and the temperature and time during polymerization, and the degree of saponification of polyvinyl alcohol can be controlled by adjusting the type and amount of the saponification catalyst, and the temperature and time during saponification. The degree of polymerization and the degree of saponification of polyvinyl alcohol are preferably adjusted within the above-mentioned ranges.

[0064] [Method of producing resin composition] The manufacturing method according to one embodiment of the present invention preferably includes a step of graft copolymerizing a raw material containing at least polyvinyl alcohol and a first monomer, and the raw material containing at least polyvinyl alcohol and the first monomer may further include a crosslinking agent. Also, the raw material containing at least polyvinyl alcohol and the first monomer may further include a second monomer. In the production method according to one embodiment of the present invention, the component ratio of each component included in the free induction decay curve obtained by measurement by pulse NMR can be adjusted within the above-mentioned range by adjusting the types and amounts of raw materials provided during graft copolymerization and the polymerization conditions, etc. The polyvinyl alcohol used in the graft copolymerization preferably has the above-mentioned degree of polymerization and degree of saponification, and the first monomer, the second monomer, and the crosslinking agent used in the graft copolymerization preferably are the above-mentioned types of the first monomer, the second monomer, and the crosslinking agent. The blending amount during graft copolymerization is preferably adjusted so that the content of each component in the resin composition satisfies the requirements for the content of each component in the resin composition described above. For example, when the raw material to be subjected to graft copolymerization is 100 parts by mass, the raw material to be subjected to graft copolymerization preferably contains 0.2 to 10 parts by mass of the crosslinking agent, more preferably contains 0.5 to 8 parts by mass, and particularly preferably contains 1 to 5 parts by mass. The content of the crosslinking agent in the raw material to be subjected to graft copolymerization is, for example, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0065] The method for graft-copolymerizing a monomer onto polyvinyl alcohol includes, for example, a solution polymerization method, and examples of the solvent used include water, dimethyl sulfoxide, and N-methylpyrrolidone.

[0066] As the initiator used in the graft copolymerization, a peroxide is preferable. Examples of the peroxide include organic peroxides such as benzoyl peroxide and inorganic peroxides. Among the peroxides, inorganic peroxides are preferable. Examples of the inorganic peroxides that can be used include potassium persulfate and ammonium persulfate. Among the inorganic peroxides, ammonium persulfate is preferable.

[0067] The graft copolymer according to one embodiment of the present invention can be used by dissolving it in a solvent. Examples of the solvent include dimethyl sulfoxide, N-methylpyrrolidone, etc. The composition and the slurry for the positive electrode described below may contain these solvents.

[0068] 1-12.Other The composition according to one embodiment of the present invention may contain other components, such as resins, within a range that does not impair the effects of the present invention. Examples of such resins include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene, styrene-butadiene copolymers (styrene butadiene rubber, etc.), and acrylic copolymers. Among these, fluororesins, particularly polyvinylidene fluoride, are preferred from the viewpoint of stability.

[0069] 2. Positive electrode slurry The composition according to one embodiment of the present invention can be a resin composition and can be used as a binder for forming a positive electrode of a secondary battery. That is, the resin composition according to one embodiment of the present invention can be a resin composition for a positive electrode. The slurry for a positive electrode according to one embodiment of the present invention contains the above composition and has excellent stability. In addition, the slurry for a positive electrode according to one embodiment of the present invention contains the above composition and can produce a positive electrode with excellent rate characteristics. The slurry for a positive electrode may contain a composition and a conductive assistant, or may contain a composition, a positive electrode active material, and a conductive assistant.

[0070] In the positive electrode slurry according to one embodiment of the present invention, the solid content of the positive electrode (binder) composition is preferably 0.1 to 20 mass %, and more preferably 1 to 10 mass %, relative to the total amount of solids in the positive electrode slurry.

[0071] 3. Lithium-ion secondary battery A secondary battery is preferred as a battery having a positive electrode according to an embodiment of the present invention. The secondary battery is preferably one or more selected from a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, and a potassium ion secondary battery, and more preferably a lithium ion secondary battery. The positive electrode according to one embodiment of the present invention and the lithium ion secondary battery including the positive electrode can be produced using a positive electrode slurry containing the above composition. Preferably, the positive electrode, the negative electrode, the separator, and the electrolyte solution (hereinafter, also referred to as electrolyte or electrolyte solution) are included.

[0072] [Positive electrode] The positive electrode according to one embodiment of the present invention can be produced by applying a positive electrode slurry containing a composition, a conductive assistant, and a positive electrode active material used as necessary onto a current collector such as aluminum foil, removing the solvent contained in the slurry by heating, and then pressing the current collector and the electrode mixture layer together by a roll press or the like to make them adhere to each other. That is, a positive electrode is obtained that includes a metal foil and a coating of the positive electrode slurry formed on the metal foil.

[0073] [Conductive additive] The conductive assistant is preferably at least one selected from the group consisting of (i) fibrous carbon, (ii) carbon black, and (iii) a carbon composite in which fibrous carbon and carbon black are mutually linked. Examples of fibrous carbon include vapor-grown carbon fiber, carbon nanotubes, and carbon nanofibers. Examples of carbon black include acetylene black, furnace black, and Ketjen Black (registered trademark). These conductive assistants may be used alone or in combination of two or more. Among these, from the viewpoint of a high effect of improving the dispersibility of the conductive assistant, one or more selected from acetylene black, carbon nanotubes, and carbon nanofibers are preferred. In the positive electrode slurry according to one embodiment of the present invention, the solid content of the conductive assistant is preferably 0.01 to 20 mass %, and more preferably 0.1 to 10 mass %, relative to the total solid content in the positive electrode slurry.

[0074] [Positive electrode active material] The positive electrode active material may be used as necessary. The positive electrode active material is preferably a positive electrode active material capable of reversibly occluding and releasing cations. The positive electrode active material has a volume resistivity of 1×10 4 Ω·cm or more and is preferably a lithium-containing composite oxide or a lithium-containing polyanion compound containing Mn. For example, LiCoO2, LiMn2O4, LiNiO2, LiMPO4, Li2MSiO4, LiNi X Mn (2-X) O4, Li(Co X Ni Y Mn Z )O2, Li(Ni X Co Y Al Z )O2 or xLi2MnO3-(1-X)LiMO2, etc. However, X in LiNi X Mn (2-X) O4 satisfies the relationship of 0 < X < 2, and X, Y, and Z in Li(Co X Ni Y Mn Z )O2 or Li(Ni X Co Y Al Z )O2 satisfy the relationship of X + Y + Z = 1, and also satisfy the relationships of 0 < X < 1, 0 < Y < 1, 0 < Z < 1. X in XLi2MnO3-(1-X)LiMO2 satisfies the relationship of 0 < X < 1. Furthermore, M in LiMPO4, Li2MSiO4, or XLi2MnO3-(1-X)LiMO2 is preferably one or more elements selected from Fe, Co, Ni, and Mn. Among the positive electrode active materials, LiNi X Mn (2-X) O4 (however, 0 < X < 2), Li(Co X Ni Y Mn Z )O2 (however, 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) and Li(Ni X Co Y Al Z )O2 (however, 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) selected from one or more of them are preferred, LiNiX Mn (2-X) O4 (where 0 < X < 2) and Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1, and X + Y + Z = 1) is more preferably one or more selected therefrom. The slurry for the positive electrode according to one embodiment of the present invention preferably has a solid content of the positive electrode active material of 50 to 99.8% by mass, more preferably 80 to 99.5% by mass, and most preferably 95 to 99.0% by mass, based on the total solid content in the slurry for the positive electrode.

[0075] [Negative electrode] The negative electrode used in the lithium-ion secondary battery according to one embodiment of the present invention is not particularly limited, but can be manufactured using a slurry for the negative electrode containing a negative electrode active material. This negative electrode can be manufactured, for example, using a metal foil for the negative electrode and a slurry for the negative electrode provided on the metal foil. The slurry for the negative electrode preferably contains a binder for the negative electrode (composition for the negative electrode), a negative electrode active material, and the above-described conductive auxiliary agent. The binder for the negative electrode is not particularly limited, but for example, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene copolymer (such as styrene-butadiene rubber), and acrylic copolymer can be used. As the binder for the negative electrode, a fluororesin is preferred. As the fluororesin, one or more selected from the group consisting of polyvinylidene fluoride and polytetrafluoroethylene are more preferred, and polyvinylidene fluoride is most preferred.

[0076] Examples of the negative electrode active material used for the negative electrode include carbon materials such as graphite, polyacene, carbon nanotubes, and carbon nanofibers, alloy-based materials such as tin and silicon, or oxide materials such as tin oxide, silicon oxide, and lithium titanate. One or more of these may be used. As the metal foil for the negative electrode, foil-shaped copper is preferably used, and the thickness is preferably 5 to 30 μm from the viewpoint of workability. The negative electrode can be manufactured using the slurry for the negative electrode and the metal foil for the negative electrode by a method according to the manufacturing method of the above-described positive electrode.

[0077] [Separator] The separator can be made of an electrically insulating porous film, net, nonwoven fabric, fiber, or the like, as long as it has sufficient strength. In particular, it is preferable to use a separator that has low resistance to ion movement of the electrolyte and excellent solution retention. The material is not particularly limited, but examples include inorganic fibers such as glass fibers or organic fibers, olefins such as polyethylene and polypropylene, synthetic resins such as polyester, polytetrafluoroethylene, and polyflon, or layered composites thereof. From the viewpoint of binding and stability, olefins or layered composites thereof are preferred. As the olefin, one or more members of the group consisting of polyethylene and polypropylene are preferred.

[0078] [Electrolytes] As the electrolyte, any of the known lithium salts can be used, for example, LiClO4, LiBF4, LiBF6, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiI, LiB(C2H5)4, LiCF3SO3, LiCH3SO3, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiC(CF3SO2)3, and lithium lower fatty acid carboxylates.

[0079] [Electrolyte] The electrolyte in which the electrolyte is dissolved is not particularly limited. Examples of the electrolyte include carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate, lactones such as γ-butyrolactone, ethers such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, and 2-methyltetrahydrofuran, sulfoxides such as dimethyl sulfoxide, oxolanes such as 1,3-dioxolane and 4-methyl-1,3-dioxolane, nitrogen-containing compounds such as acetonitrile, nitromethane, and N-methyl-2-pyrrolidone, methyl formate, methyl acetate, and the like. Examples of the electrolyte include esters such as ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, and phosphoric acid triesters, inorganic acid esters such as sulfates, nitrates, and hydrochlorides, amides such as dimethylformamide and dimethylacetamide, glymes such as diglyme, triglyme, and tetraglyme, ketones such as acetone, diethyl ketone, methyl ethyl ketone, and methyl isobutyl ketone, sulfolanes such as sulfolane, oxazolidinones such as 3-methyl-2-oxazolidinone, and sultones such as 1,3-propane sultone, 4-butane sultone, and naphtha sultone. At least one of these electrolytes can be used. The electrolyte preferably contains a carbonate, and more preferably contains ethylene carbonate or diethyl carbonate.

[0080] Among the above electrolytes and electrolytic solutions, an electrolytic solution in which LiPF6 is dissolved in a carbonate is preferred, an electrolytic solution in which LiPF6 is dissolved in a mixed solution containing ethylene carbonate and diethyl carbonate is more preferred, and an electrolytic solution in which LiPF6 is dissolved in a mixed solution in which ethylene carbonate and diethyl carbonate are mixed in a volume ratio of 1:2 is even more preferred. The concentration of the electrolyte in the solution varies depending on the electrode and electrolytic solution used, but is preferably 0.5 to 3 mol / L.

[0081] Applications of the lithium ion secondary battery according to the embodiment of the present invention are not particularly limited, and examples thereof include portable AV devices such as digital cameras, video cameras, portable audio players, and portable LCD televisions, portable information terminals such as notebook personal computers, smartphones, and mobile PCs, as well as a wide range of other fields such as portable game devices, power tools, electric bicycles, hybrid automobiles, electric automobiles, and power storage systems. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples. These are merely illustrative examples and do not limit the scope of the present invention. Data are shown in Table 1.

[0083] [Example 1] <Preparation of polyvinyl alcohol (PVA)> The PVA used was PVA (B-24) manufactured by Denka Co., Ltd. The average polymerization degree and saponification degree of the PVA are shown in Table 1.

[0084] <Preparation of Composition> A reaction vessel was charged with 1,804 parts by mass of pure water, and nitrogen gas was bubbled through it to deoxygenate it. Then, 100 parts by mass of partially saponified PVA (saponification degree 85.6%, polymerization degree 2400) was charged at room temperature and dissolved by heating to 90°C. The reaction vessel was adjusted to 60°C, and 170 parts by mass of a 10% aqueous solution of ammonium persulfate that had been deoxygenated by bubbling nitrogen gas through it was added all at once, followed by 96 parts by mass of acrylonitrile and the crosslinking agent oligoethylene glycol diacrylate (the number of ethylene glycol repeats in general formula (B) is n = 9, R 21 , R 22 is hydrogen.) (manufactured by Shin-Nakamura Chemical Co., Ltd., product name: A-400) 8 parts by mass of the mixed solution was added over 5 hours to polymerize. 100 parts by mass of the obtained polymerization solution was added to 300 parts by mass of methanol, and the precipitate was filtered under reduced pressure and dried at 40°C for 12 hours to obtain a resin composition. The composition of the obtained composition containing the graft copolymer is shown in Table 1.

[0085] <Reaction rate and composition ratio> For the resulting composition, the reaction rate of each raw material and the composition ratio of each component were calculated. The reaction rate of polyvinyl alcohol was determined by the following method. First, the concentration of PVA in the raw material solution was determined by absorbance. Next, 50 g of the polymerization reaction solution obtained in the polymerization reaction was centrifuged at 3000G for 30 minutes to obtain a supernatant. The absorbance of the supernatant was measured to determine the PVA concentration. The reaction rate of PVA (%) was calculated by {1-(PVA concentration in the supernatant) / (PVA concentration at the time of charging)}×100. The reaction rate of PVA was 93%.

[0086] The reaction rates of the first monomer and the crosslinking agent were determined by the following method. After the polymerization was completed, the product was precipitated with methanol, and the dried product was dissolved in deuterated DMSO. 1 H-NMR was measured. From the intensity of the signals corresponding to PVA, the first monomer, and the crosslinking agent in the obtained spectrum, the composition of each component was calculated with PVA as the standard. Signals from PVA, PAN and vinyl acetate, PAN, and the crosslinking agent were observed at 1 to 1.7 ppm, 1.7 to 2.3 ppm, 3 to 3.2 ppm, and 3.5 to 3.7 ppm, respectively. The reaction rate was calculated by comparing the composition calculated from NMR with the composition of each component at the time of charging. The reaction rate indicates the extent to which the first monomer and crosslinking agent are contained in the composition out of the first monomer and crosslinking agent charged. The reaction rate of the first monomer was 98%, and the reaction rate of the crosslinking agent was 100%.

[0087] In addition, the composition ratio of each component of the composition according to Example 1 was calculated from the reaction rate. When the composition was 100 parts by mass, the content of the polyvinyl alcohol structure was 47.7 parts by mass, the content of the first monomer unit was 48.2 parts by mass, and the content of the structure derived from the crosslinking agent was 4.2 parts by mass. This composition ratio includes a free polymer that is a homopolymer of the first monomer.

[0088] <Evaluation method> (Pulsed NMR) Using pulse NMR, the free induction decay curve of the resin composition was obtained under each temperature condition by the Solid Echo method. Measurement equipment: JEOL JNM-MU25 (25MHz) Observed nucleus: 1H Measurement: T2 Measurement method: Solid echo method Pulse width: 90° pulse, 25μs Pulse interval: 10μs Number of times: 8 Measurement temperature: 27℃, 120℃, 150℃, 180℃ (The measurement temperature is the temperature inside the sample. The device temperature was adjusted so that the internal temperature of the sample reached the measurement temperature 5 minutes after the device temperature reached the set temperature, and measurement was started.) Repeat time: 4s

[0089] Analysis method: Using equation (4), fitting was performed with analysis software (built-in NM-MU25), and the obtained free induction decay curve was approximated to three components. The obtained free induction decay curve was separated into three curves derived from the three components, H component, M component, and S component, in the order of shortest relaxation time. In other words, the actually measured free induction decay curve is a superposition of the free induction decay curves derived from the three components, H component, M component, and S component. The Weibull coefficient is the H component w H In the case of 2, M component w M and S component w S In this case, the value is 1. M(t) = Σ(M(0) i × exp((-t / T 2i )^w i ))...Equation (4) M(t): signal strength at time t t: time T 2i :Relaxation time of each component M(0)i: Signal intensity at t=0 for each component wi: Weibull coefficient

[0090] <Evaluation method> (DMSO insoluble matter (gel fraction)) 1 g of the obtained composition and 300 ml of DMSO were added to a 500 ml beaker and stirred at 60° C. for 15 hours. The obtained mixture was then filtered with a Kiriyama funnel using No. 5C filter paper specified in JIS P 3801, and the residue remaining on the filter paper was taken as the insoluble part (gel content), and the filtrate was taken as the soluble part. The insoluble part (gel content) was vacuum dried at 100° C. for 24 hours and weighed. The insoluble part was taken as Ag, and the gel fraction (%) was calculated as A×100 / 1.

[0091] (graft rate) 1.00 g of the obtained composition containing the graft copolymer was weighed out and added to 50 cc of special grade DMF (manufactured by Kokusan Chemical Co., Ltd.), and stirred at 1000 rpm for 24 hours at 80°C. Next, this was centrifuged at 10000 rpm for 30 minutes in a centrifuge (model: H2000B, rotor: H) manufactured by Kokusan Co., Ltd. The filtrate (DMF soluble matter) was carefully separated, and the DMF insoluble matter was vacuum dried at 100°C for 24 hours, and the graft ratio was calculated using the following formula. [(GF) / (G×(100-H) / 100)]×100...Equation (3) F: Mass of component dissolved in DMF (g) G: Mass of the composition used in the test (g) H: Total content (mass%) of the first monomer unit and the second monomer unit in the composition

[0092] (Swelling ratio of composition (25°C, 15 days)) The obtained composition was dissolved in NMP to prepare 4% by mass NMP. 5.6 g of the obtained solution was added to a petri dish of PTFE (tetrafluoroethylene) and dried at 105 ° C for 8 h with a blower dryer to obtain a film with a thickness of 250 μm. The center part of the obtained film was cut to 5 mm × 5 mm to be used as a test film. The obtained test film was measured for mass, and then immersed in an electrolyte solution in which ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed at a volume ratio of 1:2. After leaving it at 25 ° C for 15 days, the liquid on the film surface was wiped off and the mass after immersion was measured. The swelling ratio was calculated from the change in mass before and after immersion using the following formula. The swelling ratio was calculated from the following formula, with the mass before immersion being WA (g) and the mass after immersion being WB (g). Swelling ratio (25°C, 15 days) (%) = WB × 100 / WA Equation (4) WA: Mass before immersion (g) WB: Mass after immersion (g)

[0093] (Swelling ratio of composition (60°C, 48 hours)) The swelling ratio when immersed in the electrolyte at 60°C for 48 hours was determined in the same manner as in (Swelling ratio of composition (25°C, 15 days)), except that the immersion conditions in the electrolyte were set to 60°C for 48 hours.

[0094] <Preparation of slurry> A mixture of 1 part by mass of the obtained binder, 2 parts by mass of acetylene black (manufactured by Denka Co., Ltd., Denka Black (registered trademark) "Li435"), and NMC532 (LiNi 0.5 Mn 0.3 Co 0.2 O2 (Umicore, TX-10) (97 parts by mass) was dissolved in 66 parts by mass of N-methyl-2-pyrrolidone (hereinafter abbreviated as NMP) to prepare a slurry for forming a positive electrode.

[0095] <Preparation of positive electrode> The prepared positive electrode slurry was applied to an aluminum foil having a thickness of 20 μm at a rate of 140 g / m using an automatic coater. 2The coating was applied so that the thickness of the positive electrode plate was 75 μm, and the positive electrode plate was pre-dried at 105°C for 30 minutes. The positive electrode plate was then pressed with a roll press at a linear pressure of 0.1 to 3.0 ton / cm, and the thickness of the positive electrode plate was adjusted to 75 μm. The positive electrode plate was then punched out into a circle of 13 mm in diameter. In order to completely remove volatile components such as residual solvent and adsorbed moisture, the positive electrode was obtained by drying at 170°C for 6 hours. The electrode area density was 29.0 mg / cm. 2 , volume density is 3.4g / cm 3 It was.

[0096] <Production of lithium-ion secondary battery> A 2032-type coin cell was fabricated using the obtained positive electrode and metallic lithium as a counter electrode. An electrolyte (a mixed solution of ethylene carbonate / diethyl carbonate = 1 / 2 (volume ratio)) in which LiPF6 was dissolved at a concentration of 1 mol / L was used as the electrolyte. A 15Φmm nonwoven fabric made of olefin fiber was used as a separator to electrically isolate them. The battery performance of the fabricated lithium-ion secondary battery was evaluated by the following method.

[0097] <Battery characteristics> The battery characteristics of the obtained battery were evaluated under the following measurement conditions. Charging conditions: CC-CV method, CC current = 0.2C, CV voltage = 4.2V, cutoff current = 1 / 20C Discharge conditions: CC method, CC current = 0.2, 0.5, 1.0, 2.0, 2.8C, cutoff voltage = 3.0V Temperature conditions: 25℃ After first charging the battery, confirm that the charge / discharge efficiency is close to 100%, then charge at 0.20mA / cm 2 The discharge capacity was measured when constant current discharge was performed at a current density of 100 V to 3.0 V, and the capacity density (mAh / g) was calculated by dividing the capacity by the amount of positive electrode active material. The current value at which this capacity (mAh) can be charged and discharged in 1 hour was defined as "1C."

[0098] <DC resistance> Currents of 0.2, 0.4, 0.6, 0.8, and 1.0 mmA were applied to an electrode of φ13 mm × 75 μm prepared in the same manner as the positive electrode described above, and the voltage was read after 10 seconds, and the resistance value was calculated using Ohm's law. Volume resistivity (Ω cm) was measured using the two-terminal method. It can be expressed by the following formula, where V is the potential difference, S is the cross-sectional area, I (A) is the current, and L (cm) is the electrode thickness. Volume resistivity (Ω cm) = (V×S) / (I×L) Formula (3)

[0099] <High temperature storage characteristics> The obtained lithium secondary battery was charged to 4.3 V at a constant current of 0.2 C (fully charged). It was placed in an environmental test chamber at 60° C. and stored for 30 days. After 30 days, it was discharged to 3.0 V at a constant current of 0.2 C at 25° C., and the high-temperature storage characteristics were calculated using the following formula. The high temperature storage characteristic (%) was calculated as follows: [(discharge capacity after storage)÷(charge capacity before storage)]×100. The obtained high-temperature storage characteristics were compared with those of a lithium secondary battery using PVDF as a positive electrode binder according to Reference Example 2 described later, and evaluated according to the following criteria. The results are shown in Table 1. A: Equivalent to a lithium secondary battery using PVDF as a binder for the positive electrode B: Compared to the lithium secondary battery using PVDF as the positive electrode binder, the high-temperature storage characteristics are poor, and the difference is within 5%. C: Compared to the lithium secondary battery using PVDF as the positive electrode binder, the high-temperature storage characteristics are poor, and the difference is more than 5% and less than 15%.

[0100] [Examples 2 to 4] <Preparation of Composition> A composition was obtained in the same manner as in Example 1, except that the blending amounts were as shown in Table 1. The results are shown in Table 1.

[0101] [Comparative Example 1] <Preparation of Composition> A composition was obtained in the same manner as in Example 1, except that the PVA was changed and the blending amounts were as shown in Table 1.

[0102] [Comparative Example 2] <Preparation of Composition> The PVA shown in Table 1 was used to prepare a resin composition.

[0103] [Reference example 1] The PVA shown in Table 1 was used to prepare a resin composition.

[0104] [Reference example 2] The resin composition used was polyvinylidene fluoride resin (HSV900: manufactured by Arkema). The results are shown in Table 1.

[0105] The abbreviations used in the following tables represent the following compounds. The monomer units represent the monomers from which the monomer units are derived. AN: Acrylonitrile OEG: Oligoethylene glycol diacrylate

[0106] [Table 1] *Indicates that the analysis results showed that there was no corresponding relaxation time component.

Claims

1. A composition for a positive electrode, comprising: The free induction decay curve of the positive electrode composition measured at 180° C. by the Solid Echo method using pulse NMR was 180 , component M 180 , component H 180 When separated into the three components, The component S 180 The component ratio is 10% or more and 80% or less, The component S 180 The relaxation time is 500 μs or more. Positive electrode composition.

2. Component H 180 The component ratio is 20% or more and 80% or less, Component H 180 The relaxation time is 100 μsec or less. The positive electrode composition according to claim 1 .

3. The free induction decay curve of the positive electrode composition measured at 27° C. by the Solid Echo method using pulse NMR was 27 , component M 27 , component H 27 When separated into the three components, Component H 27 The component ratio is 60% or more and less than 100%, Component H 27 The relaxation time is 50 μsec or less. The positive electrode composition according to claim 1 or 2.

4. The component M 180 The component ratio is 30% or more, The component M 180 The relaxation time is greater than 100 μsec and less than 500 μsec, The component S 180 The component ratio is 50% or less, Component H 180 The component ratio is 60% or less. The positive electrode composition according to any one of claims 1 to 3.

5. The component S 180 The component ratio of the component M 180 The sum of the component ratios of the components H 180 The ratio of components is greater than The positive electrode composition according to any one of claims 1 to 4.

6. The positive electrode composition contains a graft copolymer, The graft copolymer has a trunk polymer and a branch polymer, the trunk polymer comprises a polyvinyl alcohol structure, 6. The positive electrode composition according to claim 1, wherein the branch polymer comprises a first monomer unit comprising a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer.

7. The positive electrode composition according to claim 6 , wherein the first monomer unit includes a (meth)acrylonitrile monomer unit.

8. The positive electrode composition further comprises a free polymer, the free polymer has no covalent bond to the graft copolymer; The free polymer comprises at least a polymer comprising the first monomer unit, The positive electrode composition according to claim 6 or 7.

9. The positive electrode composition according to any one of claims 6 to 8, wherein the graft copolymer further contains a crosslinked portion derived from a crosslinking agent.

10. The positive electrode composition according to claim 9, wherein the positive electrode composition contains 0.2 to 10 parts by mass of a structure derived from the crosslinking agent when the positive electrode composition is taken as 100 parts by mass.

11. The positive electrode composition according to any one of claims 6 to 10, wherein the graft ratio of the graft copolymer is 40 to 3000%.

12. The positive electrode composition according to any one of claims 6 to 11, wherein the degree of saponification of the polyvinyl alcohol structure in the positive electrode composition is 60 to 100 mol %.

13. The positive electrode composition according to any one of claims 6 to 12, wherein an average degree of polymerization of the polyvinyl alcohol structure in the positive electrode composition is 300 to 4000.

14. A resin composition for a positive electrode, comprising the composition for a positive electrode according to any one of claims 1 to 13.

15. A slurry for a positive electrode comprising the composition for a positive electrode according to any one of claims 1 to 13, a positive electrode active material, and a conductive assistant.

16. The positive electrode slurry according to claim 15, wherein the solid content of the positive electrode composition is 1 to 20 mass% when the total solid content in the positive electrode slurry is 100 mass%.

17. 17. The positive electrode slurry according to claim 15, wherein the conductive assistant is at least one selected from the group consisting of fibrous carbon, carbon black, and a carbon composite in which fibrous carbon and carbon black are mutually bonded.

18. A positive electrode comprising a metal foil and a coating of the positive electrode slurry according to any one of claims 15 to 17 formed on the metal foil.

19. 20. A secondary battery comprising the positive electrode according to claim 18, wherein the secondary battery is one or more selected from the group consisting of a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, or a potassium ion secondary battery.

20. The positive electrode active material is LiNi X Mn (2-X) O 4 (where 0<X<2), Li(Co X Ni Y Mn Z ) O 2 (where 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1), and Li(Ni X Co Y A Z ) O 2 (wherein 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1), and the secondary battery is a lithium ion secondary battery.

Citation Information

Patent Citations

  • Vinylidene fluoride-based copolymer

    JP1994172452A

  • Wrinkled absorbent particles with highly available surface area for fast absorption

    JP1994506252A

  • Production of water absorptive gel solution

    JP2000095823A

  • Binder for lithium ion secondary battery electrode and its utlization

    JP2001256980A

  • Slurry composition for electrode, electrode and secondary battery

    JP2004227974A