Monodisperse spherical silicon dioxide with adjustable particle size and preparation method thereof

By adjusting the concentration of CTAB aqueous solution under diethanolamine catalysis and controlling the particle size of spherical silica microspheres, the problem of difficult particle size regulation and poor operability in the prior art is solved, and particle size uniformity and dispersion are achieved. Improve and simplify the preparation process.

CN118908232APending Publication Date: 2024-11-08WUHAN UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411017573.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, when preparing spherical silica microspheres, operability and economicality are not conducive to widespread promotion and application, and it is difficult to effectively control the particle size and improve the dispersion.

Method used

The concentration of CTAB aqueous solution and ethyl orthosilicate under diethanolamine catalyzed by stirring, centrifugation, washing, drying and calcining is used to control the particle size of silica microspheres to achieve accurate control of the particle size. .

Benefits of technology

The particle size of silica microspheres was successfully controlled between 0.8μm-2μm, ensuring particle size uniformity, good spherical structure, smooth appearance and dispersion, simplifying the operation process and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004966200440000011
    Figure HDA0004966200440000011
  • Figure HDA0004966200440000012
    Figure HDA0004966200440000012
  • Figure HDA0004966200440000021
    Figure HDA0004966200440000021
Patent Text Reader

Abstract

The invention provides a preparation method of monodisperse spherical silicon dioxide microspheres with adjustable particle size, which comprises the following steps: by taking tetraethoxysilane (TEOS) as a silicon source, diethanol amine (DEA) as a catalyst, cetyltrimethylammonium bromide (CTAB) as a surfactant and an aqueous solution of ethanol as a solvent, firstly dissolving CTAB in deionized water; after the TEOS is completely dissolved, dropwise adding a certain volume of TEOS into a CTAB solution, uniformly stirring, adding a certain volume of DEA ethanol water solution, uniformly stirring, continuously stirring at room temperature to obtain a dispersion solution of a reaction product, centrifuging, washing and drying the reaction product to obtain a precursor product, and drying the precursor product to obtain the TEOS / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA / DEA composite material. The precursor product is placed in a muffle furnace to be subjected to calcination treatment, and an obtained calcined product is spherical silicon dioxide. The spherical silicon dioxide microspheres obtained by the invention have the characteristics of monodispersity and adjustable particle size, the particle size of the prepared silicon dioxide is in a range of 0.8-2 microns, and the method has the advantages of simple preparation method, safety, environmental protection and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing monodisperse spherical silicon dioxide microspheres with adjustable particle size. Background Art

[0002] Micron-sized silica has the advantages of large specific surface area, strong adsorption, non-toxicity, and good biocompatibility, so it is widely used in catalysis, medicine, coatings and other fields.

[0003] At present, the main methods for preparing spherical silica are: sol-gel method, microemulsion method, template method and vapor phase precipitation method. However, due to operability and economy, they are not conducive to widespread promotion and application.

[0004] The publication number is CN102491353A, which invented a method for preparing transparent microporous silica microspheres. Water, octylamine and ethyl orthosilicate are used as raw materials. After mixing water and octylamine, ethyl butyrate is added to react. After the reaction, the reaction liquid is filtered, the obtained particles are washed and dried, and the dried particles are heated to 550℃-950℃, kept warm for 6 hours, and transparent microporous silica microspheres are obtained after natural cooling. This invention can synthesize transparent microporous silica microspheres using only water, octylamine and ethyl orthosilicate, without using alkali and alcohol, with less raw materials, easy to obtain silicon source, cheap price, and reduced production cost. However, the calcination and insulation time are too long, which increases the time cost of the experiment.

[0005] The publication number is CN115477307A. The prepared silica seed dispersion liquid is centrifuged, washed, frozen, and dried to obtain silica powder, a certain amount of ethanol is added thereto to obtain a silica dispersion liquid, a certain amount of ammonia solution is added to the dispersion liquid after ultrasonication to form a uniform solution, and then ethyl orthosilicate is slowly and uniformly dropped into the dispersion liquid to continue the reaction for 3 hours to form micron-sized silica microspheres. The reaction is fast and the cost is low, and silica microspheres with uniform particle size and large size can be obtained, but the lack of an initiator solution makes the experimental reaction time longer.

[0006] The publication number is CN106009346A, which invented a method for preparing monodisperse silica microspheres. First, a seed suspension, an ethyl orthosilicate solution, and an initiator solution are prepared for use. Then, the ethyl orthosilicate solution and the initiator solution are added to the seed suspension at the same time, and the addition speeds are controlled respectively. After the reaction is completed, the silica composite microspheres are allowed to stand, and centrifuged to obtain the silica composite microspheres. Finally, the impurities are removed by calcination in a muffle furnace to obtain monodisperse silica microspheres. The silica microspheres that can be prepared by this method have highly uniform particle size, high chemical stability, good dispersibility, and controllable particle size. However, the preparation of a silica seed dispersion separately increases the difficulty of the experiment. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing monodisperse spherical silica microspheres with adjustable particle size. By changing the experimental conditions, the purpose of adjusting the particle size of the spherical silica microspheres can be achieved, so that the particle size is controlled between 0.8 μm and 2 μm. At the same time, the obtained silica microspheres are uniform in size, have a good spherical structure, a smooth appearance and good dispersibility.

[0008] The present invention is to obtain monodisperse spherical silica microspheres of different particle sizes by mixing CTAB aqueous solutions of different concentrations with a silicon source under stirring at normal temperature and pressure, and centrifuging, washing, drying and calcining under the catalysis of diethanolamine. This preparation method has the characteristics of simple operation, uniform size of spherical silica microspheres and smooth appearance, and more importantly, the purpose of controlling the size of spherical silica microspheres can be achieved by simple regulation (controlling the concentration of CTAB aqueous solution).

[0009] Specifically, a method for preparing monodisperse spherical silica microspheres with adjustable particle size is characterized by:

[0010] (1) Using tetraethyl orthosilicate as a silicon source, diethanolamine as a catalyst, hexadecyltrimethylammonium bromide as a surfactant, and water and ethanol as solvents; preparing CTAB into aqueous solutions of different mass concentrations, preparing tetraethyl orthosilicate into an ethanol solution of tetraethyl orthosilicate, and preparing diethanolamine into an aqueous solution of diethanolamine;

[0011] (2) preparing aqueous solutions of CTAB with different mass concentrations, heating them to 30° C. in a water bath, adding an ethanol solution of ethyl orthosilicate to the above solution, stirring and reacting for a period of time, then dropping an aqueous solution of diethanolamine under stirring conditions, and stopping stirring to allow precipitation to occur;

[0012] (3) washing the obtained precipitate with ethanol and water alternately, drying it, and then calcining it at 450° C.-650° C. to obtain monodisperse spherical silica microspheres of different particle sizes;

[0013] (4) The particle size of monodisperse spherical silica microspheres changes with the mass concentration of CTAB aqueous solution.

[0014] Preferably, the mass concentration of the CTAB aqueous solution is controlled to be 2 mg / mol-14 mg / mol, and the particle size range of the prepared spherical silica microspheres is 0.8 μm-2 μm.

[0015] Preferably, the concentration of the ethanol solution of tetraethyl orthosilicate is 0.1 mol / L.

[0016] Preferably, the stirring rate is 300 rpm-500 rpm, and the stirring time is 30 min-120 min.

[0017] Preferably, the concentration of the aqueous solution of diethanolamine is 0.1 mol / L.

[0018] Preferably, the drying process is carried out in a vacuum drying oven at 60° C.-80° C., and the drying time is 4 h-8 h.

[0019] Preferably, the calcination is carried out in a muffle furnace at 500° C.-600° C. for 4 h-8 h.

[0020] According to the present invention, silica microspheres of various particle sizes can be synthesized. Silica microspheres of different particle sizes can be widely used in multiple industries and fields, and can also be used as material parts of catalysts, catalyst carriers, coatings, cosmetics, optoelectronic materials, semiconductors, etc.

[0021] The method of the present invention uses diethanolamine to prepare an alkaline solution, adjusts the solution environment to catalyze the hydrolysis reaction of tetraethyl orthosilicate, and then changes the amount of a surfactant (CTAB) in the reaction system to achieve the purpose of accurately controlling the particle size of the silica microspheres. The operation is convenient, the equipment is simple, and the prepared spherical silica has good dispersibility, uniform size, smooth appearance, high yield, and no adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 SEM image of spherical nano-silicon dioxide prepared in Example 1

[0023] Figure 2 SEM image of spherical nano-silicon dioxide prepared in Example 2

[0024] Figure 3 SEM image of spherical nano-silicon dioxide prepared in Example 3

[0025] Figure 4 SEM image of spherical nano-silicon dioxide prepared in Example 4

[0026] Figure 5 SEM image of spherical nano-silicon dioxide prepared in Comparative Example 5

[0027] Figure 6 The particle size comparison diagram of spherical silicon dioxide prepared in Examples 1-4 and Comparative Example DETAILED DESCRIPTION

[0028] In order to better understand the above technical solution, the technical solution of the present application is described in detail through specific embodiments below. It should be understood that the embodiments of the present application and the specific features in the embodiments are detailed descriptions of the technical solution of the present application, rather than limitations on the technical solution of the present application. In the absence of conflict, the embodiments of the present application and the technical features in the embodiments can be combined with each other. It should be understood that the term "and / or" used herein includes any and all combinations of one or more of the listed associated items.

[0029] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0030] In view of the defects in existing silicon dioxide preparation methods and technologies, silicon dioxide is an oxide material with great application potential and excellent physical and chemical properties, such as stable chemical properties, non-toxicity and environmental friendliness. The present invention uses tetraethyl orthosilicate as a silicon source, hexadecyltrimethylammonium bromide as a surfactant, and diethanolamine as a catalyst to prepare a monodisperse spherical silicon dioxide microsphere with adjustable particle size. The method has the characteristics of simple operation and green environmental protection.

[0031] The main idea of ​​the embodiment of the present invention is: a method for preparing monodisperse spherical silica microspheres with adjustable particle size, comprising the following steps:

[0032] Dissolve hexadecyltrimethylammonium bromide in deionized water and stir to obtain solution I;

[0033] Dissolve ethyl orthosilicate in anhydrous ethanol and stir to obtain solution II;

[0034] Add solution II to solution I and stir evenly to obtain solution III;

[0035] DEA was dissolved in deionized water, and then the stirred solution was added dropwise into solution III, and then stirred and allowed to stand to obtain a mixed solution;

[0036] The obtained mixed solution is centrifuged, washed and dried in sequence to obtain a precursor product of silica microspheres.

[0037] The obtained silica microsphere precursor product is placed in a muffle furnace for programmed temperature calcination treatment, and the obtained calcination product is monodisperse spherical silica microspheres.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the embodiments of the present invention can be purchased from the market or prepared by existing methods. The preparation method is described in detail below.

[0039] Example 1

[0040] Dissolve 0.08g CTAB in a conical flask filled with 15mL distilled water, transfer to an oil bath, stir and heat to 30°C. Add 15mL 0.1mol / L LTEOS ethanol solution to the conical flask and stir evenly, then slowly drop 2mL 0.1 mol / L DEA solution into the conical flask and stir for 30min. Stop stirring when transparent colloidal particles are generated in the solution and let it stand for 10h.

[0041] The obtained silica microspheres were centrifuged, washed alternately with distilled water and ethanol three times, and finally dried in a vacuum drying oven at 60°C for 6 hours. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min and calcined for 2 hours. The obtained calcined product was monodisperse spherical silica microspheres.

[0042] Example 2

[0043] Dissolve 0.04g CTAB in a conical flask filled with 15mL distilled water, transfer to an oil bath, stir and heat to 30°C. Add 15mL 0.1mol / L TEOS ethanol solution to the conical flask and stir evenly, then slowly drop 2mL 0.1 mol / L DEA solution into the conical flask and stir for 30min. Stop stirring when transparent colloidal particles are generated in the solution and let it stand for 10h.

[0044] The obtained silica microspheres were centrifuged, washed alternately with distilled water and ethanol three times, and finally dried in a vacuum drying oven at 60°C for 6 hours. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min and calcined for 2 hours. The obtained calcined product was monodisperse spherical silica microspheres.

[0045] Example 3

[0046] Dissolve 0.10g CTAB in a conical flask filled with 15mL distilled water, transfer to an oil bath, stir and heat to 30°C. Add 15mL 0.1mol / LTEOS ethanol solution to the conical flask and stir evenly, then slowly drop 2mL 0.1 mol / L DEA solution into the conical flask and stir for 30min. Stop stirring when transparent colloidal particles are generated in the solution and let it stand for 10h.

[0047] The obtained silica microspheres were centrifuged, washed alternately with distilled water and ethanol three times, and finally dried in a vacuum drying oven at 60°C for 6 hours. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min and calcined for 2 hours. The obtained calcined product was monodisperse spherical silica microspheres.

[0048] Example 4

[0049] Dissolve 0.15g CTAB in a conical flask filled with 15mL distilled water, transfer to an oil bath, stir and heat to 30°C. Add 15mL 0.1mol / LTEOS ethanol solution to the conical flask and stir evenly, then slowly drop 2mL 0.1 mol / L DEA solution into the conical flask and stir for 30min. Stop stirring when transparent colloidal particles are generated in the solution and let it stand for 10h.

[0050] The obtained silica microspheres were centrifuged, washed alternately with distilled water and ethanol three times, and finally dried in a vacuum drying oven at 60°C for 6 hours. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min and calcined for 2 hours. The obtained calcined product was monodisperse spherical silica microspheres.

[0051] Comparative Example

[0052] Dissolve 0.20g CTAB in a conical flask filled with 15mL distilled water, transfer to an oil bath, stir and heat to 30°C. Add 15mL 0.1mol / LTEOS ethanol solution to the conical flask and stir evenly, then slowly drop 2mL 0.1 mol / L DEA solution into the conical flask and stir for 30min. Stop stirring when transparent colloidal particles are generated in the solution and let it stand for 10h.

[0053] The obtained silica microspheres were centrifuged, washed alternately with distilled water and ethanol three times, and finally dried in a vacuum drying oven at 60°C for 6 hours. The dried product was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min and calcined for 2 hours. The obtained calcined product was monodisperse spherical silica microspheres.

[0054] In summary, the present invention adopts a water bath heating method to synthesize micron-sized monodisperse spherical silica, the synthesis steps are simple and the particle size of the target product can be accurately controlled.

[0055] Obviously, the above embodiments of the present invention are merely examples for clearly explaining the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing monodisperse spherical silica microspheres with adjustable particle size, characterized in that: The method for preparing monodisperse spherical silica microspheres with adjustable particle size comprises the following steps: (1) Add a certain amount of CTAB into deionized water, stir at room temperature for 5-25 minutes, and stir evenly to obtain dispersion I; (2) Add a certain amount of ethyl orthosilicate to anhydrous ethanol, stir at room temperature for 10-30 minutes, and stir evenly to obtain solution II; (3) adding solution II to solution I while stirring, and stirring under heating in a water bath until uniform solution III is obtained; (4) adding the aqueous solution of diethanolamine dropwise into solution III under stirring, stirring at room temperature for 15-150 minutes, and stirring evenly to obtain a mixed solution; (5) subjecting the mixed solution to centrifugation, washing and drying treatments in sequence, wherein the washing process is washing with deionized water and anhydrous ethanol alternately, and then drying the centrifuged product, and the obtained dry product is a silica microsphere precursor; (6) The dried silica microsphere precursor product is placed in a muffle furnace for calcination, and the calcined product is silica microspheres.

2. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The mass concentration of the CTAB aqueous solution is 2 mg / mol to 14 mg / mol.

3. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The concentration of the ethyl orthosilicate ethanol solution is 0.02 mol / L to 0.2 mol / L.

4. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The water bath heating temperature is 20°C-50°C.

5. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The stirring rate is 300rpm-500rpm, and the stirring time is 30min-120min.

6. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The concentration of the diethanolamine aqueous solution is 0.05 mol / L to 0.15 mol / L.

7. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The washing process is washing with deionized water and anhydrous ethanol alternately.

8. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The drying treatment is carried out in a vacuum drying oven at 60°C-80°C, and the drying time is 4h-8h.

9. The method for preparing monodisperse spherical silica microspheres with adjustable particle size according to claim 1, characterized in that: The calcination treatment is carried out in a muffle furnace at 450° C.-650° C., with a heating rate of 1-4° C. / min and a calcination time of 4h-8h.

Citation Information

Cited By

  • Preparation method of monodisperse submicron spherical silicon dioxide

    CN120903513A

  • Preparation method of high-monodisperse micron-sized silicon dioxide microspheres, microspheres and chip

    CN122144747A

  • Preparation method of high monodisperse micron-sized silica microspheres, microspheres and chip

    CN122144747B