Silicon-based particles having a core-shell structure and a method for producing the same, anode material, electrode piece and battery

Silicon-based particles with a core-shell structure address the limitations of silicon anodes by stabilizing the SEI film and reducing expansion, enhancing electron and lithium ion transmission, thereby improving the performance of lithium-ion batteries.

JP7575600B2Active Publication Date: 2024-10-29BERZELIUS (NANJING) CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023528730
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-10
Filing Date
2021-12-10
Publication Date
2024-10-29
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

Current lithium-ion batteries using graphite as the negative electrode material are limited by low energy density, and silicon-based anode materials face challenges such as severe volume change, electrode pulverization, and unstable solid electrolyte interface (SEI) film formation, leading to poor cycle stability and electrolyte consumption.

Method used

The development of silicon-based particles with a core-shell structure, comprising an oxygen-containing silicon-based compound matrix, monomeric nanosilicon particles, a silicon carbide shell layer, and a carbon layer, which are produced through surface treatment, carbon coating, and lithium insertion processes to enhance mechanical strength and electron/lithium ion transmission.

Benefits of technology

The core-shell structure improves the connection strength between particles, reduces expansion, stabilizes the SEI film, and enhances electron and lithium ion transmission, resulting in higher capacity, longer cycle life, and improved coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575600000001
    Figure 0007575600000001
  • Figure 0007575600000002
    Figure 0007575600000002
  • Figure 0007575600000003
    Figure 0007575600000003
Patent Text Reader

Abstract

The present invention provides silicon-based particles having a core-shell structure, a method for producing the same, a negative electrode material, a pole piece, and a battery. The silicon-based particles include core particles containing an oxygen-containing silicon-based compound matrix and monomeric nanosilicon particles, with the molar ratio of oxygen to silicon in the core particles being 0.5 to 1.5, a silicon carbide shell layer covering the core particles, and a carbon layer covering the silicon carbide shell layer. The silicon-based particles can be used in batteries and have features such as low expansion coefficient, longer cycle life, high capacity, and high coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of batteries, and in particular to silicon-based particles having a core-shell structure and their preparation method, anode material, pole piece and battery. [Background technology]

[0002] In recent years, with the rapid development and widespread application of various portable electronic devices, electric vehicles and energy storage systems, the demand for lithium-ion batteries with high energy density and long cycle life is becoming more and more urgent. Currently, the negative electrode active material of commercialized lithium-ion batteries is mainly graphite, but its low theoretical capacity limits the further improvement of the energy density of lithium-ion batteries. Silicon negative electrode materials have the advantage of high capacity that other negative electrode active materials cannot match, so they have become the focus of research and development in recent years, and are gradually moving from laboratory research and development to commercial application. In addition, monomeric silicon negative electrode materials have a serious volume effect during the lithium insertion and desorption process, with a volume change rate of about 300%, which leads to the powdering of the electrode material and the separation of the electrode material and the collecting fluid. In addition, silicon negative electrode materials constantly expand and contract during the charging and discharging of the battery and continue to burst, so that when the fresh interface generated is exposed to the electrolyte, a new SEI film is formed, which continues to consume the electrolyte and reduces the cycle performance of the electrode material. To address the above problems of monomeric silicon-based negative electrodes, scientific researchers have used silicon oxide as the negative electrode material of the battery. The theoretical capacity of silicon oxide is about 1700mAh / g, which is lower than that of monomeric silicon anode materials, but its expansion rate and cycle stability have obvious advantages, making it easier to realize industrial applications than monomeric silicon. However, compared with conventional graphite anode materials, silicon oxide still has technical challenges such as large expansion, unstable SEI formed in the battery, and rather poor cycle stability.

[0003] The contents of the background art are only those technologies known to the applicant and do not represent prior art in this technical field. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a silicon-based particle having a core-shell structure, which can be used in batteries and has the characteristics of low expansion rate, longer cycle life, high capacity, high coulombic efficiency, etc. [Means for solving the problem]

[0005] According to one embodiment of the present invention, the silicon-based particle having a core-shell structure includes an oxygen-containing silicon-based compound matrix and a monomeric nanosilicon particle, the molar ratio of oxygen element to silicon element in the core particle being 0.5 to 1.5, preferably 0.8 to 1.2, and more preferably 0.9 to 1.1, a silicon carbide shell layer covering the core particle, and a carbon layer covering the silicon carbide shell layer.

[0006] According to some embodiments of the present invention, the oxygen-containing silicon-based compound matrix is ​​silicon oxide (SiO X ,0 <X<1.5)である。

[0007] According to some embodiments of the present invention, the oxygen-containing silicon-based compound matrix is ​​a lithium silicate-based compound matrix, and the molar ratio of lithium element to silicon element in the core particle is 0.1-2.

[0008] According to some embodiments of the present invention, the median diameter of the core particles is 0.05 to 20 μm, preferably 0.3 to 15 μm, and more preferably 3 to 10 μm.

[0009] According to some embodiments of the present invention, the particle size SPAN value (SPAN=(D90-D10) / D50) of the core particles is ≦2.0, preferably ≦1.5, more preferably ≦1.3, and even more preferably ≦1.0.

[0010] According to some embodiments of the present invention, the monomeric nanosilicon particles are uniformly dispersed in the oxygen-containing silicon-based compound matrix.

[0011] According to some embodiments of the present invention, the median diameter of the monomeric nanosilicon particles is 0.1-25 nm, preferably 0.1-20 nm, more preferably 0.3-15 nm, and even more preferably 0.3-10 nm.

[0012] According to some embodiments of the present invention, the silicon carbide shell layer has a thickness of 1-200 nm, preferably 8-100 nm, and more preferably 10-80 nm.

[0013] According to some embodiments of the present invention, the carbon layer has a thickness of 1-2000 nm, preferably 3-500 nm, and more preferably 5-200 nm.

[0014] According to some embodiments of the present invention, the mass ratio of the carbon layer in the silicon-based particle is 0.1-15 wt.%, preferably 0.5-10 wt.%, more preferably 1-7 wt.%, and even more preferably 1-5 wt.%.

[0015] According to some embodiments of the present invention, the specific surface area of ​​the silicon-based particles is 0.1 to 20 m 2 / g, preferably 0.8 to 10m 2 / g, more preferably 1 to 7m 2 / g, and more preferably 1 to 5 m 2 / g.

[0016] According to some embodiments of the present invention, the tap density of the silicon-based particles is ≥ 0.4 g / cm 3 and preferably ≧0.7 g / cm 3 and more preferably ≧0.9 g / cm 3 It is.

[0017] According to another aspect of the present invention, there is provided a method for producing silicon-based particles having a core-shell structure, comprising the steps of surface treating silicon oxide particles, carbon coating the surface-treated silicon oxide particles to form a silicon carbide layer and a conductive carbon layer, and sieving and demagnetizing the carbon-coated material.

[0018] According to some embodiments of the present invention, the method further comprises subjecting the carbon coated material to a lithium intercalation treatment.

[0019] According to some embodiments of the present invention, the lithium insertion process is carried out using at least one of the following methods: electrochemical method, liquid phase lithium insertion method, thermal lithium insertion method, high temperature kneading method, and high energy mechanical method.

[0020] According to some embodiments of the present invention, surface treating the silicon oxide particles includes a gas phase treatment or a liquid phase treatment.

[0021] Specifically, the purpose of the surface treatment is to form an active oxygen-rich silicon oxide shell layer on the surface of the silicon oxide particles, which can react with a carbon source precursor in a subsequent carbonization process to produce the desired silicon carbide shell layer.

[0022] According to some embodiments of the present invention, silicon oxide particles are heat-treated in an oxygen-containing atmosphere, the oxygen content is between 100 ppm and 100 vol%, the water vapor content is between 1 ppm and 20 vol%, the heating time is 10 to 600 minutes, and the heat treatment temperature is 300 to 1100° C. The oxygen-containing atmosphere includes one or more of oxygen, water vapor, and air. The gas-phase treatment can be performed using any one of equipments such as a tube furnace, an atmospheric box furnace, a pusher kiln, a roller kiln, or a rotary kiln.

[0023] According to some embodiments of the present invention, surface treating the silicon oxide particles includes a liquid phase treatment of immersing the silicon oxide particles in water, or an aqueous hydrogen peroxide solution or a nitric acid solution, the mass concentration of the aqueous hydrogen peroxide solution or the nitric acid solution being ≦30 wt.%, the liquid phase treatment temperature being 0 to 100° C., preferably 10 to 85° C., and more preferably 20 to 60° C., and the liquid phase treatment time being 10 to 600 minutes, preferably 20 to 360 minutes, more preferably 20 to 300 minutes, even more preferably 40 to 240 minutes, and even more preferably 40 to 120 minutes.

[0024] According to some embodiments of the present invention, immersing the silicon oxide particles in water, an aqueous hydrogen peroxide solution, or a nitric acid solution further includes stirring the silicon oxide particles to uniformly contact the silicon oxide particles with the water, the aqueous hydrogen peroxide solution, or the nitric acid solution.

[0025] According to some embodiments of the present invention, carbon coating the surface-treated silicon oxide particles may be achieved by a chemical vapor deposition process or a thermal carbonization process that includes first mixing the surface-treated silicon oxide particles with a carbon precursor and carbonizing them by thermal treatment in a non-oxidizing atmosphere.

[0026] According to some embodiments of the present invention, the temperature of the chemical vapor deposition method or the heat treatment carbonization method is 800-1200° C., and is kept constant for 0.5-24 hours.

[0027] Specifically, the carbon layer material for chemical vapor deposition can be one or more of methane, ethane, ethylene, acetylene, propane, propylene, butane, butene, butadiene, benzene, toluene, xylene, styrene, or phenol, and the silicon carbide layer is obtained by reacting the above material with the surface treatment layer of silicon oxide particles during the chemical vapor deposition process.

[0028] Specifically, the carbon precursor in the heat treatment carbonization method includes one or more of glucose, sucrose, shell polysaccharide, starch, citric acid, gelatin, alginic acid, carboxymethyl cellulose, coal tar pitch, petroleum asphalt, phenolic resin, tar, naphthalene oil, anthracene oil, polyacrylic acid, polyacrylic acid ester, polystyrene, polyvinylpyrrolidone, polyoxyethylene, polyvinyl alcohol, epoxy resin, polyacrylonitrile, and polymethyl methacrylate, and the silicon carbide layer is obtained by reacting the above materials with the surface treatment layer of silicon oxide particles during the heat treatment process.

[0029] According to some embodiments of the present invention, the non-oxidizing atmosphere includes one or more of nitrogen gas, argon gas, hydrogen gas, or helium gas.

[0030] Furthermore, the surface-treated silicon oxide particles and the carbon precursor are mixed by using any one of a VC mixer, a two-dimensional mixer, a three-dimensional mixer, a V-type mixer, a horizontal mixer, a double cone mixer, and a ribbon mixer to uniformly mix the silicon oxide particles and the carbon precursor, followed by heat treatment. Alternatively, the silicon oxide particles and the carbon precursor are mixed by adding a solvent by using any one of a VC mixer, a coating, and a high-speed disperser, followed by drying to obtain a composite of the silicon oxide particles and the carbon precursor. Furthermore, the added solvent includes one or more combinations of water, methanol, ethanol, isopropanol, N-butanol, ethylene glycol, ethyl ether, acetone, N-methylpyrrolidone, methylbutanone, tetrahydrofuran, benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, and trichloromethane.

[0031] Furthermore, the carbon coating equipment includes a tube furnace, an atmosphere box furnace, a pusher kiln, a roller kiln or a rotary kiln.

[0032] According to some embodiments of the present invention, the carbon coating of the surface-treated silicon oxide particles further includes performing a scattering treatment, and the scattering equipment includes any one of an airflow mill, a ball mill, a turbine mill, a Raymond mill, a plow mill, and a gear mill.

[0033] According to another aspect of the invention there is also provided an anode material for a battery comprising silicon-based particles as described above.

[0034] Furthermore, the negative electrode material is prepared by mixing silicon-based particles having a core-shell structure with a carbon-based powder material, and the carbon-based powder material is any combination of one or more selected from the group consisting of natural graphite, artificial graphite, surface-modified natural graphite, hard carbon, soft carbon, or mesophase carbon microspheres.

[0035] According to another aspect of the invention, there is also provided a pole piece comprising the anode material as described above.

[0036] According to another aspect of the invention, there is also provided a battery including a pole piece as described above. Effect of the Invention

[0037] According to some embodiments, the core-shell structure of the silicon-based particles of the present invention can increase the connection strength between the core particles and the outer carbon layer, and reduce the falling off of the carbon layer caused by the repeated expansion of the material particles during the battery cycle process.When the oxygen-containing silicon-based compound matrix is ​​a lithium silicate-based compound matrix, the provision of the core-shell structure can improve the water resistance of the material.

[0038] In addition, the high mechanical strength of silicon carbide can effectively suppress the expansion of material particles during the lithium insertion / extraction process, reducing damage to the SEI film and improving battery cycle performance.

[0039] In addition, the carbon layer coating provides excellent electron and lithium ion transmission paths, ensuring that the silicon-based particles with core-shell structure can fully participate in the electrochemical reaction, reducing the polarization of the battery and improving the battery's power supply performance.

[0040] The drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their explanations are used to interpret the present invention and do not constitute undue limitations on the present invention. [Brief description of the drawings]

[0041] [Figure 1] FIG. 2 is a schematic diagram of a silicon-based grain structure according to an exemplary embodiment of the present invention. [Diagram 2] 1 is a scanning electron microscope (SEM) photograph of a cross-section of a silicon-based particle according to an exemplary embodiment of the present invention. [Diagram 3] 1 is a flow chart of a manufacturing process for silicon-based particles according to an exemplary embodiment of the present invention. [Figure 4] 4 is a SEM photograph of a cross-section of a silicon-based particle according to another exemplary embodiment of the present invention. [Diagram 5] 4 is a flow chart of a manufacturing process for silicon-based particles according to another exemplary embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] Hereinafter, specific embodiments of the present invention will be described in more detail in conjunction with the drawings and embodiments, so that the aspects of the present invention and the advantages of each aspect can be more fully understood. However, the specific embodiments and examples described below are for the purpose of explanation only and are not limitations on the present invention.

[0043] In view of the above background, the present invention will now be described with reference to specific examples.

[0044] [Silicon-based particles] FIG. 1 is a schematic diagram of a silicon-based grain structure according to an exemplary embodiment of the present invention.

[0045] 1, according to an exemplary embodiment, the silicon-based particle of the present invention includes a core particle 101, a silicon carbide shell layer 103, and a carbon layer 105. The core particle 101 includes an oxygen-containing silicon-based compound matrix and a monomeric nanosilicon particle. Alternatively, the oxygen-containing silicon-based compound matrix is ​​a silicon oxide matrix or a lithium silicate-based compound matrix.

[0046] Alternatively, the molar ratio of oxygen element to silicon element in the core particle 101 is 0.5 to 1.5, preferably 0.8 to 1.2, and more preferably 0.9 to 1.1. When the oxygen-containing silicon-based compound matrix is ​​a lithium silicate compound matrix, the molar ratio of lithium element to silicon element in the core particle is 0.1 to 2.

[0047] According to some embodiments, the median diameter of the core particles is 0.05-20 μm, preferably 0.3-15 μm. In some embodiments of the present invention, when the silicon-based particles do not contain lithium (i.e., the oxygen-containing silicon-based compound matrix is ​​a silicon oxide matrix), the particle size span value of the core particles is ≦2.0, preferably ≦1.5, more preferably ≦1.0. In some embodiments of the present invention, when the silicon-based particles contain lithium (i.e., the oxygen-containing silicon-based compound matrix is ​​a lithium silicate-based compound matrix), the particle size span value of the core particles is ≦2.0, preferably ≦1.5, more preferably ≦1.3. According to an exemplary embodiment, the monomeric nanosilicon particles are uniformly dispersed in the oxygen-containing silicon-based compound matrix. In some embodiments of the present invention, when the silicon-based particles do not contain lithium, the median diameter of the monomeric nanosilicon particles is 0.1-20 nm, preferably 0.3-10 nm. In some embodiments of the present invention, when the silicon-based particles contain lithium, the median diameter of the monomeric nanosilicon particles is 0.1-25 nm, preferably 0.3-15 nm.

[0048] As shown in Figure 1, according to an exemplary embodiment, a silicon carbide shell layer 103 covers the core particle 101. The core-shell structure is clearly shown in the SEM photographs of the cross-section of the silicon-based particle of the embodiment shown in Figures 2 and 4. The thickness of the silicon carbide shell layer 103 is 1-200 nm, preferably 8-100 nm, and more preferably 10-80 nm.

[0049] As shown in FIG. 1, according to some embodiments, a carbon layer (also referred to as a conductive carbon layer in the present invention) 105 covers the silicon carbide shell layer 103. The thickness of the carbon layer 105 is 1-2000 nm, preferably 3-500 nm, and more preferably 5-200 nm. In some embodiments of the present invention, when the silicon-based particle does not contain lithium, the mass ratio of the carbon layer in the silicon-based particle is 0.1-15 wt.%, preferably 0.5-10 wt.%, and more preferably 1-7 wt.%. In some embodiments of the present invention, when the silicon-based particle contains lithium, the mass ratio of the carbon layer in the silicon-based particle is 0.1-15 wt.%, preferably 0.5-10 wt.%, and more preferably 1-5 wt.%.

[0050] In some embodiments of the present invention, when the silicon-based particles do not contain lithium, the silicon-based particles have a specific surface area of ​​0.1 to 20 m 2 / g, preferably 0.8 to 10m 2 / g, more preferably 1 to 5m 2 In some embodiments of the present invention, when the silicon-based particles contain lithium, the specific surface area of ​​the silicon-based particles is 0.1 to 20 m 2 / g, preferably 0.8 to 10m 2 / g, more preferably 1 to 7m 2 In some embodiments of the present invention, when the silicon-based particles are lithium-free, the tap density is ≥ 0.4 g / cm 3 and preferably ≧0.7 g / cm 3 and more preferably ≧0.9 g / cm 3 In some embodiments of the present invention, when the silicon-based particles contain lithium, the tap density is ≧0.4 g / cm 3 and preferably ≧0.7 g / cm 3 It is.

[0051] [Method of manufacturing silicon-based particles] FIG. 3 is a flow chart of a process for producing silicon-based particles according to an exemplary embodiment of the present invention.

[0052] As shown in Figure 3, in S301, silicon oxide particles are surface-treated. The general formula of silicon oxide used in the present invention is SiO X X is 0.5 to 1.5, preferably 0.8 to 1.2, and more preferably 0.9 to 1.1. Silicon oxides with X close to 1 are generally called silicon oxides. The specific manufacturing process of silicon oxide particles can be performed in the following steps. First, in an inert gas atmosphere or under reduced pressure conditions, a mixture of metal silicon powder and silicon dioxide powder is heated within a temperature range of 900°C to 1600°C to generate silica gas. This gas is deposited on an adsorption plate. When the temperature in the reactor is lowered to below 100°C, the deposit is removed and crushed and powdered using equipment such as a ball mill and an airflow crusher to obtain silicon oxide particles.

[0053] In S301, the surface treatment includes a gas-phase or liquid-phase treatment, the purpose of which is to form an oxygen-rich active silicon oxide shell layer on the surface of the silicon oxide particles, which can be reacted with a carbon source precursor in a subsequent carbonization process to produce the desired silicon carbide shell layer.

[0054] According to some embodiments, the gas phase treatment includes heat treating the core particles in an oxygen or water vapor atmosphere, where the heating time is 10-600 minutes and the heat treatment temperature is 300-1100° C. The heat treatment atmosphere can be selected as water vapor, and the content of water vapor is between 1 ppm and 20 vol%.

[0055] The liquid-phase treatment includes immersing silicon oxide particles in water, an aqueous hydrogen peroxide solution, or a nitric acid solution, where the solution concentration is ≦30 wt.%, the liquid-phase treatment temperature is 0-100° C., and the treatment time is 10-600 minutes. In this process, immersing silicon oxide particles in water, an aqueous hydrogen peroxide solution, or a nitric acid solution also includes stirring so that the silicon oxide particles are uniformly contacted with the water, the aqueous hydrogen peroxide solution, or the nitric acid solution.

[0056] When the surface treatment of the silicon oxide particles is completed, the process proceeds to S303.

[0057] In S303, the surface-treated silicon oxide particles are carbon-coated to form a silicon carbide layer and a conductive carbon layer. According to an exemplary embodiment, the main methods of carbon coating include adopting chemical vapor deposition, heat-treatment carbonization, etc.

[0058] If chemical vapor deposition is used, the temperature is controlled to 800°C to 1200°C and kept constant for 0.5 to 24 hours. The carbon layer material can include one or more of methane, ethane, ethylene, acetylene, propane, propylene, butane, butene, butadiene, benzene, toluene, xylene, styrene, or phenol.

[0059] When the heat treatment carbonization method is adopted, specifically, the surface-treated silicon oxide particles are mixed with a carbon precursor and heat-treated and carbonized in a non-oxidizing atmosphere. The temperature is 800-1200°C, and is kept constant for 0.5-24 hours. According to an exemplary embodiment, the carbon precursor includes one or more of glucose, sucrose, shell polysaccharide, starch, citric acid, gelatin, alginic acid, carboxymethyl cellulose, coal tar pitch, petroleum asphalt, phenolic resin, tar, naphthalene oil, anthracene oil, polyacrylic acid, polyacrylic acid ester, polystyrene, polyvinylpyrrolidone, polyoxyethylene, polyvinyl alcohol, epoxy resin, polyacrylonitrile, and polymethyl methacrylate. The non-oxidizing atmosphere includes one or more of nitrogen gas, argon gas, hydrogen gas, and helium gas.

[0060] According to some embodiments, the mixing process uses any one of a VC mixer, a two-dimensional mixer, a three-dimensional mixer, a V-type mixer, a horizontal mixer, a double cone mixer, and a ribbon mixer to uniformly mix the silicon oxide particles and the carbon precursor, followed by heat treatment. Alternatively, any one of a VC mixer, a coating, and a high-speed disperser is used to uniformly mix the silicon oxide particles and the carbon precursor, and then the mixture is dried to obtain a composite of the silicon oxide particles and the carbon precursor. Furthermore, the additive solvent includes one or more of water, methanol, ethanol, isopropanol, N-butanol, ethylene glycol, ethyl ether, acetone, N-methylpyrrolidone, methylbutanone, tetrahydrofuran, benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, and trichloromethane.

[0061] According to an exemplary embodiment, the equipment used for carbon coating in S303 includes a tube furnace, an atmosphere box furnace, a pusher kiln, a roller kiln, or a rotary kiln. In addition, after carbon coating is completed, scattering treatment can be performed, and the scattering equipment includes any one of an airflow mill, a ball mill, a turbine mill, a Raymond mill, a plow mill, and a gear mill. Then, proceed to S305.

[0062] In S305, according to an exemplary embodiment, the carbon-coated material is sieved and demagnetized to obtain silicon-based particles with a core-shell structure for use in the negative electrode material.

[0063] FIG. 5 is a flow chart of a manufacturing process for silicon-based particles according to another exemplary embodiment of the present invention, which includes the following steps.

[0064] S501: Surface-treat silicon oxide particles.

[0065] S503: Carbon-coating the surface-treated silicon oxide particles to form a silicon carbide layer and a conductive carbon layer.

[0066] S505: The carbon-coated material is subjected to a lithium insertion process.

[0067] S507: The lithium-intercalated material is screened and demagnetized.

[0068] However, steps S501, S503 and S507 are similar to steps S301, S303 and S305 described above, and therefore the description thereof will be omitted here.

[0069] In S505, according to an exemplary embodiment, a lithium insertion process is performed to insert lithium into the silicon oxide particles having the silicon carbide layer and the conductive carbon layer. The lithium insertion process includes electrochemical method, liquid phase lithium insertion method, thermal lithium insertion method, high temperature kneading method, high energy mechanical method, etc. Among them, electrochemical method, liquid phase lithium insertion method and thermal lithium insertion method are preferred.

[0070] According to some embodiments, when performing lithium insertion processing using electrochemical methods, it is necessary to provide an electrochemical cell including four components, a bath, an anode electrode, a cathode electrode, and a power source, and the anode electrode and the cathode electrode are respectively connected to both ends of the power source. At the same time, the anode electrode is turned on with a lithium source, and the cathode electrode is connected to a container containing silicon oxide particles. The bath is filled to the brim with an organic solvent, and the lithium source (anode electrode) and the container containing silicon oxide particles (cathode electrode) are immersed in the organic solvent. After the power is turned on, the lithium ions are inserted into the silicon oxide structure due to the occurrence of an electrochemical reaction, and silicon oxide particles that have been subjected to lithium insertion processing are obtained. As the organic solvent, solvents such as vinyl carbonate, propylene carbonate, butene carbonate, fluorovinyl carbonate, dimethyl carbonate, ethyl carbonate, diethyl carbonate, ethyl acetate, ethyl acetate, propyl acetate, ethyl propionate, dimethyl sulfoxide, etc. can be used. This organic solvent also contains an electrolyte lithium salt, and lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), etc. can be used. The lithium source (anode electrode) can be a lithium foil or a lithium compound such as lithium carbonate, lithium oxide, lithium hydroxide, lithium cobalt oxide, lithium iron phosphate, lithium manganate, lithium vanadium phosphate, or lithium nickel oxide.

[0071] Silicon oxide can also be lithium-inserted using the liquid-phase lithium insertion method. In a specific implementation, metallic lithium, an electron transfer catalyst, and silicon oxide particles are added to an ether-based solvent, and the mixture is stirred in a non-oxidizing atmosphere until the metallic lithium in the solution is completely eliminated, and the mixture is heated to maintain a constant temperature reaction. Under the action of the electron transfer catalyst, metallic lithium can be dissolved in an ether-based solvent to form a lithium ion coordination compound, which has a relatively low reduction potential, and can react with silicon oxide, and the lithium ion can enter the silicon oxide structure. The electron transfer catalyst includes biphenyl, naphthalene, etc. The ether-based solvent includes methyl butyl ether, ethylene glycol butyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, etc. The constant temperature reaction temperature is 25°C to 200°C. The material can then be further heat-treated in a non-oxidizing atmosphere, and the temperature of the heat treatment is 400°C to 900°C, preferably 500°C to 850°C. The non-oxidizing atmosphere is provided by at least one gas selected from the group consisting of nitrogen gas, argon gas, hydrogen gas, and helium gas.

[0072] Silicon oxide can also be lithium-inserted using a thermal lithium insertion method. In a specific implementation, silicon oxide particles are uniformly mixed with a lithium-containing compound and then heat-treated in a non-oxidizing atmosphere. The lithium-containing compound includes lithium hydroxide, lithium carbonate, lithium oxide, lithium peroxide, lithium hydride, lithium nitrate, lithium acetate, lithium oxalate, etc. The mixing method uses any one of a high-speed disperser, a high-speed stirrer, a ball mill, a taper mixer, a spiral mixer, a stirring mixer, and a VC mixer. The heat treatment equipment is any one of a rotary furnace, a ladle refining furnace, an inner pot furnace, a roller kiln, a pusher kiln, an atmospheric box furnace, and a tube furnace. The temperature of the heat treatment is 400 to 900°C, preferably 550 to 850°C, the warming time is 0.1 to 12 hours, and the heating rate is greater than 0.1°C / min and less than 20°C / min. The non-oxidizing atmosphere is provided by at least one gas selected from the group consisting of nitrogen gas, argon gas, hydrogen gas, and helium gas.

[0073] [Characteristics of silicon-based particles] 1. The equipment used to detect silicon-based particles is as follows:

[0074] A Hitachi SU8010 cold field emission scanning electron microscope was used to observe the surface morphology of the samples and the thicknesses of the silicon carbide shell layer and the conductive carbon film layer.

[0075] The particle size and particle size distribution of the materials were measured using a Dandong Baite Bettersize 2000LD laser particle sizer.

[0076] The specific surface area of ​​the materials was measured using a Conta Quantachrome Nova4200e specific surface area measurement device.

[0077] The tap density of the materials was measured using a Dandong Baite BT-301 tap density meter.

[0078] The carbon content in the carbon layer of the materials was measured using an elementarvario EL cube elemental analyzer.

[0079] The crystal structure of the materials was measured using a Rigaku MiniFlex600 X-ray diffractometer.

[0080] The silicon carbide content in the material was measured using a LabRamHR800 Raman scattering spectrometer, and the TO (transverse optical) vibration mode peak of silicon carbide was found to be in the range of 700 to 800 cm -1 That was about it.

[0081] 2.Performance measurement Preparation of electrode pieces: 9 parts of silicon-based particles having the above core-shell structure, 43.5 parts of artificial graphite, 43.5 parts of natural graphite, 1 part of conductive additive SuperP, 0.5 parts of multi-walled carbon nanotubes, 1 part of binder sodium carboxymethylcellulose CMC, and 1.5 parts of modified polyacrylate were taken, homogenized under an aqueous system, coated, dried, and roll-pressed to obtain negative electrode pieces containing silicon-based particles.

[0082] Half-cell evaluation: The above-prepared core-shell structured silicon-based particle negative electrode, separator, lithium piece, and stainless steel spacer were stacked in order, 200μL of electrolyte was dripped onto them, and then sealed to create a 2016-type lithium-ion half-cell. The capacity and discharge efficiency were measured using a small (micro) current range device from Wuhan Landen Electronics Co., Ltd. The initial reversible desorption lithium specific capacity of the negative half-cell and the initial charge / discharge coulombic efficiency were measured.

[0083] Whole battery evaluation: The negative electrode piece of the silicon-based particles with the core-shell structure prepared above was rolled, cut, lug-welded, etc., and then paired with a positive electrode piece (ternary nickel-cobalt-manganese material, LiNi 0.8 Co 0.1 Mn 0.1O2) and a separator, then put into an aluminum shell of the corresponding size, vacuum baked, and then injected with a certain amount of electrolyte, sealed, and formed to obtain a complete silicon-based particle anode-containing lithium-ion monolayer stacked whole battery. The battery capacity is about 50mAh. At least five stacked whole batteries were manufactured for each material for measurement. Performance measurements were performed on the whole battery of this group using a battery tester from Wuhan Lanhe Co., Ltd., with a voltage range of 4.2 to 2.75V. The main measurement items were the discharge capacity and average voltage at 0.2C, and the capacity retention rate data for 200 cycles at a charge and discharge rate of 0.5C. The electrochemical data obtained from the above measurements were combined with the areal density of the positive electrode, negative electrode, and separator obtained by weighing them during battery production, and the unit (i.e., the combination of the positive electrode, negative electrode, and separator) weight energy density of the whole battery was calculated and obtained. The battery in a charged state after one charge-discharge cycle in an inert atmosphere was disassembled, and the thickness of the negative electrode piece excluding the thickness of the negative electrode piece before the battery was assembled was measured to obtain the expansion rate of the negative electrode piece.

[0084] Water resistance measurement: 1 g of the silicon-based particles having a core-shell structure obtained above was taken and placed in a small bottle, 50 g of ion-depleted water and a magnetic rotor were added, and the bottle was placed on a magnetic stirrer at room temperature and stirring was started. After sealing, the amount of gas generated was measured using a wastewater gas collection method, and the time when gas generation began was recorded.

[0085] In view of the above examples, the silicon-based particles of the present invention have a core-shell structure, and the silicon carbide shell layer increases the connection strength between the core particle and the outermost carbon layer, effectively preventing the destruction of the particle outer carbon shell during the negative electrode material, battery electrode and battery processing process, and effectively mitigating the detachment of the outer conductive carbon layer due to the repeated expansion and contraction of the material particles during the battery cycle process.

[0086] Compared with the oxygen-containing silicon-based compound in the core particle and the outermost conductive carbon film layer, the silicon carbide shell layer has higher mechanical strength and can effectively suppress the expansion of the material particles during the lithium insertion process, thereby effectively reducing the expansion rate of the electrode surface and the battery surface. Moreover, the suppression of particle expansion can reduce the damage of the SEI film on the particle surface and promote the cycle performance of the battery.

[0087] The carbon layer coating simultaneously provides excellent electron and lithium ion transmission paths, ensures that the silicon-based particles with core-shell structure can fully participate in the electrochemical reaction, reduces the polarization of the battery, and improves the charge-dissipation performance.

[0088] When the oxygen-containing silicon-based compound matrix of the core is a lithium silicate-based compound matrix, the silicon carbide shell layer itself has water resistance and is denser than the conductive carbon layer, which can block the dissolution and erosion of water into the lithium-containing core particles during the environmental humidity and aqueous homogenization process, and the material can be applied to the currently commonly used aqueous homogenization coating system, which can reduce the performance degradation caused by the side effects of materials and moisture during the processing process, improve the flow deformation properties and adhesion properties of the negative electrode slurry, and improve the quality of the pole pieces.

[0089] Example 1-1 Silicon suboxide particle powder (D50=3.0 μm, SPAN=2.0) was taken and placed in humid air with a relative humidity (the ratio of the actual water vapor content in air to the saturated water vapor content at a constant temperature) of 100% at 25°C, the temperature was 600°C, and the time was 60 minutes, resulting in silicon suboxide particles with an oxygen-rich shell layer.

[0090] 2 kg of the above surface-treated silicon suboxide particle powder and 7 wt.% petroleum asphalt were added to a VC mixer and mixed for 30 min at a linear velocity of 8 m / s at the maximum diameter of the mixing part to uniformly mix the two raw materials.

[0091] The above mixture was placed in a graphite crucible and placed in a box furnace, where it was heated to 1000°C at 3°C / min with nitrogen gas protection, kept at that temperature for 4 hours, and then naturally cooled to room temperature to complete the carbonization process. In this step, the asphalt was carbonized by high-temperature treatment in an oxygen-free atmosphere, and partially reacted with the oxygen-rich shell layer on the surface of the silicon suboxide particles to produce a silicon carbide shell layer. The heat-treated material was scattered, sieved, and demagnetized.

[0092] The specific surface area of ​​the silicon-based particles of Example 1-1 measured using the above equipment was 4.0 m 2 / g and the tap density is 1.0 g / cm 3 and the carbon content was 4.8 wt.%. From the results of the X-ray diffraction pattern, by substituting the Sherrer equation, it was possible to calculate that the size of the crystal grains corresponding to the Si(111) crystal plane in the material obtained in Example 1-1 was 4.2 nm. The Raman scattering spectrum indicated the presence of silicon carbide in the material. When the cross-section of the sample was observed with a scanning electron microscope, it was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 55 nm thick, and the outermost layer was covered with a carbon layer about 60 nm thick.

[0093] 9 parts of the above-mentioned core-shell structured silicon-based particles, 43.5 parts of artificial graphite, 43.5 parts of natural graphite, 1 part of conductive additive SuperP, 0.5 parts of multi-walled carbon nanotubes, 1 part of binder sodium carboxymethylcellulose CMC, and 1.5 parts of modified polyacrylate were taken, homogenized under an aqueous system, coated, dried, and roll-pressed to obtain negative electrode pieces containing silica lithium particles.

[0094] Using the above half-cell evaluation measurement method, the initial reversible lithium desorption specific capacity of the negative electrode half-cell obtained in Example 1-1 was 453.6 mAh / g, and the initial charge / discharge coulombic efficiency was 88.2%.

[0095] Using the above-mentioned whole battery evaluation measurement method, the expansion rate of the negative electrode piece obtained in Example 1-1 was 26.3%, the unit weight energy density was 382.5Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 91.3%.

[0096] Example 1-2 Silicon suboxide particle powder (D50=3.0μm, SPAN=2.0) was taken, placed in a 20wt% aqueous hydrogen peroxide solution, heated to 30℃, and held for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0097] Subsequent treatment was carried out in the same manner as in Example 1-1.

[0098] The specific surface area of ​​the silicon-based particles in Example 1-2 is 4.0 m 2 / g and the tap density is 0.9 g / cm 3 The carbon content was 4.7 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.2 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 55 nm thick, and the outermost layer was covered with a carbon layer about 60 nm thick.

[0099] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 455.2 mAh / g, the initial charge / discharge coulombic efficiency was 88.5%, the negative electrode piece expansion rate of the resulting full cell was 26.4%, the unit weight energy density was 385.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 91%.

[0100] Examples 1-3 Silicon suboxide particle powder (D50=7.5μm, SPAN=2.0) was taken, placed in a hydrogen peroxide aqueous solution with a concentration of approximately 20wt%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0101] Subsequent treatment was carried out in the same manner as in Example 1-1, except that the carbon precursor used was 5 WT.% coal tar pitch.

[0102] The specific surface area of ​​the silicon-based particles in Example 1-3 is 1.6 m 2 / g and the tap density is 1.3 g / cm 3 The carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.2 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 45 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0103] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 463.6 mAh / g, the initial charge / discharge coulombic efficiency was 89.8%, the negative electrode piece expansion rate of the resulting full cell was 27.3%, the unit weight energy density was 398.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 91%.

[0104] Examples 1-4 Silicon suboxide particle powder (D50=7.5μm, SPAN=1.5) was taken, placed in a hydrogen peroxide aqueous solution with a concentration of approximately 20wt%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon-based particles with an oxygen-rich shell layer.

[0105] Subsequent processing was carried out in the same manner as in Example 1-3.

[0106] The specific surface area of ​​the silicon-based particles in Examples 1-4 is 1.4 m 2 / g and the tap density is 1.3 g / cm 3The carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.2 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 55 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0107] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 467.6 mAh / g, the initial charge / discharge coulombic efficiency was 90.3%, the negative electrode piece expansion rate of the resulting full cell was 26.6%, the unit weight energy density was 400.4 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 93.8%.

[0108] Examples 1-5 Silicon suboxide particle powder (D50 = 7.5 μm, SPAN = 1.0) was taken, placed in a hydrogen peroxide aqueous solution with a concentration of approximately 20 wt.%, heated to 30°C, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0109] Subsequent processing was carried out in the same manner as in Example 1-3.

[0110] The specific surface area of ​​the silicon-based particles in Examples 1-5 is 1.3 m 2 / g and the tap density is 1.2 g / cm 3 and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 65 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0111] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 472.6 mAh / g, the initial charge / discharge coulombic efficiency was 91%, the negative electrode piece expansion rate of the resulting full cell was 26%, the unit weight energy density was 402.3 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 95.4%.

[0112] Examples 1-6 Silicon suboxide particle powder (D50=3.0μm, SPAN=1.5) was taken, placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0113] Subsequent treatment was carried out in the same manner as in Example 1-1.

[0114] The specific surface area of ​​the silicon-based particles of Examples 1-6 is 3.5 m 2 / g and the tap density is 0.9 g / cm 3 The carbon content was 4.8 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 3.9 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 70 nm thick, and the outermost layer was covered with a carbon layer about 60 nm thick.

[0115] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 458.7mAh / g, the initial charge / discharge coulombic efficiency was 89.3%, the negative electrode piece expansion rate of the resulting full cell was 25.7%, the unit weight energy density was 391.9Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 91.2%.

[0116] Examples 1-7 Silicon suboxide particle powder (D50=3.0μm, SPAN=1.0) was taken, placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0117] Subsequent treatment was carried out in the same manner as in Example 1-1.

[0118] The specific surface area of ​​the silicon-based particles of Examples 1-7 is 3.0 m 2 / g and the tap density is 0.9 g / cm 3 The carbon content was 4.9 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 80 nm thick, and the outermost layer was covered with a carbon layer about 60 nm thick.

[0119] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 460.3 mAh / g, the initial charge / discharge coulombic efficiency was 90%, the negative electrode piece expansion rate of the resulting full cell was 25%, the unit weight energy density was 394.7 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 92.4%.

[0120] Examples 1-8 Silicon suboxide particle powder (D50=10.0μm, SPAN=1.5) was taken, placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed in stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0121] Subsequent treatment was carried out in the same manner as in Example 1-1, except that 4 WT.% petroleum asphalt was used.

[0122] The specific surface area of ​​the silicon-based particles of Examples 1-8 is 1.0 m 2 / g and the tap density is 1.3 g / cm 3The carbon content was 3.0 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 45 nm thick, and the outermost layer was covered with a carbon layer about 45 nm thick.

[0123] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 470.2 mAh / g, the initial charge / discharge coulombic efficiency was 90.8%, the negative electrode piece expansion rate of the resulting full cell was 27.1%, the unit weight energy density was 402.1 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 95.4%.

[0124] Examples 1-9 Silicon suboxide particle powder (D50=5.0μm, SPAN=1.0) was taken and placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0125] Subsequent treatment was carried out in the same manner as in Example 1-1, except that 6 WT.% petroleum asphalt was used.

[0126] The specific surface area of ​​the silicon-based particles of Examples 1-9 is 2.0 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.0 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 75 nm thick, and the outermost layer was covered with a carbon layer about 55 nm thick.

[0127] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 468.3 mAh / g, the initial charge / discharge coulombic efficiency was 90.6%, the negative electrode piece expansion rate of the resulting full cell was 25.5%, the unit weight energy density was 397.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 94%.

[0128] Examples 1-10 Silicon suboxide particle powder (D50=5.0μm, SPAN=1.0) was taken and placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0129] Subsequent treatment was carried out in the same manner as in Example 1-9, except that the heat treatment temperature was 800° C. and the heat retention time was 6 hours.

[0130] The specific surface area of ​​the silicon-based particles of Examples 1-10 is 2.1 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.0 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 3.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 45 nm thick, and the outermost layer was covered with a carbon layer about 55 nm thick.

[0131] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 462.2 mAh / g, the initial charge / discharge coulombic efficiency was 90.1%, the negative electrode piece expansion rate of the resulting full cell was 26.7%, the unit weight energy density was 395.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 94.9%.

[0132] Examples 1-11 Silicon suboxide particle powder (D50 = 5.0 μm, SPAN = 1.5) was taken, placed in a hydrogen peroxide aqueous solution with a concentration of approximately 20 wt.%, heated to 30°C, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0133] Subsequent treatment was carried out in the same manner as in Example 1-9, except that the heat treatment temperature was 1200° C. and the heat retention time was 3 hours.

[0134] The specific surface area of ​​the silicon-based particles of Examples 1-11 is 2.0 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.2 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 6.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 100 nm thick, and the outermost layer was covered with a carbon layer about 55 nm thick.

[0135] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 511.3 mAh / g, the initial charge / discharge coulombic efficiency was 90.7%, the negative electrode piece expansion rate of the resulting full cell was 24.7%, the unit weight energy density was 381.6 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 92.6%.

[0136] Examples 1-12 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.0) was taken, placed in dry air with a flow rate of 200 sccm, heated to 600° C. and held for 60 minutes to perform a surface treatment, thereby obtaining silicon suboxide particles having an oxygen-rich shell layer.

[0137] Subsequent processing was carried out in the same manner as in Example 1-9.

[0138] The specific surface area of ​​the silicon-based particles of Examples 1-12 is 2.0 m 2 / g and the tap density is 1.2 g / cm 3The carbon content was 4.2 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 5 nm thick, and the outermost layer was coated with a carbon layer about 55 nm thick.

[0139] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 461.2 mAh / g, the initial charge / discharge coulombic efficiency was 90.4%, the negative electrode piece expansion rate of the resulting full cell was 27.7%, the unit weight energy density was 394.7 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.8%.

[0140] Examples 1-13 Silicon suboxide particle powder (D50 = 5.0 μm, SPAN = 1.0) was taken, placed in dry air with a flow rate of 100 sccm and oxygen with 100 sccm, heated to 500°C and held for 60 minutes, and surface-treated to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0141] Subsequent processing was carried out in the same manner as in Example 1-9.

[0142] The specific surface area of ​​the silicon-based particles of Examples 1-13 is 2.0 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.1 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 5 nm thick, and the outermost layer was covered with a carbon layer about 55 nm thick.

[0143] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 460.3 mAh / g, the initial charge / discharge coulombic efficiency was 90%, the negative electrode piece expansion rate of the resulting full cell was 27.5%, the unit weight energy density was 393.1 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.4%.

[0144] Examples 1-14 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.0) was taken, placed in oxygen with a flow rate of 200 sccm, heated to 400° C. and held for 60 minutes to perform a surface treatment, thereby obtaining silicon suboxide particles having an oxygen-rich shell layer.

[0145] Subsequent processing was carried out in the same manner as in Example 1-9.

[0146] The specific surface area of ​​the silicon-based particles of Examples 1-14 is 2.0 m 2 / g and the tap density is 1.2 g / cm 3 The carbon content was 4.1 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 5 nm thick, and the outermost layer was covered with a carbon layer about 55 nm thick.

[0147] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 459.7mAh / g, the initial charge / discharge coulombic efficiency was 90.3%, the negative electrode piece expansion rate of the resulting full cell was 27.6%, the unit weight energy density was 395.8Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.9%.

[0148] Examples 1-15 Silicon suboxide particle powder (D50=5.0μm, SPAN=1.0) was taken and placed in a nitric acid solution with a concentration of approximately 20wt.%, heated to 30℃, and immersed with stirring for 2 hours for surface treatment to obtain silicon suboxide particles with an oxygen-rich shell layer.

[0149] The surface-treated silicon suboxide particles were placed in a graphite crucible, placed in a box furnace, and heated to 1000°C at 3°C / min with acetylene gas, kept at that temperature for 4 hours, and then naturally cooled to room temperature to complete the carbonization process. The heat-treated material was scattered, sieved, and demagnetized.

[0150] The specific surface area of ​​the silicon-based particles of Examples 1-15 is 2.1 m 2 / g and the tap density is 1.2 g / cm 3 The carbon content was 5.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 10 nm thick, and the outermost layer was covered with a carbon layer about 75 nm thick.

[0151] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 463.4 mAh / g, the initial charge / discharge coulombic efficiency was 90.4%, the negative electrode piece expansion rate of the resulting full cell was 26.7%, the unit weight energy density was 392.7 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 91.2%.

[0152] Comparison 1-1 500 g of silicon suboxide particle powder with a median diameter D50 of 5.0 μm and SPAN=1.0 was placed in a rotary furnace, heated to 1000°C, and filled with methane. The methane flow rate was 1 L / min. After maintaining the temperature constant for 60 minutes, the filling of methane was stopped and the temperature was lowered to room temperature to obtain the product, which was then demagnetized and sieved to obtain a silica particle composite negative electrode material.

[0153] The specific surface area of ​​the silicon-based particles in comparison 1-1 is 2.2 m 2 / g and the tap density is 1.2 g / cm 3The carbon content was 4.1 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the resulting material was 4.2 nm. The outer surface of the relatively coarse core particles was observed to be free of silicon carbide shell and to have a 65 nm carbon film layer.

[0154] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 459.8 mAh / g, the initial charge / discharge coulombic efficiency was 89.2%, the negative electrode piece expansion rate of the resulting full cell was 29.4%, the unit weight energy density was 393.0 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 85.6%.

[0155] Comparison 1-2 The median diameter D50 is 5.0 μm, SPAN=1.0, and the chemical formula is SiO X 500 g of silicon oxide particle powder (0.6≦X≦1.1) was placed in a rotary furnace, heated to 300° C., and filled with oxygen at an oxygen flow rate of 200 mL / min. After maintaining the temperature constant for 20 minutes, the filling with oxygen was stopped and the temperature was lowered to room temperature.

[0156] The product obtained above was placed in a rotary furnace, heated to 1100°C, filled with methane, the methane flow rate was 1 L / min, and kept at a constant temperature for 60 minutes, after which the filling with methane was stopped and the temperature was lowered to room temperature. The product was demagnetized and sieved to obtain a silicon-based particle negative electrode material.

[0157] The specific surface area of ​​the silicon-based particles in comparison 1-2 is 2.2 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.2 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.5 nm. The outer surface of the relatively coarse core particles was observed to have a silicon carbide shell layer of about 3 nm and a carbon film layer of 65 nm.

[0158] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 462.5 mAh / g, the initial charge / discharge coulombic efficiency was 88.3%, the negative electrode piece expansion rate of the resulting full cell was 29.8%, the unit weight energy density was 391.4 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 88.4%.

[0159] Comparison 1-3 Silicon suboxide raw material was processed with a jaw crusher, pulverized with an airflow pulverizer, and sieved to obtain silicon suboxide particle powder with a median diameter of 5 μm and a SPAN of 1.0. The silicon suboxide particle powder was taken and placed in 20 wt. % hydrogen peroxide water at a temperature of 30° C., and immersed with stirring for 2 hours to perform surface treatment.

[0160] 2 kg of the surface-treated silicon suboxide particles were taken and put into a VC mixer together with 120 g of petroleum asphalt, and mixed for 30 minutes at a linear velocity of 8 m / s at the maximum diameter of the stirring member to uniformly mix the two raw materials. Subsequent processing was carried out in the same manner as in Example 1-1, except that the end temperature of the heating was 700°C.

[0161] The specific surface area of ​​the silicon-based particles in comparison 1-3 is 2.0 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.1 wt.%. It was observed that the outer surface of the relatively coarse core particle was covered with a carbon layer about 60 nm thick. Because the carbonization temperature was low, carbon could not react with the oxygen-rich shell layer on the surface of the silicon suboxide particle, and the presence of a silicon carbide shell layer was not observed.

[0162] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 457.3 mAh / g, the initial charge / discharge coulombic efficiency was 88.5%, the expansion rate of the resulting negative electrode piece was 30.1%, the unit weight energy density was 390.6 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.1%.

[0163] Comparison 1-4 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.0) was taken, placed in moist air with a relative humidity of about 80%, heated to 1000° C., and held for 60 minutes to perform a surface treatment.

[0164] Subsequent processing was carried out in the same manner as in Example 1-9.

[0165] The specific surface area of ​​the silicon-based particles in comparison 1-4 is 2.1 m 2 / g and the tap density is 1.1 g / cm 3 The carbon content was 4.0 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 4.1 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 500 nm thick, and the outermost layer was covered with a carbon layer about 60 nm thick.

[0166] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 443.2mAh / g, the initial charge / discharge coulombic efficiency was 85.2%, the expansion rate of the resulting negative electrode piece was 29.5%, the unit weight energy density was 367.8Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 88.4%.

[0167] Example 2-1 Silicon suboxide particle powder (D50 = 5 μm, SPAN = 1.3) was taken, placed in air (25 °C) with a relative humidity of approximately 100%, heated to 600 °C and held for 60 minutes to perform surface treatment, resulting in silicon suboxide particles with an oxygen-rich shell layer.

[0168] 2 kg of the surface-treated silicon suboxide particles were taken and placed in a VC mixer together with 120 g of petroleum asphalt powder, and mixed for 30 minutes at a linear velocity of 8 m / s at the maximum diameter of the stirring member to uniformly mix the two raw materials.

[0169] The above mixture was placed in a graphite crucible, placed in a box furnace, and nitrogen gas protective gas was added, and the temperature was raised to 1000°C at 3°C / min, kept at that temperature for 4 hours, and then naturally cooled to room temperature to complete the heat treatment. In this step, the asphalt was carbonized under high temperature treatment in an oxygen-free atmosphere to obtain a conductive carbon layer, and also partially reacted with the oxygen-rich shell layer on the surface of the silicon suboxide particles to produce a silicon carbide shell layer. The above carbide was pulverized with a gear mill at a linear speed of about 5m / s, and the composite material obtained after heat treatment was crushed into fine powder.

[0170] In a drying room with a relative humidity of less than 30%, 100g of the powder obtained in the above step, 9g of metallic lithium ribbon, 2g of biphenyl were put into a sealable glass container, along with 200g of methyl butyl ether and a large stirring magnetic element. At this time, the container was filled with argon gas and sealed, and the container was placed on a magnetic stirrer to stir, with the rotation speed set to 200r / min. After 5 hours of constant temperature reaction at 70°C, the methyl butyl ether in the container was evaporated or filtered out, and then dried. The resulting powder was then placed in a tube furnace and heat-treated under an argon atmosphere, heated to 750°C at a heating rate of 10°C / min, and then held for 3 hours. After natural cooling, a lithium-intercalated oxygen-containing silicon-based compound powder was obtained. Finally, after sieving and demagnetization, a product that can finally be used as a negative electrode material was obtained.

[0171] The silicon-based particle diameter D50 of Example 2-1 measured using the above-mentioned equipment was 6.2 μm, SPAN=1.40, and specific surface area was 3.1 m 2 / g, and the carbon content was 3.6 wt.%. From the results of the X-ray diffraction pattern, by substituting into the Sherrer equation, it was possible to calculate that the size of the crystal grains corresponding to the Si(111) crystal plane in the material obtained in Example 2-1 was 5.0 nm. The Raman scattering spectrum indicated the presence of silicon carbide in the material. When the cross section of the sample was observed with a scanning electron microscope, it was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 50 nm thick, and the outermost layer was covered with a carbon layer about 30 nm thick.

[0172] Using the above water resistance test method, it was detected that the silicon-based particles obtained in Example 2-1 started to generate gas after immersion in water for 5 days.

[0173] Using the above pole piece manufacturing method, a silicon-based particle negative pole piece was obtained.

[0174] Using the above half-cell evaluation test method, the initial reversible lithium desorption specific capacity of the negative electrode half-cell obtained in Example 2-1 was 428.1 mAh / g, and the initial charge / discharge coulombic efficiency was 93.6%.

[0175] Using the above-mentioned whole battery evaluation test method, the negative electrode piece expansion rate of the whole battery obtained in Example 2-1 was 27.4%, the unit weight energy density was 414.2Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 92.3%.

[0176] Example 2-2 Silicon suboxide particle powder (D50=5 μm, SPAN=1.3) was taken and placed in 20 wt. % hydrogen peroxide solution, the temperature was kept at 50° C. and stirring was maintained for 4 hours, then it was cooled to room temperature, filtered and dried.

[0177] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0178] The silicon-based particles of Example 2-2 had a particle size D50 of 6.3 μm, a SPAN of 1.40, and a specific surface area of ​​3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 60 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0179] The resulting silicon-based particles started to generate gas after six days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half cell was 425.9 mAh / g, and the initial charge / discharge coulombic efficiency was 93.6%. The negative electrode piece expansion rate of the resulting full cell was 28.4%, the unit weight energy density was 413.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 89.2%.

[0180] Example 2-3 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.3) was taken and placed in nitric acid with a concentration of 20 wt. % at 60° C., and stirred for 4 hours, then cooled to room temperature, filtered, and dried.

[0181] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0182] The silicon-based particle diameter D50 of Example 2-3 is 6.3 μm, SPAN=1.4, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 70 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0183] The resulting silicon-based particles started to generate gas after 7 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half cell was 425.1 mAh / g, and the initial charge / discharge coulombic efficiency was 93.8%. The negative electrode piece expansion rate of the resulting full cell was 28.2%, the unit weight energy density was 413.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 89.5%.

[0184] Examples 2-4 Silicon suboxide particle powder (D50=5 μm, SPAN=1.3) was taken and placed in water, and the temperature was 80° C., and the mixture was immersed in water with stirring for 4 hours, and then cooled to room temperature, filtered, and dried.

[0185] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0186] The silicon-based particle diameter D50 of Example 2-4 is 6.3 μm, SPAN=1.40, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 40 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0187] The resulting silicon-based particles started to generate gas after 5 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half-cell was 425.4 mAh / g, and the initial charge / discharge coulombic efficiency was 93.7%. The negative electrode piece expansion rate of the resulting full cell was 27.9%, the unit weight energy density was 413.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 92.1%.

[0188] Examples 2-5 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.3) was taken and placed in dry air (water content about 500 ppm) with a flow rate of 200 sccm, surface treatment was performed, and the temperature was controlled to 600° C. and held for 60 minutes.

[0189] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0190] The silicon-based particle diameter D50 of Example 2-5 is 6.1 μm, SPAN=1.40, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 5 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0191] The silicon-based particles obtained started to generate gas after 4 days of immersion in water. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 426.7 mAh / g, and the initial charge / discharge coulombic efficiency was 93.5%. The negative electrode piece expansion rate of the obtained full cell was 28.7%, the unit weight energy density was 413.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 89.3%.

[0192] Examples 2-6 Silicon suboxide particle powder (D50=5.0 μm, SPAN=1.3) was taken and placed in a mixture of dry air and oxygen at 500° C., and held for 60 minutes with an air flow rate of 100 sccm and an oxygen flow rate of 100 sccm, for surface treatment.

[0193] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0194] The silicon-based particle diameter D50 of Example 2-6 is 6.1 μm, SPAN=1.40, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 5 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0195] The silicon-based particles obtained started to generate gas after 4 days of immersion in water. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 425.8 mAh / g, and the initial charge / discharge coulombic efficiency was 93.6%. The negative electrode piece expansion rate of the obtained full cell was 28.6%, the unit weight energy density was 413 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 89.2%.

[0196] Examples 2-7 Silicon suboxide particle powder (D50=5 μm, SPAN=1.3) was taken and placed in oxygen with a flow rate of 200 sccm for surface treatment, the temperature was adjusted to 400° C., and the powder was held for 60 minutes.

[0197] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0198] The silicon-based particle diameter D50 of Example 2-7 is 6.1 μm, SPAN=1.40, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.6 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 5 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0199] The silicon-based particles obtained started to generate gas after 4 days of immersion in water. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 426.2 mAh / g, and the initial charge / discharge coulombic efficiency was 93.5%. The negative electrode piece expansion rate of the obtained full cell was 28.5%, the unit weight energy density was 413.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 88.9%.

[0200] Examples 2-8 Silicon suboxide particle powder (D50=5 μm, SPAN=1.8) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment at a temperature of 600° C. for 60 minutes.

[0201] Subsequent treatment was carried out in the same manner as in Example 2-1.

[0202] The silicon-based particle diameter D50 of Example 2-8 is 6 μm, SPAN=1.90, and the specific surface area is 3.1 m 2 / g and the carbon content was 3.8 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 30 nm thick, and the outermost layer was coated with a carbon layer about 30 nm thick.

[0203] The resulting silicon-based particles started to generate gas after 5 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half cell was 426.5 mAh / g, and the initial charge / discharge coulombic efficiency was 93.8%. The negative electrode piece expansion rate of the resulting full cell was 27.6%, the unit weight energy density was 414 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90%.

[0204] Examples 2-9 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment at a temperature of 600° C. for 60 minutes.

[0205] Using the same coating method and heat treatment as in Example 2-1, silicon suboxide particles having a silicon carbide layer and a conductive carbon layer were obtained.

[0206] Next, the lithium metal lithium insertion process is carried out using the solid-phase lithium insertion method. Specifically, 500g of the above particles are taken and mixed with 40g of lithium hydride powder, the mixed powder is placed in a tube furnace and heat-treated under an argon atmosphere, the temperature is increased to 650°C at a heating rate of 10°C / min and held for 6 hours, the material is taken out of the tube furnace after natural cooling, and finally, after sieving and demagnetization, a product that can be used as a negative electrode material is obtained.

[0207] The silicon-based particle diameter D50 of Example 2-9 is 6.3 μm, SPAN=1.20, and the specific surface area is 2.3 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 30 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0208] The resulting silicon-based particles started to generate gas after 9 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half-cell was 429.6 mAh / g, and the initial charge / discharge coulombic efficiency was 93.8%. The negative electrode piece expansion rate of the resulting full cell was 27.3%, the unit weight energy density was 415.3 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 92.7%.

[0209] Example 2-10 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment at a temperature of 600° C. for 60 minutes.

[0210] The same coating method and heat treatment as in Example 2-1 were used, except that the carbonization temperature was kept at 900°C for 6 hours to obtain silicon suboxide particle powder having a silicon carbide layer and a conductive carbon layer.

[0211] Lithium metal lithium insertion treatment was carried out using the same solid phase lithium insertion method as in Example 2-9.

[0212] The silicon-based particle diameter D50 of Example 2-10 is 6.3 μm, SPAN=1.20, and the specific surface area is 2.3 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 20 nm thick, and the outermost layer was covered with a carbon layer about 50 nm thick.

[0213] The resulting silicon-based particles started to generate gas after six days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half-cell was 430.4 mAh / g, and the initial charge / discharge coulombic efficiency was 93.6%. The negative electrode piece expansion rate of the resulting full cell was 27.9%, the unit weight energy density was 414.8 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.9%.

[0214] Example 2-11 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment at a temperature of 600° C. for 60 minutes.

[0215] The same coating method and heat treatment as in Example 2-1 were used, except that the carbonization temperature was 850° C. and the temperature was maintained for 6 hours.

[0216] Lithium metal lithium insertion treatment was carried out using the same solid phase lithium insertion method as in Example 2-9.

[0217] The silicon-based particle diameter D50 of Example 2-11 is 6.3 μm, SPAN=1.20, and the specific surface area is 2.3 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 15 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0218] The silicon-based particles obtained started to generate gas after 5 days of immersion in water. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 432.3 mAh / g, and the initial charge / discharge coulombic efficiency was 93.4%. The negative electrode piece expansion rate of the obtained full cell was 28%, the unit weight energy density was 415.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 90.5%.

[0219] Example 2-12 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment at a temperature of 600° C. for 60 minutes.

[0220] The same coating method and heat treatment as in Example 2-1 were used, except that the carbonization temperature was kept at 1100°C for 2 hours to obtain silicon suboxide particle powder having a silicon carbide layer and a conductive carbon layer.

[0221] Lithium metal lithium insertion treatment was carried out using the same solid phase lithium insertion method as in Example 2-9.

[0222] The silicon-based particle diameter D50 of Example 2-12 is 6.3 μm, SPAN=1.20, and the specific surface area is 2.3 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 50 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0223] The silicon-based particles obtained started to generate gas after 9 days of immersion in water. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 427.4 mAh / g, and the initial charge / discharge coulombic efficiency was 93.8%. The negative electrode piece expansion rate obtained in Example 2-12 was 27.1%, the unit weight energy density was 414.3 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 88.5%.

[0224] Example 2-13 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in moist air (25° C.) with a relative humidity of 100% to perform surface treatment, the temperature was approximated to 600° C., and the time was approximated to 60 minutes.

[0225] The same coating method and heat treatment as in Example 2-1 were used, except that the carbonization temperature was 1100° C. and the temperature was maintained for 6 hours.

[0226] Lithium metal lithium insertion treatment was carried out using the same solid phase lithium insertion method as in Example 2-9.

[0227] The silicon-based particle diameter D50 of Example 2-13 is 6.3 μm, SPAN=1.20, and the specific surface area is 2.3 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 6.0 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 110 nm thick, and the outermost layer was coated with a carbon layer about 35 nm thick.

[0228] The resulting silicon-based particles started to generate gas after 10 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half-cell was 424.4 mAh / g, and the initial charge / discharge coulombic efficiency was 93.7%. The negative electrode piece expansion rate of the resulting full cell was 27.0%, the unit weight energy density was 413 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 89.3%.

[0229] Example 2-14 Silicon suboxide particle powder (D50=5 μm, SPAN=1) was taken and placed in humid air (25° C.) with a relative humidity of 100% to perform surface treatment, the temperature was approximated to 600° C., and the time was approximated to 60 minutes.

[0230] The surface-treated silicon suboxide particles were taken and placed in a rotary furnace using a CVD method, and methane gas was introduced, the methane flow rate was 1 L / min, the set temperature was 1000°C, and the heat treatment was completed by keeping the temperature for 2 hours. In this step, the methane was deposited and carbonized under high temperature treatment in an oxygen-free atmosphere, and partially reacted with the oxygen-rich shell layer on the surface of the silicon suboxide particles to generate a silicon carbide shell layer. The carbide was crushed with a gear mill and crushed into fine powder.

[0231] Lithium metal lithium insertion treatment was carried out using the same solid phase lithium insertion method as in Example 2-9.

[0232] The silicon-based particle diameter D50 of Example 2-14 is 5.6 μm, SPAN=1.30, and the specific surface area is 5.0 m 2 / g and the carbon content was 3.5 wt.%. The grain size corresponding to the Si(111) crystallographic plane in the obtained material was 5 nm. Raman scattering spectrum indicated the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was coated with a dense silicon carbide shell about 10 nm thick, and the outermost layer was coated with a carbon layer about 50 nm thick.

[0233] The resulting silicon-based particles started to generate gas after 5 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half cell was 424.5 mAh / g, and the initial charge / discharge coulombic efficiency was 93.8%. The negative electrode piece expansion rate of the resulting full cell was 28.1%, the unit weight energy density was 413.2 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 88.6%.

[0234] Comparison 2-1 Untreated silicon suboxide particle powder (D50=5 μm, SPAN=1.30) was taken, placed in a rotary furnace, heated to 1000°C, and filled with methane. The methane flow rate was 1 L / min. After maintaining the temperature constant for 60 minutes, the methane filling was stopped and the temperature was lowered to room temperature. The product was obtained, demagnetized, and sieved to obtain silicon-based particles with a conductive carbon layer.

[0235] Silicon-based particle diameter D50 is 5.6μm, SPAN=1.50, specific surface area is 5.0m 2 / g and the carbon content was 3.5 wt.%. The size of the crystal grains corresponding to the Si(111) crystal plane in the material obtained in Comparative Example 2-1 was 4 nm. It was observed that there was no silicon carbide shell on the outer surface of the relatively coarse core particle, and the outermost layer was covered with a carbon layer 40 nm thick.

[0236] Since the silicon suboxide particles of Comparative Example 2-1 were not subjected to lithium insertion treatment, there was no need to measure the water resistance.

[0237] The initial reversible lithium desorption capacity of the resulting negative electrode half cell was 465 mAh / g, the initial charge / discharge coulombic efficiency was 88.4%, the negative electrode piece expansion rate of the resulting full cell was 31.4%, the unit weight energy density was 412 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 84.1%.

[0238] Comparison 2-2 Silicon suboxide particles (D50=5 μm, SPAN=1) were taken and not surface-treated. Using the same coating method and heat treatment as in Example 2-1, silicon suboxide particles having only a conductive carbon layer were obtained.

[0239] The silicon suboxide particles were subjected to a liquid phase lithium intercalation treatment using the same method as in Example 2-1. Finally, the particles were sieved and demagnetized to obtain a product that can be used as a negative electrode material.

[0240] The silicon-based particle diameter D50 of comparative example 2-2 is 6.1 μm, SPAN=1.4, and the specific surface area is 3 m 2 / g and the carbon content was 3.8 wt.%. X-ray diffraction pattern showed that the silicon grain size of the material was 5 nm. It was observed that the outer surface of the relatively coarse core particles was free of silicon carbide shell and the carbon layer was about 40 nm thick.

[0241] The silicon-based particles obtained started to generate gas after immersion in water for 3 days. The initial reversible lithium desorption specific capacity of the obtained negative electrode half cell was 424.3 mAh / g, and the initial charge / discharge coulombic efficiency was 93.2%. The negative electrode piece expansion rate of the obtained full cell was 29.6%, the unit weight energy density was 411.5 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 87.3%.

[0242] Comparison 2-3 Silicon suboxide particle powder (D50=5 μm, SPAN=1.3) was taken and placed in moist air (25° C.) with a relative humidity of 100%, the temperature was kept at 1150° C. for 30 minutes, and then cooled to room temperature.

[0243] Subsequent treatment was carried out in the same manner as in Example 2-1, except that in Comparative Example 2-3, the amount of petroleum asphalt relative to the silicon suboxide particles was 10 WT.%.

[0244] The silicon-based particle diameter D50 of comparative example 2-3 is 6.3 μm, SPAN=1.4, and the specific surface area is 2.5 m 2 / g, and the carbon content was 3.8 wt.%. The size of the crystal grains corresponding to the Si(111) crystal plane in the obtained material was 5 nm, and it was also found that the Si-O peak had an enhancement phenomenon for each example. Raman scattering spectrum showed the presence of silicon carbide in the material. It was observed that the outer surface of the relatively coarse core particle was covered with a dense silicon carbide shell about 300 nm thick, and the outermost layer was covered with a carbon layer about 40 nm thick.

[0245] The resulting silicon-based particles started to generate gas after 12 days of immersion in water. The initial reversible lithium desorption specific capacity of the resulting negative electrode half-cell was 403.4 mAh / g, and the initial charge / discharge coulombic efficiency was 93.1%. The negative electrode piece expansion rate of the resulting full cell was 29.6%, the unit weight energy density was 402.6 Wh / kg, and the capacity retention rate after 200 charge / discharge cycles was 83.3%.

[0246] It is clear that the above examples are only for clarifying the examples described herein, and do not limit the embodiments. Those skilled in the art can make other different types of changes and variations based on the above description. It is not necessary and cannot be exhaustively described here. Any obvious changes or variations caused thereby are still within the protection scope of the present invention.

Claims

1. A method for producing silicon-based particles having a core-shell structure, comprising the steps of: A step of surface treating SiOx particles (0.5≦x≦1.5); carbon-coating the surface-treated SiOx particles to form a silicon carbide layer and a conductive carbon layer; sieving and demagnetizing the carbon coated material; The surface treatment includes a gas phase treatment or a liquid phase treatment, The gas phase treatment includes heat treating the SiOx particles in an oxygen-containing atmosphere, the heating time is 10 to 600 minutes, and the heat treatment temperature is 300 to 1100° C.; The oxygen-containing atmosphere may include one or more of oxygen, water vapor, and air; The liquid phase treatment includes immersing the SiOx particles in water, an aqueous hydrogen peroxide solution, or a nitric acid solution; The mass concentration of the hydrogen peroxide solution or the nitric acid solution is ≦30 wt. %, the liquid phase treatment temperature is 0 to 100° C., and the time is 10 to 600 minutes; The method for producing said silicon carbide layer is characterized in that the thickness of said silicon carbide layer is 8 to 200 nm.

2. The method of claim 1 further comprising subjecting the carbon coated material to a lithium intercalation treatment.

3. 3. The method according to claim 2, wherein the lithium insertion process is carried out by using at least one of electrochemical method, liquid phase lithium insertion method, thermal lithium insertion method, high temperature kneading method, and high energy mechanical method.

4. The step of coating the surface-treated SiOx oxide particles with carbon comprises: By chemical vapor deposition; or 2. The method according to claim 1, further comprising: first mixing the surface-treated SiOx particles with a carbon precursor; and then subjecting the mixture to a heat-treatment carbonization process in a non-oxidizing atmosphere.

5. The temperature of the chemical vapor deposition method or the heat treatment carbonization method is 800 to 1200° C., and the temperature is kept constant at 0 The method according to claim 4, characterized in that the mixture is kept for 5 to 24 hours.

Citation Information

Patent Citations

  • Lithium ion battery, negative electrode, negative electrode conductive paste and preparation method of negative electrode conductive paste

    CN108598404A

  • Anode active material and preparation method and application thereof

    CN111180693A

  • Silicon oxide / carbon composite anode material and preparation method thereof and lithium ion battery

    CN112018334A

  • Negative electrode material for nonaqueous secondary battery and method for producing the material, and lithium ion secondary battery

    JP2011222151A

  • Negative electrode active material for lithium ion secondary battery, and lithium ion secondary battery comprising the negative electrode active material

    JP2012178269A