Resin composition and injection molded product using same
A resin composition combining block polypropylene, ethylene-propylene rubber, and additives improves the durability and weather resistance of thin-walled hinges in integrated resin molded bodies, addressing issues of damage and UV degradation.
Patent Information
- Application Number
- JP2024049203
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Resin molded bodies with integrated lids, such as wiring boxes and closures, face issues with thin-walled hinge sections that are prone to damage from repeated opening and closing and UV degradation, leading to poor weather resistance and durability.
A resin composition comprising block polypropylene, ethylene-propylene rubber, a hindered amine light stabilizer, and carbon black in specific ratios, enhancing the durability and weather resistance of thin-walled hinge portions.
The composition provides excellent repeated bending durability and weather resistance, preventing damage to thin-walled hinges even under UV exposure, ensuring long-term functionality.
Smart Images

Figure 0007575631000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and an injection molded article using the same. [Background technology]
[0002] Various resin molded articles are used in automobiles, electric and electronic devices, etc. For example, resin molded articles for vehicles such as automobiles include resin molded articles such as bumpers, skid garnishes, dashboards, body panels, wiring connectors, and wiring boxes that house electrical components. In addition, resin molded articles called closures (junction boxes) for connecting and branching optical or metal communication cables are also included. As a resin composition for forming a resin molded body, various resin compositions are already known, and resin compositions that satisfy the characteristics suitable for the intended use have also been developed. For example, in Patent Document 1, a resin composition for automobile exteriors that has color stability and weather resistance is proposed in claim 1, which contains polypropylene, rubber, talc, a colorant, an ultraviolet absorber, and a hindered amine light stabilizer at a specific content, although the specific composition is not disclosed in the examples. In addition, Patent Document 2 proposes a dynamically vulcanized alloy composition (DVA) having an improved stiffness / impact balance in claim 1, which contains a cured elastomer, a thermoplastic polyolefin resin, and a solid granular component selected from the group consisting of a filler, an additive, and a mixture thereof. However, Patent Document 2 only specifically discloses a composition containing an ethylene propylene elastomer, a random polypropylene (PPRC), and glass fiber. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2008-537568 [Patent Document 2] Japanese Patent Application Publication No. 3-54237 Summary of the Invention [Problem to be solved by the invention]
[0004] Among the resin molded bodies, wiring boxes, closures, etc. are formed as box-shaped molded bodies having openable and closable cover members, flap members, etc., or resin molded bodies having cover-shaped molded bodies having openable and closable cover members, flap members, etc. Some of these molded bodies are made of separate bodies, such as a body and a cover member or flap member that covers the body, but when liquid-tightness for waterproofing, etc., or airtightness for stain resistance, etc., is required, a body and a cover body integrated together are preferably used. An integrally molded body in which the body and the cover body are integrated is usually provided with a connection mechanism that connects and links the body and the cover body. As such a connection mechanism, various mechanisms such as hinges are known, but an integrally molded body in which the body and the cover body are integrally formed from the same resin composition is advantageous in terms of cost, productivity, etc. The hinge portion provided as a connection mechanism in this integrally molded body is usually formed thinner than the thickness of the body or the cover body in terms of ease of opening and closing. In such an integrally molded body, in actual use, it is necessary to open the lid when manufacturing and inspecting the internal mechanism. However, the hinge portion formed in a thin wall (also called a thin-walled hinge portion) is thin, and is therefore prone to damage such as cracks and fissures due to repeated opening and closing of the lid, and is poor in opening and closing durability (repeated bending durability). Moreover, resin molded bodies such as closures installed outdoors (aerial installation) are exposed to ultraviolet rays, and therefore the resin composition, particularly the resin composition forming the thin-walled hinge portion, is prone to deterioration. As a result, when the lid is opened and closed after installation (after exposure to ultraviolet rays), particularly after installation, the thin-walled hinge portion is prone to damage and is poor in weather resistance. However, Patent Documents 1 and 2 do not consider the above viewpoint.
[0005] An object of the present invention is to provide an injection-molded article that exhibits excellent durability against repeated bending and weather resistance, and a resin composition capable of forming the injection-molded article. [Means for solving the problem]
[0006] The present inventors have thoroughly investigated materials for forming a resin molded body having a thin-walled hinge portion, and have found that by selecting block polypropylene from among polypropylenes as a resin component, using this in combination with a specific amount of ethylene-propylene rubber, and further combining a hindered amine-based light stabilizer and carbon black in a specific mass ratio, when a molded body is formed, the repeated bending durability of the thin-walled hinge portion can be improved, excellent weather resistance can be imparted not only to the resin molded body but also to the thin-walled hinge portion, and damage caused by opening and closing operations at the thin-walled hinge portion can be suppressed even after exposure to ultraviolet light. Based on this finding, the present inventors have conducted further research and have come up with the present invention.
[0007] That is, the object of the present invention has been achieved by the following means. <1> A resin composition comprising 100 parts by mass of block polypropylene, 6 to 10 parts by mass of ethylene-propylene rubber, 0.05 to 2.0 parts by mass of a hindered amine light stabilizer, and 1.5 to 3.0 parts by mass of carbon black. <2> The ethylene-propylene rubber contains an ethylene-propylene rubber having an ethylene content of 60% or more. <1> The resin composition according to claim 1. <3> The carbon black comprises furnace black. <1> or <2> The resin composition described above. <4> The carbon black has a specific surface area (m 2 / g) versus DBP absorption (cm 3 / 100g) [DBP absorption (cm 3 / g) / Specific surface area (m 2 / g)] is 0.018 to 0.040 (cm 3 / m 2 ) carbon black, <1> ~ <3> The resin composition according to any one of claims 1 to 10. <5> The melt flow rate (measurement temperature 230°C, load 2.16 kg) is 3.0 to 5.0 g / 10 min. <1> ~ <4> The resin composition according to any one of claims 1 to 10. <6> the above <1> ~ <5> 13. An injection-molded article formed from the resin composition according to any one of claims 1 to 12.
[0008] In the present invention and this specification, when describing physical properties and the like by showing a numerical range, when the upper limit and lower limit of the numerical range are described separately, any of the upper limit and lower limit can be appropriately combined to form a specific numerical range. On the other hand, when describing multiple numerical ranges represented by "~", the upper limit and lower limit forming the numerical range are not limited to the specific combination described before and after "~" as a specific numerical range, and can be a numerical range obtained by appropriately combining the upper limit and lower limit of each numerical range. Note that in the present invention and this specification, a numerical range represented by "~" means a range including the numerical values described before and after "~" as the upper limit and lower limit. Effect of the Invention
[0009] The present invention can provide an injection molded article exhibiting excellent repeated bending durability and weather resistance, particularly an injection molded article having a thin-walled hinge portion, and a resin composition capable of forming an injection molded article exhibiting such excellent properties. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic exploded front view showing an example of a closure used for installing an optical or metallic communication cable, disassembled into a main body and an end plate. [Diagram 2] FIG. 2 is a schematic exploded cross-sectional view showing a cross section perpendicular to the axis of a semi-tubular body constituting an example of a closure used for installing an optical or metallic communication cable. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Resin composition] The resin composition of the present invention contains 6 to 10 parts by mass of ethylene-propylene rubber, 0.05 to 2.0 parts by mass of a hindered amine light stabilizer, and 1.5 to 3.0 parts by mass of carbon black, relative to 100 parts by mass of block polypropylene, and may contain other components. The resin composition of the present invention having the above composition has excellent repeated bending durability and weather resistance by itself, and can impart excellent repeated bending durability and weather resistance to its injection molded article.
[0012] In the present invention, unless otherwise specified, the term "resin" is used as a concept including elastomer and rubber. In the present invention, even when a resin composition contains an elastomer (including rubber), it is referred to as a resin composition, a resin molded body, etc. for convenience, but this does not exclude an elastomer composition and an elastomer molded body from the technical scope of the present invention. Each component that may be contained in the resin composition of the present invention and the content thereof will be described below. Each component may be used alone or in combination of two or more kinds.
[0013] <Block polypropylene> Known polypropylenes include propylene homopolymers (homopolypropylene: h-PP), random polypropylenes (also called ethylene-propylene random copolymers, r-PP), and block polypropylenes (also called ethylene-propylene block copolymers, b-PP). In the present invention, among the above, block polypropylene is used in combination with ethylene-propylene rubber, which will be described later, as the resin component (base resin). This allows for a synergistic effect with the hindered amine light stabilizer and carbon black, which will be described later, to achieve both excellent repeated bending durability and high weather resistance, and also improves brittleness. This excellent effect is unique to block polypropylene, which cannot be achieved with homopolypropylene or random polypropylene.
[0014] Block polypropylene is generally a composition (mixture) in which a rubber component is dispersed in polypropylene (homopolypropylene or random polypropylene), and has a sea-island structure in which the rubber component exists independently in the polypropylene. The rubber component is not particularly limited, but examples thereof include polymers of ethylene, octene, butene, hexene, and the like, and ethylene-propylene rubber (EPR). The rubber component is usually contained in the block polypropylene in an amount of 1 to 20% by mass, and preferably 5 to 20% by mass. The content of the rubber component in the block polypropylene can be measured by Fourier transform infrared spectroscopy (FT-IR) or the like.
[0015] The melt flow rate (MFR, measurement temperature 230°C, load 2.16 kg) of the block polypropylene is not particularly limited, and is appropriately determined in consideration of the MFR of the resin composition of the present invention, injection moldability, etc. The MFR of the block polypropylene is, for example, preferably 2.0 to 30 g / 10 min, more preferably 2.0 to 10 g / 10 min. The MFR of polypropylene refers to a value measured in accordance with JIS K 7210-1 (2014) under conditions of a measurement temperature of 230°C and a load of 2.16 kg.
[0016] <Ethylene-propylene rubber> The ethylene-propylene rubber (also called EP rubber) is not particularly limited as long as it is a rubber (including elastomer) made of a copolymer obtained by copolymerizing ethylene and propylene, and any known rubber can be used. Preferred examples of the ethylene-propylene rubber include a rubber made of a binary copolymer of ethylene and propylene, and a rubber made of a ternary copolymer of ethylene, propylene, and a diene. Terpolymers include terpolymers of ethylene, propylene, and conjugated diene, and terpolymers of ethylene, propylene, and non-conjugated diene. The diene compound constituting the terpolymer is not particularly limited, and examples thereof include conjugated diene compounds such as butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene, and non-conjugated diene compounds such as dicyclopentadiene (DCPD), ethylidene norbornene (ENB), and 1,4-hexadiene, and non-conjugated diene compounds are preferred. As the binary copolymer, ethylene-propylene rubber (EPM) is preferred, and as the ternary copolymer, ethylene-propylene-diene rubber (EPDM) is preferred.
[0017] The content of the ethylene constituent in the ethylene-propylene rubber (referred to as ethylene content) is not particularly limited, but is preferably 45 to 70 mass% in terms of improving weather resistance while maintaining excellent repeated bending durability, and more preferably 60 mass% or more in terms of achieving both repeated bending durability and weather resistance at a high level and further improving brittleness. The ethylene content is a value measured in accordance with the method described in ASTM D3900. The content of the diene constituent in the terpolymer rubber (referred to as the diene content) is not particularly limited, but is preferably 2.0 to 10 mass% in terms of improving weather resistance while maintaining excellent repeated bending durability, and more preferably 3.0 to 7.0 mass% in terms of achieving both repeated bending durability and weather resistance at a high level. The diene content can be measured by proton NMR ( 1 This is a value measured by H-NMR or other methods. The ethylene-propylene rubber contained in the resin composition of the present invention may be one type or two or more types, but it is preferable that the resin composition contains an ethylene-propylene rubber having an ethylene component content of 60% or more, and more preferably an ethylene-propylene rubber having an ethylene component content of 60% or more.
[0018] <Hindered amine light stabilizer> The resin composition of the present invention contains a hindered amine light stabilizer (HALS). As the hindered amine-based light stabilizer, any known hindered amine-based light stabilizer used in a resin composition can be used without any particular limitation, and may be a polymerizable compound, but is preferably a non-polymerizable compound.
[0019] Examples of the hindered amine-based light stabilizer, which is a non-polymerizable compound, include bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl-1-oxy) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, 1,2,2,6,6-pentamethyl-4-piperidyl methyl sebacate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate. Examples of such an acid include methyl-4-piperidyl, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, 2,2,6,6-tetramethyl-4-piperidyl stearate, 3-dodecyl-1-(2,2,6,6-tetramethyl-4-piperidyl)-pyrrolidine-2,5-dione, and those used in the examples described below.
[0020] Regarding the hindered amine-based light stabilizer, the contents described in Patent Documents 1 and 2 can be appropriately referred to, and the contents thereof are incorporated as a part of the description of this specification in their entirety. Examples of commercially available hindered amine light stabilizers include high molecular weight hindered amine light stabilizers (HALS), low molecular weight hindered amine light stabilizers (HALS), and hindered amine light stabilizers (HALS) blends (all manufactured by BASF).
[0021] As the hindered amine-based light stabilizer, those used in the examples described below, such as tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, are preferred, since they can achieve both high levels of repeated bending durability and weather resistance by combining them with carbon black, which will be described later, in the above resin component.
[0022] <Carbon black> The resin composition of the present invention contains carbon black. As the carbon black, any known carbon black used in a resin composition can be used without any particular limitation. In the resin composition of the present invention, the carbon black is considered to function as a colorant and an ultraviolet absorber, and by coexisting with the hindered amine-based light stabilizer in the above-mentioned resin component, it is possible to achieve both repeated bending durability and weather resistance. Examples of types of carbon black (types by manufacturing method) include furnace black, channel black, acetylene black, thermal black, etc. The carbon black contained in the resin composition of the present invention may be one type or two or more types, but it is preferable that the resin composition contains furnace black, and more preferably furnace black, in that repeated bending durability and weather resistance can be achieved at a high level by combining the resin composition with the hindered amine light stabilizer.
[0023] The properties of the carbon black are not particularly limited and can be set appropriately. For example, when the carbon black is in powder form, its average particle size can be 10 to 120 nm. Carbon black specific surface area (m 2 / g) is not particularly limited, and may be, for example, 20 to 140 m 2 / g. The specific surface area of carbon black is the "BET specific surface area" measured using nitrogen gas as an adsorbate in accordance with the "carrier gas method" of JIS Z 8830:2013. For example, it can be measured using a specific surface area / pore distribution measuring device "Flowsorb" (manufactured by Shimadzu Corporation). The specific surface area can be controlled by the manufacturing process and treatment conditions. It can be appropriately adjusted and set by known methods such as the use of activators, adjustment of heat treatment, acid washing or immersion, control of the gas phase method, and optimization of the manufacturing process. DBP absorption of carbon black (cm 3 / 100g) is not particularly limited, and may be, for example, 80 to 200 cm 3 The DBP absorption amount of carbon black (also called DBP oil absorption amount) is a value measured in accordance with JIS K 6217-4 (2008) and is the amount of dibutyl phthalate (DBP) absorbed per 100 g of carbon black (cm 3 The DBP absorption amount can be appropriately adjusted and set by known methods such as the use of a surface treatment agent, adjustment of heat treatment, classification treatment, surface oxidation treatment, and physical treatment.
[0024] In carbon black, the specific surface area (m 2 / g) versus DBP absorption (cm 3 / 100g) [DBP absorption (cm 3 / g) / Specific surface area (m 2 / g)] is not particularly limited, but is preferably 0.018 to 0.040 (cm 3 / m 2 ) range. This allows the resin component to have good dispersibility, and allows molding while suppressing the occurrence of strand defects. As a result, it is possible to achieve both high levels of durability against repeated bending and weather resistance. 3 / g) / Specific surface area (m 2 / g)] is 0.015 to 0.037 (cm / g) in that weather resistance can be further improved to achieve a good balance between repeated bending durability and weather resistance at a higher level, and brittleness can also be improved. 3 / m 2), and more preferably in the range of 0.020 to 0.032 (cm 3 / m 2 It is more preferable that the ratio [DBP absorption amount (cm 3 / g) / Specific surface area (m 2 / g)] is the "DBP absorption (cm 3 / 100g)” was converted to the DBP absorption amount per 1g of carbon black. 3 / g)" to the specific surface area (m 2 / g) to obtain the value. In the present invention, the carbon black has the above ratio [DBP absorption amount (cm 3 / g) / Specific surface area (m 2 / g)] in the above range, or adjust the specific surface area and / or DBP absorption amount as described above to obtain the above ratio [DBP absorption amount (cm 3 / g) / Specific surface area (m 2 It is preferable to use a material in which the ratio [DBP absorption amount (cm / g)] is adjusted to fall within the above range. 3 / g) / Specific surface area (m 2 / g)] can be appropriately adjusted and set by known methods such as use of an activator, adjustment of heat treatment, acid washing or immersion, control of a gas phase method, optimization of the manufacturing process, use of a surface treatment agent, adjustment of heat treatment, classification treatment, surface oxidation treatment, and physical treatment methods.
[0025] <Other resins> The resin composition of the present invention may contain a resin other than block polypropylene and ethylene-propylene rubber (referred to as other resin) as a resin component. Examples of other resins include polyolefins (excluding block polypropylene), styrene-based elastomers, acrylic rubbers, silicone rubbers, fluororubbers, etc. The polyolefin resin is not particularly limited as long as it is a resin made of a polymer obtained by polymerizing or copolymerizing a compound having an ethylenically unsaturated bond (olefin compound), and known resins used in various resin compositions can be used. For example, polyethylene, polypropylene (excluding block polypropylene), ethylene-α-olefin copolymer (excluding ethylene-propylene rubber), polyolefin copolymer having an acid copolymer component or an acid ester copolymer component (for example, EVA, EEA), and acid-modified polyolefin resin can be mentioned. In addition, rubber or elastomer of these copolymers (excluding ethylene rubber) can also be mentioned. Furthermore, other resins include styrene-based elastomer, acrylic rubber, silicone rubber, fluororubber, etc. In addition, a mixture of the resin with a plasticizer can also be used. As the plasticizer, for example, organic oil or mineral oil can be mentioned.
[0026] <Other ingredients> In addition to the block polypropylene, ethylene-propylene rubber, hindered amine light stabilizer, and carbon black, the resin composition of the present invention may contain various other components, such as additives generally used in resin compositions, as other components within the scope of the present invention. Examples of other components include antioxidants (antioxidants), lubricants, processing heat stabilizers, flame retardants, fillers (inorganic fillers), crosslinking agents, crosslinking assistants, crosslinking catalysts, crosslinking-promoting metals, and inert agents (e.g., copper inhibitors). The antiaging agent is not particularly limited, and may be any of various known antiaging agents used in resin compositions. Examples of the antiaging agent include (hindered) phenol-based antiaging agents, benzimidazole-based antiaging agents, amine-based antiaging agents, and sulfur-based antiaging agents (excluding benzimidazole-based antiaging agents), and the like, with phenol-based antiaging agents and sulfur-based antiaging agents being preferred. The lubricant is not particularly limited, and may be any of various known anti-aging agents used in resin compositions. Examples of the lubricant include silicone compounds, fatty acids, fatty acid metal salts, and fatty acid amides, with fatty acids and fatty acid metal salts being preferred. The processing heat stabilizer is not particularly limited, and includes various known antiaging agents used in resin compositions. Examples of the processing heat stabilizer include phosphorus-based processing heat stabilizers such as tris(2,4-di-tert-butylphenyl) phosphite, and sulfur-based processing heat stabilizers such as thioester. Examples of the filler (inorganic filler) include various known fillers used in resin compositions, and can be appropriately contained in the resin composition. In the present invention, one of the preferred embodiments is not to contain talc. Not containing talc includes an embodiment in which talc is inevitably present in the resin composition, and includes, for example, an embodiment in which talc is contained in an amount of 5.0 parts by mass or less relative to 100 parts by mass of block polypropylene.
[0027] <Composition of Resin Composition> The resin composition of the present invention contains block polypropylene, ethylene-propylene rubber, hindered amine light stabilizer, and carbon black in the specific amounts described below, and thus can achieve both repeated bending durability and weather resistance. That is, the content of the ethylene-propylene rubber in the resin composition of the present invention is 6 to 10 parts by mass relative to 100 parts by mass of the block polypropylene. When the content of the ethylene-propylene rubber is within the range of 6 to 10 parts by mass, it is possible to achieve both repeated bending durability and weather resistance, and further, it is possible to suppress a decrease in brittleness (particularly low-temperature brittleness) in a molded product of the resin composition of the present invention. In the present invention, the content of the ethylene-propylene rubber is preferably 7.0 to 9.5 parts by mass, more preferably 7.5 to 9.0 parts by mass, relative to 100 parts by mass of the block polypropylene, in terms of being able to achieve both repeated bending durability and weather resistance at a high level and further being able to maintain excellent brittleness.
[0028] The content of the hindered amine light stabilizer in the resin composition of the present invention is 0.05 to 2.0 parts by mass relative to 100 parts by mass of the block polypropylene. When the content of the hindered amine light stabilizer is within the range of 0.05 to 2.0 parts by mass, both repeated bending durability and weather resistance can be achieved. In the present invention, the content of the hindered amine light stabilizer is preferably 0.06 to 1.80 parts by mass, more preferably 0.08 to 0.15 parts by mass relative to 100 parts by mass of the block polypropylene, in order to further improve the weather resistance and achieve both repeated bending durability and weather resistance at a high level. The carbon black content in the resin composition of the present invention is 1.5 to 3.0 parts by mass relative to 100 parts by mass of the block polypropylene. When the carbon black content is within the range of 1.5 to 3.0 parts by mass, both repeated bending durability and weather resistance can be achieved. In the present invention, the carbon black content is preferably 1.8 to 3.0 parts by mass relative to 100 parts by mass of the block polypropylene, in that both repeated bending durability and weather resistance can be achieved at a high level. In the resin composition of the present invention, the mass ratio of the carbon black content to the hindered amine light stabilizer content [carbon black content / hindered amine light stabilizer content] can be appropriately set in consideration of the above-mentioned respective contents. From the viewpoints of repeated bending durability and weather resistance, it is preferably 1 to 50, more preferably 10 to 40, and even more preferably 15 to 35.
[0029] The total content of the other resins in the resin composition of the present invention is set within a range that does not impair the effects of the present invention, and can be, for example, 0 to 15 parts by mass per 100 parts by mass of the block polypropylene. The total content of other components in the resin composition of the present invention is set within a range that does not impair the effects of the present invention, and can be, for example, 0 to 15 parts by mass relative to 100 parts by mass of the block polypropylene. Here, the content of the antioxidant can be appropriately set in consideration of the total content of the other components, and can be, for example, 0 to 2 parts by mass relative to 100 parts by mass of the block polypropylene. The content of the lubricant can be appropriately set in consideration of the total content of the other components, and can be, for example, 0 to 2 parts by mass relative to 100 parts by mass of the block polypropylene. The content of the processing heat stabilizer can be appropriately set in consideration of the total content of the other components, and can be, for example, 0 to 2 parts by mass relative to 100 parts by mass of the block polypropylene.
[0030] <Preparation of Resin Composition of the Present Invention> The resin composition of the present invention can be prepared by melt mixing (kneading) block polypropylene, ethylene-propylene rubber, hindered amine light stabilizer, carbon black, and optionally other resins and other components. The melt mixing method is not particularly limited as long as it is a method that is usually adopted for preparing a resin or rubber composition. For example, various mixing devices such as a single screw extruder, a twin screw extruder, a roll, a Banbury mixer, and various kneaders can be used for mixing. The melt mixing conditions such as the melt mixing temperature and the melt mixing time are not particularly limited, and can be appropriately set within a temperature range equal to or higher than the melting temperature of the resin component, usually block polypropylene. The melt mixing temperature is usually set to a temperature equal to or higher than the melting temperature of the resin component, and cannot be uniquely determined depending on the type and composition of the resin component, but, for example, 120 to 240 ° C. is preferable, and 140 to 220 ° C. is more preferable. The mixing order of each component is not particularly limited, and the above-mentioned components can be mixed (melted) at once, or each component can be mixed sequentially in an appropriate order. In this way, the resin composition of the present invention in which each component is dispersed (mixed) can be prepared.
[0031] <Characteristics of the Resin Composition of the Present Invention> The resin composition of the present invention has properties exhibited by the above-mentioned composition. For example, it has repeated bending durability and weather resistance that pass the tests in the examples described below, and desirably has brittleness that passes the tests in the examples. The melt flow rate (MFR, measurement temperature 230°C, load 2.16 kg) of the resin composition of the present invention is not particularly limited and can be appropriately determined, for example, in the range of 1.0 to 12 g / 10 min. From the viewpoint of moldability, the melt flow rate of the resin composition of the present invention is preferably in the range of 3.0 to 5.0 g / 10 min, more preferably in the range of 3.0 to 4.0 g / 10 min. The MFR of the resin composition of the present invention refers to a value measured in accordance with JIS K 7210-1 (2014) under conditions of a measurement temperature of 230°C and a load of 2.16 kg.
[0032] The resin composition of the present invention is generally made into a bulk, strand, pellet or other form as a molding material. The resin composition of the present invention may be a crosslinked resin composition (crosslinked body) having a crosslinked structure (including a dynamic crosslinked structure), but is usually preferably a non-crosslinked composition (non-crosslinked body). In the present invention, the non-crosslinked resin composition refers to a resin composition that is not actively crosslinked (including dynamic crosslinking) by electron beam irradiation, a crosslinking agent, or the like during its preparation and during molding of an injection-molded body. Thus, the non-crosslinked resin composition includes a resin composition in which crosslinking has unavoidably progressed partially after the injection-molded body is placed, for example, outdoors.
[0033] As described above, the resin composition of the present invention can realize excellent repeated bending durability and weather resistance, and furthermore, depending on the composition, it is excellent in brittleness (particularly low-temperature brittleness). The resin composition of the present invention exhibiting such excellent properties is suitable as a molding material for various resin molded bodies, and is particularly suitable as a molding material for integrally molded bodies in which a main body and a lid are integrated, particularly an integrally molded body having a thin-walled hinge portion. As a molding method, extrusion molding, injection molding, and other various molding methods can be applied, but it is preferable to apply injection molding by utilizing the above-mentioned property (MFR) of the resin composition of the present invention.
[0034] [Injection molded body] An injection molded article using the resin composition of the present invention (hereinafter referred to as the injection molded article of the present invention) will be described below. The injection molded article of the present invention is a molded article that is injection molded into a shape and size according to the application, etc., using the resin composition of the present invention as a molding material, and is preferably an injection molded article having a hinge portion (thin hinge portion) formed in a thin wall shape. This thin hinge portion is formed thinner than the thickness of the parts that are connected (integrally molded) to sandwich the thin hinge portion, and functions as a hinge by bending and stretching the thin hinge portion as a fulcrum (operation point), and is a part that rotates at least one of the connected parts. Such a thin hinge portion may be one in which a plurality of grooves (long, thin, bottomed recesses) are arranged in a straight line with a gap between the connected parts, but from the viewpoint of moldability, it is preferable that the thin hinge portion is formed as a single groove between the connected parts.
[0035] The dimensions of the thin-walled hinge portion are not particularly limited as long as it is formed thinner than the parts connected to each other by sandwiching the thin-walled hinge portion. The thickness of the thin-walled hinge portion may be set to a thickness that is thinner than the parts connected to each other by sandwiching the thin-walled hinge portion and that allows bending as a hinge. Since the resin composition of the present invention exhibits excellent repeated bending durability and weather resistance as described above, the thin-walled hinge portion can be made thinner than conventionally, but it cannot be determined univocally by the dimensions of the molded body and the connected parts. The thickness of the thin-walled hinge portion can be, for example, 50% or less of the thickness of the connected parts, and is preferably 5 to 35%, and more preferably 10 to 25%, in terms of ease of bending, repeated bending durability, and the like. An example of the thickness of the thin-walled hinge portion can be, for example, 0.4 to 0.8 mm. Here, the "connected portion" used as the basis for the thickness of the thin-walled hinge portion is the connected portion having the thinner thickness when the connected portions sandwiching the thin-walled hinge portion have different thicknesses. The width of the thin hinge portion may be any width that allows bending as a hinge, and cannot be uniquely determined by the dimensions of the molded body or the connected portion, etc. An example of the width of the thin hinge portion is, for example, 1 to 5 mm, preferably 1.5 to 3.5 mm.
[0036] The molding method and molding conditions of the resin composition of the present invention are appropriately selected according to the shape and form after molding. For example, the molding method includes extrusion molding using an extrusion molding machine, extrusion molding using an injection molding machine, and molding using other molding machines. In the present invention, injection molding is preferred. The molding temperature is not particularly limited and can be the same temperature as the melt mixing temperature when preparing the resin composition of the present invention. In the resin composition of the present invention, mixing of the components and molding can be carried out simultaneously or successively.
[0037] The injection molded body of the present invention can be used for various applications and products (including semi-finished products). It is preferably suitable as a box-shaped molded body having an openable / closable cover member or flap member, or a cover-shaped molded body having an openable / closable cover member or flap member, or further as a resin molded body having a cover-shaped molded body, and is particularly suitable as a box-shaped molded body or a cover-shaped molded body, and specific examples thereof include a wiring box, a closure, and the like.
[0038] Hereinafter, the injection molded article of the present invention will be described with reference to a semi-tubular body (a cover-shaped molded article) used in a closure for connecting and branching optical or metallic communication cables. A closure having a semi-tubular body, which is an example of the injection molded body of the present invention (hereinafter, for convenience, may be referred to as "the closure of the present invention") is the same as a known closure, except that it has a semi-tubular body of the present invention described below. The closure of the present invention is preferably a closure for outdoor aerial installation, and is composed of a tubular main body and end plates that close both axial ends of the main body, as shown in Fig. 1 for example, and is provided with fixing means for holding or fixing cables, etc., in the internal space of the main body. Cables, etc. to be connected, branched, etc. are introduced into the internal space of the main body through each end plate, and are connected, branched, etc. in the internal space of the main body.
[0039] The semi-tubular body provided in the closure of the present invention is an example of the injection molded body of the present invention, and is integrally formed by injection molding using the resin composition of the present invention. An example of the semi-tubular body provided in the closure of the present invention (hereinafter, sometimes referred to as the "semi-tubular body of the present invention") will be described with reference to the drawings. Fig. 1 is a schematic exploded front view showing the state in which the closure is disassembled into a main body and an end plate, and Fig. 2 is a schematic exploded cross-sectional view showing a cross section perpendicular to the axis of a semi-tubular body constituting the closure. In Fig. 1 and Fig. 2, the axial direction of the semi-tubular body is the left-right direction, the direction perpendicular to the axis and penetrating the side plate and the cover part described later is the front-rear direction, and the direction perpendicular to the axis and the front-rear direction (the direction penetrating the top plate and the bottom plate) is the up-down direction. In the front-rear direction, the direction from the side plate toward the cover part is called the front, and the direction from the cover part toward the side plate is called the rear. In the up-down direction, the direction from the bottom plate 7 toward the top part 13c is called the up, and the direction from the top part 13c toward the bottom plate 7 is called the down.
[0040] As shown in Fig. 2, the semi-tubular body of the present invention has a semi-tubular shape with a cross section perpendicular to the axis that is an inverted U-shape, and this cross-sectional shape is also called a gutter shape or a half-split pipe shape. In the present invention, the semi-tubular body does not have to be an exact half-split shape (a shape divided in half) of a tubular body, and includes a tubular body in which a part of the tube wall is missing and opened. This semi-tubular body 6 has a side plate 11 and a cover plate 12 that face each other, and a connecting part 13 that connects or joins the side plate 11 and the cover plate 12. This connecting part 13 is composed of shoulder parts 13a, 13b and an upper surface part 13c, and the shoulder part 13a connects the side plate 11 and the upper surface part 13c, and the shoulder part 13b connects the cover plate 12 and the upper surface part 13c. A groove is formed in the axial direction of the body at the joint (outer surface) between the top surface 13c and the shoulder 13a and at the joint (outer surface) between the top surface 13c and the shoulder 13b, forming a thin-walled hinge portion 14. The shape and size of the groove forming the thin-walled hinge portion 14 are not particularly limited as described above, but a groove having a rectangular cross section is formed in the semi-tubular body 6. This thin-walled hinge portion 14 has a thickness thinner than the thickness of the top surface 13c and the thickness of the shoulder 13a and the shoulder 13b, for example, a thickness thinner than the thickness of the top surface 13c, the shoulder 13a and the shoulder 13b by about 1 to 3 mm. The semi-tubular body 6 of the present invention is open at the bottom, and as shown in FIG. 2, a bottom plate 7 is incorporated here to form a tubular body having a hexagonal cross section. In the main body thus formed, the cover plate 12 and shoulder portion 13b are rotatable (openable and closable) around the thin-walled hinge portion 14, and the side plate 11 and shoulder portion 13a are rotatable (openable and closable) around the thin-walled hinge portion 14. The end plates 3 are plate-like members provided at both openings in the axial direction of the main body (semi-tubular body 6) and close both openings.
[0041] The closure 1, which is composed of the main body and the end plates 3, is formed by fitting the bottom plate 7 to the opening of the semi-tubular body 6 and providing the end plates 3 to both openings of the semi-tubular body 6. When a cable is arranged in this closure 1, the cover plate 12 and the shoulder 13b and / or the side plate 11 and the shoulder 13a are rotated (flipped up) from the front upwards with the thin-walled hinge portion 14 as a fulcrum, thereby exposing the internal space 15, and connection and branching of the cable or the like can be performed in this internal space 15. After the connection and branching work is completed, the flipped-up cover plate 12 and the shoulder 13b and / or the side plate 11 and the shoulder 13a are rotated downwards with the thin-walled hinge portion 14 as a fulcrum to close the internal space 15 (closure). In this closure 1, the internal space 15 (closure) can be opened and closed by the simple operation of rotating the cover plate 12 and shoulder portion 13b and / or the side plate 11 and shoulder portion 13a around the thin-walled hinge portion 14. Moreover, since the semi-tubular body 6 is made of the resin composition of the present invention, the thin-walled hinge portion 14 shows excellent characteristics without any damage such as cracks or fissures even if the above-mentioned opening and closing operations of the thin-walled hinge portion 14 are repeated or even if the above-mentioned opening and closing operations are performed after being placed outdoors and exposed to ultraviolet rays.
[0042] The dimensions of the closure of the present invention are not particularly limited and are appropriately determined depending on the application, for example, the size and number of optical or metal communication cables to be connected or branched, etc. For example, the length in the axial direction of the semi-tubular body 6 can be 455 to 620 mm.
[0043] In the semi-tubular body 6 shown in Figures 1 and 2, a groove is provided on the outer surface of the junction between the top surface portion 13c and the shoulder portion 13b to form the thin-walled hinge portion 14. However, in the present invention, a groove can also be provided on the inner surface of the junction between the top surface portion and the shoulder portion to form the thin-walled hinge portion. In addition, in the semi-tubular body 6, a thin-walled hinge portion 14 is also provided at the connection between the upper surface portion 13c and the shoulder portion 13a, so that the side panel 11 and the shoulder portion 13a can rotate around the thin-walled hinge portion 14 as a fulcrum. However, in the present invention, it is sufficient that the thin-walled hinge portion is provided at either the connection between the upper surface portion 13c and the shoulder portion 13a or the connection between the upper surface portion 13c and the shoulder portion 13b. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In the following Tables 1-1 and 1-2 (collectively referred to as Table 1), the numerical values relating to the blending amounts of each example are based on mass unless otherwise specified. Note that when the content column of each component is left blank, it indicates that the content of the component is 0 parts by mass.
[0045] Working Example , reference example Details of each compound used in the comparative examples are shown below. <Polypropylene> BC4BSW: Product name, block polypropylene, MFR (230℃, 2.16kg) 5.0g / 10min, manufactured by Japan Polypropylene Corporation PM761A: Product name, block polypropylene, MFR (230°C, 2.16 kg) 9.5 g / 10 min, manufactured by SunAllomer Co., Ltd. PM472W: Product name, block polypropylene, MFR (230°C, 2.16 kg) 2.7 g / 10 min, manufactured by SunAllomer Co., Ltd. J466: Product name, block polypropylene, MFR (230℃, 2.16kg) 3.1g / 10min, manufactured by Prime Polymer Co., Ltd. J707G: Product name, block polypropylene, MFR (230°C, 2.16 kg) 30 g / 10 min, manufactured by Prime Polymer Co., Ltd. PM600A: Product name, homopolypropylene, MFR (230°C, 2.16 kg) 7.5 g / 10 min, manufactured by SunAllomer Co., Ltd. PF621S: Product name, random polypropylene, MFR (230°C, 2.16 kg) 6.5 g / 10 min, manufactured by SunAllomer Co., Ltd. <Ethylene-propylene rubber> EPT3092: Product name, ethylene-propylene-ethylidene norbornene rubber, ethylene content 65% by mass, diene content 4.6% by mass, manufactured by Mitsui Chemicals, Inc. EPT4045M: Product name, ethylene-propylene-ethylidene norbornene rubber, ethylene content 45% by mass, diene content 7.6% by mass, manufactured by Mitsui Chemicals, Inc.
[0046] <Hindered amine light stabilizer> ADK STAB LA52: Trade name, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)butane-1,2,3,4-tetracarboxylate, manufactured by ADEKA Corporation Tinuvin 144: Trade name, Bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate, manufactured by BASF Japan Ltd. Tinuvin 770DF: Trade name, Bis(2,2,6,6-tetramethyl-4-piperidyl)Sebacate, manufactured by BASF Japan Ltd. Tinuvin 123: Trade name, Decanediol, bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl)ester, reaction products with 1,1-dimethylethylhydroperoxide and octane, manufactured by BASF Japan Ltd. <Carbon black> As carbon black, commercially available Furne Black (PK-1 to PK-7) was used. For each Furne Black, the DBP absorption (cm 3 / 100g) and specific surface area (m 2 / g) and the specific surface area (m 2 / g) versus DBP absorption (cm 3 / g) [DBP absorption (cm 3 / g) / Specific surface area (m 2 The DBP absorption (cm3 / g) of each furnace black was calculated. The results are shown in Table 1. 3 / 100g) and specific surface area (m 2 / g) were confirmed to be within the above-mentioned range.
[0047] <Other ingredients> Sumilizer TPM: Trade name, sulfur-based antioxidant, 3,3'-thiobis(tetradecyl propionate), manufactured by Sumitomo Chemical Co., Ltd. Irgafos 168: Trade name, phosphorus-based heat stabilizer, tris(2,4-di-tert-butylphenyl) phosphite, manufactured by BASF Zinc stearate: ZN-ST (product name), lubricant, manufactured by Nitto Kasei Co., Ltd. Irganox1010: Trade name, phenolic antioxidant, Pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), manufactured by BASF
[0048] [Examples 1 to 25 , Reference examples 1-3 and Comparative Examples 1 to 8] The components shown in Table 1 were fed into a co-rotating twin-screw extruder in the amounts shown in Table 1, melt-mixed at 200°C for 3 minutes, and then discharged at a material discharge temperature of 220°C and passed through a feeder rudder to obtain pellets of the resin composition.
[0049] Using each of the prepared pellets, injection molded bodies or test pieces were produced and the following tests were carried out. The results are shown in Table 1.
[0050] <Test 1: Hinge bending test (repeated bending durability test)> Each of the produced pellets was used to injection mold a semi-tubular closure body having the following dimensions. (Injection molding conditions) Melting temperature: 240℃ Mold temperature: Fixed side 60℃ Mold temperature: moving side 35℃ (Dimensions of semi-tubular body) Axial length of semi-tubular body: 620mm Parallel length (width) of thin hinge section (rectangular cross section): 2.4mm±0.5mm Thin hinge part thickness: 0.45mm±0.5mm Length of thin hinge part: 620mm Thickness of the parts (top and shoulder parts) (connected across the thin hinge part): 3.0mm ± 0.2mm
[0051] The manufactured semi-tubular body 6 was arranged with the thin-walled hinge portion 14 so that the axis was parallel to the hinge bending test movable portion of the bending test machine, and the cover plate 12 and the shoulder portion 13b were rotated 105° (from the original position) in the direction away from the side plate 11 to bend the thin-walled hinge portion 14 (cover plate 12 and shoulder portion 13b were opened), and the semi-tubular body 6 was fixed to the bending test machine. Note that the groove forming the thin-walled hinge portion 14 was fixed in a state facing the outside of the bending test machine (the bending side of the cover plate 12). Next, in a room temperature (25±3°C) environment, the cover plate 12 and the shoulder portion 13b were rotated 105° in one second in a direction approaching the side plate 11 (cover plate 12 and shoulder portion 13b were closed), and the semi-tubular body 6 was returned to its original state (the state shown in FIG. 2). Thereafter, it was rotated 105° in one second in a direction away from the side plate 11 (returning the cover plate 12 and shoulder portion 13b to their initial open state). The rotational movement (opening and closing movement) to rotate the cover plate 12 and the shoulder portion 13b to the closed state and the open state in this way was considered as one cycle, and the presence or absence of cracks in the thin-walled hinge portion 14 was confirmed by rotating the cover plate 12 and the shoulder portion 13b multiple times. This test was conducted to evaluate the repeated bending durability of the semi-tubular body 6, which was an injection molded product of the resin composition of the present invention, and Table 1 shows the number of cycles of rotation at which cracks or breaks occurred in the thin-walled hinge portion 14. Note that the test involved 30,000 cycles of rotation, and if no cracks or breaks occurred in the thin-walled hinge portion 14 after 30,000 cycles, this was indicated as "30,000>". In the present invention, if the number of rotational cycles at which cracks or fissures occur in the thin-walled hinge portion 14 is 25,000 or more, it is considered to be "pass", and if it is less than 25,000, it is considered to be "fail".
[0052] <Test 2: Weather resistance test> Using each of the produced pellets, dumbbell-shaped test pieces of the following dimensions were prepared, with one groove (corresponding to a thin-walled hinge portion) parallel to the width direction at the center of the length of the parallel part, in accordance with JIS K7113. (Production conditions) Melting temperature: 240℃ Mold temperature: Fixed side 60℃ Mold temperature: moving side 35℃ (Dumbbell specimen dimensions) Total length A: 70mm Width B at both ends: 12.5mm Length of parallel part C: 12.5 mm Parallel part width D: 3mm Groove length: 3mm Groove width: 2.4mm±0.5mm Thickness I: 3.0mm±0.2mm Thin hinge part thickness: 0.45mm±0.5mm
[0053] Weather resistance was evaluated using a sunshine carbon arc lamp weather resistance tester (filter A type) (model number: Sunshine Weather Meter S80, manufactured by Suga Test Instruments Co., Ltd.) and the prepared dumbbell-shaped test pieces. Specifically, each dumbbell test piece was irradiated in accordance with JIS B 7753. However, the black panel temperature in the chamber was set to 63±3°C, and the cycle was 120 minutes (102 minutes of irradiation followed by 18 minutes of irradiation and spraying). When the irradiation time from the start of irradiation reached 2000 hours, 4000 hours, and 6000 hours, the dumbbell test piece was removed from the weather resistance tester and subjected to 100 cycles of hinge bending test. After 100 cycles of the hinge bending test, the appearance of the thin-walled hinge portion 14 (inner surface and back surface) of the dumbbell test piece was visually confirmed. The hinge bending test was performed in the same manner as in <Test 1: Hinge bending test (repeated bending durability test)> above, except that a dumbbell test piece was used. This test is a test to evaluate the weather resistance of a dumbbell test piece which is an injection mold of the resin composition of the present invention, and the case where cracks or fissures were confirmed in the thin-walled hinge part 14 at each irradiation time was marked as "X", and the case where cracks or fissures were not confirmed was marked as "◯". In this test, the case where cracks or fissures were confirmed in the thin-walled hinge part 14 after 4000 hours of irradiation was marked as "fail", the case where cracks or fissures were not confirmed in the thin-walled hinge part 14 after 4000 hours of irradiation was marked as "pass", and the case where cracks or fissures were not confirmed in the thin-walled hinge part 14 after 6000 hours of irradiation was marked as excellent (pass).
[0054] <Test 3: Measurement of MFR> Using each of the prepared pellets, the MFR (230° C., 2.16 kg) of each resin composition was measured by the method described above. This test is a reference test, and the MFR (230° C., 2.16 kg) is preferably within the range of 3.0 to 5.0 g / 10 min.
[0055] <Test 4: Embrittlement test> Embrittlement tests were conducted on five A-type test pieces made from each of the prepared pellets in accordance with JIS K 7216. A-type test piece grips and striking hammers were used, and the minimum temperatures at which the number of breakages for all five test pieces was zero are shown in Table 1. Breakage was determined according to the breakage criteria, with the occurrence of cracks being considered as breakage. This test is a reference test, and it is preferable that the above minimum temperature be -25°C or lower.
[0056] [Table 1-1]
[0057] [Table 1-2]
[0058] In Table 1, "b-pp" stands for block polypropylene, "h-pp" for homopolypropylene, and "r-pp" for random polypropylene. The conditions and units for the MFR of the polypropylene and resin composition are as described above, but are omitted here. The "absorption amount / specific surface area" in the carbon black column is the ratio [DBP absorption amount (cm 3 / g) / Specific surface area (m 2 / g), and "mass ratio of content" represents the mass ratio of the carbon black content to the hindered amine light stabilizer content [carbon black content / hindered amine light stabilizer content].
[0059] As is clear from the results shown in Table 1, the comparative resin compositions that do not satisfy the components and their contents specified in the present invention exhibited poor results in at least one of the hinge bending test and the weather resistance test, and the injection molded articles were unable to achieve both repeated bending durability and weather resistance. In contrast, the resin compositions of Examples 1 to 25, which contain specific amounts of block polypropylene, ethylene-propylene rubber, hindered amine-based light stabilizer, and carbon black, all showed excellent results in the hinge bending test and weather resistance test, and were capable of producing injection-molded articles that exhibited excellent repeated bending durability and weather resistance. [Explanation of symbols]
[0060] 1. Closures 3 End plate 6 semi-tubular body 7 Bottom plate 11 Side plate 12 Cover plate 13 Connection part 13a, 13b Shoulder 13c Top part 14 Thin hinge part 15. Interior Space
Claims
1. The composition contains 6 to 10 parts by mass of ethylene-propylene rubber, 0.05 to 2.0 parts by mass of a hindered amine-based light stabilizer, and 1.5 to 3.0 parts by mass of carbon black, relative to 100 parts by mass of block polypropylene; The resin composition comprises carbon black having a ratio of DBP absorption (cm 3 / g), calculated by converting the DBP absorption (cm 3 / 100 g) to the specific surface area (m 2 / g) and converting it into DBP absorption per 1 g of carbon black [DBP absorption (cm 3 / g) / specific surface area (m 2 / g)] of 0.018 to 0.040 (cm 3 / m 2 ).
2. The resin composition according to claim 1, wherein the ethylene-propylene rubber contains an ethylene-propylene rubber having an ethylene component content of 60% or more.
3. The resin composition of claim 1 , wherein the carbon black comprises furnace black.
4. A resin composition as described in claim 1, wherein the mass ratio of the carbon black content to the hindered amine light stabilizer content [carbon black content / hindered amine light stabilizer content] is 25 to 50.
5. The resin composition according to claim 1, having a melt flow rate (measurement temperature: 230° C., load: 2.16 kg) of 3.0 to 5.0 g / 10 min.
6. An injection molded article formed from the resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Dynamically vulcanized alloy having improved rigidity / impact balance
JP1991054237A
Polypropylene-based resin composition having improved coating ability
JP1991252444A
Reinforced polypropylene molding composition
JP1993194804A
Polypropylene resin composition for coated
JP1994107897A
Polyolefin resin composition
JP1996041251A